Metal base material with adhesive and laminate
The laminate configuration with a smooth copper foil, specific adhesive resin layer, and prepreg layer addresses the skin effect and adhesive strength issues, enhancing transmission characteristics and preventing peeling in high-frequency applications.
Patent Information
- Application Number
- JP2024034981
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-11
AI Technical Summary
In high-frequency transmission, the skin effect causes increased transmission loss due to non-smooth metal wiring surfaces, and this leads to reduced adhesive strength between resin and metal layers, increasing the risk of circuit peeling.
A laminate configuration using a copper foil with a surface roughness of 1.0 μm or less, an adhesive resin layer composed of a specific polyimide resin and maleimide compound with a radical initiator, and a prepreg layer, with thickness ratios optimized to ensure adhesive strength and low dielectric properties.
The solution provides excellent transmission characteristics and sufficient adhesive strength between resin and metal layers, reducing transmission loss and preventing peeling, while maintaining low dielectric properties in high-frequency bands.
Smart Images

Figure 2024144195000011 
Figure 2024144195000012 
Figure 2024144195000013
Abstract
Description
[Technical field]
[0001] The present invention relates to adhesive-backed metal substrates and laminates. [Background technology]
[0002] Copper clad laminates (hereinafter sometimes referred to as "CCL"), which are used for transmitting high-frequency signals, are manufactured by laminating copper foil and resin layers. In recent years, with the increasing speed of transmitted signals, further improvement in the transmission characteristics of CCL is required.
[0003] For example, Patent Document 1 discloses a laminate in which a resin substrate and a metal substrate are laminated with an adhesive layer interposed therebetween. The adhesive layer of the laminate disclosed in Patent Document 1 is in a low frequency band relative to the 5G frequency band, but has a relative dielectric constant of 3.0 or less and a dielectric loss tangent of 0.02 or less at a frequency of 1 MHz. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-3886 Summary of the Invention [Problem to be solved by the invention]
[0005] In high-frequency transmission, the current tends to flow only on the surface of the metal wiring as the frequency band increases. Therefore, if the surface shape is not smooth, the transmission loss increases. This is a well-known phenomenon called the skin effect. To reduce the transmission loss due to the skin effect, for example, there is a tendency to use metal foil with a small surface roughness for metal substrates.
[0006] The lower the surface roughness of the metal foil, the less the anchoring effect is achieved, and the lower the adhesion between the resin substrate and the metal foil. In this case, there is a problem that the circuit of the printed circuit board is easily peeled off.
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide an adhesive-backed metal substrate and laminate that have excellent transmission characteristics and can ensure sufficient adhesive strength between a resin substrate and a metal layer. [Means for solving the problem]
[0008] That is, the present invention employs the following configuration. [1] An adhesive-bonded metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, the adhesive resin composition comprising a polyimide resin (A), a maleimide compound (B) and a radical initiator, the weight ratio of the polyimide resin (A) to the maleimide compound (B) being 10:1 to 3:2, the content of the radical initiator relative to 100 parts by mass of the maleimide compound (B) being 1 part by mass or more and less than 25 parts by mass, and the adhesive resin layer having a thickness of 0.1 μm or more and 10 μm or less. [2] The adhesive-backed metal substrate according to [1], wherein the metal layer is a copper foil having a surface roughness Rzjis of 1.0 μm or less. [3] A laminate comprising an adhesive-backed metal substrate according to [1] or [2] on both sides of a prepreg, the prepreg being laminated on a side of the adhesive-backed metal substrate opposite to a side on which the adhesive resin layer of the adhesive-backed metal substrate is in contact with the metal layer, the prepreg being one or more types selected from the group consisting of modified polyimide resin prepregs, polyester resin prepregs, liquid crystal polymer prepregs, cyclic olefin resin prepregs, polyphenylene ether resin prepregs, polyphenylene sulfide resin prepregs, polyether ether ketone resin prepregs, bismaleimide resin prepregs, triazine resin prepregs, bismaleimide-triazine resin prepregs, benzocyclobutene resin prepregs and low dielectric epoxy resin prepregs. [4] The laminate according to [3], wherein the adhesive resin layer has a thickness of 0.1 μm or more and 10 μm or less, the prepreg has a thickness of 50 μm or more and 1000 μm or less, and the metal layer has a thickness of 1 μm or more and 35 μm or less, and the following formula (1) is satisfied: 0.05≦(X / Y)×100≦7 (1) [In (1), X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg.] Effect of the Invention
[0009] According to the present invention, it is possible to provide an adhesive-attached metal substrate and a laminate which have excellent transmission characteristics and can ensure sufficient adhesive strength between a resin substrate and a metal layer. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view of an example of an adhesive-backed metal substrate according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an example of a laminate according to the present embodiment. [Diagram 3] FIG. 13 is a graph showing the results of measuring the transmission loss (dB / 100 mm) of the laminates of Example 11, Comparative Example 11, and Comparative Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Metal substrate with adhesive> 1 is a schematic diagram showing a cross section of an adhesive-coated metal substrate 1 of this embodiment. The adhesive-coated metal substrate 1 comprises a metal layer 10 and an adhesive resin layer 11.
[0012] A rigid substrate for high-speed transmission can be manufactured by combining the adhesive-backed metal substrate 1 with any low-dielectric substrate and thermally laminating them. For example, when a prepreg using a polyphenylene ether resin is used as the low dielectric substrate, a rigid substrate can be manufactured.
[0013] (metal layer 10) Any known conductive material that can be used for a circuit board can be used for the metal layer 10. Specifically, metal materials such as SUS, copper, aluminum, iron, steel, zinc, nickel, etc., and alloys of the above metal materials. The metal layer 10 is preferably a metal foil, more preferably a copper foil.
[0014] When the metal layer 10 is a copper foil, a rolled copper foil or an electrolytic copper foil can be used.
[0015] Furthermore, the material of the copper foil may be pure copper or a copper alloy in which a small amount of tin (Sn) or silver (Ag) is added to pure copper.
[0016] The metal layer 10 is a metal foil having a surface roughness of 1.5 μm or less, preferably 1.4 μm or less, particularly preferably 1.3 μm or less, and most preferably 1.0 μm or less. The metal layer 10 is preferably a copper foil having a surface roughness of 1.5 μm or less, more preferably a copper foil having a surface roughness of 1.4 μm or less, particularly preferably a copper foil having a surface roughness of 1.3 μm or less, and most preferably a copper foil having a surface roughness of 1.0 μm or less.
[0017] In this specification, the surface roughness means the ten-point average roughness (Rzjis). The surface roughness of a metal foil, for example a copper foil, can be measured using a surface roughness measuring instrument manufactured by Tokyo Seimitsu Co., Ltd., product name: SURFCOM1900DX.
[0018] The thickness of the metal layer 10 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the metal layer 10 is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. The above upper and lower limits for the thickness of the metal layer 10 can be combined in any desired manner. Examples of combinations include a thickness of the metal layer 10 of 5 μm or more and 50 μm or less, 10 μm or more and 45 μm or less, and 15 μm or more and 40 μm or less.
[0019] (Adhesive resin layer 11) The adhesive resin layer 11 is formed from an adhesive resin composition described below. According to the adhesive-backed metal substrate 1, the metal layer 10 can be bonded to any low dielectric substrate via the adhesive resin layer 11. The thickness of the adhesive resin layer 11 provided on the adhesive-coated metal substrate 1 is 0.2 μm to 9 μm, preferably 0.5 μm to 9 μm, more preferably 0.6 μm to 8 μm, and even more preferably 0.7 μm to 7 μm.
[0020] When the thickness of the adhesive resin layer 11 is equal to or greater than the above lower limit, the metal layer 10 and the low dielectric substrate can be bonded to each other. When the thickness of the adhesive resin layer 11 is equal to or less than the above upper limit, the adhesive resin layer 11 has a low residual solvent ratio, and delamination due to volatile gases during the heating step is less likely to occur.
[0021] (Adhesive resin composition) The adhesive resin composition for forming the adhesive resin layer 11 will be described. In this embodiment, by forming an adhesive resin layer 11 using a specific adhesive resin composition, it is possible to provide an adhesive-coated metal substrate and a laminate that can exhibit low dielectric properties in the high frequency range of 10 GHz, which is a frequency band of 6 GHz or higher assuming 5G.
[0022] The specific adhesive resin composition described below has a specific content of the maleimide compound, which is one component of the precursor of the polyimide resin (A), and is therefore considered to provide a low dielectric property in the high frequency range of the resulting adhesive resin layer 11. The maleimide group of the maleimide compound maintains a cyclic structure even after crosslinking, and crosslinking between maleimide groups results in a symmetrical structure. In this case, molecular motion is easily suppressed, and it is considered that the resulting adhesive resin layer 11 provides a low dielectric property in the high frequency range.
[0023] The adhesive resin composition contains a polyimide resin (A), a maleimide compound (B), and a radical initiator. As the adhesive resin composition, the resin composition disclosed in WO 2022 / 004583 can be used. The details are described below.
[0024] [Polyimide resin (A)] The polyimide resin (A) is an isocyanate-modified polyimide resin (A1) or a terminal-modified isocyanate-modified polyimide resin (A2). The isocyanate-modified polyimide resin (A1) is referred to as "polyimide resin (A1)", and the terminal-modified isocyanate-modified polyimide resin (A2) is referred to as "polyimide resin (A2)".
[0025] Polyimide resin (A1) The polyimide resin (A1) is obtained by reacting a diisocyanate compound (a) with an intermediate polyimide resin. The diisocyanate compound (a) is referred to as "component (a)".
[0026] The intermediate polyimide resin is a reaction product of the following components (b), (c), and (d). (b) Component: Aliphatic diamino compound (b) (c) Component: Tetrabasic acid dianhydride (c) (d) Component: Aromatic diamino compound (d)
[0027] The polyimide resin (A1) is a reaction product of either or both of an amino group and an acid anhydride group present at both ends of the intermediate polyimide resin with an isocyanate group present in the component (a).
[0028] The reaction between the intermediate polyimide resin and component (a) is a copolymerization reaction between an amino group or an acid anhydride group at the terminal of the intermediate polyimide resin and an isocyanate group in component (a). In other words, a urea bond is formed by the reaction between an amino group and an isocyanate group, and an imide bond is formed by the reaction between an acid anhydride and an isocyanate group.
[0029] The amount of component (a) used in the copolymerization reaction between the intermediate polyimide resin and component (a) is preferably less than 1 equivalent of the isocyanate group of component (a) relative to 1 equivalent of the terminal functional group of the intermediate polyimide resin, more preferably 0.50 to 0.99 equivalents, and even more preferably 0.67 to 0.98 equivalents.
[0030] By using the component (a) in the above-mentioned range relative to the intermediate polyimide resin, the polyimide resin (A1) can be sufficiently polymerized, and the residual rate of unreacted raw materials can be reduced, improving various properties such as heat resistance and flexibility after curing of the adhesive resin composition.
[0031] The terminal functional equivalent of the intermediate polyimide resin herein means a value calculated from the amounts of each raw material used in synthesizing the intermediate polyimide resin.
[0032] The component (a) used in the synthesis of the polyimide resin (A1) can be any compound having two isocyanate groups in the molecule, and a plurality of diisocyanate compounds can be reacted simultaneously.
[0033] As the (a) component, phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tetramethyl xylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, tridenediisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, allylene sulfone ether diisocyanate, allylcyanate diisocyanate, N-acyl diisocyanate, trimethylhexamethylene diisocyanate, 1,3-bis(isocyanate methyl)cyclohexane or norbornane-diisocyanate methyl is preferred. Among them, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate or isophorone diisocyanate, which are excellent in balance of flexibility, adhesiveness, etc., are more preferred.
[0034] The reaction between the intermediate polyimide resin and the component (a) may be carried out by a known synthesis method. Specifically, the polyimide resin (A1) can be obtained by adding the component (a) to an intermediate polyimide resin solution obtained by the synthesis method described below, and heating and stirring at a temperature of 80° C. or higher and 150° C. or lower.
[0035] The reaction time for the synthesis reaction of the intermediate polyimide resin and the reaction of the intermediate polyimide resin with component (a) is greatly affected by the reaction temperature. It is preferable to carry out the reaction until the increase in viscosity accompanying the progress of the reaction reaches equilibrium and the maximum molecular weight is obtained, which is usually several tens of minutes to 10 hours.
[0036] The isocyanate-modified polyimide resin solution obtained above can be poured into a poor solvent such as water, methanol, or hexane to separate the produced polymer, and then a solid content of the polyimide resin (A1) can be obtained by a reprecipitation method.
[0037] Polyimide resin (A2) The polyimide resin (A2) has either or both of an amino group and an acid anhydride group at both ends, and therefore, the ends can be modified by reacting it with a compound having one functional group capable of reacting with these functional groups to prepare a terminally modified isocyanate-modified polyimide resin, i.e., the polyimide resin (A2).
[0038] Examples of the compound capable of reacting with either or both of an amino group and an acid anhydride group include a compound having an acid anhydride group such as maleic anhydride, a compound having an alcoholic hydroxyl group such as hydroxyethyl acrylate, a compound having a phenolic hydroxyl group such as phenol, a compound having an isocyanate group such as 2-methacryloyloxyethyl isocyanate, and a compound having an epoxy group such as glycidyl methacrylate.
[0039] By modifying the terminals, both terminals of the isocyanate compound of the present invention can be changed to functional groups other than amino groups and acid anhydride groups (for example, when terminal modification is performed with hydroxyethyl acrylate, the terminals of the isocyanate-modified polyimide resin can be changed to acryloyl groups), so it is also possible to prepare a composition in which the compound is combined with a compound that reacts with functional groups other than amino groups or acid anhydride groups.
[0040] ··Intermediate polyimide resin The intermediate polyimide resin is a reaction product of the above-described components (b), (c), and (d). The reaction of components (b), (c), and (d) includes a step of obtaining a polyamic acid by a copolymerization reaction between the amino groups in components (b) and (d) and the acid anhydride groups in component (c), and a step of obtaining an intermediate polyimide resin by a dehydration cyclization reaction (imidization reaction) of the polyamic acid. These two steps may be carried out separately, but it is more efficient to carry them out continuously in one batch.
[0041] When the number of moles of component (b) used in the copolymerization reaction is MB, the number of moles of component (c) is MC, and the number of moles of component (d) is MD, if the relationship MB + MD > MC is satisfied, both ends of the obtained intermediate polyimide resin will be amino groups; if the relationship MB + MD < MC is satisfied, both ends of the obtained intermediate polyimide resin will be acid anhydride groups.
[0042] Also, when the relationship MB + MD = MC is satisfied, the theoretically obtained intermediate polyimide resin will have an infinite molecular weight and will have one amino group and one acid anhydride group at both ends.
[0043] An example of the amount of component (b) used in the copolymerization reaction is an amount in the range of 10% by mass or more and 50% by mass or less of the mass obtained by subtracting the mass of water generated in the dehydration cyclization reaction step during the synthesis of the intermediate polyimide resin from the total mass of components (b), (c), (d) used in the synthesis step of the intermediate polyimide resin and component (a) used in the synthesis step of the above-described polyimide resin (A1) (this mass is substantially equal to the mass of the finally obtained isocyanate-modified polyimide resin).
[0044] If the amount of component (b) is below the above range, the proportion of the aliphatic chain derived from component (b) in the intermediate polyimide resin will be too small, resulting in high relative permittivity and dielectric loss tangent. If it exceeds the above range, the proportion of the aliphatic chain derived from component (b) in the intermediate polyimide resin will be too large, leading to a decrease in the heat resistance of the cured product.
[0045] The component (b) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aliphatic compound having two amino groups in one molecule, but an aliphatic diamino compound having 6 to 36 carbon atoms is preferred.
[0046] Specific examples of the component (b) include hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, C14 branched diamine, C18 branched diamine, dimer diamine, and diaminopolysiloxane, etc. These may be used alone or in combination of two or more.
[0047] The dimer diamine described as a specific example of component (b) in this specification is a dimer acid, which is a dimer of an unsaturated fatty acid such as oleic acid, in which the two carboxy groups of the dimer acid are substituted with primary amino groups (see, for example, JP-A-9-12712).
[0048] Specific examples of commercially available dimer diamines include PRIAMINE 1074 and PRIAMINE 1075 (both manufactured by Croda Japan Co., Ltd.), and Versamine 551 (manufactured by Cognis Japan Co., Ltd.) These may be used alone or in combination of two or more.
[0049] The component (c) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it has two acid anhydride groups in one molecule.
[0050] Specific examples of component (c) include pyromellitic anhydride, ethylene glycol bis(anhydrotrimellitate), glycerin bis(anhydrotrimellitate) monoacetate, 1,2,3,4-butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3 -methylcyclohexene-1,2-dicarboxylic acid anhydride, 3a,4,5,9b-tetrahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-1,3-dione, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, bicyclo(2,2,2)-oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic acid dianhydride, 5,5'-((propane-2,2-diylbis(4,1-phenylene))bis(oxy))bis(isobenzofuran-1,3-dione), and the like.
[0051] Among these, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, or 3,3',4,4'-diphenylethertetracarboxylic dianhydride are preferred from the viewpoints of solvent solubility, adhesion to a substrate, and photosensitivity. These may be used alone or in combination of two or more.
[0052] The component (c) used in the synthesis of the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following formulas (1) to (4).
[0053] [ka]
[0054] In formula (4), Y represents C(CF3)2, SO2, CO, O, a direct bond, or a divalent linking group represented by the following formula (5): The two linking moieties represented by formula (5) are each a moiety that bonds to phthalic anhydride.
[0055] [ka]
[0056] The component (d) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aromatic compound having two amino groups in one molecule.
[0057] Specific examples of component (d) include m-phenylenediamine, p-phenylenediamine, m-tolylenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl thioether, 3,3'-dimethyl-4,4'-diaminodiphenyl thioether, 3,3'-diethoxy-4,4'-diaminodiphenyl thioether, and 3,3 '-Diaminodiphenylthioether, 4,4'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-dimethoxy-4,4'-diaminodiphenylthioether, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(4-aminophenyl)propane, 4,4'-diamino Diphenyl sulfoxide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, benzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 3,3'-diaminobiphenyl, p-xylylenediamine, m-xylylenediamine, o-xylylenediamine, 2,2'-bis(3-aminophenoxyphenyl)propane, 2,2'-bis(4-aminophenoxyphenyl)propane, 1,3-bis(4 bis(4-aminophenoxyphenyl)benzene, 1,3'-bis(3-aminophenoxyphenyl)propane, bis(4-amino-3-methylphenyl)methane, bis(4-amino-3,5-dimethylphenyl)methane, bis(4-amino-3-ethylphenyl)methane, bis(4-amino-3,5-diethylphenyl)methane, bis(4-amino-3-propylphenyl)methane, and bis(4-amino-3,5-dipropylphenyl)methane. These may be used alone or in combination of two or more.
[0058] The component (d) used in the synthesis of the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following formulas (6) and (8).
[0059] [ka]
[0060] In formula (6), R 1 represents a methyl group or a trifluoromethyl group, and in formula (8), Z represents CH(CH3), SO2, CH2, O-C6H4-O, O, a direct bond, or a divalent linking group represented by formula (5), R 3 represents a hydrogen atom, a methyl group, an ethyl group, or a trifluoromethyl group. The two linking moieties represented by formula (5) are each a moiety that bonds to phthalic anhydride.
[0061] The intermediate polyimide resin can be synthesized by a known method. For example, a solvent, a dehydrating agent, and a catalyst are added to a mixture of the components (b) to (d) used in the synthesis, and the mixture is heated and stirred at 100 to 300°C under an inert gas atmosphere such as nitrogen, whereby an imidization reaction (a ring-closing reaction accompanied by dehydration) occurs via the polyamic acid, and an intermediate polyimide resin solution is obtained. At this time, water generated during the imidization is distilled out of the system, and after the reaction is completed, the dehydrating agent and catalyst are also distilled out of the system, making it possible to obtain a highly pure intermediate polyimide resin without the need for washing. Examples of dehydrating agents include toluene and xylene, and examples of catalysts include pyridine and triethylamine.
[0062] Solvents that can be used in the synthesis of the intermediate polyimide resin include methyl ethyl ketone, methyl propyl ketone, methyl isopropyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl n-hexyl ketone, diethyl ketone, diisopropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, acetylacetone, γ-butyrolactone, diacetone alcohol, cyclohexen-1-one, dipropyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, tetrahydropyran, ethyl isoamyl ether, ethyl-t-butyl ether, ethyl benzyl ether, cresyl methyl ether, anisole, phenetole, methyl acetate, ethyl acetate, propyl acetate, isoacetate, and the like. Propyl acetate, butyl acetate, isobutyl acetate, amyl acetate, isoamyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, benzyl acetate, methyl acetoacetate, ethyl acetoacetate, methyl propionate, ethyl propionate, butyl propionate, benzyl propionate, methyl butyrate, ethyl butyrate, isopropyl butyrate, butyl butyrate, isoamyl butyrate, methyl lactate, ethyl lactate, butyl lactate, ethyl isovalerate, isoamyl isovalerate, diethyl oxalate, dibutyl oxalate, methyl benzoate, ethyl benzoate, propyl benzoate, methyl salicylate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc. may be mentioned, but are not limited thereto. These may be used alone or in a mixture of two or more.
[0063] [Maleimide compound (B)] The compound having a maleimide group is not particularly limited as long as it is a compound having one or more maleimide groups in one molecule, but a compound having two or more maleimide groups in one molecule is preferred, and examples thereof include polyfunctional maleimide compounds obtained by reacting 3,4,4'-triaminodiphenylmethane, triaminophenol, or the like with maleic anhydride, maleimide compounds obtained by reacting tris-(4-aminophenyl)-phosphate, tris(4-aminophenyl)-phosphate, or tos(4-aminophenyl)-thiophosphate with maleic anhydride, trismaleimide compounds such as tris(4-maleimidophenyl)methane, bis(3,4-dimaleimidophenyl)methane, tetrahydrofuran ... Examples of the maleimide compounds include tetramaleimide compounds such as tramaleimide benzophenone, tetramaleimide naphthalene, and maleimide obtained by reacting triethylenetetramine with maleic anhydride, phenol novolac type maleimide resins, isopropylidenebis(phenoxyphenylmaleimide)phenylmaleimide aralkyl resins, and biphenylene type phenylmaleimide aralkyl resins. Commercially available products include MIR-3000, MIR-5000 (all manufactured by Nippon Kayaku Co., Ltd.), BMI-70, BMI-80 (all manufactured by K.I. Kasei Co., Ltd.), BMI-1000, BMI-2000, and BMI-3000 (all manufactured by Daiwa Kasei Kogyo Co., Ltd.).
[0064] Since a compound having a maleimide group undergoes self-crosslinking between itself due to the action of a radical initiator, a resin composition using an isocyanate-modified polyimide resin having an amino group at its terminal, a compound having a maleimide group, and a radical initiator becomes a cured product in which the maleimide groups self-crosslink when heated and the polyimide resin and the maleimide resin are copolymerized.
[0065] [Radical initiator] Radical initiators that can be used for self-crosslinking between maleimide groups include peroxides such as dicumyl peroxide and dibutyl peroxide, and azo compounds such as 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0066] In the adhesive resin composition used in this embodiment, the weight ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2, and preferably 7:1 to 5:2. When the weight ratio of the polyimide resin (A) to the maleimide compound (B) is within the above range, the adhesive-coated metal substrate or laminate has low dielectric properties in the high frequency range. In addition, the adhesive is easy to adhere to even metal foils with a low surface roughness of 1.5 μm or less, and is easy to exhibit high adhesive strength.
[0067] In the adhesive resin composition used in this embodiment, the content of the radical initiator relative to 100 parts by mass of the maleimide compound (B) is 1 part by mass or more and less than 25 parts by mass, and preferably 5 parts by mass or more and 20 parts by mass or less. When the content of the radical initiator satisfies the above range, the adhesive-coated metal substrate or laminate can ensure sufficient adhesive strength between the resin film and the metal layer. In particular, it is easy to adhere to metal foils with a low surface roughness of 1.5 μm or less, and is easy to exhibit high adhesive strength.
[0068] The adhesive resin composition may contain an organic solvent. Specific examples of the organic solvent include amide-based solvents such as γ-butyrolactones, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone; sulfones such as tetramethylene sulfone; ether-based solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate, and propylene glycol monobutyl ether; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; and aromatic solvents such as toluene and xylene.
[0069] The organic solvent is preferably used in such a proportion that the solids concentration in the adhesive resin composition excluding the organic solvent is generally 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 70% by mass or less.
[0070] The adhesive resin composition can be produced by adding a base material containing the polyimide resin (A) and the maleimide compound (B) to an organic solvent, and further adding a radical initiator.
[0071] <Laminate> The laminate of the present embodiment includes the adhesive-backed metal substrate of the present embodiment on both sides of a prepreg. 2 is a schematic diagram of a cross section of a laminate 2 of this embodiment. The laminate 2 includes adhesive-coated metal substrates 1 on both sides of a prepreg 12. The prepreg 12 is laminated on a surface 11 a of the adhesive-coated metal substrate 1 opposite to the surface of the adhesive resin layer 11 that is in contact with the metal layer 10 . That is, the laminate 2 is formed by laminating the metal layer 10 / the adhesive resin layer 11 / the prepreg 12 / the adhesive resin layer 11 / the metal layer 10 in this order.
[0072] (Prepreg) The prepreg 12 is preferably one or more selected from the group consisting of modified polyimide resin prepreg, polyester resin prepreg, liquid crystal polymer prepreg, cyclic olefin resin prepreg, polyphenylene ether resin prepreg, polyphenylene sulfide resin prepreg, polyether ether ketone resin prepreg, bismaleimide resin prepreg, triazine resin prepreg, bismaleimide-triazine resin prepreg, benzocyclobutene resin prepreg, and low dielectric epoxy resin prepreg.
[0073] An example of the laminate 2 is a copper clad laminate.
[0074] In the laminate 2, the adhesive resin layer 11 preferably has a thickness of 0.2 μm or more and 9 μm or less, the metal layer 10 preferably has a thickness of 1 μm or more and 35 μm or less, and the prepreg preferably has a thickness of 50 μm or more and 1000 μm or less.
[0075] It is preferable that the laminate 2 satisfies formula (1). 0.01≦(X / Y)×100≦7 (1) [In (1), X is the thickness of the adhesive resin layer (μm), and Y is the thickness of the prepreg (μm).]
[0076] The above (1) is preferably any one of the following (1)-1 to (1)-3. 0.05≦(X / Y)×100≦7 ···(1)-1 0.2≦(X / Y)×100≦6.5 ···(1)-2 0.4≦(X / Y)×100≦6 ···(1)-3 EXAMPLES
[0077] The present invention will be explained more specifically below with reference to examples, but the present invention is not limited to these examples.
[0078] <Preparation of Adhesive Resin Composition> ≪Material≫ The polyimide resin (A) and the maleimide compound (B) were mixed in a ratio of polyimide resin (A):maleimide compound (B)=4:1 and used. The radical initiator used was dicumyl peroxide (Sigma-Aldrich). Anisole was used as the solvent.
[0079] ≪Preparation≫ The base material was mixed with a solvent so that the weight ratio of the polyimide resin (A) to the maleimide compound (B) was 4:1, and the base material was dissolved. Further, 17 parts by mass of dicumyl peroxide was added to 100 parts by mass of the maleimide compound (B), and the mixture was diluted with an organic solvent (anisole:toluene=9:1) to prepare an adhesive resin composition 1 with an adjusted solid content concentration. The solid content concentration was adjusted to the following concentrations depending on the thickness of the adhesive resin layer. Adhesive resin layer thickness of 1 to 6 μm: The solid content was adjusted to 11% by mass and applied using a bar coater. Adhesive resin layer thickness exceeds 10 μm: Adjust the solid concentration to 11% by mass and apply using an applicator. Adhesive resin layer thickness less than 0.1 μm: Adjust the solid concentration to 1% by mass and apply using a bar coater.
[0080] <Production of adhesive-coated metal substrate> Example 1 Adhesive resin composition 1 was applied to an electrolytic copper foil (Fukuda Metal Foil & Powder Co., Ltd., CF-T9DA-SV) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm using an applicator or a bar coater. The amount of coating was set so that the adhesive resin layer after drying had a thickness of 6 μm. After coating, the coating was dried at 140° C. for 1 minute until the residual solvent ratio became 1%, thereby producing an adhesive-coated metal substrate of Example 1.
[0081] <Examples 2 to 6, Comparative Examples 1 to 2> Adhesive-coated metal substrates of Examples 2 to 6 and Comparative Examples 1 and 2 were produced in the same manner as in Example 1, except that the thickness of the adhesive resin layer was changed to the thickness shown in Table 1A below.
[0082] [Table 1A]
[0083] <Processability evaluation> The processability was evaluated based on the residual solvent rate and the processing speed.
[0084] <Residual solvent rate> Adhesive resin layers having the same thickness as those in Examples 1 and 3 and Comparative Example 1 were formed on polyimide sheets and dried at 120° C. for 10 minutes, after which the residual rate of organic solvent was measured. For the measurement, TG / DTA was used. The results are shown in Table 1A. As shown in Table 1A, Comparative Example 1, in which the adhesive resin layer had a thickness of 10 μm, had a high residual solvent ratio of 0.85%. If the residual solvent ratio is high, gas will evaporate from the adhesive resin layer during the heating process, causing delamination. On the other hand, it was found that in Examples 1 and 3 in which the adhesive resin layer had a thickness of 3 μm or 6 μm, the residual solvent rate was low and the possibility of delamination due to gas generation was low.
[0085] ≪Processing speed≫ A coater test was conducted simulating the adhesive coating process when the copper foil was in a rolled state, and the processing speed was measured when the same residual solvent rate (0.7% or less) was achieved under the same drying conditions (drying oven (8 zones, 1 m each) set at 70 to 140°C). In order to reduce the residual solvent content, the drying conditions are not changed to a higher temperature or a longer time because this makes it difficult for the curing reaction to proceed. Therefore, when the residual solvent content of the adhesive resin layer to be formed is to be reduced, the processing speed is slowed down to perform drying. However, if the processing speed is too slow, this is not preferable because it reduces productivity. As shown in the results in Table 1B, if the adhesive resin layer is 1.5 μm to 6 μm thick, processing is possible at a processing speed of about 3 to 5 m / min, and productivity can be maintained. On the other hand, if the adhesive resin layer is 9 μm thick, the processing speed is 1 m / min, and there is a concern that productivity may decrease.
[0086] [Table 1B]
[0087] ≪Reference example 1≫ As Reference Example 1, an electrolytic copper foil (Fukuda Metal Foil & Powder Co., Ltd., CF-T9DA-SV) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm was used.
[0088] ≪Reference example 2≫ As Reference Example 2, an electrolytic copper foil (Fukuda Metal Foil & Powder Co., Ltd., CF-T9DA-SV) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm was used.
[0089] ≪Reference example 3≫ As Reference Example 3, an electrolytic copper foil (Mitsui Mining & Smelting, HS1-VSP) having a surface roughness Rzjis of 1.5 μm and a thickness of 18 μm was used.
[0090] <Production of Laminate> <Types of prepregs> Three types of polyphenylene ether resin prepregs were used. The polyphenylene ether resin prepregs are referred to as PPE-based prepregs.
[0091] (PPE prepreg) PPE prepreg 1: AGC Nelco, meteorwave4000, thickness: 110.3μm. PPE-based prepreg 2: Panasonic, MEGTRON6, thickness: 130.3μm. PPE prepreg 3: Panasonic, MEGTRON7, thickness: 140.5μm. PPE-based prepreg 4: A commercially available prepreg with a dielectric constant of 3.6 and a dielectric tangent of 0.0041 at 10 GHz, thickness: 100 μm.
[0092] On both sides of each prepreg, the adhesive-backed metal substrate of each of Examples 1 to 6 and Comparative Examples 1 and 2 was laminated in the following order: copper foil / adhesive resin layer / prepreg / adhesive resin layer / copper foil. When the metal base material of Reference Example 1 was used, the layers were laminated in the order of copper foil / prepreg copper foil. The lamination conditions differed depending on the type of prepreg, and lamination was performed under the conditions shown in Table 2 below.
[0093] [Table 2]
[0094] In this way, laminates 1A to 1I, 2A to 2I, and 3A to 3I were produced, respectively.
[0095] <Measurement of adhesive strength> For the resulting laminate, the adhesive strength between the copper foil and the prepreg was measured. The resulting laminate was cut to a width of 10 mm to obtain a test piece. The prepreg side was attached to a ring core with a diameter of 11 cm, and a 90° peel test was performed by pulling the copper foil portion at a speed of 50 mm / min. When the adhesive strength was 0.53 N / mm or more (3.0 lbs / inch or more) by this measurement, it was evaluated as “adequate adhesive strength is ensured.” The adhesive strengths of the produced laminates are shown in Table 2. As an index of adhesive strength between the prepreg and the metal layer, from the viewpoint of preventing peeling of the metal layer during the manufacturing process, an adhesive strength of 0.53 N / mm or more (3.0 lbs / inch or more) is required. For this reason, 0.53 N / mm or more (3.0 lbs / inch or more) was set as the pass value.
[0096] <Solder heat resistance> The manufactured laminate was left in a thermostatic chamber at 23°C and 50% humidity for 24 hours, and then floated in a solder bath at 288°C to measure the time until deformation or bubbling occurred and evaluate heat resistance. The results are shown in Table 2. If no deformation or bubbling occurred within 300 seconds, it was evaluated as passing.
[0097] <Measurement of dielectric properties> The copper foil was removed from each of the resulting laminates by etching to obtain a test piece (50 mm wide, 100 mm long) in which adhesive resin layer / prepreg / adhesive resin were laminated in this order. The obtained test pieces were dried at 135° C. for 1 hour to prepare dried test pieces. After drying, the test pieces were left to stand for 24 hours under conditions of 23° C. and 50% humidity to prepare humidity-conditioned test pieces, and the dielectric properties of each were measured.
[0098] The dielectric properties were measured by using a resonator manufactured by QWED Corporation and the relative dielectric constant and dielectric loss tangent were measured at a frequency of 10 GHz by the split post dielectric resonator method.
[0099] For laminates 1A to 1I, 2A to 2I, and 3A to 3I, the type of adhesive-backed metal base material, the type of prepreg, adhesive strength, solder heat resistance, X / Y (X is the thickness of the adhesive resin layer (μm), and Y is the thickness of the prepreg (μm)), and dielectric properties are shown in Tables 3 to 5, respectively.
[0100] [Table 3]
[0101] [Table 4]
[0102] [Table 5]
[0103] As shown in Tables 3 to 5, in each laminate, when Reference Example 1 was compared with each Example, the Examples had higher adhesive strength than Reference Example 1. In addition, when comparing each laminate between Example 1 and Comparative Example 1, the adhesive strength was equivalent. In Comparative Example 1, in which the adhesive resin layer had a thickness of 10 μm, delamination was a concern based on the evaluation results of the processing speed. Therefore, it was confirmed that the thickness of the adhesive resin layer is superior to that of the adhesive resin layer of 0.1 μm or more and 10 μm or less. In addition, when Example 1 and Comparative Example 2 were compared for each laminate, the adhesive strength of Comparative Example 2 was NG or lower than the Examples.
[0104] Furthermore, when the dielectric properties of the prepreg in the laminate are poorer than those of the adhesive resin, comparing the examples and comparative example 1, it is expected that the transmission loss of comparative example 1 will be better than that of the examples. However, when the dielectric properties of the prepreg are better than those of the adhesive resin, it is expected that the thicker the adhesive resin layer is, the greater the influence on the transmission loss will be. Therefore, taking other performance properties into consideration, it is preferable that the thickness of the adhesive resin layer be 10 μm or less.
[0105] In addition, when Example 1 and Reference Example 1 are compared, the adhesive strength of Reference Example 1 was evaluated as "NG" and the relative dielectric constant of the Examples was lower than that of Reference Example 1. Therefore, it was confirmed that the Examples were better in both adhesive strength and transmission characteristics than Reference Example 1.
[0106] <Measurement of transmission characteristics> The laminates of Example 11, Comparative Example 11 and Comparative Example 12 shown in Table 6 below were produced.
[0107] [Table 6]
[0108] The transmission loss (dB / 100 mm) was measured for the laminates of Example 11, Comparative Example 11, and Comparative Example 12 using the following device. The results are shown in FIG.
[0109] [Device] KEISIGHT TECHNOLOGIES 10MHz-67GHz: Network analyzer PNA Series N5227B 55GHZ-95GHz: Frequency extender for WR12 signal analyzer N9029AV12
[0110] 3, even at high frequencies, the transmission loss in Example 11 was smaller than those in Comparative Examples 12 and 13. Furthermore, as shown in Table 3, Example 11 also had high adhesive strength. On the other hand, in Comparative Example 11, since the surface roughness Rzjis was high at 1.5 μm, the adhesive strength was exhibited, but the transmission loss increased as the frequency increased. In Comparative Example 12, the surface roughness Rzjis was 0.85 μm, and therefore the transmission loss was smaller than that of Comparative Example 11, but the adhesive strength was low because no adhesive resin layer was provided. [Explanation of symbols]
[0111] 1: adhesive-coated metal substrate, 2: laminate, 10: metal layer, 11: adhesive resin layer, 12: prepreg
Claims
1. An adhesive-coated metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, The adhesive resin composition comprises a polyimide resin (A), a maleimide compound (B), and a radical initiator, the weight ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2; the content of the radical initiator relative to 100 parts by mass of the maleimide compound (B) is 1 part by mass or more and less than 25 parts by mass, The adhesive-coated metal substrate, wherein the adhesive resin layer has a thickness of 0.2 μm or more and 9 μm or less.
2. 2. The adhesive-backed metal substrate according to claim 1, wherein the metal layer is a copper foil having a surface roughness Rzjis of 1.0 μm or less.
3. A laminate comprising the adhesive-backed metal substrate according to claim 1 or 2 on both sides of a prepreg, The prepreg is laminated on a surface of the adhesive-bonded metal substrate opposite to a surface in contact with the metal layer, The prepreg is at least one type selected from the group consisting of modified polyimide resin prepregs, polyester resin prepregs, liquid crystal polymer prepregs, cyclic olefin resin prepregs, polyphenylene ether resin prepregs, polyphenylene sulfide resin prepregs, polyether ether ketone resin prepregs, bismaleimide resin prepregs, triazine resin prepregs, bismaleimide-triazine resin prepregs, benzocyclobutene resin prepregs, and low dielectric epoxy resin prepregs.
4. The adhesive resin layer has a thickness of 0.1 μm or more and 10 μm or less, The thickness of the prepreg is 50 μm or more and 1000 μm or less, The thickness of the metal layer is 1 μm or more and 35 μm or less, The laminate according to claim 3 , which satisfies the following formula (1): 0.05≦(X / Y)×100≦7...(1) [In (1), X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg.]
Citation Information
Patent Citations
Low dielectric fire-resistant adhesive composition