Polyarylate resin, and coating layer and laminate each including the same
A polyarylate resin with specific monomer ratios and production methods addresses the shortcomings of existing resins by enhancing abrasion resistance, flexibility, and heat resistance, ensuring effective film formability and reduced curling.
Patent Information
- Application Number
- JP2024024774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polyarylate resins fail to meet the increasing demands for abrasion resistance, flexibility, tensile fracture strain characteristics, and heat resistance, particularly due to issues such as high glass transition points, curling during solvent drying, and poor film formability, which are exacerbated by the use of aromatic hydrocarbons and high inherent viscosities.
A polyarylate resin composition comprising specific ratios of 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, terephthalic acid, and isophthalic acid, with inherent viscosities between 1.00 and 1.30 dl/g, and a terminal capping agent, produced via interfacial polymerization, to achieve balanced properties.
The resin exhibits excellent abrasion resistance, flexibility, tensile fracture strain, and film formability, with minimal curling and improved heat resistance, meeting modern performance standards.
Smart Images

Figure 2024144155000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyarylate resin having excellent abrasion resistance, flexibility, tensile strain at break, heat resistance and film formability, and to a coating film and a laminate containing the same. [Background technology]
[0002] Polyarylate resins are widely used in the electrical and electronics fields and the automotive field for injection molding because of their excellent heat resistance, flexibility, dimensional stability, and transparency. In recent years, because of their excellent transparency, heat resistance, and flexibility, they have been made into films by extrusion molding or solution processing, and are expected to be used as glass substrate materials and materials for foldable applications. Glass substrate materials require abrasion resistance and scratch resistance, and foldable applications often require flexibility, tensile fracture strain characteristics, and heat resistance. Moreover, these required properties are increasingly being required at even higher levels.
[0003] Film formation by solution processing is described, for example, in Patent Documents 1, 2, and 3. Patent Documents 1, 2, and 3 describe a technology in which the blending amount of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane is increased to 25 mol % or more to increase solubility in a solvent and form a film by solution processing.
[0004] Regarding the solubility of polyarylate resins having high inherent viscosity in solvents, for example, Patent Document 4 is mentioned.
[0005] Patent Document 5 describes a polyarylate resin made of a bisphenol having a cyclohexane ring structure and a bisphenol having an isopropylidene skeleton.
[0006] Patent Document 6 discloses a method for improving film formability while improving mechanical properties by blending an amorphous polyester resin other than a polyarylate resin. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2016 / 163462 Brochure [Patent Document 2] JP 2013-173928 A [Patent Document 3] JP 2015-174908 A [Patent Document 4] JP 2011-246551 A [Patent Document 5] JP 2009-167291 A [Patent Document 6] JP 2020-50877 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, when the resin composition described in Example 1 of Patent Documents 1, 2, and 3 was actually examined, it was confirmed that the resin composition did not satisfy the abrasion resistance and flexibility required in recent years. It is generally known that in order to improve such properties, the inherent viscosity corresponding to the molecular weight is increased. In the resin compositions described in Patent Documents 1, 2, and 3, the glass transition point was too high due to the large amount of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane blended, and problems occurred such as curling due to thermal shrinkage during drying of the solvent and curling due to thermal shrinkage during extrusion molding. Such problems revealed the problem of very poor film-forming moldability, which was a problem that arose even before the abrasion resistance and flexibility were improved.
[0009] In particular, Patent Document 3 describes that the solvent contains aromatic hydrocarbons, but aromatic hydrocarbons have poor drying properties and tend to remain in the resin coating film, so that a large amount of solvent may remain in the resin coating film, which may reduce the abrasion resistance and / or flexibility.
[0010] In Patent Document 4, since the phenol component is composed of 2,2-bis(4-hydroxyphenyl)propane, even if the inherent viscosity is increased, the glass transition point is 210° C. or lower, and the heat resistance may be poor. Patent Document 5 had problems of low inherent viscosity and poor wear resistance and flexibility. Patent Document 5 also describes the use of a catalyst in combination, but there were problems such as an increase in the number of catalyst types increasing not only the polymerization property but also the decomposition property after molding, which is likely to lead to a decrease in wear resistance and / or flexibility. In recent years, it has become possible to increase polymerization with one type of catalyst by lowering the polymer concentration in the solvent during polymerization, increasing the stirring efficiency, or changing the amount of end-capping agent. In Patent Document 6, the glass transition point is 200° C. or lower, and the heat resistance is sometimes poor.
[0011] An object of the present invention is to provide a polyarylate resin having an excellent balance of abrasion resistance, flexibility, tensile strain at break, heat resistance, and formability into a film. Another object of the present invention is to provide a polyarylate resin which is excellent in all of the properties, such as abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability. [Means for solving the problem]
[0012] As a result of extensive research, the present inventors have found that the above object can be achieved by using a polyarylate resin having a specific composition and a specific inherent viscosity, and have arrived at the present invention.
[0013] The gist of the present invention is as follows. <1> (A) 2,2-bis(4-hydroxyphenyl)propane; (B) 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; (C) terephthalic acid; and (D) Isophthalic acid A polyarylate resin comprising: The content ratio ((A) / (B)) of the component (A) to the component (B) is 72 / 28 to 95 / 5 (mol%), The polyarylate resin has an inherent viscosity (ηinh) of more than 1.00 dl / g and less than 1.30 dl / g. <2> The content ratio ((C) / (D)) of the component (C) to the component (D) is 90 / 10 to 10 / 90 (mol%). <1> The polyarylate resin according to claim 1. <3> A 5 μm thick film made of the polyarylate resin exhibits an abrasion amount of 1.0 mg or less in an abrasion test based on JIS K7204. <1> or <2> The polyarylate resin according to claim 1. <4> A film having a thickness of 5 μm and composed of the polyarylate resin exhibits a tensile breaking strain of 100% or more. <1> ~ <3> 2. The polyarylate resin according to claim 1 . <5> The glass transition temperature is 200 to 245°C. <1> ~ <4> 2. The polyarylate resin according to claim 1 . <6> The content ratio ((A) / (B)) of the component (A) to the component (B) is 76 / 24 to 85 / 15 (mol%), the content ratio ((C) / (D)) of the component (C) to the component (D) is 80 / 20 to 10 / 90 (mol%); The inherent viscosity (ηinh) is 1.03 to 1.29 dl / g. <1> ~ <5> The polyarylate resin according to any one of claims 1 to 5. <7> The content ratio ((A) / (B)) of the component (A) to the component (B) is 76 / 24 to 85 / 15 (mol%), the content ratio ((C) / (D)) of the component (C) to the component (D) is 80 / 20 to 10 / 90 (mol%); The inherent viscosity (ηinh) is 1.03 to 1.18 dl / g. <1> ~ <6> The polyarylate resin according to any one of claims 1 to 5. <8> The polyarylate resin further contains a terminal blocking agent, and the content of the terminal blocking agent is more than 0.30 mol % and less than 2.00 mol % based on the phenol component. <1> The polyarylate resin according to claim 1. <9> By interfacial polymerization method, <1> ~ <8> 2. A method for producing a polyarylate resin, comprising the steps of: producing the polyarylate resin according to any one of claims 1 to 11; <10> The method for producing the polyarylate resin according to claim 9, wherein the following raw materials are used: (A) 2,2-bis(4-hydroxyphenyl)propane; (B) 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; (C') terephthalic acid dichloride; and (D') Isophthalic acid dichloride. <11> A single type of quaternary ammonium salt is used as a polymerization catalyst. <9> or <10> A method for producing the polyarylate resin described in claim 1. <12> <1> ~ <8> A coating film comprising the polyarylate resin according to any one of claims 1 to 5. <13> <1> ~ <8> 2. A laminate comprising a layer containing the polyarylate resin according to claim 1. Effect of the Invention
[0014] According to the present invention, by making a polyarylate resin of a specific composition have a specific inherent viscosity, it is possible to provide a polyarylate resin that is excellent in all of the properties such as abrasion resistance, flexibility, tensile strain at break (characteristics), heat resistance, and film formability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. The polyarylate resin of the present invention is a polyester resin that contains a dihydric phenol component and an aromatic dicarboxylic acid component, and contains 75 to 100 mol % (particularly 90 to 100 mol %, preferably 100 mol %) of the dihydric phenol component when the total of the components (constituent monomer components) having a hydroxyl group (e.g., a phenol-based hydroxyl group or an alcohol-based hydroxyl group) is taken as 100 mol %. The polyarylate resin of the present invention also preferably contains 75 to 100 mol % (particularly 90 to 100 mol %, preferably 100 mol %) of the aromatic dicarboxylic acid component when the total of the components (constituent monomer components) having a carboxyl group is taken as 100 mol %. Note that in the present invention, the polyarylate resin does not include so-called liquid crystal polymers having a mesogenic group.
[0016] The polyarylate resin of the present invention contains, as dihydric phenol components, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A (BisA)) (hereinafter sometimes referred to as "component (A)") and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (BisTMC) (hereinafter sometimes referred to as "component (B)"). If at least one of components (A) and (B) is not contained, the heat resistance, abrasion resistance, and tensile strain at break properties are reduced.
[0017] The polyarylate resin of the present invention contains terephthalic acid (TPA) (hereinafter sometimes referred to as "component (C)") and isophthalic acid (IPA) (hereinafter sometimes referred to as "component (D)") as aromatic dicarboxylic acid components. If component (C) is not contained, the tensile strain at break property and film formability are reduced. If component (D) is not contained, the flexibility, tensile strain at break property and film formability are reduced.
[0018] Therefore, the polyarylate resin of the present invention contains at least components (A) to (D) as monomer components or copolymer components. More specifically, the polyarylate resin of the present invention contains at least residues of components (A) to (D). For this reason, with regard to components (C) to (D), the polyarylate resin can also be expressed as containing residues of terephthalic acid (TPA) and isophthalic acid (IPA).
[0019] In this specification, the abrasion resistance refers to a property that the amount of abrasion of a polyarylate resin is smaller in an abrasion test based on JIS K7204. The flexibility is a property that makes it more difficult for the polyarylate resin to break in a folding endurance (MIT) test based on JIS P 8115. The tensile strain at break characteristic is a characteristic in which the tensile strain at break of a polyarylate resin is larger in a tensile test based on JIS K7127. Heat resistance refers to the property of a polyarylate resin having a higher glass transition temperature. The film formability refers to the property of the polyarylate resin film produced by extrusion molding and solution processing being less likely to curl. Curling is a phenomenon in which the film naturally rolls up while taking on a rounded shape from the edge.
[0020] The polyarylate resin may contain other diol components other than the components (A) and (B), for example, dihydric phenols other than the components (A) and (B) (e.g., 4,4'-cyclohexylidene bisphenol), aliphatic diols (e.g., ethylene glycol, propylene glycol, etc.), and alicyclic diols (e.g., 1,4-cyclohexanediol, 1,3-cyclohexanediol, 1,2-cyclohexanediol, etc.), within the range that does not impair the effects of the present invention. The other diol components are preferably dihydric phenols other than the components (A) and (B). The content ratio of the other diol components is usually 20 mol% or less, preferably 10 mol% or less, and more preferably 0 mol%, relative to the total amount of the diol components (100 mol%). When the polyarylate resin contains two or more kinds of the other diol components, the total amount of them may be within the above range. The diol component is a monomer component having two hydroxyl groups in one molecule.
[0021] The polyarylate resin may contain other dicarboxylic acid components other than the components (C) and (D), for example, aromatic dicarboxylic acids other than the components (C) and (D) (e.g., 4,4'-oxydibenzoyl chloride, etc.), aliphatic dicarboxylic acids (e.g., sebacic acid, etc.), and alicyclic dicarboxylic acids (e.g., 1,4-cyclohexanedicarboxylic acid, etc.) within the range that does not impair the effects of the present invention. The other dicarboxylic acid components are preferably aromatic dicarboxylic acids other than the components (C) and (D). The content ratio of the other dicarboxylic acid components is usually 20 mol% or less, preferably 10 mol% or less, and more preferably 0 mol%, relative to the total amount of the dicarboxylic acid components (100 mol%). When the polyarylate resin contains two or more kinds of the other dicarboxylic acid components, the total amount of them may be within the above range. The dicarboxylic acid component is a monomer component having two carboxyl groups in one molecule.
[0022] The content ratio of component (A) to component (B) is 72 / 28 to 95 / 5 in terms of (A) / (B) (mol%), and from the viewpoint of further improving abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability, it is preferably 76 / 24 to 85 / 15, more preferably 77 / 23 to 83 / 17, even more preferably 78 / 22 to 82 / 18, and most preferably 80 / 20. In this content ratio, if the proportion of component (A) is too small, the abrasion resistance decreases. On the other hand, if the proportion of component (A) is too large, the abrasion resistance and tensile strain at break decrease. The content ratio is the content ratio of the residues of each component.
[0023] The content ratio of component (C) and component (D) is not particularly limited, and is usually 10 / 90 to 90 / 10 in terms of (C) / (D) (mol%). From the viewpoint of further improving abrasion resistance, bending property, tensile strain at break property, heat resistance, and film forming moldability, it is preferably 20 / 80 to 90 / 10, more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, sufficiently preferably 30 / 70 to 70 / 30, more sufficiently preferably 35 / 65 to 65 / 35, more particularly preferably 40 / 60 to 60 / 40, and most preferably 50 / 50. The content ratio is the content ratio of the residue of each component.
[0024] The ratio of the total amount of components (A) and (B) to the total amount of components (C) and (D) is not particularly limited, and is usually 90 / 100 to 110 / 100 in terms of "(A) + (B)" / "(C) + (D)" (mol %), and from the viewpoint of further improving abrasion resistance, flexibility, tensile strain at break properties, heat resistance, and film formability, it is preferably 95 / 100 to 105 / 100, more preferably 98 / 100 to 102 / 100, and most preferably 100 / 100. The ratio is the ratio of residues of each component.
[0025] The inherent viscosity (ηinh) of the polyarylate resin is greater than 1.00 dl / g and less than 1.30 dl / g. From the viewpoint of further improving the abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability, it is preferably 1.03 to 1.29 dl / g, more preferably 1.03 to 1.25 dl / g, even more preferably 1.03 to 1.22 dl / g, sufficiently preferably 1.03 to 1.18 dl / g, more sufficiently preferably 1.03 to 1.15 dl / g, particularly preferably 1.08 to 1.15 dl / g, and most preferably 1.08 to 1.12 dl / g. If the viscosity is 1.00 dl / g or less, the abrasion resistance, tensile strain at break, and / or flexibility are poor. If the viscosity is 1.30 dl / g or more, the high resin viscosity leaves a problem in productivity.
[0026] In this specification, the inherent viscosity is a value calculated based on the relative viscosity (ηrel) measured using 1,1,2,2-tetrachloroethane as a solvent at a concentration of 1 g / dL and a temperature of 25° C. The inherent viscosity may be the inherent viscosity of a polyarylate resin that does not contain any compounding agents. In the specification of the physical properties of a polyarylate resin, a compounding agent is a material that is mixed or added after polymerization of the polyarylate resin, and does not include additives such as terminal blocking agents, antioxidants, and polymerization catalysts, which are added during polymerization of the polyarylate resin, as described below.
[0027] The glass transition temperature of the polyarylate resin is preferably 200 to 245°C, more preferably 205 to 240°C, even more preferably 210 to 235°C, sufficiently preferably 215 to 230°C, and most preferably 215 to 220°C.
[0028] In this specification, the glass transition temperature is defined as the starting temperature of an endothermic change occurring due to transition from a solid state to a molten state in a temperature rise curve obtained by raising the temperature from 30° C. to 400° C. at a heating rate of 10° C. / min using a differential scanning calorimeter. The glass transition temperature may be the glass transition temperature of a polyarylate resin that does not contain any compounding agents.
[0029] From the viewpoint of further improving abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability, the polyarylate resin preferably exhibits an abrasion amount of 1.0 mg or less in an abrasion test, more preferably an abrasion amount of 0.8 mg or less, even more preferably an abrasion amount of 0.5 mg or less, and most preferably an abrasion amount of 0.2 mg or less. The abrasion amount is usually 0.05 mg or more.
[0030] In this specification, the abrasion amount is a value measured by subjecting a 5 μm thick film of polyarylate resin to an abrasion test based on JIS K7204. The abrasion amount may be the abrasion amount of a film of only polyarylate resin without any compounding agent. The thickness may be the average thickness of 100 arbitrary points.
[0031] From the viewpoint of further improving abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability, the polyarylate resin preferably exhibits a tensile strain at break of 100% or more in a tensile test, more preferably a tensile strain at break of 120% or more, even more preferably a tensile strain at break of 130% or more, and most preferably a tensile strain at break of 133% or more. The tensile strain at break is usually 150% or less.
[0032] In this specification, the tensile breaking strain is a value measured by subjecting a 5 μm thick film of polyarylate resin to a tensile test based on JIS K7127. The tensile breaking strain may be the tensile breaking strain of a film of only polyarylate resin without any compounding agent. The thickness may be the average thickness of 100 arbitrary points.
[0033] The polyarylate resin may have any shape, and usually has a fine particle shape. Fine particle shape means granular. The major axis is usually 5 mm or less (particularly 2 mm or more and 5 mm or less). The major axis means the maximum length of the fine particle shape.
[0034] In this specification, the major axis is the average value of 100 arbitrary polyarylate resin fine particles.
[0035] The bulk density of the polyarylate resin is usually 0.1 to 0.5 g / ml, particularly 0.15 to 0.30 g / ml.
[0036] In this specification, the bulk density is a value measured by the following method. Fill a 1000ml container with polyarylate resin and measure the mass (g). Calculate the bulk density by dividing the mass (g) by 1000 (ml).
[0037] The method for producing the polyarylate resin is not particularly limited, and examples thereof include an interfacial polymerization method and a solution polymerization method. Compared with the solution polymerization method, the interfacial polymerization method has a faster reaction rate, and therefore the hydrolysis of the acid halide can be suppressed, and as a result, a polymer having a high molecular weight can be obtained. The interfacial polymerization method includes a method in which a solution (organic phase) in which a halide of a dicarboxylic acid component is dissolved in an organic solvent that is not compatible with water is mixed with an alkaline aqueous solution (aqueous phase) containing additives such as a diol component, an end-capping agent, an antioxidant, and a polymerization catalyst, and a polymerization reaction is carried out while stirring at a temperature of 50°C or less (particularly 20°C or less) for 1 to 8 hours (particularly 1 to 3 hours). As the solvent used for the organic phase, a solvent that is not compatible with water and dissolves the polyarylate resin is preferable. Examples of such a solvent include methylene chloride, chloroform, etc., and methylene chloride is preferable because it is easy to use in production. In the interfacial polymerization method, terephthalic acid dichloride and isophthalic acid dichloride are used as raw materials for terephthalic acid and isophthalic acid dichloride as components (C) and (D), respectively. When terephthalic acid and isophthalic acid are used as raw materials, the interfacial polymerization method cannot be carried out.
[0038] Examples of the end-capping agent include monohydric phenols, monoacid chlorides, monohydric alcohols, and monocarboxylic acids. Examples of monohydric phenols include phenol, o-cresol, m-cresol, p-cresol, p-tert-butylphenol [PTBP], o-phenylphenol, m-phenylphenol, p-phenylphenol, o-methoxyphenol, m-methoxyphenol, p-methoxyphenol, 2,3,6-trimethylphenol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol, 2-phenyl-2-(4-hydroxyphenyl)propane, 2-phenyl-2-(2-hydroxyphenyl)propane, and 2-phenyl-2-(3-hydroxyphenyl)propane. Examples of the monovalent acid chloride include benzoyl chloride, benzoic acid chloride, methanesulfonyl chloride, and phenyl chloroformate. Examples of monohydric alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, pentanol, hexanol, dodecyl alcohol, stearyl alcohol, benzyl alcohol, and phenethyl alcohol. Examples of the monovalent carboxylic acid include acetic acid, propionic acid, octanoic acid, cyclohexanecarboxylic acid, benzoic acid, toluic acid, phenylacetic acid, p-tert-butylbenzoic acid, and p-methoxyphenylacetic acid. Of these, the end-capping material is preferably PTBP because of its high reactivity and thermal stability.
[0039] The content of the terminal blocking agent is not particularly limited and may be, for example, more than 0.30 mol % and less than 2.00 mol % relative to the phenol component. From the viewpoint of further improving abrasion resistance, flexibility, tensile strain at break, heat resistance, and film formability (particularly, from the viewpoint of further improving abrasion resistance at a lower inherent viscosity), the content is preferably 0.30 to 1.90 mol %, more preferably 0.40 to 1.80 mol %, even more preferably 0.50 to 1.70 mol %, sufficiently preferably 0.60 to 1.60 mol %, even more sufficiently preferably 0.70 to 1.50 mol %, particularly preferably 0.80 to 1.30 mol %, and most preferably 0.90 to 1.20 mol %.
[0040] Examples of the antioxidant include sodium hydrosulfite, L-ascorbic acid, erythorbic acid, catechin, tocopherol, and butylhydroxyanisole, with sodium hydrosulfite being preferred because it dissolves quickly in water. This antioxidant is added and used during polymerization of the polyarylate resin, and is different in type from the antioxidant described below that is added and used as a compounding agent during production of the polyarylate resin composition after polymerization of the polyarylate resin.
[0041] Examples of the polymerization catalyst include quaternary ammonium salts such as tri-n-butylbenzyl ammonium halide, tetra-n-butyl ammonium halide, trimethylbenzyl ammonium halide, and triethylbenzyl ammonium halide; and quaternary phosphonium salts such as tri-n-butylbenzyl phosphonium halide, tetra-n-butyl phosphonium halide, trimethylbenzyl phosphonium halide, and triethylbenzyl phosphonium halide. Among them, tri-n-butylbenzyl ammonium halide, trimethylbenzyl ammonium halide, tetra-n-butyl ammonium halide, tri-n-butylbenzyl phosphonium halide, and tetra-n-butyl phosphonium halide are preferred because they can produce a polymer with a high molecular weight and a low terminal acid value. The polymerization catalyst is preferably produced using one compound selected from the group consisting of the above polymerization catalysts (particularly quaternary ammonium salts) from the viewpoint of preventing a decrease in heat resistance, abrasion resistance, flexibility, and tensile strain at break due to a decrease in molecular weight caused by decomposition of the resin after molding.
[0042] The polyarylate resin of the present invention may be in the form of a polyarylate resin composition containing additives such as antioxidants, flame retardants, ultraviolet absorbers, flow modifiers, inorganic particulate fillers, pigments, dyes, and resin polymers other than polyarylate resins, as long as the effects of the present invention are not impaired. In this specification, the polyarylate resin obtained by adding the above additives to the polyarylate resin after polymerization of the polyarylate resin and melt-kneading the mixture is referred to as a polyarylate resin composition. The polyarylate resin composition may usually be in the form of pellets. Examples of the antioxidant that is added after polymerization of the polyarylate resin include hindered phenol-based antioxidants, hindered amine-based antioxidants, thioether-based antioxidants, and phosphorus-based antioxidants. Examples of the flame retardant include halogen-based flame retardants, phosphorus-based flame retardants, and metal hydroxide-based flame retardants. Examples of ultraviolet absorbents include ethylhexyl methoxycinnamate, octyl salicylate, octocrylene, t-butyl methoxybenzoylmethane, and the like, and different ones can be used depending on the desired absorption wavelength. Examples of the flowability modifier include Metablen manufactured by Mitsubishi Chemical Corporation, various plasticizers, and the like. Examples of the particulate inorganic filler include zirconia-based, silica-based, silicon-acrylic, melamine-based, acrylic, calcium carbonate, and other inorganic fillers. Examples of the pigment include titanium oxide and carbon black. Examples of the dye include natural dyes, oil-soluble dyes, basic dyes, and acid dyes. Examples of the other resin polymer include polycarbonate, polystyrene, polyester, acrylic resin, polyphenylene ether, polysulfone, polyethersulfone, and polyetherimide. As the other resin polymer, a polyarylate resin other than the polyarylate resin of the present invention may be used.
[0043] The polyarylate resin or polyarylate resin composition of the present invention may have the form of a coating (or film) or layer. Such coating (or film) or layer is useful as a glass substrate material and a material for foldable applications in the electric / electronic field and the automotive field. When the polyarylate resin or polyarylate resin composition of the present invention has the form of a layer, the present invention may constitute a laminate having the layer on a substrate. Examples of the substrate include polyester film and metal.
[0044] Glass substrate materials are specifically polymeric materials used in conjunction with epoxy resins to impregnate glass fiber cloth in the electrical and electronics and automotive fields. More specifically, materials for foldable applications refer to transparent polymer materials that make up the screen portion in the electrical and electronics field. EXAMPLES
[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0046] 1.Measurement method (1) Inherent viscosity (ηinh) The relative viscosity (ηrel) of the polyarylate resin was measured using 1,1,2,2-tetrachloroethane as a solvent at a concentration of 1 g / dL and a temperature of 25° C. The inherent viscosity was calculated from the obtained relative viscosity and the following formula. In the formula, "c" is the concentration. ηinh=ln(ηrel) / c
[0047] (2) Composition of polyarylate resin Using an NMR measurement device (JNM-LA400 manufactured by JEOL Ltd.), 1 The compositions of the respective compounds were determined by H-NMR measurement. Deuterated trifluoroacetic acid was used as the measurement solvent.
[0048] (3) Glass transition temperature Using a differential scanning calorimeter (Diamond DSC manufactured by PerkinElmer), the polyarylate resin was heated from 30°C to 400°C at a heating rate of 10°C / min, and the starting temperature of the endothermic change occurring due to the transition from a solid state to a molten state in the obtained heating curve was determined as the glass transition temperature.
[0049] (4) Heat resistance The glass transition temperature measured in the above (3) was evaluated according to the following criteria. ◎: 210℃ or higher. ○: 205℃ or higher and less than 210℃. △: 200°C or higher and less than 205°C. ×: Less than 200°C.
[0050] (5) Preparation of evaluation samples Polyarylate resin was dissolved in chloroform to a solid content concentration of 10 wt%, and a coating was formed on a polyester film (thickness 75 μm) and evaluated. For abrasion resistance, tensile strain at break characteristics, and film formability (solution processing), the film was prepared so that the film thickness after drying was 5 μm. For flexibility evaluation, the film was prepared so that the film thickness after drying was 50 μm.
[0051] (6) Abrasion resistance The film prepared by the method described in (5) above was subjected to an abrasion test described in JIS K7204, and the weight loss (mg) of the film before and after the test was evaluated according to the following criteria. The abrasion test was performed using a CS-10F abrasion wheel and a load of 250 g. ◎: The amount of wear is 0.5 mg or less. ◯: The amount of wear is more than 0.5 and 0.8 mg or less. △: Wear amount is more than 0.8 and 1.0 mg or less ×: Amount of wear is more than 1.0 mg.
[0052] (7) Flexibility The film prepared by the method described in (5) above was subjected to a folding endurance (MIT) test described in JIS P 8115, and the number of times the film broke was evaluated according to the following criteria. ◎: 10,000 times or more; ○: 9,000 or more and less than 10,000 times; △: 7000 or more and less than 9000 times; ×: Less than 7000 times.
[0053] (8) Tensile fracture strain characteristics The film prepared by the method described in (5) above was subjected to a tensile test according to JIS K7127, and the tensile breaking strain was evaluated according to the following criteria. A test sample was cut out to a width of 10 mm, and the test speed was 500 mm / min. ◎: 130% or more. ○: 120% or more and less than 130%. △: 100% or more but less than 120%. ×: Less than 100%.
[0054] (9) Film-forming moldability (extrusion molding) The polyarylate resin was extruded into a film having a thickness of 100 μm using a single screw extruder with a diameter of 50 mm (L / D=30). The obtained film was evaluated according to the following criteria. ◎: No curl. ◯: Curling was observed, but the curl origin was within 1 cm from the edge of the film. △: Curling was observed, but the curl originated within 3 cm from the edge of the film. ×: Curling was observed, and the curling originated more than 3 cm inside from the edge of the film.
[0055] (10) Film formability (solution processing) The film prepared by the method described in (5) above was dried at 100° C. for 5 minutes, and the degree of curling at the edges was evaluated according to the following criteria. ◎: No curl. ◯: Curling was observed, but the curl origin was within 3 cm from the edge of the film. Δ: Curling was observed, but the curl originated within 5 cm from the edge of the film. ×: Curling was observed, and the curling originated more than 5 cm inside from the edge of the film.
[0056] (11) Overall rating The worst evaluation result of all the coating film performances was adopted as the overall evaluation result.
[0057] Example 1 In a 2L reaction vessel equipped with a paddle-type two-blade stirrer, 14.1 parts by mass of BisTMC as a dihydric phenol component, 41.4 parts by mass of BisA, 0.3 parts by mass of PTBP as an end-capping agent, 32.6 parts by mass of sodium hydroxide (NaOH) as an alkali, 1.0 part by mass of a 50% by mass aqueous solution of tri-n-butylbenzylammonium chloride [TBBAC] as a polymerization catalyst, and 0.3 parts by mass of sodium hydrosulfite as an antioxidant were charged and dissolved in 1040 parts by mass of water (aqueous phase). In addition, 23.0 parts by mass of terephthalic acid dichloride (TPC) and 23.0 parts by mass of isophthalic acid dichloride (IPC) were dissolved in 910 parts by mass of methylene chloride (organic phase). The charged composition ratio was as follows. BisTMC:BisA:TPC:IPC:PTBP:TBBAC:NaOH=20.0:80.0:50.0:50.0:1.0:0.68:360 (mol%). The total amount of the aqueous phase and the organic phase was 1L. The aqueous phase was stirred at 400 rpm in advance, and the organic phase was added to the aqueous phase while maintaining the stirring speed, and polymerization was performed by interfacial polymerization at 15°C for 2 hours. After this, the stirring was stopped, and the aqueous phase and the organic phase were separated by decantation. After removing the aqueous phase, 500 parts by mass of methylene chloride, 2000 parts by mass of pure water, and 2 parts by mass of acetic acid were added to stop the reaction, and the mixture was stirred at 15°C for 30 minutes. Then, the organic phase was washed 10 times with pure water, and the organic phase was added to methanol to precipitate the polymer. The precipitated polymer was filtered and dried to obtain a polyarylate resin (major axis 3 mm).
[0058] Examples 2 to 18 and Comparative Examples 1 to 15 As shown in Table 1, polymerization of polyarylate resin and preparation of film were carried out in the same manner as in Example 1, except that the monomer charging ratio was changed and the amount of end-capping agent (PTBP) in the interfacial polymerization method was adjusted to have a predetermined inherent viscosity. Particularly in Examples 13 and 14 and Comparative Examples 7 to 10, the monomers shown in Table 1 were used in the ratios shown in Table 1.
[0059] Table 1 shows the composition of the polyarylate resin, as well as its characteristic values and evaluation results.
[0060] [Table 1]
[0061] The abbreviations in Table 1 stand for the following: TPC: Terephthalic acid dichloride IPC: Isophthalic acid dichloride OBC: 4,4'-oxydibenzoyl chloride TPA: Terephthalic acid IPA: Isophthalic acid OBA: 4,4'-dicarboxydiphenyl ether BisA: 2,2-bis(4-hydroxyphenyl)propane BisTMC: 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane BisZ: 4,4'-cyclohexylidene bisphenol
[0062] In Table 1, the polyarylate resins of Examples 1 to 14 were excellent in abrasion resistance, flexibility, tensile strain at break characteristics, heat resistance and film formability.
[0063] Generally, it is expected that the smaller the molecular weight of a polymer is, the lower its inherent viscosity is, and the lower the abrasion resistance of the polymer is. However, the following phenomena (1) and (2) were found; Phenomenon (1): Comparing Examples 1, 3, 4, and 9 to 12 with Examples 2 and 5, when the content ratio ((A) / (B)) of the polyarylate resin between the components (A) and (B) is 76 / 24 to 85 / 15 (particularly 77 / 23 to 83 / 17) in terms of molar ratio and the content ratio ((C) / (D)) of the components (C) and (D) is 80 / 20 to 10 / 90 in terms of molar ratio, the polyarylate resin exhibits better abrasion resistance (◎) even when the inherent viscosity is in a relatively wide range (for example, 1.03 to 1.29 dl / g).
[0064] Phenomenon (2): Comparison of Examples 1, 3, 4, and 9-10 with Examples 2 and 5 (particularly Example 2) revealed that when the content ratio ((A) / (B)) of the polyarylate resin between the components (A) and (B) is 76 / 24 to 85 / 15 (particularly 77 / 23 to 83 / 17) in terms of molar ratio and the content ratio ((C) / (D)) of the components (C) and (D) is 80 / 20 to 10 / 90 in terms of molar ratio, the polyarylate resin exhibits better abrasion resistance (◎) even when the inherent viscosity is in a relatively low range (for example, 1.03 to 1.18 dl / g, particularly 1.03 to 1.15 dl / g).
[0065] In Table 1, Comparative Example 1 had a small amount of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane as component (B), resulting in poor wear resistance. In Comparative Example 2, the blended amount of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane as component (B) was large, and the result was poor wear resistance. Although the mechanism by which wear resistance is exhibited is unclear, when the molar ratio of component (A) / component (B) was more than 95 / 5 or less than 72 / 28, the wear resistance was poor.
[0066] Comparative Example 3 had a low inherent viscosity and was poor in flexibility. Comparative Example 4 had a high inherent viscosity and was poor in film formability. Comparative Example 5, which did not contain 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, was inferior in heat resistance, abrasion resistance, and tensile strain at break properties. In Comparative Example 6, the mass ratio of component (A) to component (B) was not within the range specified in the present invention, and therefore the wear resistance and flexibility were poor. In Comparative Example 7, since 4,4'-dicarboxydiphenyl ether was blended instead of terephthalic acid dichloride, the film processability was poor. In Comparative Example 8, since 4,4'-dicarboxydiphenyl ether was blended instead of isophthalic acid dichloride, the bending property, tensile breaking strain and film formability were inferior. Comparative Example 9, in which 4,4'-cyclohexylidenebisphenol was blended instead of 2,2-bis(4-hydroxyphenyl)propane, resulted in poor wear resistance. Comparative Example 10 contained 4,4'-cyclohexylidenebisphenol instead of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and therefore had inferior abrasion resistance and tensile strength at break. In Comparative Example 11, since 2,2-bis(4-hydroxyphenyl)propane was not blended, the abrasion resistance was poor. In Comparative Example 12, since isophthalic acid chloride was not blended, the abrasion resistance, flexibility, tensile strain at break, and film formability were poor. In Comparative Example 13, since terephthalic acid chloride was not blended, the abrasion resistance, tensile breaking strain, and film formability were poor. In Comparative Example 14, since isophthalic acid chloride was not blended, the flexibility and tensile breaking strain were inferior. In Comparative Example 15, since terephthalic acid chloride was not blended, the abrasion resistance and tensile breaking strain were inferior. [Industrial Applicability]
[0067] The polyarylate resin and polyarylate resin composition of the present invention are useful in all applications requiring wear resistance, flexibility, tensile strain at break, heat resistance, and film formability. Examples of such applications include glass substrate materials and foldable materials in the electrical and electronic fields and automotive fields.
Claims
1. (A) 2,2-bis(4-hydroxyphenyl)propane; (B) 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; (C) terephthalic acid; and (D) Isophthalic acid A polyarylate resin comprising: The content ratio ((A) / (B)) of the component (A) to the component (B) is 72 / 28 to 95 / 5 (mol%), The polyarylate resin has an inherent viscosity (ηinh) of more than 1.00 dl / g and less than 1.30 dl / g.
2. The polyarylate resin according to claim 1, wherein the content ratio ((C) / (D)) of the component (C) to the component (D) is 90 / 10 to 10 / 90 (mol%).
3. 2. The polyarylate resin according to claim 1, wherein a 5 μm-thick film made of the polyarylate resin exhibits an abrasion amount of 1.0 mg or less in an abrasion test based on JIS K7204.
4. 2. The polyarylate resin according to claim 1, wherein a 5 μm thick film made of the polyarylate resin exhibits a tensile break strain of 100% or more.
5. The polyarylate resin according to claim 1, having a glass transition temperature of 200 to 245°C.
6. The content ratio ((A) / (B)) of the component (A) to the component (B) is 76 / 24 to 85 / 15 (mol%), The content ratio ((C) / (D)) of the component (C) to the component (D) is 80 / 20 to 10 / 90 (mol%), The polyarylate resin according to claim 1, wherein the inherent viscosity (ηinh) is 1.03 to 1.29 dl / g.
7. The content ratio ((A) / (B)) of the component (A) to the component (B) is 76 / 24 to 85 / 15 (mol%), The content ratio ((C) / (D)) of the component (C) to the component (D) is 80 / 20 to 10 / 90 (mol%), The polyarylate resin according to claim 1, wherein the inherent viscosity (ηinh) is 1.03 to 1.18 dl / g.
8. The polyarylate resin according to claim 1, further comprising a terminal blocking agent, the content of the terminal blocking agent being more than 0.30 mol % and less than 2.00 mol % based on the phenol component.
9. A method for producing a polyarylate resin, comprising producing the polyarylate resin according to any one of claims 1 to 8 by an interfacial polymerization method.
10. The method for producing the polyarylate resin according to claim 9, using the following raw materials: (A) 2,2-bis(4-hydroxyphenyl)propane; (B) 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; (C') terephthalic acid dichloride; and (D') Isophthalic acid dichloride.
11. The method for producing a polyarylate resin according to claim 9, wherein one type of quaternary ammonium salt is used as the polymerization catalyst.
12. A coating film comprising the polyarylate resin according to any one of claims 1 to 8.
13. A laminate comprising a layer containing the polyarylate resin according to any one of claims 1 to 8.
Citation Information
Patent Citations
Polyarylate and its manufacturing method
JP2009167291A
Coating agent
JP2011246551A
Polyarylate resin and film comprising the same
JP2013173928A
Varnish and method of producing the same
JP2015174908A
Resin composition and film thereof
JP2020050877A