Preliminary treatment method of molten iron

The method addresses inefficiencies in conventional hot metal pretreatment by controlling oxygen collision pressure and using a CaO-based medium to minimize equipment damage and reduce costs while enhancing dephosphorization efficiency.

JP2024144157AActive Publication Date: 2024-10-11JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024025113
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-22
Publication Date
2024-10-11
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

Conventional hot metal pretreatment methods lack specific values for oxygen delivery rate, lance height, and bottom blowing gas flow rate, leading to issues such as metal ejection onto converter equipment and increased operating costs.

Method used

A method involving a first blowing process with controlled oxygen collision pressure, followed by slag discharge and introduction of a CaO-based medium, with specific oxygen collision pressure ranges in the second blowing process to manage metal scattering and enhance dephosphorization efficiency.

Benefits of technology

Reduces metal adhesion to converter equipment, lowers operating costs, and improves dephosphorization efficiency by controlling oxygen collision pressure within specified ranges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144157000001_ABST
    Figure 2024144157000001_ABST
Patent Text Reader

Abstract

To provide a preliminary treatment method of molten iron capable of suppressing occurrence of a base metal sticking trouble and performing economically advantageous refining.SOLUTION: A preliminary treatment method of molten iron includes a first blowing step in which a gas oxygen source is supplied to molten iron in a converter type refining furnace from a top blow lance for desiliconization and dephosphorization of the molten iron, a slag discharge step in which at least a part of the slag produced in the first blowing step is discharged from the converter type refining furnace, and a second blowing step in which, after the slag discharge step, a CaO-based solvent is added to the converter type refining furnace and a gas oxygen source is supplied from the top blow lance for dephosphorization and decarbonization of the residual molten iron. In the second blowing step, when the gas oxygen source is supplied from the top blow lance to the molten iron bath surface, the blowing is carried out so that an oxygen collision pressure PC obtained by a predetermined relation becomes 58800 Pa or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steelmaking process using a converter or a converter-type refining furnace, and a pretreatment method for hot metal for the steelmaking process, including desiliconization, dephosphorization, and decarburization of hot metal. 3 kg. Furthermore, the "N" attached to the unit of gas volume represents the volume of the gas under standard conditions, which are 0°C and 101325 Pa. In this specification, "x to y" representing a numerical range represents not less than x and not more than y, and includes the boundary value. [Background technology]

[0002] In the conventional hot metal pretreatment method including the desiliconization, dephosphorization, and decarburization processes, a gaseous oxygen source is supplied from a top-blowing lance to perform the desiliconization, dephosphorization, and decarburization processes of the hot metal. In order to perform the desiliconization, dephosphorization, and decarburization processes efficiently, a treatment method is used in which three values, the oxygen blowing rate, the lance height, and the bottom-blowing gas flow rate, are changed.

[0003] For example, Patent Document 1 discloses a method for pre-treatment of molten pig iron, in which desiliconization and dephosphorization are carried out continuously with a slag removal process in between using a converter-type refining furnace. It is said that a sufficient amount of slag can be quickly discharged outside the furnace in the slag removal process after the desiliconization process, and that this makes it possible to perform sufficient dephosphorization in the next dephosphorization process from the standpoints of cost and quality. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-159632 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques have the following problems. The technology disclosed in Patent Document 1 does not establish specific values ​​for the oxygen flow rate, lance height, and bottom blown gas flow rate. Therefore, the quality of the dephosphorization treatment was improved in the dephosphorization and decarburization treatment process. However, there were cases where the ingots ejected or generated during blowing adhered to or fell onto the hood of the converter equipment. And there was room for improvement in the increased operating costs caused by removing the ingots.

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for preliminary treatment of molten iron which can suppress the occurrence of troubles such as metals generated during blowing adhering to and falling onto the hood of a converter furnace and which enables economically advantageous refining. [Means for solving the problem]

[0007] The present invention provides a method for pretreating molten pig iron, which advantageously solves the above problems, comprising a first blowing step of supplying a gaseous oxygen source from a top-blowing lance to the molten pig iron in a converter-type refining furnace to desiliconize and dephosphorize the molten pig iron, a slag removal step of discharging at least a part of the slag generated in the first blowing step from the converter-type refining furnace, and a second blowing step of adding a CaO-based flux into the converter-type refining furnace after the slag removal step and supplying a gaseous oxygen source from the top-blowing lance to dephosphorize and decarburize the remaining molten pig iron, wherein in the second blowing step, when the gaseous oxygen source is supplied from the top-blowing lance to the surface of the molten pig iron bath, an oxygen impingement pressure P C The method is characterized in that the blowing is performed at a pressure of 58,800 Pa or less. P C =ρ V 2 / twenty one) V / (V0-V loss )=d e / (2 C Z) (2) C = 0.016 + 18600 / (P0 - P e ) (3) Here, P C : Oxygen impingement pressure on the bath surface (Pa), ρ: Gas density of the gaseous oxygen source (1.43 kg / m 3 ), V: central flow velocity of the gaseous oxygen source (m / s), V0: Nozzle outlet flow velocity (m / s), V loss : Flow velocity loss due to improper expansion (m / s), d e : Nozzle outlet diameter (m), C: Constant, Z: lance height (m), P0: Nozzle absolute pressure (Pa), P e : Atmospheric pressure (Pa) Represents.

[0008] In the second blowing step, in the hot metal pretreatment method according to the present invention, the oxygen collision pressure P C is in the range of 10800 to 11800 Pa, and when the cumulative oxygen supply amount is in the range of 30% or more and less than 70% of the total oxygen supply amount, the oxygen collision pressure P C In the remaining range of the cumulative oxygen supply amount being 70% or more of the total oxygen supply amount, the oxygen collision pressure P C Setting the pressure in the range of 49,000 to 50,000 Pa may be a more preferable solution. Effect of the Invention

[0009] According to the present invention, the oxygen impingement pressure during oxygen blowing is appropriately controlled, which makes it possible to suppress the occurrence of troubles such as the metal generated during blowing adhering to and falling onto the hood of the converter, and to perform economically advantageous preliminary treatment of molten pig iron. [Brief description of the drawings]

[0010] [Figure 1] 1(A) to 1(E) are schematic diagrams showing the order of steps in a molten iron pretreatment method according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a blowing pattern of the present invention. [Diagram 3] FIG. 1 is a diagram showing a blowing pattern outside the scope of the present invention. [Figure 4] 1 is a graph showing a comparison of the number of troubles caused by metals between the method of the present invention and outside the scope of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The following is a detailed description of the embodiments of the present invention. The following embodiments are merely examples of equipment and methods for embodying the technical idea of ​​the present invention, and are not intended to limit the configuration to those described below. In other words, the technical idea of ​​the present invention can be modified in various ways within the technical scope described in the claims.

[0012] 1(A)-(E) are schematic diagrams showing the steps of a molten pig iron pretreatment method according to an embodiment of the present invention. In this embodiment, first, new molten pig iron 9a is received from a charging ladle 14 into a converter-type refining furnace 1 (FIG. 1(A)), and a first blowing step (FIG. 1(B)) is performed in which oxygen-containing gas 12 as a gaseous oxygen source is supplied from a top-blowing lance 2 to the molten pig iron 9 in the converter-type refining furnace 1 to desiliconize and dephosphorize the molten pig iron 9. Next, a slag removal step (FIG. 1(C)) is performed in which at least a part of the slag 10 generated in the first blowing step is discharged from the converter-type refining furnace 1. Next, after the slag removal step, a second blowing step (FIG. 1(D)) is performed in which a CaO-based flux is added into the converter-type refining furnace 1, and oxygen-containing gas 12 as a gaseous oxygen source is supplied from the top-blowing lance 2 to dephosphorize and decarburize the remaining molten pig iron 9. Next, the molten iron 9 is tapped after the blowing is completed (Fig. 1(E)).

[0013] In this embodiment, the oxygen impingement pressure P C The oxygen impingement pressure from the top blowing lance 2 can be calculated by the following formulas (1) to (3). P C =ρ V 2 / twenty one) V / (V0-V loss )=d e / (2 C Z) (2) C = 0.016 + 18600 / (P0 - P e ) (3) Here, P C : Oxygen impingement pressure on the bath surface (Pa), ρ: Gas density of the gaseous oxygen source (1.43 kg / m3 ), V: central flow velocity of the gaseous oxygen source (m / s), V0: Nozzle outlet flow velocity (m / s) V loss : Flow velocity loss due to improper expansion (m / s) d e : Nozzle outlet diameter (m), C: Constant, Z: lance height (m), P0: Nozzle absolute pressure (Pa), P e : Atmospheric pressure (Pa) Represents.

[0014] In the second blowing process, in order to improve the dephosphorization efficiency, the amount of oxygen sent per unit time was increased and the height of the top blowing lance was lowered to reduce the oxygen impingement pressure P C In this case, the oxygen impingement pressure P C If the oxygen impingement pressure P of the oxygen-containing gas 12 blown from the top lance 2 to the molten iron in the second blowing process exceeds 58,800 Pa, a large amount of iron particles will be scattered from the surface of the molten iron 9 by the oxygen jet. There is a risk that the iron particles will accumulate on the hood of the converter equipment and become ingots or fall and damage surrounding equipment. C is limited to a maximum of 58,800 Pa.

[0015] On the other hand, if the oxygen impingement pressure is too low, the dephosphorization efficiency decreases and the treatment time is extended. C It is preferable that the pressure is at least 9800 Pa or more.

[0016] The molten iron pretreatment method according to this embodiment will be described in detail. The molten iron pretreatment method according to this embodiment using a converter-type refining furnace 1 is carried out in the following order, as shown in the flow chart of FIG. 1: (A) molten iron charging step, (B) first blowing step, (C) slag removal step, (D) second blowing step, and (E) tapping step. It is particularly preferable to repeatedly carry out these steps in the same furnace, since this enables efficient pretreatment of the molten iron.

[0017] [Hot metal charging process] First, the hot metal charging step (A) will be described. In this step (A), it is preferable to charge new hot metal 9a from the charging ladle 14 while leaving the slag (hereinafter simply referred to as "slag after dephosphorization and decarburization treatment") 17 generated after the second blowing step in the preliminary treatment of the previous hot metal in the converter-type refining furnace 1. On the other hand, the slag after the previous pretreatment of the hot metal often adheres to the furnace wall of the converter-type refining furnace 1. In addition, before the hot metal charging, a cold iron source 11 such as iron scrap is charged, and then the hot metal 9a is charged. The cold iron source 11 to be charged in advance may be iron scrap as specified in the "Unified Standard for Iron Scrap Inspection" of the Japan Iron Source Association, or may be iron-based, such as direct reduced iron or cold iron.

[0018] Here, the slag 17 after the previous dephosphorization and decarburization treatment, which is left in the refining furnace 1 in preparation for the next refining or remains attached to the furnace wall, is used for the purpose of adjusting the slag basicity in the following first blowing step. The basicity of the slag after the dephosphorization and decarburization treatment, that is, the concentration ratio (CaO) / (SiO2) of (CaO) to (SiO2) in the slag on a mass basis (hereinafter simply referred to as "basicity"), is preferably 1.2 or more, more preferably 1.4 or more. The reason is that if the basicity of the slag after the previous dephosphorization and decarburization treatment 17 at the end of the second blowing step is less than 1.2, even if this slag is left, it may not be sufficient for adjusting the basicity in the first blowing step. For this reason, it is necessary to add a large amount of lime-based flux in the desiliconization treatment in the first blowing step. There is no particular upper limit on the basicity of the slag after the dephosphorization and decarburization treatment. Normally, the basicity of the slag used in the dephosphorization and decarburization of molten iron is set to about 3.0 or less, so there is no need to increase the basicity any further.

[0019] In addition, the amount of the slag 17 left in the furnace after the previous dephosphorization and decarburization process is preferably 30% by mass or more of the amount of slag generated during the previous dephosphorization and decarburization process of the hot metal in order to effectively adjust the basicity. More preferably, it is 60% by mass or more. In this embodiment, if the entire amount of the slag left in the furnace after the second blowing process and the molten iron are used for the desiliconization process of new hot metal, it is more effective for adjusting the basicity in the desiliconization process. Furthermore, if this method is performed continuously, the pretreatment slag discharged is homogeneous, consisting only of the slag after the first blowing process. Therefore, the pretreatment slag does not contain the slag after the dephosphorization and decarburization process, which has a high basicity. Therefore, problems such as the expansion of the slag due to the hydration reaction and the elution of alkali do not occur. Therefore, this embodiment is extremely effective in utilizing the slag as a material.

[0020] The slag after dephosphorization and decarburization has a relatively high basicity, a relatively high melting point, and a relatively low temperature (below about 1350℃), so it has low fluidity. Therefore, even if a cold iron source is charged on the slag after dephosphorization and decarburization, the cold iron source is not enveloped in the slag and its melting is not delayed. There is no need for an operation that is inefficient in terms of heat and material balance, such as adding a large amount of coolant to solidify the slag, which is used when the so-called decarburized slag is left in the furnace. In addition, the slag after dephosphorization and decarburization is rich in solid phase and has low fluidity due to the above characteristics, so it contains a large amount of fine metallic iron in its structure. Therefore, even after the slag is solidified, crushed, and magnetically separated, it still contains metallic iron of about 10% by mass or more. Conventionally, this slag was discharged outside the system. According to this embodiment, the dephosphorized and decarburized slag can be carried over to the next refining process, and most of the metallic iron in the dephosphorized and decarburized slag can be recovered in the molten pig iron, which has the effect of reducing iron loss. On the other hand, the slag after the first blowing step has a relatively high fluidity, so the metallic iron in the slag is likely to become coarse. Therefore, in such slag, there is little metallic iron that remains in the slag after the pulverization and magnetic separation processes. Therefore, in this embodiment, the iron loss in the slag can be reduced throughout the entire preliminary treatment of the molten pig iron.

[0021] [First blowing process] Next, the first blowing step (B) shown in FIG. 1(B) will be described. In this step (B), the converter-type refining furnace 1 is placed upright, and oxygen-containing gas 12 as a gaseous oxygen source is supplied to the molten pig iron 9 through the oxygen supply lance 2 to perform desiliconization and dephosphorization. In this first blowing step, the Si source contained in the hopper and the lime-based flux contained in the hopper can be added into the converter-type refining furnace 1 through the chute. In addition, carbonaceous material as a heat source, Si source, and iron oxide as an oxygen source can also be added in the same manner. As the oxygen source for the desiliconization and dephosphorization treatment, it is preferable to use only the oxygen-containing gas 12 without using iron oxide, which has a large heat absorption, from the viewpoint of dissolving a large amount of cold iron source 11. In particular, it is preferable to use pure oxygen. It is preferable to inject bottom-blowing gas 13 from the bottom-blowing tuyere 3 and stir the mixture.

[0022] In this desiliconization process, Si contained in the molten pig iron 9a or Si contained in the Si source and the cold iron source 11 that transfers to the molten pig iron through melting is desiliconized by reacting with the oxygen source (Si+O2→SiO2). This helps to increase the efficiency of the dephosphorization reaction in the subsequent second blowing process. At the same time, P contained in the molten pig iron 9a is dephosphorized. In this first blowing process, oxidation heat of silicon and phosphorus is generated, which increases the molten iron temperature and promotes the melting of the cold iron source 11 in the molten pig iron. The composition of the slag in this first blowing process is determined taking into consideration the amount and estimated composition of the slag 17 after the previous dephosphorization and decarburization process that was left in the furnace in advance, as well as the amount of SiO2 produced by the above reaction.

[0023] That is, the basicity of the slag during the first blowing step is preferably adjusted to 0.8 or more and 1.5 or less. The reason is that if the slag basicity during the first blowing step is less than 0.8, depending on the [Si] (mass%) concentration in the molten pig iron, the phenomenon of rephosphorization due to a decrease in the dephosphorization ability of the slag 17 after the dephosphorization and decarburization treatment, that is, an increase in the [P] concentration in the molten pig iron, is observed. On the other hand, if the slag basicity is greater than 1.5, the solid fraction increases due to an increase in undissolved CaO, so that the fluidity of the slag during the first blowing step becomes poor, and there are cases in which the slag cannot be discharged. The preferable upper limit of the slag basicity is about 1.2.

[0024] Next, the basicity of the slag at the end of the first blowing step is preferably adjusted to 0.5 or more and 1.5 or less. If the basicity of the slag at this stage is less than 0.5, the viscosity of the slag increases, and there is a risk that a good slag removal rate cannot be ensured in the next slag removal step. Therefore, the basicity of the slag at the end of the first blowing step is preferably 0.5 or more, more preferably 0.8 or more. If the slag basicity at this stage is higher than 1.5, the fluidity of the slag decreases, so there is a problem that the amount of slag removed in the next slag removal step is small or the amount of slag removed is difficult to control. This is also not efficient in terms of reducing the amount of lime-based solvent. Therefore, the basicity of the slag at the end of the first blowing step is preferably 1.5 or less, more preferably 1.2 or less. In addition, in order to adjust the basicity, lime-based solvents such as quicklime, limestone, and dolomite, as well as steelmaking slag selected from decarburization slag, dephosphorization slag, and ladle slag can be used as solvents.

[0025] The molten metal temperature at the end of the first blowing process is preferably adjusted to 1240°C or higher and 1400°C or lower. If the temperature is higher than 1400°C, the slag 17 left or left in the furnace after dephosphorization and decarburization treatment will rephosphorize, leading to an increase in the [P] concentration in the molten metal. This increases the dephosphorization load in the subsequent process, which is not efficient. In addition, it is necessary to increase the magnesia (MgO) concentration in the slag to prevent wear of the magnesia carbon bricks lining, which increases the cost. More preferably, the temperature is 1350°C or lower. On the other hand, if the temperature is lower than 1240°C, the fluidity of the slag will decrease, and the amount of slag discharged in the next slag discharge process will decrease or it will be difficult to control the amount of slag discharged. In addition, the melting speed of the scrap will decrease. More preferably, the temperature is 1260°C or higher.

[0026] In addition, the molten metal temperature at this stage must be controlled in order to perform dephosphorization efficiently in the second blowing process. For example, if the molten metal temperature at the end of the first blowing process is set to 1350°C or less, the amount of coolant such as iron ore added to adjust the temperature in the second blowing process can be significantly reduced. When desiliconization / dephosphorization and dephosphorization / decarburization processes are performed consecutively in the same furnace, it is difficult to add scrap before the dephosphorization / decarburization process in terms of work time. In addition, the cold iron source that can be added from the furnace during the process is expensive and granulated, or is limited in quantity, such as ingots generated in the steelworks. Therefore, it is difficult to use a large amount of cold iron source regularly during the dephosphorization / decarburization process. In reality, the number of types of auxiliary materials that can be used in the furnace top charging device is also limited. In such cases, the cold iron source may not be added from the furnace. In short, the coolant used in the dephosphorization and decarburization processes has traditionally been limited to iron oxide such as iron ore, and it has generally not been possible to fully utilize inexpensive cold iron sources such as scrap.

[0027] The molten metal temperature after the first blowing process may be measured using a thermocouple or estimated from the heat balance. In the case of estimation from the heat balance, coefficients may be adjusted and variables may be added or removed depending on the individual equipment and operating conditions. If there is residual scrap after the desiliconization and dephosphorization processes, the measured value tends to be slightly higher than the estimated value, but this is within the margin of error and does not interfere with use.

[0028] The additive may also contain carbon. Examples of carbon include carbonaceous materials such as coke or graphite, as well as carbon in carbides such as silicon carbide. Examples of solvents include auxiliary materials such as quicklime, lightly burned dolomite, and magnesia clinker. Other slags such as dephosphorization slag, decarburization slag, and ladle slag can also be used as calcium oxide or magnesium oxide sources. Examples of inexpensive auxiliary materials include calcium or magnesium carbonates and hydroxides. However, because these have a large heat absorption, it is preferable to distinguish them from other solvents and revise the estimated heat balance when using large quantities.

[0029] Ferrosilicon can be used as the Si source to be added. It is preferable to use cheaper silicon carbide briquettes or waste refractories mainly composed of silicon carbide. It is not necessary to use only this silicon source as the heat source, and other heat sources such as carbonaceous materials may be used in combination as long as the productivity is not reduced. It is preferable to add the carbonaceous materials by predicting the amount of decarburization so that the [C] concentration in the molten iron at the end of the first blowing process is 3.3 mass% or more. This is because if it is less than 3.3 mass%, the heat source will be insufficient in the subsequent dephosphorization and decarburization processes. At the same time, the carburization rate on the surface of the cold iron source such as scrap will decrease, leading to a decrease in the melting rate of the cold iron source.

[0030] As will be described in detail later, in order to improve the slag removal property of the slag 10 after the first blowing step, it is preferable to cause moderate foaming of the slag in the converter-type refining furnace 1. For this purpose, it is effective to increase the rate of generation of CO gas generated by the reaction between carbon in the molten pig iron and iron oxide in the slag. Therefore, in order to obtain a stable slag removal rate in the next slag removal step, it is preferable to supply oxygen in an amount equal to or greater than the stoichiometric amount required to oxidize the Si in the molten pig iron and the added Si source.

[0031] The unit oxygen consumption to be supplied to the hot metal during the first blow process is the amount required stoichiometrically for desiliconization plus 2 Nm 3 / t hot metal or more, preferably 4Nm 3 It is preferable that the amount of oxygen is equal to or more than 1 / t-molten pig iron. In this embodiment, it is preferable that the [Si] concentration in the molten pig iron at the end of the first blowing step is 0.2 mass% or less by blowing oxygen in this manner. It is more preferable to make it 0.1 mass% or less, and even more preferable to make it 0.05 mass% or less. This makes it possible to maintain the foaming state and keep the slag removal performance good even when removing the slag after the first blowing step. At the same time, it becomes possible to suppress rephosphorization from the slag to the molten pig iron. In the oxygen blowing for desiliconization treatment, the top blowing oxygen flow rate is 1 to 2 Nm 3 The top blowing lance height Z is preferably 2.2 to 3.3 m. The oxygen impingement pressure P calculated by the above formula is C At the same time, the blowing rate of the bottom blown gas is preferably 0.02 to 0.2 Nm 3 It has been confirmed that the above-mentioned effect can be obtained when the temperature is about / (min·t-molten iron).

[0032] It is preferable to combine the control of the [Si] concentration in the molten pig iron with the control of the slag basicity and the molten iron temperature. By doing so, even if the second blowing process is performed while leaving all of the slag after the previous dephosphorization and decarburization process in the furnace, the lime content in the slag after the dephosphorization and decarburization process can be effectively utilized without causing rephosphorization. In addition, by combining the control of the [Si] concentration in the molten pig iron, the slag basicity, and the molten iron temperature, and leaving the slag after the previous dephosphorization and decarburization process in the furnace, the (P2O5) concentration in the slag can be increased. This also promotes the foaming of the slag. In particular, the (P2O5) in the slag has the effect of lowering the surface tension of the slag, promoting the reaction with the molten pig iron and the dispersion of fine bubbles. Therefore, it is considered that the foaming of the slag can be maintained and the slag removal can be maintained well even at a relatively low iron oxide concentration, such as a total iron concentration (T.Fe) of about 10 mass%.

[0033] [Slag removal process] Next, the slag removal step (C) shown in FIG. 1(C) will be described. In the hot metal pretreatment method according to this embodiment, the slag removal process is performed after the first blowing process described above. That is, the slag removal process is performed to remove the low basicity treated slag containing a large amount of SiO2 generated during the first blowing process from the converter-type refining furnace 1. The removal of the treated slag 10 is effective in reducing the amount of lime-based flux used to adjust the slag basicity to an appropriate level in the next second blowing process. In this embodiment, the desiliconization and dephosphorization process of new hot metal is performed while leaving a large amount of the dephosphorization and decarburization process slag generated during the previous hot metal pretreatment in the furnace. In this case, the desiliconization and dephosphorization process is performed to prevent rephosphorization from the slag to the hot metal, so that the (P2O5) concentration in the slag becomes higher than in the past. If a large amount of slag is left after treatment, the amount of (P2O5) in the slag in the furnace in the next second blowing process will become excessive, which will reduce the dephosphorization effect, so it is also important to prevent this.

[0034] A characteristic feature of the hot metal pretreatment method according to this embodiment is that when the above-mentioned treatments (A) to (E) are repeatedly and continuously performed, if the slag is not sufficiently discharged after the first blowing step, the accumulation of (P2O5) in the furnace progresses, so care must be taken. This is because if the amount of (P2O5) in the slag in the furnace becomes too large during the dephosphorization and decarburization treatment stage, the increase in the (P2O5) concentration in the slag reduces the efficiency of the dephosphorization reaction, and the [P] concentration in the hot metal after treatment increases. In addition, the amount of lime-based flux required for the dephosphorization reaction increases.

[0035] Therefore, in this embodiment, the slag discharge rate after the first blowing step is preferably at least 40 mass% or more, and more preferably 60 mass% or more. Here, the slag discharge rate (mass%) is the percentage obtained by dividing the mass of the discharged slag by the mass of the slag in the furnace at the end of the first blowing step. If the slag discharge rate is less than 40 mass%, the amount of lime-based solvent used in the dephosphorization treatment in the next step will increase as described above. Furthermore, if the amount of slag increases as a result, slag foaming cannot be suppressed, and slag will erupt from the furnace throat during the dephosphorization treatment, which may cause operational problems.

[0036] In this way, in the method for pre-treating molten pig iron according to the present embodiment, it is preferable that the temperature of the molten iron at the end of the first blowing process is set to 1240°C or more and 1400°C or less so that the basicity of the slag at the end of the first blowing process is within the range of 0.5 to 1.5. Furthermore, by optimizing the oxygen consumption rate to promote slag foaming, good slag fluidity and gas hold-up can be ensured. Then, a good slag removal rate can be obtained simply by tilting the furnace body after the end of the first blowing process to allow the slag to flow out of the furnace throat. When the tilting angle of the furnace body is adjusted so as not to allow the molten pig iron to flow out, a certain amount of slag must remain in the furnace. However, the volume ratio of the foamed slag is about 1 / 10, and the bulk density is lower than the true density. Therefore, the amount of slag remaining in the furnace can be controlled to be low. If the foaming of the slag subsides, the slag removal rate will decrease. Therefore, it is preferable to keep the time from the end of the first blowing step to the start of tilting the furnace body for slag removal within 4 minutes.

[0037] If the basicity of the slag at the end of the first blowing step required in the slag removal step is less than 0.5, the viscosity of the slag increases, and there is a risk that a good slag removal rate cannot be ensured. On the other hand, if the basicity of the slag at the end of the first blowing step exceeds 1.5, solid slag is generated, the fluidity of the slag decreases, and there is a risk that the slag removal rate decreases. Thus, from the viewpoint of ensuring the slag removal property and the slag removal rate, it is preferable to set the basicity of the slag to about 0.5 to 1.5. However, from the viewpoint of preventing rephosphorization from the slag in the first blowing step and reducing the amount of lime-based solvent used, it is more preferable to adjust the basicity of the slag to the range of 0.8 to 1.2.

[0038] In addition, slag foaming progresses due to fine CO bubbles generated by the reaction of the total iron (T.Fe) in the slag at the end of the first blowing process in the slag removal process, i.e., iron oxide and the iron particles containing carbon suspended in the molten iron or slag. In order to verify the appropriate (T.Fe) concentration range, a separate check was conducted and it was found that slag foaming was insufficient when the total iron (T.Fe) was less than 5 mass%. Therefore, the driving force when discharging the slag by tilting the converter was small, and sufficient discharge was difficult. On the other hand, when the total iron (T.Fe) exceeded 25 mass%, the generation of CO bubbles in the slag rapidly progressed and the bumping phenomenon was confirmed, so that the slag discharge work had to be interrupted. Thus, it is preferable that the appropriate range of the total iron (T.Fe) in the slag at the end of the first blowing process, i.e., in the slag removal process, is 5 to 25 mass%.

[0039] In addition, in the slag removal process, if the temperature of the slag at the end of the first blowing step is low, for example, below 1240°C, the slag viscosity increases due to the generation of solid slag and the viscosity of the liquid slag increases. This leads to a decrease in the fluidity of the slag and a decrease in the slag removal rate. Therefore, it is preferable to adjust the cold iron source consumption rate according to the initial conditions of the molten pig iron used, and to adjust at least one of the amount of heat source added, such as silicon carbide or ferrosilicon, and the oxygen consumption rate. By setting the molten iron temperature at the end of the first blowing step to 1240°C or higher, the slag temperature also becomes 1240°C or higher. It is more preferable to set the molten iron temperature to 1260°C or higher.

[0040] However, if all of the slag generated after the first blowing process is removed, the slag formation of the newly added lime-based flux in the next dephosphorization and decarburization process will be delayed. This will hinder the dephosphorization reaction. To address this issue, fluorite can be added to promote slag formation. However, as mentioned above, this will restrict the uses of the slag and hinder its utilization. There is also a method of promoting slag formation by adding iron oxide such as iron ore. However, this method involves a large heat loss due to the endothermic decomposition reaction of the iron oxide. As a result, the amount of heat available for melting the cold iron source will decrease, making it unwise.

[0041] Therefore, in order to promote slag formation of the lime-based flux without using fluorite or iron oxide in the dephosphorization and decarburization treatment stage, it is preferable to leave an appropriate amount of slag 10 with a preferable composition and temperature after the first blowing step in the furnace. It is effective to promote slag formation by using SiO2 and iron oxide in the slag. When discharging the slag after the first blowing step, it is preferable to discharge the slag after the first blowing step of 4 to 20 kg / t-molten pig iron by adjusting the tilt angle of the furnace body. A suitable slag discharge rate of 40 mass% or more, more preferably 60 mass% or more, can be maintained. This makes it possible to efficiently promote the dephosphorization reaction without using iron oxide in the second blowing step. And it becomes possible to indirectly utilize the reaction heat due to the decomposition endothermic heat of iron oxide as heat for melting the cold iron source in the first blowing step. In this regard, if the amount of slag remaining after the first blow is less than 4 kg / t-hot metal, it is necessary to use iron oxide to promote the slag formation of the lime-based flux in the second blow. On the other hand, if the amount of slag remaining exceeds 20 kg / t-hot metal, the amount of lime-based flux must be increased and the operation of the second blow may be hindered.

[0042] [Second blowing process] Next, the second blowing step (D) shown in FIG. 1(D) will be described. After the slag removal step (C), a lime-based flux is added to the molten pig iron 9 remaining in the same converter-type refining furnace 1, and oxygen is blown as a gaseous oxygen source to dephosphorize and decarburize the molten pig iron 9. In order to reduce heat loss, it is preferable to use only oxygen-containing gas 12 from the oxygen supply lance 2 as the oxygen source used in this second blowing step. It is preferable to inject bottom blown gas 13 from the bottom blowing tuyeres 3 for stirring. [P] in the molten pig iron is oxidized by oxygen in the supplied oxygen source to become phosphorus oxide (P2O5). This phosphorus oxide is stably incorporated into the slag generated by the slagification of the lime-based flux, and the dephosphorization of the molten pig iron progresses. In order to efficiently advance the dephosphorization reaction, it is preferable to add a lime-based flux so that the basicity of the slag after the second blowing step (slag 17 after the dephosphorization and decarburization treatment in the pretreatment) is 1.2 to 3.0, and to perform the second blowing step by supplying oxygen so that the temperature of the molten metal after the completion of the second blowing step is 1280° C. to 1360° C. More preferably, the basicity of the slag is 1.4 or more.

[0043] If the slag basicity of the dephosphorization and decarburization slag 17 generated in the second blowing process is less than 1.2 or the molten metal temperature exceeds 1360°C, the dephosphorization ability of the slag decreases, and the [P] concentration in the molten pig iron after the treatment may not be reduced sufficiently. On the other hand, if the slag basicity exceeds 3.0, it becomes difficult to turn the lime-based flux into slag, which may reduce the utilization efficiency of the lime-based flux and increase the cost. Even if the molten metal temperature is less than 1280°C, it becomes difficult to turn the lime-based flux into slag, which may reduce the dephosphorization ability and may cause a shortage of heat in the subsequent decarburization process. In order to ensure a sufficient amount of heat in the decarburization process, it is preferable to set the molten metal temperature after the second blowing process to 1280°C or more and 1360°C or less. At the same time, it is preferable to adjust the amount of oxygen used and the amount of carbon added in the first and second blowing steps so that the carbon concentration in the molten iron at the end of the second blowing step is 2.5 mass % or more.

[0044] In the operation according to the present embodiment, the [Si] concentration, [P] concentration, and molten metal temperature change, and there are cases where the molten metal temperature at the end of the first blowing process is low, or where the [P] concentration of the molten metal is high and the dephosphorization load is large. In such cases, in order to promote the dissolution of lime in the second blowing process, it is effective to blow powdered lime or a lime source such as calcium carbonate onto the molten metal surface using oxygen gas or inert gas from an oxygen supply lance or a separately installed lance. In the region where the molten metal surface is irradiated with top-blown oxygen, the temperature becomes high at about 2000°C due to direct decarburization reaction and iron oxidation, and the addition of a powdered lime source to this region promotes melting.

[0045] In the hot metal pretreatment method according to the present embodiment, SiO2-containing slag that contributes to the melting of lime is discharged after the first blowing step, so that early melting by blasting powdered lime source is effective. In addition, in this method, the oxidation heat of Si in the hot metal is utilized to promote the melting of the cold iron source. Therefore, in terms of the melting rate of scrap in the hot metal, operation at a higher temperature is preferable. However, in terms of preventing rephosphorization and promoting the dephosphorization reaction during the second blowing step, high-temperature treatment is rather disadvantageous. Therefore, in this embodiment, it is preferable to locally cool only the reaction region by the decomposition reaction (endothermic reaction) of iron oxide by simultaneously top-blowing powdered iron oxide into the region where the above-mentioned top-blown oxygen is injected. Then, it becomes possible to promote dephosphorization or suppress rephosphorization under macroscopically high temperature conditions. Here, the auxiliary materials containing lime and calcium carbonate may be not only each of them alone, but also recycled materials such as slag generated during converter decarburization blowing, etc. As for the iron oxide, not only simple substances such as iron ore but also recycled materials such as rolling scale, sintered ore powder, and collected dust may be used.

[0046] In this embodiment, in order to prevent the trouble of the oxygen jet scattering the iron nuggets, the oxygen collision pressure P C On the other hand, from the viewpoint of dephosphorization efficiency, the oxygen impingement pressure P CIt is preferable that the oxygen impingement pressure P is at least 9800 Pa. As described above, in the second blowing step, the slag remaining after the first blowing step is foaming at first, and the foaming subsides with the addition of a lime-based flux, and the oxygen jet from the top lance reaches the molten iron significantly. For example, when the ratio of the cumulative oxygen supply amount to the total oxygen supply amount in the second blowing step is in the range of less than 30%, the oxygen impingement pressure P C is in the range of 10800 to 11800 Pa, and when the cumulative oxygen supply amount is in the range of 30% to less than 70% of the total oxygen supply amount, the oxygen collision pressure P C In the remaining range of 14700 to 15700 Pa, the oxygen impingement pressure P C It is preferable that the oxygen flow rate in the second blowing process is in the range of 49,000 to 50,000 Pa. This range suppresses the occurrence of troubles such as the metal generated during blowing adhering to and falling onto the hood of the converter furnace, and makes refining economically advantageous. In addition, the [P] concentration in the molten pig iron can be stably reduced to a lower level than in the past. Also, the oxygen flow rate in the second blowing process is 2.2 to 2.6 Nm 3 / (min / t-molten iron) is preferable. The bottom blowing gas flow rate is 0.04~0.15Nm 3 / (min / t-hot metal) is preferred.

[0047] [Potting process] Next, the tapping step (E) shown in Fig. 1 (E) will be described. In this step (E), when the [P] concentration in the molten pig iron has decreased to a predetermined value through the second blowing step, the converter-type refining furnace 1 is tilted to the side where the tapping port is installed, and the molten pig iron in the converter-type refining furnace is tapped into a molten metal holding vessel (not shown). The predetermined [P] concentration is preferably 0.030 mass% or less. In the tapping step, it is preferable to leave 30 mass% or more of the slag after dephosphorization and decarburization treatment, in which the slag has a basicity of 1.2 or more, in the vessel.

[0048] As described above, in the method for pretreatment of molten iron according to the present embodiment, the oxygen impingement pressure P CBy appropriately controlling this, it is possible to prevent the occurrence of problems such as the metal generated during blowing adhering to and falling onto the hood of the converter equipment, and to realize preliminary treatment of molten iron that enables economical refining.

[0049] In addition, in this embodiment, the amount of lime-based flux added in the second blowing step can be minimized, which contributes to reducing the unit consumption of auxiliary materials in the entire molten iron refining process. EXAMPLES

[0050] Example 1 Figure 2 shows the blowing patterns according to the present invention. Figure 2(a) shows the blowing pattern for the first blowing step, and Figure 2(b) shows the blowing pattern for the second blowing step. Table 1 shows the values ​​of various blowing parameters at the blowing time (ratio of cumulative oxygen supply to total oxygen supply) according to this example. Additionally, the metallurgical properties and ingot attachment are evaluated and listed. The evaluation criteria are as follows: (1) Metallurgical properties (compared to conventional examples) The following evaluation was carried out to see whether the P concentration in the molten iron was worse than in the conventional example. 〇: Lower than the conventional molten iron [P] concentration △: The P concentration in the molten iron is equal to or lower than that of the conventional example. ×: Higher P concentration than conventional molten iron (2) With metal (compared to conventional examples) The following evaluation was carried out based on whether or not the metal adhered to the hood part of the converter equipment. Small: No metal ingots on the hood, no trouble with metal ingots Middle: Hood has metal ingots, but no problems with metal ingots. Large: Hood with metal ingots and problems with metal ingots

[0051] Figure 3 shows the blowing patterns of the conventional example. Figure 3(a) shows the blowing pattern of the first blowing process, and Figure 3(b) shows the blowing pattern of the second blowing process. Table 2 summarizes the values ​​of various blowing parameters at the blowing time (ratio of cumulative oxygen supply to total oxygen supply) of this conventional example. Additionally, the metallurgical properties and ingot attachment are evaluated and listed.

[0052] [Table 1]

[0053] [Table 2]

[0054] Figure 4 shows a comparison of the frequency of metal ingot trouble occurring in the hood of a converter furnace equipment between the invention example and the conventional example. In Figure 4, the frequency of metal ingot trouble occurring in the invention example is standardized to 1. The conventional example had metal ingot trouble 14 times more frequently than the invention example.

[0055] Example 2 Tables 3 and 4 show various blowing conditions, and also show the evaluation of metallurgical properties and ingot deposition. The results of operation under those blowing conditions are summarized below. In Tables 3 and 4, the cumulative oxygen supply rate / total oxygen supply rate (%) for Steps 1 to 4 and 5 to 8 are the same as in Tables 1 and 2. In the cases of No. 1 and No. 2, the oxygen impingement pressure in the second blowing process was within the optimum range and operation was possible without ingot adhesion. The [P] concentration in the molten iron was the same as or lower than that of the conventional case. Process No. 3 is an example of the invention in which the maximum oxygen impingement pressure in the second blowing process was increased within the preferred range compared to processes No. 1 and 2. Although there was some ingot adhesion to the hood, there were no ingot troubles. The [P] concentration in the molten iron was lower than in the conventional process. In the treatments No. 4 and 5, the second blowing step was in the suitable range, and the oxygen impingement pressure P C This is an example of the invention in which excessive foaming occurred due to the high concentration of phosphorus. Although there was some metal ingot on the hood, there were no metal troubles. The phosphorus concentration in the molten iron was the same as or lower than the conventional level. Treatment No. 6 is the oxygen impingement pressure P C This is a comparative example in which the P concentration in the molten iron was higher than in the past, causing frequent problems with ingot adhesion. In the case of No. 7, the second blowing process was in the optimum range, there was no hood ingot adhesion, and it was the most economical operation of the hot metal pretreatment. The [P] concentration in the hot metal was lower than the conventional one. In the treatment No. 8, the oxygen impingement pressure P C There was no hood ingot attached, and the P concentration in the molten iron was the same as or lower than that of the conventional method. In the treatment No. 9, the oxygen impingement pressure P C is low, and the oxygen impingement pressure P C In this example, the concentration of [P] in the molten iron was the same as in the conventional case or was lower than that in the conventional case. In the treatment No. 10, the oxygen impingement pressure P C This is an example of the invention in which the dephosphorization efficiency was low and the treatment time was extended. There was no hood ingot attached, and the [P] concentration in the molten iron was the same as or lower than the conventional example.

[0056] [Table 3]

[0057] [Table 4] [Explanation of symbols]

[0058] 1 Converter-type refining furnace 2 Oxygen supply lance (top blowing lance) 3 Bottom-blown tuyere 4. Tap hole 9. Molten Iron 9a Hot metal 10 (After desiliconization and dephosphorization, after the first blowing process) Slag 11 Cold Iron Source 12 Oxygen-containing gases (gaseous oxygen sources) 13 Bottom blown gas 14 Charging pot 17 Slag after dephosphorization and decarburization (after the second blowing process)

Claims

1. a first blowing step in which a gaseous oxygen source is supplied from a top blowing lance to the molten iron in a converter-type refining furnace to desiliconize and dephosphorize the molten iron; a slag removal step of removing at least a portion of the slag generated in the first blowing step from the converter-type refining furnace; a second blowing step of adding a CaO-based flux into the converter-type refining furnace after the slag removal step, and supplying a gaseous oxygen source from the top blowing lance to dephosphorize and decarburize the remaining molten iron, In the second blowing step, when a gaseous oxygen source is supplied from the top blowing lance to the molten iron bath surface, the oxygen impingement pressure P is calculated by the following formulas (1) to (3): C The method for pre-treatment of molten iron comprises blowing the mixture at a pressure of 58,800 Pa or less. P C = ρ V 2 / 2 (1) V / (V 0 -V loss ) = d e / (2・C・Z) (2) C=0.016+18600 / (P 0 -P e ) (3) Here, P C : Oxygen impingement pressure on the bath surface (Pa), ρ: gas density of the gaseous oxygen source (1.43 kg / m 3 ), V: central flow velocity of the gaseous oxygen source (m / s), V 0 : nozzle outlet jet velocity (m / s), V loss : Flow velocity loss due to improper expansion (m / s), d e :Nozzle outlet diameter (m), C: constant, Z: lance height (m), P 0 : nozzle absolute pressure (Pa), P e : Atmospheric pressure (Pa) Represents.

2. In the second blowing step, when the cumulative oxygen supply amount from the start of blowing is less than 30% of the total oxygen supply amount, the oxygen collision pressure P C is in the range of 10800 to 11800 Pa, and when the cumulative oxygen supply amount is in the range of 30% or more and less than 70% of the total oxygen supply amount, the oxygen collision pressure P C is in the range of 14700 to 15700 Pa, and in the remaining range where the cumulative oxygen supply amount is 70% or more of the total oxygen supply amount, the oxygen collision pressure P C The method for pre-treating molten iron according to claim 1, wherein the pressure is in the range of 49,000 to 50,000 Pa.

Citation Information

Patent Citations

  • Method for preliminary treatment of molten iron

    JP2013189714A

  • Dephosphorization processing method for changing top-blown condition in converter type vessel

    JP2015140462A

  • Refining method of molten iron

    JP2017052976A

  • Dephosphorization method of molten pig iron excellent in dephosphorization efficiency

    JP2017226874A

  • Preliminary processing method for molten iron

    WO2014115526A1