Catalyst for carbon dioxide hydrogenation to methanol and method of preparation thereof

The catalyst composition optimized by DFT simulations addresses the challenge of high CO2 conversion to methanol, achieving efficient hydrogenation with enhanced conversion and selectivity through a co-precipitation and calcination process.

JP2024144143APending Publication Date: 2024-10-11HINDUSTAN PETROLEUM CORP LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
JP2024021339
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing catalysts for the hydrogenation of carbon dioxide to methanol face challenges in achieving high conversions and methanol yields due to the thermodynamic stability of CO2, necessitating improved catalyst design and reaction conditions.

Method used

A catalyst composition comprising 80-95% w/w of catalyst metals and oxides, 5-20% w/w structural promoters, and 5-10% w/w binder is prepared through co-precipitation and calcination processes, utilizing density functional theory (DFT) simulations to optimize adsorption energies.

Benefits of technology

The method enhances catalyst activity, resulting in efficient hydrogenation of CO2 to methanol with improved conversion rates and selectivity, as demonstrated by optimal catalyst formulations like 55%Cu+5%Ti+20%Zn+5%Zr+5%Al+10%Ce achieving 19% CO2 conversion and 69% methanol selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144143000001_ABST
    Figure 2024144143000001_ABST
Patent Text Reader

Abstract

To provide a catalyst for carbon dioxide hydrogenation to methanol, which yields higher methanol with higher selectivity, and to provide a method of preparation thereof.SOLUTION: There is provided a catalyst for carbon dioxide hydrogenation to methanol having 80 to 95% w / w of a metal and their oxides; 5 to 20% w / w of a structural promoter; and 5 to 10% w / w of a binder of the total weight of the catalyst. There is also provided a method for preparation of a catalyst for carbon dioxide hydrogenation to methanol, comprising: a) co-precipitating of 80 to 95% w / w of a metal precursors of the total weight of the catalyst under with a 1.0 to 1.8 M precipitating agent followed by adding 5 to 20% w / w of a structural promoter of the total weight of the catalyst to obtain an active metal precipitate, b) washing and drying the active metal precipitate under conditions to obtain a dried active metal precipitate followed by calcination under conditions to form a mixed metal oxide, c) adding 5 to 10% w / w of a binder of the total weight of the catalyst to the 90 to 95% w / w mixed metal oxides along with 0.5 to 1.5 M peptizing agent, followed by drying and calcination under conditions to obtain a catalyst for carbon dioxide hydrogenation to methanol.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for the hydrogenation of carbon dioxide to methanol. The present invention also relates to a method for the preparation of a catalyst for the hydrogenation of carbon dioxide to methanol. [Background technology]

[0002] The Background Discussion contains information useful for understanding the present invention. No admission is made that any of the information provided herein is prior art or relevant to the presently claimed invention, or that any publication specifically or implicitly referenced is prior art.

[0003] Catalytic hydrogenation of CO2 has the potential to convert industrial emissions into value-added chemicals like methanol, a key intermediate in several industrially important chemical processes in the production of dimethyl ether (DME), gasoline, biodiesel, formaldehyde, acetic acid etc. This is essential to mitigate these CO2 emissions, which are a major contributor to global warming. In India, domestic methanol production declined by 57% from 2010-2011 to 2015-2016, while consumption of the chemical increased by 61% during the same period. The CO2 emission target will not only work towards net-zero emissions but will also help improve domestic production.

[0004] CO2 is a thermodynamically stable molecule, and achieving high conversion and methanol yield purely depends on proper catalyst design and finding the optimal reaction process conditions.

[0005] There have been continuous efforts in designing catalysts for hydrogenating CO2 to methanol. CN103263926A discloses a catalyst for synthesizing methanol by hydrogenating carbon dioxide, which is composed of a combination of ions of monovalent (Ma) or divalent metal (Ma) and trivalent (Mb) or tetravalent (Mb) ions. The molar ratio of each metal is [n(Cu)+n(Zn)+n(Ma)]:[n(Al)+n(Mb)]=2-15, n(Cu):n(Zn)=0.5-4, n(Ma):n(Zn)=0-1, n(Mb):n(Al) is equal to 0-9. CN110252308B discloses that active metals dispersed at the atomic level in a support metal oxide are suitable for hydrogenating CO2 to methanol. The active metal comprises one or more of Cr, Mn, Fe, Co, Ni, Cu, Zn, Mo, Ru, Rh, Pd, Ag, W, Ir, Pt, and Au, and the support metal comprises one or more of Ti, Zr, Nb, Ce, Al, Ga, In, Si, Ge, and Sn.

[0006] Although many prior arts have reported improvements in catalyst formulations, there remains a need in the art for a better understanding of catalytic activity and, in turn, its design.Density Functional Theory (DFT) calculations and related computational methods have evolved into predictive tools for materials design due to advances in mathematical algorithms and computational hardware. One approach according to the claimed invention is the use of DFT modeling to design catalyst compositions by understanding the optimal CO2 adsorption energy required for efficient hydrogenation of CO2 to methanol. Summary of the Invention [Problem to be solved by the invention]

[0007] It is an object of the present invention to provide a catalyst for the hydrogenation of carbon dioxide to methanol.

[0008] Another object of the present invention is to provide a method for preparing a catalyst for hydrogenating carbon dioxide to methanol. [Means for solving the problem]

[0009] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0010] The present disclosure discloses a catalyst for hydrogenating carbon dioxide to methanol comprising a metal and its oxide in an amount of 80-95% w / w of the total weight of the catalyst, a structural promoter in an amount of 5-20% w / w of the total weight of the catalyst, and a binder in an amount of 5-10% w / w of the total weight of the catalyst.

[0011] The present disclosure relates to a) co-precipitation of metal precursors at 80-95% w / w of the total weight of the catalyst using 1.0-1.8M precipitant, followed by addition of a structural promoter at 5-20% w / w of the total weight of the catalyst to obtain an active metal precipitate; b) washing and drying the active metal precipitate at a temperature in the range of 70-90°C for a period in the range of 8-12 hours to obtain a dried active metal precipitate, followed by calcination at a temperature in the range of 300-400°C for a period in the range of 3-5 hours to form a mixed metal oxide; c) Adding 5-10% w / w of binder with 0.5-1.5M of peptizer to 90-95% w / w of mixed metal oxides of the total weight of catalyst followed by drying at a temperature in the range of 70-90°C for a period in the range of 8-12 hours and calcining at a temperature in the range of 300-400°C for a period in the range of 3-5 hours to obtain a shaped final catalyst for hydrogenation of CO2 to methanol. A method for preparing a catalyst for hydrogenating carbon dioxide to methanol is disclosed, comprising:

[0012] Various objects, features, aspects and advantages of the present subject matter will become more apparent from the following detailed description of preferred embodiments. [Brief description of the drawings]

[0013] [Figure 1] X-ray diffraction (XRD) analysis is shown. [Diagram 2] A CO2-Temperature Programmed Desorption (TPD) study is shown. [Diagram 3] A temperature programmed reaction (TPR) study is presented. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The following is a detailed description of the embodiments of the present disclosure. The embodiments are described in sufficient detail to clearly convey the present disclosure. However, the amount of detail provided is not intended to limit the anticipated variations of the embodiments, but rather to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the present disclosure as defined by the appended claims.

[0015] Throughout the following specification, unless the context requires otherwise, the word "consisting of" and variations thereof are to be interpreted in their open and inclusive sense as "including, but not limited to."

[0016] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates otherwise. It should also be noted that the term "or" is generally used in its sense to include "and / or" unless the content clearly dictates otherwise.

[0017] In some embodiments, the numbers expressing properties such as amounts of ingredients, concentrations, reaction conditions, and the like, used to describe and claim certain embodiments of the invention should be understood as being modified in some cases by the term "about". Accordingly, in some embodiments, the numerical parameters set forth in the written description are approximations that may vary depending on the desired properties sought to be obtained by a particular embodiment. In some embodiments, the numerical parameters should be construed in light of the number of reported significant digits and by applying ordinary rounding techniques. Notwithstanding that the numerical ranges and parameters setting forth the broad scope of some embodiments of the invention are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible.

[0018] The recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of referring individually to each separate value falling within the range, and unless otherwise indicated herein, each separate value is incorporated herein as if each separate value was individually set forth herein.

[0019] All processes described herein can be performed in any suitable order unless otherwise indicated herein or clearly contradicted by context. Any examples provided herein with respect to specific embodiments, or the use of exemplary language (e.g., "etc.") is intended merely to facilitate a better understanding of the invention and does not impose limitations on the scope of the invention as otherwise claimed. No language in the specification should be construed as indicating any non-claimed element essential to the practice of the invention.

[0020] The headings and abstracts of the invention provided herein are for convenience only and do not interpret the scope or meaning of the embodiments.

[0021] The following description provides a number of exemplary embodiments of the inventive subject matter, and although each embodiment represents a single combination of inventive elements, the inventive subject matter is considered to include all possible combinations of the disclosed elements. Thus, if one embodiment includes elements A, B, and C, and a second embodiment includes elements B and D, the inventive subject matter is deemed to also include other remaining combinations of A, B, C, or D, even if not explicitly so.

[0022] All publications herein are incorporated by reference to the same extent as if each individual publication or patent application was specifically and individually indicated to be incorporated by reference. If a definition or use of a term in an incorporated reference is inconsistent with or contradicts the definition of that term provided herein, the definition of that term provided herein applies and the definition of that term in the reference does not apply.

[0023] Grouping of alternative elements or embodiments of the invention disclosed herein should not be construed as limiting. Each group member may be referenced individually or in combination with other members of the group or other elements described herein and claimed. One or more members of a group may be included in or deleted from a group for reasons of convenience and / or patentability. When such inclusion or deletion is made, the specification is deemed to include the group as modified to satisfy the following written description, and the embodiments described herein are provided to illustrate one or more examples of specific embodiments of the principles and aspects of the present disclosure. These examples are provided for illustrative purposes and are not intended to limit these principles and disclosures.

[0024] It should also be understood that the present invention can be implemented in various ways, including as a system, a method, or a device. These implementations, or other forms that the present invention may take, may be referred to herein as processes. In general, the order of steps of disclosed processes may be varied within the scope of the present invention.

[0025] Various terms used in this specification are set forth below. Unless a term used in the claims is defined below, it should be given the broadest definition that people in the relevant art have given that term, as reflected in printed publications and issued patents at the time of filing.

[0026] One embodiment of the present disclosure discloses a catalyst for hydrogenating carbon dioxide to methanol, comprising a metal and its oxide in an amount of 80-95% w / w of the total weight of the catalyst, a structural promoter in an amount of 5-20% w / w of the total weight of the catalyst, and a binder in an amount of 5-10% w / w of the total weight of the catalyst.

[0027] One embodiment of the present disclosure discloses that the metal and its oxide are selected from the group consisting of copper, cobalt, zinc oxide, indium oxide, zirconia, gallium oxide, nano-zirconia, lanthanum, ceria, nickel oxide, palladium, titania, and combinations thereof.

[0028] One embodiment of the present disclosure discloses that the structural promoter is selected from the group consisting of silica, alumina, alumina-silica, magnesium silicate, zirconia, ceria, titania, and combinations thereof.

[0029] An embodiment of the present disclosure discloses that the binder is selected from the group consisting of pseudoboehmite, ludox silica, precipitated silica, hydroxypropyl methylcellulose, and combinations thereof.

[0030] One embodiment of the present disclosure discloses that the catalyst comprises 55% w / w Cu, 5% w / w Ti, 20% w / w Zn, 5% w / w Zr, 5% w / w Al, and 10% w / w Ce.

[0031] Another embodiment of the present disclosure is a) co-precipitation of metal precursors at 80-95% w / w of the total weight of the catalyst using 1.0-1.8M precipitant, followed by addition of a structural promoter at 5-20% w / w of the total weight of the catalyst to obtain an active metal precipitate; b) washing and drying the active metal precipitate at a temperature in the range of 70-90°C for a period in the range of 8-12 hours to obtain a dried active metal precipitate, followed by calcination at a temperature in the range of 300-400°C for a period in the range of 3-5 hours to form a mixed metal oxide; c) Adding 5-10% w / w of binder with 0.5-1.5M of peptizer to 90-95% w / w of mixed metal oxides of the total weight of catalyst followed by drying at a temperature in the range of 70-90°C for a period in the range of 8-12 hours and calcining at a temperature in the range of 300-400°C for a period in the range of 3-5 hours to obtain a shaped final catalyst for hydrogenation of CO2 to methanol. A method for preparing a catalyst for hydrogenating carbon dioxide to methanol is disclosed, comprising:

[0032] Another embodiment of the present disclosure discloses that the precipitating agent and the metal precursor are co-precipitated at a pH in the range of 7.5-9.

[0033] Another embodiment of the present disclosure discloses that the metal precursor and the structural promoter are preferably nitrates.

[0034] Another embodiment of the present disclosure discloses that the precipitating agent is selected from the group consisting of plasticizers, sodium carbonate, sodium hydroxide, cetyltrimethylammonium bromide (CTAB), ethylenediamine, and combinations thereof.

[0035] Another embodiment of the present disclosure discloses that the deflocculating agent is selected from the group consisting of nitric acid, acetic acid, citric acid, formic acid, phosphoric acid, and combinations thereof.

[0036] Another embodiment of the present disclosure discloses that the plasticizer is hydroxypropyl methylcellulose, hydroxyethyl cellulose, polyethylene glycol, starch, sugar, and combinations thereof.

[0037] Another embodiment of the present disclosure discloses that the washing is done with hot water.

[0038] In one embodiment, the present invention relates to the design of active catalysts for the hydrogenation of CO to methanol via a thermal catalytic route. Density functional theory calculations are performed to simulate the catalytic properties for CO adsorption on the catalyst surface and this data is used as a key parameter for designing active catalyst formulations.

[0039] In one embodiment, the synthesis of the catalyst is carried out by precipitation, co-precipitation, wet and incipient (dry) impregnation methods.

[0040] In one embodiment, the methods of catalyst characterization are BET surface area, pore volume, pore size, X-ray diffraction spectrophotometer (XRD), X-ray fluorescence spectrophotometer (XRF), compressive strength, FE-SEM-EDX, CO2 desorption, ammonia temperature programmed desorption (NH3-TPD), H2 temperature programmed reduction (H2-TPR).

[0041] In one embodiment, the activity of the catalyst was measured in a tubular fixed bed reactor at different temperatures from 230 to 300 °C, pressures from 30 to 40 bar, and gas hourly space velocities (GHSVs) from 4000 to 15000 h while maintaining a CO2 to H2 ratio of 1:3. -1 Throughout the reaction, N2 was used as an internal standard for data analysis. Liquid and gas samples were analyzed by gas chromatography (GC) and refinery gas analyzer (RGA).

[0042] Simulation studies are used to design catalysts. Density Functional Theory (DFT) simulation studies are used to estimate the CO2 adsorption energy on the catalyst surface, which is identified as a key parameter to arrive at a suitable catalyst and correlated with experimental data.

[0043] The catalyst systems prepared and evaluated for this reaction are multimetal oxides, and the table below shows a list of the metals that were tested in this reaction.

[0044] [Table 1]

[0045] While various embodiments of the present disclosure have been described above, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the present disclosure. The present invention is not limited to the described embodiments, variations, or examples, which are included to enable those skilled in the art to make and use the present invention in combination with the information and knowledge available to them. EXAMPLES

[0046] The present invention is further described in the form of the following examples. However, it should be understood that the following examples are merely illustrative and should not be construed as limiting the scope of the present invention. EXAMPLES

[0047] 60%CuO+25%ZnO+5%ZrO2+10%Al2O3 The catalyst was prepared by a simple co-precipitation method using Na2CO3 as the precipitant. Under vigorous stirring, a mixed aqueous solution of Cu(NO3)2·3H2O (0.5 M), Zn(NO3)2·6H2O (0.5 M), zirconium nitrate hydrate (0.5 M), and aluminum nitrate nonahydrate (0.5 M) was added to form a homogeneous solution. Then, an aqueous solution of Na2CO3 (1.2 M) was added dropwise to the solution at 75 °C until the pH = 8 was reached. The solution was aged at the same temperature for 15 h, and then thoroughly washed with hot distilled water to remove all the Na. + The ions were removed. The resulting material was dried at 80°C overnight and calcined at 350°C for 4 hours (rate 2°C / min) in static air. X-ray diffraction (XRD) analysis of the resulting catalyst is shown in Figure 1. EXAMPLES

[0048] 55%CuO+25%ZnO+10%Al2O3+5%SiO2+5%ZrO2 The catalyst was prepared by a simple co-precipitation method using Na2CO3 as the precipitant. Under vigorous stirring, a mixed aqueous solution of zirconium oxychloride octahydrate (0.5 M), zinc nitrate hexahydrate (0.5 M), and SiO2 gel support was added to form a homogeneous solution. Then, an aqueous solution of Na2CO3 (1.2 M) was added dropwise to the solution at 75 °C until pH = 8. The solution was aged at the same temperature for 15 h, and then thoroughly washed with hot distilled water to remove all the Na. + The ions were removed. The resulting material was dried at 80°C overnight and calcined at 350°C for 4 hours (rate 2°C / min) in static air. X-ray diffraction (XRD) analysis of the resulting catalyst is shown in Figure 1. EXAMPLES

[0049] Optimal catalyst formulation Several catalysts were synthesized and evaluated in a laboratory-scale reactor, two examples of which are described above. After data analysis, the optimal catalyst formulation was identified as follows: XRD analysis of the resulting catalysts is shown in Figure 1.

[0050] 55%Cu+5%Ti+20%Zn+5%Zr+5%Al+10%Ce EXAMPLES

[0051] Optimal catalyst blending method The catalyst was prepared by a simple co-precipitation method using Na2CO3 as the precipitant. Under vigorous stirring, a mixed aqueous solution of copper nitrate trihydrate (0.5 M), zinc nitrate hexahydrate (0.5 M), zirconium oxychloride octahydrate (0.5 M), aluminum nitrate nonahydrate (0.5 M), CeO2, and TiO2 support was added to form a homogeneous solution. Then, Na2CO3 aqueous solution (1.2 M) was added dropwise to the solution at 75 °C until pH = 8. The solution was aged at the same temperature for 15 h, and then thoroughly washed with hot distilled water to remove all the Na. + The ions were removed. The resulting material was dried overnight at 80°C and calcined in static air at 350°C for 4 hours (rate 2°C / min). EXAMPLES

[0052] The TPD study of CO2 shown in Figure 2 provides information on the CO2 absorption by the different catalytic systems described in the examples. The results show that the catalysts have different CO2 absorption capacities, and that too strong or too weak adsorption is not suitable for increasing activity, indicating that optimal CO2 absorption is a prerequisite for efficient CO2 conversion. Similarly, the TPR study shown in Figure 3 provides information on the appropriate temperature required for reduction / pretreatment of the catalyst before the reaction. EXAMPLES

[0053] Catalyst evaluation data Catalytic evaluation data of several catalysts from different batches and their comparison. The optimal catalyst formulation clearly shows that this composition is necessary to achieve the best activity in terms of CO2 conversion and methanol yield. Example 3 (55%Cu+5%Ti+20%Zn+5%Zr+5%Al+10%Ce) showed the highest CO2 conversion of 19 and good methanol selectivity of 69, STY462. The CO2 adsorption energy (kJ / mol) was -1.22.

[0054] [Table 2]

[0055] One skilled in the art will understand that the amounts and types of each component can be used in different combinations or alone, and all such variations and combinations are within the scope of the present disclosure.

[0056] The above examples are merely illustrative and should not be construed as limiting the scope of the present invention. Various changes and modifications to the disclosed embodiments will be apparent to those skilled in the art. Such changes and modifications can be made without departing from the scope of the present invention.

Claims

1. 1. A catalyst for the hydrogenation of carbon dioxide to methanol comprising a metal and its oxide in an amount of 80-95% w / w of the total weight of the catalyst, a structural promoter in an amount of 5-20% w / w of the total weight of the catalyst, and a binder in an amount of 5-10% w / w of the total weight of the catalyst.

2. 2. The catalyst of claim 1, wherein the metal and its oxide are selected from the group consisting of copper, cobalt, zinc oxide, indium oxide, zirconia, gallium oxide, nano-zirconia, lanthanum, ceria, nickel oxide, palladium, titania, and combinations thereof.

3. 2. The catalyst of claim 1, wherein the structural promoter is selected from the group consisting of silica, alumina, alumina-silica, magnesium silicate, zirconia, ceria, titania, and combinations thereof.

4. 2. The catalyst of claim 1, wherein the binder is selected from the group consisting of pseudoboehmite, ludox silica, precipitated silica, hydroxypropyl methylcellulose, and combinations thereof.

5. 2. The catalyst of claim 1, wherein the catalyst comprises 55% w / w Cu, 5% w / w Ti, 20% w / w Zn, 5% w / w Zr, 5% w / w Al, and 10% w / w Ce.

6. a) co-precipitation of metal precursors at 80-95% w / w of the total weight of the catalyst using 1.0-1.8M precipitant, followed by addition of structural promoter at 5-20% w / w of the total weight of the catalyst to obtain active metal precipitate; b) washing and drying the active metal precipitate at a temperature in the range of 70-90°C for a period in the range of 8-12 hours to obtain a dried active metal precipitate, followed by calcination at a temperature in the range of 300-400°C for a period in the range of 3-5 hours to form a mixed metal oxide; c) Adding 5-10% w / w of binder with 0.5-1.5M of peptizer to 90-95% w / w of mixed metal oxides of the total weight of catalyst followed by drying at a temperature ranging from 70-90° C. for a period ranging from 8-12 hours and calcining at a temperature ranging from 300-400° C. for a period ranging from 3-5 hours to obtain a shaped final catalyst for hydrogenation of carbon dioxide to methanol.

1. A method for preparing a catalyst for hydrogenating carbon dioxide to methanol, comprising:

7. The method of claim 6, wherein the precipitating agent and the metal precursor are co-precipitated at a pH in the range of 7.5 to 9.

8. 7. The method of claim 6, wherein the metal precursor and the structural promoter are preferably nitrates.

9. 7. The method of claim 6, wherein the precipitating agent is selected from the group consisting of plasticizers, sodium carbonate, sodium hydroxide, cetyltrimethylammonium bromide (CTAB), ethylenediamine, and combinations thereof.

10. 7. The method of claim 6, wherein the deflocculating agent is selected from the group consisting of nitric acid, acetic acid, citric acid, formic acid, phosphoric acid, and combinations thereof.

11. 10. The method of claim 9, wherein the plasticizer is hydroxypropyl methylcellulose, hydroxyethyl cellulose, polyethylene glycol, starch, sugar, and combinations thereof.

12. The method of claim 6, wherein the washing is performed with hot water.

Citation Information

Cited By

  • Catalyst for converting carbon dioxide to methanol and method for preparing methanol

    JP2026109478A