Method for precipitating polyvinyl alcohol-based resin

By controlling the mixing process of PVA resin with alcohol-based precipitates, the method produces fine PVA resin particles for efficient recovery, addressing the inefficiencies of existing methods and reducing collection costs.

JP2024144212APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024039084
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for recovering polyvinyl alcohol (PVA) resin from waste liquids result in fibrous precipitates that require cutting devices for collection, leading to inefficiencies and increased costs.

Method used

A method involving the controlled mixing of a PVA resin aqueous solution with an alcohol-based precipitate, governed by specific time and mass ratios, using stirring conditions to produce fine PVA resin particles that can be easily recovered without cutting equipment.

Benefits of technology

The method achieves a high recovery rate of fine PVA resin particles, facilitating easy collection and reducing operational costs by eliminating the need for cutting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144212000001
    Figure 2024144212000001
  • Figure 2024144212000002
    Figure 2024144212000002
  • Figure 2024144212000003
    Figure 2024144212000003
Patent Text Reader

Abstract

To provide a method for precipitating a fine polyvinyl alcohol (PVA)-based resin, which has an excellent recovery rate.SOLUTION: There is provided a method for precipitating a polyvinyl alcohol-based resin in which a polyvinyl alcohol-based resin aqueous solution and a precipitation solution containing alcohol as a main component are mixed under stirring and time from the start of mixing to the completion of mixing is defined as time A and the time A is divided into 60, the mixing start time is defined as A0, the time of n / 60 is defined as An and the mixing completion time is defined as A60 (provided, 0<n<60), a value calculated by the following expression (I) is 0.010 to 20 in A1 and 0.05 to 0.75 in A60. (The mass of the polyvinyl alcohol-based resin+the mass of water) / the mass of alcohol...Expression (I)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for precipitating a polyvinyl alcohol-based resin, and more particularly to a method for precipitating a polyvinyl alcohol-based resin from an aqueous solution of the polyvinyl alcohol-based resin. [Background technology]

[0002] Polyvinyl alcohol resins (hereinafter, also referred to as PVA resins) have been widely used industrially as water-soluble synthetic polymers, and are widely utilized as raw materials for synthetic fibers or films, fiber processing agents, paper processing agents, adhesives, inorganic binders, polymerization stabilizers for polyvinyl chloride resins, etc.

[0003] Among these applications, PVA resins are preferably used as support materials when producing molded bodies using 3D printers, as cores when producing molded bodies with hollow parts, as dispersants when producing water-insoluble resin microparticles, etc. This is because by using PVA resins to produce support materials and cores and dispersing microparticles, it is possible to finally separate the molded body and microparticles from the support materials, cores, and dispersants by contacting them with water.

[0004] On the other hand, when the PVA resin is finally separated by contacting with water, a PVA resin waste liquid is generated. From the viewpoint of reducing the burden on the environment, it is required to remove the PVA resin from the waste liquid. In addition, if it becomes possible to recover the PVA resin from the waste liquid, the recovered PVA resin can be reused, which is also preferable in terms of cost.

[0005] As a method for recovering a PVA-based resin from an aqueous solution containing the PVA-based resin, for example, Patent Document 1 proposes a method in which a polyvinyl alcohol-based resin molded body containing an inorganic filler is dissolved in water, and then brought into contact with a precipitating liquid containing an alcohol having 3 to 6 carbon atoms as a main component to precipitate a polyvinyl alcohol-based resin containing an inorganic filler, and the precipitate is separated and recovered. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-218642 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the technique described in Patent Document 1, although the recovery rate of the PVA resin is high, since the precipitated PVA resin is fibrous, the fibrous PVA resin becomes entangled with each other and forms a mass. Therefore, when transporting the precipitated PVA resin, it is necessary to use a device having a cutting function such as a cutter pump, and there is room for improvement in terms of ease of recovery and cost.

[0008] Therefore, an object of the present invention is to provide a method for precipitating a fine PVA-based resin with an excellent recovery rate. [Means for solving the problem]

[0009] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by mixing an aqueous polyvinyl alcohol-based resin solution with a precipitating liquid containing alcohol as a main component, and mixing the solutions so that the masses of the alcohol, PVA-based resin, and water in the mixed solution satisfy a specific relationship, thereby completing the present invention.

[0010] That is, the present invention has the following configuration.

[0011] A first aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin, comprising the steps of: The polyvinyl alcohol resin aqueous solution and the alcohol-based precipitating liquid are mixed under stirring, If the time from the start of mixing to the end of mixing is A time and A time is divided into 60 parts, the start of mixing is A0, the n / 60th hour is An, and the end of mixing is A60 (however, 0 <n<60)、 This is a method for precipitating a polyvinyl alcohol-based resin, in which the value calculated by the following formula (I) is 0.010 to 20 for A1 and 0.05 to 0.75 for A60. (mass of polyvinyl alcohol resin + mass of water) / mass of alcohol... formula (I)

[0012] A second aspect of the present invention is the method for precipitating a polyvinyl alcohol-based resin according to the first aspect, A2, the method for precipitating a polyvinyl alcohol-based resin, wherein the value calculated by the formula (I) is 0.020 to 16.

[0013] A third aspect of the present invention is the method for precipitating a polyvinyl alcohol-based resin according to the first or second aspect, A3, the method for precipitating a polyvinyl alcohol-based resin, wherein the value calculated by the formula (I) is 0.030 to 12.

[0014] A fourth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to third aspects, A20, the value calculated by the formula (I) is 0.040 to 3.

[0015] A fifth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to fourth aspects, The polyvinyl alcohol-based resin is a polyvinyl alcohol-based resin containing a 1,2-diol structural unit in a side chain.

[0016] A sixth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to fifth aspects, In the method for precipitating a polyvinyl alcohol-based resin, the particle size of the precipitated polyvinyl alcohol-based resin is 0.1 to 50 mm.

[0017] A seventh aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to sixth aspects, This is a method for precipitating a polyvinyl alcohol-based resin, in which stirring is carried out so that the value calculated by the following formula (II) becomes 100 or more. (d / D) × N (II) In the above formula (II), d is the blade diameter (m) of the stirring blade, D is the vessel diameter (m) of the stirring vessel, and N is the rotation speed (rpm) of the stirring blade.

[0018] An eighth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to seventh aspects, A method for precipitating a polyvinyl alcohol-based resin, comprising using an edged turbine blade as an agitating blade.

[0019] A ninth aspect of the present invention is The present invention is a method for recycling a polyvinyl alcohol-based resin, which comprises recovering a polyvinyl alcohol-based resin precipitated by the method for precipitating a polyvinyl alcohol-based resin according to any one of the first to eighth aspects. Effect of the Invention

[0020] According to the precipitation method of the present invention, the precipitated PVA-based resin is fine, so that it can be easily recovered without using a device with a cutting function such as a cutter pump, and the PVA-based resin can be precipitated with a high recovery rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following embodiments of the present invention will be described in detail. The following description is merely an example of the present invention, and the present invention is not limited thereto. In this specification, the notation "~" indicates a numerical value including the numbers before and after it.

[0022] <Polyvinyl alcohol resin> First, the PVA resin used in this embodiment will be described. PVA resins are resins mainly composed of vinyl alcohol structural units, obtained by saponifying polyvinyl ester resins obtained by copolymerizing vinyl ester monomers, and are composed of vinyl alcohol structural units and vinyl ester structural units with a degree of saponification corresponding to the degree of saponification.

[0023] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate. From an economical standpoint, vinyl acetate is preferably used.

[0024] The average degree of polymerization of the PVA resin used in this embodiment (measured in accordance with JIS K6726:1994) is preferably 350-1,000, more preferably 400-800, and even more preferably 450-600. If the average degree of polymerization is 350 or more, the resin has sufficient strength, and if the average degree of polymerization is 1000 or less, decomposition of the resin due to generation of shear heat during injection molding can be suppressed.

[0025] The saponification degree (average saponification degree measured in accordance with JIS K6726:1994) of the PVA resin used in the present embodiment is preferably 60 to 99.9 mol %, more preferably 80 to 99.5 mol %, and even more preferably 90 to 99.5 mol %. If the saponification degree is 60 mol % or more, the water solubility is improved, and if it is 99.9 mol % or less, melt molding becomes easy.

[0026] In addition to unmodified PVA resins, the PVA resins of this embodiment may be modified PVA resins obtained by copolymerizing various monomers during the production of polyvinyl ester resins and saponifying the copolymerized PVA resins, or various post-modified PVA resins obtained by introducing various functional groups into unmodified PVA resins through post-modification. Such modification may be performed within a range in which the water solubility of the PVA resin is not lost. In some cases, the modified PVA resin may be further post-modified.

[0027] Examples of monomers copolymerizable with vinyl ester monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, and 3,4-dihydroxy-1-butene; acylated derivatives thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid; salts, monoesters, or dialkyl esters thereof; nitriles such as acrylonitrile and methacrylonitrile; and diacetone acrylate. amides such as ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, and other olefin sulfonic acids or their salts; alkyl vinyl ethers, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, glycerin monoallyl ether, 3,4-diacetoxy-1-butene, and other vinyl compounds; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; vinylidene chloride, 1,4-diacetoxy-2-butene, and vinylene carbonate.

[0028] In addition, examples of modified PVA-based resins into which functional groups have been introduced by a post-reaction include those having acetoacetyl groups by reaction with diketene, those having polyalkylene oxide groups by reaction with ethylene oxide, those having hydroxyalkyl groups by reaction with epoxy compounds, etc., and those obtained by reacting aldehyde compounds having various functional groups with PVA.

[0029] When the PVA-based resin is a modified PVA-based resin, the content (modification amount) of the modified species in the modified PVA-based resin, i.e., the constituent units derived from various monomers in the copolymer or the functional groups introduced by a post-reaction, cannot be generally determined because the characteristics vary greatly depending on the modified species, but is preferably in the range of 0.1 to 20 mol %, more preferably in the range of 0.5 to 12 mol %.

[0030] Among these various modified PVA resins, in the present embodiment, a PVA resin having a hydrophilic modified group is preferably used. Examples of the hydrophilic modified group include a hydroxyl group, a carboxyl group, and an amino group. In particular, from the viewpoint of water solubility, a PVA-based resin containing a structural unit having a 1,2-diol modifying group is preferred.

[0031] Among such PVA-based resins containing structural units having 1,2-diol modifying groups, it is preferable to use a PVA-based resin containing a 1,2-diol structural unit in the side chain, represented by the following general formula (1) (hereinafter, sometimes referred to as a "PVA-based resin containing a 1,2-diol structural unit in the side chain"). By using a PVA-based resin containing a 1,2-diol structural unit in the side chain, the melting point can be lowered, and the temperature range during melt molding can be expanded. The portions other than the 1,2-diol structural units are vinyl alcohol structural units and unsaponified vinyl ester structural units, like ordinary PVA resins.

[0032] [ka]

[0033] (In formula (1), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and X represents a single bond or a bonding chain.

[0034] In the above general formula (1), R 1 ~R 6 R each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. 1 ~R 6are preferably all hydrogen atoms, but may be alkyl groups having 1 to 5 carbon atoms in an amount that does not significantly impair the resin properties. The alkyl group is not particularly limited, but examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and pentyl groups, and the alkyl group may have a substituent such as a halogeno group, a hydroxyl group, an ester group, a carboxylic acid group, or a sulfonic acid group, as necessary.

[0035] In addition, X in the 1,2-diol structural unit represented by general formula (1) is most preferably a single bond in terms of thermal stability and stability under high temperature and acidic conditions, but may be a linking chain as long as it does not impair the effects of the present invention. Examples of such linking chains include hydrocarbons such as alkylene groups, alkenylene groups, alkynylene groups, phenylene groups, and naphthylene groups (these hydrocarbons may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms), as well as -O-, -(CHO)-, -(OCH) m -, -(CH2O) m CH2-, -CO-, -COCO-, -CO(CH2) m Examples of such groups include CO-, -CO(CH)CO-, -S-, -CS-, -SO-, -SO2-, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO4-, -Si(OR)2-, -OSi(OR)2-, -OSi(OR)2O-, -Ti(OR)2-, -OTi(OR)2-, -OTi(OR)2O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, etc. (each R is independently an arbitrary substituent, preferably a hydrogen atom or an alkyl group, and m is an integer of 1 to 5). Among these, an alkylene group having 6 or less carbon atoms, particularly a methylene group, or -CH2OCH2- is preferred from the viewpoint of stability during production or use.

[0036] A particularly preferred structure in the 1,2-diol structural unit represented by the above general formula (1) is R 1 ~R 6 are all hydrogen atoms and X is a single bond, and is a structural unit represented by the following formula (1a).

[0037] [ka]

[0038] When the PVA resin is a PVA resin containing a 1,2-diol structural unit in a side chain, the content (modification amount) of the structural unit represented by general formula (1) contained in the PVA resin containing a 1,2-diol structural unit in a side chain is preferably 0.1 to 10 mol%, more preferably 0.5 to 9 mol%, and even more preferably 1 to 8 mol%. When the content is 0.1 mol% or more, the effect of the 1,2-diol structure in the side chain is sufficiently obtained. Also, when the content is 10 mol% or less, the melt moldability is improved.

[0039] The content (modification amount) of 1,2-diol structural units in the PVA resin is the same as that of the PVA resin that has been completely saponified. 1 It can be obtained from the H-NMR spectrum (solvent: DMSO-d6, internal standard: tetramethylsilane). Specifically, it may be calculated from the peak areas derived from the hydroxyl group protons, methine protons, and methylene protons in the 1,2-diol structural unit, the methylene protons in the main chain, the protons of the hydroxyl groups linked to the main chain, etc.

[0040] When a PVA resin having a 1,2-diol structural unit in a side chain is used, the saponification degree is preferably 80 to 99.9 mol%, more preferably 98.5 to 99.5 mol%. If the saponification degree is 80 mol% or more, the resin is less likely to decompose and deformation at high temperatures can be suppressed.

[0041] The PVA resin having a 1,2-diol structural unit in the side chain can be produced by a known production method. For example, (i) a method of saponifying a copolymer of a vinyl ester monomer and a compound represented by the following general formula (2), (ii) a method of saponifying and decarbonating a copolymer of a vinyl ester monomer and a compound represented by the following general formula (3), or (iii) a method of saponifying and deketalizing a copolymer of a vinyl ester monomer and a compound represented by the following general formula (4) is preferably used.

[0042] [ka]

[0043] (In formula (2), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, X represents a single bond or a bonding chain, R 7 and R 8 are each independently a hydrogen atom or R 9 -CO-(wherein, R 9 represents an alkyl group having 1 to 6 carbon atoms.

[0044] [ka]

[0045] (In formula (3), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and X represents a single bond or a bonding chain.

[0046] [ka]

[0047] (In formula (4), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, X represents a single bond or a bonding chain, R 10 and R11 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.

[0048] R in the above general formulas (2) to (4) 1 ~R 6 Specific examples and preferred examples of X are the same as those in the above formula (1). 7 and R 8 are each independently a hydrogen atom or R 9 -CO-(wherein, R 9 R is an alkyl group having 1 to 6 carbon atoms. 10 and R 11 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and specific and preferred examples of the alkyl group having 1 to 5 carbon atoms are the same as those in formula (1).

[0049] As for the methods (i), (ii), and (iii), for example, the methods described in JP-A-2006-95825 can be used. Among the above methods, the method (i) is preferred from the viewpoint of excellent copolymerization reactivity and industrial handling properties. In particular, the method (i) is preferred in which R 1 ~R 6 is a hydrogen atom, X is a single bond, R 7 , R 8 R 9 -CO-, R 9 It is preferable to use 3,4-diacyloxy-1-butene, in which R is an alkyl group having 1 to 4 carbon atoms. 9 In particular, 3,4-diacetoxy-1-butene, in which R is a methyl group, is preferably used.

[0050] The PVA-based resin used in this embodiment may be of one type or a mixture of two or more types. In that case, the above-mentioned unmodified PVAs, an unmodified PVA and a PVA-based resin having a structural unit represented by the general formula (1), PVA-based resins having structural units represented by the general formula (1) with different saponification degrees, average polymerization degrees, modification amounts, etc., an unmodified PVA, or a PVA-based resin having a structural unit represented by the general formula (1) and other modified PVA-based resins, etc. can be used in combinations.

[0051] [Other Components] As long as the effects of the present invention are not impaired, lubricants such as magnesium stearate and magnesium 12-hydroxystearate may be added as additives to the PVA-based resin. Further, plasticizers such as glycerin, diglycerin, polyglycerin, ethylene oxide adducts of glycerin, and glycerin fatty acids may be contained as necessary.

[0052] 《Precipitation Method》 Next, the precipitation method of the PVA-based resin according to this embodiment will be described. The precipitation method according to this embodiment is such that when a PVA-based resin aqueous solution and a precipitation liquid mainly composed of alcohol are mixed under stirring, and the time from the start of mixing to the end of mixing is set as A hours, and when A hours is divided into 60 equal parts, with the start of mixing being A0, the n / 60-th hour being An, and the end of mixing being A60 (where 0 < n < 60), the value calculated by the following formula (I) is 0.010 to 20 at A1 and 0.05 to 0.75 at A60. (Mass of PVA-based resin + Mass of water) / Mass of alcohol ··· Formula (I)

[0053] In the precipitation method of the PVA-based resin according to this embodiment, in the mixed liquid obtained by mixing a PVA-based resin aqueous solution and a precipitation liquid mainly composed of alcohol under stirring, the proportion of the precipitation liquid gradually increases. In this specification, "end of mixing" means the time when the contact of the total amount of the precipitation liquid to be mixed with the PVA-based resin aqueous solution is completed. For example, when the precipitation liquid is dropped into the PVA-based resin aqueous solution, the time when the dropping of the total amount of the precipitation liquid to be mixed is completed is the "end of mixing".

[0054] Here, the PVA-based resin aqueous solution is an aqueous solution containing the above-mentioned PVA-based resin. The PVA-based resin aqueous solution is obtained by contacting the PVA-based resin with water to dissolve the PVA-based resin (dissolving step).

[0055] The method for contacting the PVA-based resin with water is not particularly limited, but examples thereof include a normal pressure room temperature dissolution method, a high pressure room temperature dissolution method, a normal pressure hot water dissolution method, and a high pressure hot water dissolution method. As the apparatus, an ultrasonic homogenizer, a three-one motor, a homomixer, or the like can be used. The temperature of the water to be contacted is preferably 0 to 200° C., more preferably 50 to 150° C., and more preferably 80 to 120° C. If the water temperature is 0° C. or higher, the PVA resin can be dissolved, and if the water temperature is 200° C. or lower, decomposition of the PVA resin can be suppressed. The dissolution time, i.e., the contact time between the PVA resin and water, is preferably 0.5 to 50 hours, more preferably 1 to 25 hours, and further preferably 1.5 to 5 hours. If the dissolution time is 0.5 hours or more, it is possible to prevent undissolved matter from remaining, and if it is 50 hours or less, it is economically preferable.

[0056] The concentration of the aqueous PVA resin solution obtained by the dissolving step varies somewhat depending on the type and dissolving apparatus, but is preferably 1 to 40% by mass, more preferably 5 to 35% by mass, and even more preferably 10 to 30% by mass. When the concentration of the PVA-based resin aqueous solution is 1% by mass or more, the number of repetitions of the recovery step described below can be reduced, which is efficient. On the other hand, when the concentration is 40% by mass or less, the solubility is increased, and the efficiency of the dissolution step can be sufficiently increased.

[0057] The deposition solution used in this embodiment is mainly composed of alcohol, and the alcohol content in the deposition solution is preferably 50 to 100% by mass, more preferably 80 to 100% by mass, and further preferably 100% by mass. If the content is 50% or more, a sufficient deposition effect can be obtained. As components other than alcohol, those that do not inhibit precipitation are not particularly limited, but usually methyl acetate, ethyl acetate or water can be used, and water is particularly preferably used.

[0058] From the viewpoint of the recovery rate, it is preferable to use an alcohol having 1 to 6 carbon atoms as the alcohol. Specific examples of the alcohol having 1 to 6 carbon atoms include methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), tert-butyl alcohol, n-butyl alcohol, isobutanol, 1-pentanol, 2-butanol and the like. Among these, from the viewpoint of suppressing the adhesiveness of the precipitate and preventing it from becoming块状, methanol, 2-propanol, ethanol, 1-propanol, and tert-butyl alcohol are preferable, and methanol and IPA are more preferably used. The alcohol may be used alone or in combination of two or more. By having the carbon number within the above range, the precipitation amount of the PVA-based resin can be increased.

[0059] In the precipitation method according to the present embodiment, a precipitation liquid mainly composed of an aqueous PVA-based resin solution and alcohol is mixed with stirring, and when the time from the start of mixing to the end of mixing is set as A hours and A hours is divided into 60 equal parts, when the start of mixing is A0, the n / 60 hour is An, and the end of mixing is A60 (where 0 < n < 60), the value calculated by the following formula (I) is set to be 0.010 to 20 at A1. (Mass of PVA-based resin + Mass of water) / Mass of alcohol ··· Formula (I)

[0060] By making the value calculated by formula (I) be 0.010 or more at A1, the precipitated PVA-based resin becomes a PVA-based resin with a small particle diameter rather than a fibrous shape. As a result, it can be easily recovered without using a device having a cutting function such as a cutter pump. At A1, the value calculated by formula (I) is preferably 0.012 or more, more preferably 0.015 or more, further preferably 0.020 or more, and particularly preferably 0.025 or more. In addition, precipitation is facilitated by making the value calculated by formula (I) in A1 20 or less. In A1, the value calculated by formula (I) is preferably 19 or less, more preferably 18 or less, even more preferably 17 or less, particularly preferably 16 or less, and most preferably 15 or less.

[0061] In this embodiment, the value calculated by the above formula (I) is set to 0.05 to 0.75 in A60. The amount of PVA-based resin recovered from the precipitation solution can be increased by setting the value calculated by the formula (I) to 0.05 or more in A60. The value calculated by the formula (I) in A60 is preferably 0.06 or more, more preferably 0.08 or more, even more preferably 0.1 or more, and particularly preferably 0.15 or more. In addition, the recovery rate can be increased by making the value calculated by formula (I) at A60 0.75 or less. At A60, the value calculated by formula (I) is preferably 0.7 or less, more preferably 0.5 or less, even more preferably 0.4 or less, and particularly preferably 0.3 or less.

[0062] In addition, in A2, it is preferable that the value calculated by the above formula (I) is 0.020 to 16. In A2, by making the value calculated by the formula (I) 0.020 or more, the precipitated PVA-based resin is prevented from becoming fibrous, and a PVA-based resin having a finer particle size can be precipitated. In A2, it is more preferable that the value calculated by the formula (I) is 0.030 or more, further preferably 0.035 or more, particularly preferably 0.040 or more, and most preferably 0.045 or more. In addition, the recovery rate can be increased by making the value calculated by formula (I) in A2 16 or less. In A2, the value calculated by formula (I) is more preferably 14 or less, further preferably 12 or less, particularly preferably 10 or less, and most preferably 9 or less.

[0063] In addition, it is preferable that the value calculated by the above formula (I) in A3 is 0.030 to 12. By making the value calculated by the formula (I) in A3 0.030 or more, the precipitated PVA-based resin is prevented from becoming fibrous, and a PVA-based resin having a finer particle size can be precipitated. In A3, it is more preferable that the value calculated by the formula (I) is 0.040 or more, further preferably 0.050 or more, and particularly preferably 0.060 or more. In addition, the recovery rate can be increased by making the value calculated by formula (I) in A3 12 or less. In A3, the value calculated by formula (I) is more preferably 10 or less, further preferably 8 or less, and particularly preferably 6 or less.

[0064] In addition, in A10, the value calculated by the above formula (I) is preferably 0.035 to 7. By adjusting the value calculated by the formula (I) in A10 to be within the above range, the precipitated PVA-based resin is prevented from becoming fibrous, and a PVA-based resin having a finer particle size can be precipitated. In A10, the value calculated by the formula (I) is more preferably 0.040 to 6, further preferably 0.050 to 5, particularly preferably 0.070 to 4, and most preferably 0.10 to 3.

[0065] In addition, it is preferable that the value calculated by the above formula (I) in A20 is 0.040 to 3. By making the value calculated by the formula (I) in A20 0.040 or more, the precipitated PVA-based resin is prevented from becoming fibrous, and a PVA-based resin with a particle size can be precipitated. It is more preferable that the value calculated by the formula (I) in A20 is 0.045 or more, further preferably 0.060 or more, particularly preferably 0.080 or more, and most preferably 0.120 or more. In addition, the PVA-based resin can be recovered with high efficiency by making the value calculated by formula (I) in A20 3 or less. The value calculated by formula (I) in A20 is more preferably 2 or less, even more preferably 1.5 or less, particularly preferably 1 or less, and most preferably 0.9 or less.

[0066] In addition, it is preferable that the value calculated by the above formula (I) in A30 is 0.045 to 1. By making the value calculated by the formula (I) in A30 within the above range, the precipitated PVA-based resin is prevented from becoming fibrous, and a PVA-based resin having a finer particle size can be precipitated. The value calculated by the formula (I) in A30 is more preferably 0.050 to 0.9, further preferably 0.065 to 0.8, particularly preferably 0.085 to 0.7, and most preferably 0.13 to 0.6.

[0067] The liquid temperature when the PVA-based resin aqueous solution and the precipitating liquid are mixed may be room temperature, and is preferably adjusted to 5 to 40° C., and more preferably 10 to 35° C. By keeping the temperature during mixing within the above range, evaporation of the alcohol can be suppressed.

[0068] The method for mixing the precipitation liquid and the aqueous PVA resin solution is not particularly limited. From the viewpoint of mixability, however, it is preferable to mix the precipitation liquid and the aqueous PVA resin solution under stirring in a stirring tank having stirring blades for circulation within the tank.

[0069] When the aqueous PVA resin solution and the precipitation liquid are mixed under stirring, it is preferable to stir the mixture so that the value calculated by the following formula (II) is 100 or more. (d / D)×N...Equation (II) In the formula (II), d is the impeller diameter (m), D is the vessel diameter (m) of the stirring vessel, and N is the rotation speed (rpm) of the impeller. The vessel diameter of the stirring vessel means the inner diameter (inner diameter) of the stirring vessel.

[0070] When the value calculated by the above formula (II) is 100 or more, the precipitated PVA-based resin is not fibrous but granular. The value calculated by the above formula (II) is preferably 110 or more, more preferably 120 or more, and particularly preferably 130 or more. From the viewpoint of stirring force, the value calculated by the above formula (II) is preferably 3000 or less, more preferably 1000 or less, more preferably 500 or less, and particularly preferably 300 or less.

[0071] The ratio (d / D) of the impeller diameter d of the stirring impeller to the vessel diameter D of the stirring vessel is preferably 0.1 to 0.95, more preferably 0.2 to 0.9, and particularly preferably 0.25 to 0.8. By having d / D within the above range, more efficient stirring can be achieved, which is preferable. The blade diameter d is twice the length from the stirring shaft to the tip of the blade.

[0072] From the viewpoint of stirring power, the rotation speed N of the stirring blade is preferably from 50 to 5000 rpm, more preferably from 100 to 4000 rpm, and even more preferably from 150 to 3000 rpm.

[0073] Examples of stirring blades include edged turbine blades (also called dispersers), paddle blades, etc. Among these, it is preferable to use edged turbine blades for stirring, since the shear force during stirring is likely to be large. The impellers may be installed in one stage or multiple stages on the stirring shaft, and when installed in multiple stages, they may be the same or different. When installing impellers in multiple stages on the stirring shaft, it is preferable that the impeller with the largest blade diameter satisfies the above formula (II) and d / D.

[0074] The shape of the stirring vessel is not particularly limited, but examples thereof include a vertical cylindrical type, a semi-elliptical type, a semi-circular type, and a conical type.

[0075] From the viewpoint of mixability, the total mixing time is preferably from 0.2 to 48 hours, more preferably from 0.5 to 24 hours, and even more preferably from 1 to 12 hours. After the contact of the entire amount of the precipitation liquid to be mixed with the aqueous PVA resin solution is completed, for example, in the case where the precipitation liquid is added dropwise to the aqueous PVA resin solution, stirring may be continued for any time after the dropwise addition of the entire amount of the precipitation liquid to be mixed is completed.

[0076] By mixing the aqueous PVA resin solution with the precipitating liquid, the PVA resin is precipitated, and a mixed solution and the precipitated PVA resin are obtained.

[0077] The particle size of the PVA-based resin precipitated by the precipitation method according to the present embodiment is preferably 0.1 to 50 mm. By precipitating the PVA-based resin in the form of fine particles by the method of the present invention and the particle size of the precipitated PVA-based resin being within the above range, the precipitated PVA-based resin can be transported through a pipe without using a cutter pump or the like, which is preferable in terms of easy recovery and cost. The particle size of the precipitated PVA resin is more preferably from 0.1 to 30 mm, further preferably from 0.1 to 10 mm, and particularly preferably from 0.5 to 5 mm. The particle size is determined as the average of the maximum diameters of 10 particles randomly taken from the precipitated PVA resin and measured with a vernier caliper.

[0078] The ratio (recovery rate) of the mass of the PVA-based resin precipitated by the above-mentioned precipitation method to the mass of the PVA-based resin in the aqueous PVA-based resin solution is preferably 50% or more. If the recovery rate is 50% or more, the PVA-based resin in the solution can be sufficiently recovered. The higher the recovery rate, the more preferable it is, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more, with the upper limit being 100%. Here, the recovery rate can be calculated by the following method. The PVA-based resin precipitated by the above precipitation method is dried for 3 hours at 140° C. using a dryer (for example, SPH-102 manufactured by ESPEC Co., Ltd.). The mass of the dried PVA-based resin is measured, and the recovery rate is calculated based on the following formula. Recovery rate (%) = {mass of PVA-based resin after drying (g) / mass of PVA-based resin used (g)} × 100

[0079] "Recycling Method" The recycling method according to this embodiment includes recovering the PVA-based resin deposited by the deposition method according to this embodiment (recovery step).

[0080] The method for recovering the PVA-based resin deposited by the PVA-based resin deposition method according to this embodiment is not particularly limited and can be performed by a known method. Specifically, for example, the deposited PVA-based resin can be filtered from the mixed solution, centrifuged, and then dried using a vibration fluidized dryer, a vacuum dryer, or the like to obtain the PVA-based resin. The drying time is preferably 2 to 130 hours, more preferably 10 to 80 hours. Also, the drying temperature is not particularly limited, but is preferably 150°C or lower.

Examples

[0081] Hereinafter, the present invention will be described more specifically with reference to examples, but the present invention is not limited to the following examples as long as the gist thereof is not exceeded. In the examples, "parts" and "%" mean mass basis unless otherwise specified.

[0082] (Example 1) <Production of PVA-based Resin> A PVA-based resin (a) having a 1,2-diol structural unit represented by the general formula (1a) (saponification degree: 99.2 mol%, degree of polymerization: 350, content of 1,2-diol structural unit: 6 mol%) was pelletized by melt extrusion using a twin-screw extruder. Such pellets are cylindrical with a total length of 3 mm and an outer diameter of 2 mm.

[0083] (A) Dissolution Step Water was put into a reaction vessel equipped with a stirring blade, and the above pellets were added while stirring at 500 rpm. After heating to 85°C, the above pellets were completely dissolved in water to obtain an aqueous solution of PVA-based resin (a) of about 27% by mass. Next, the solid content was calculated by the volatile matter method {(mass of solid after drying / mass of aqueous solution) × 100}, and an aqueous solution of 25% by mass of PVA resin (a) was adjusted by adding water.

[0084] (B) Precipitation Step 100 g of methanol was placed in a 2 L stirring tank (tank diameter D: 0.13 m). Using an edged turbine blade (blade diameter d: 0.1 m) as an agitator blade in a Three-One Motor (manufactured by EYELA), 900 g of a precipitation solution consisting of methanol was dropped at a rate of 900 g / hour and 200 g of a 25% by mass aqueous solution of PVA-based resin (a) was dropped at a rate of 200 g / hour using a dropping funnel while stirring at a rotation speed N of 200 rpm. The period from the start of mixing to the end of mixing is designated time A, which is divided into 60 parts. The values ​​of formula (I) below at A0, A1, A2, A3, A20 and A60 are shown in Tables 1 and 2. (mass of polyvinyl alcohol resin + mass of water) / mass of alcohol... formula (I) In Example 1, the time A was 1 hour.

[0085] In addition, the impeller diameter d (m) of the stirring blade, the vessel diameter D (m) of the stirring vessel, and the stirring speed N (rpm) were used to calculate the following formula (II), and the obtained values ​​are shown in Table 3. (d / D) × N (II)

[0086] (C) Recovery process The PVA-based resin (a') precipitated in the above precipitation step was filtered through a mesh and dried at 140°C for 3 hours to obtain a PVA-based resin (a').

[0087] Evaluation Method <Particle size of precipitated PVA resin> Ten randomly selected PVA resin particles were taken from the PVA resin (a') obtained in the precipitation step, and the average value of the maximum diameters measured with a vernier caliper was used. The results are shown in Table 1. In addition, when the precipitated PVA resin was in a lump form (a state in which the fibrous resin was entangled), it was marked with "X" in Table 1.

[0088] <Recovery rate> The mass of the PVA resin (a') obtained in the above recovery step was measured, and the recovery rate was calculated based on the following formula. The results are shown in Table 1. Recovery rate (%) = {mass (g) of dried PVA-based resin (a') / mass (g) of PVA-based resin (a) used} × 100

[0089] Example 2 The evaluation was carried out in the same manner as in Example 1, except that the rotation speed N of the stirring impeller and the blade diameter d of the stirring impeller were changed to those shown in Table 3. The results are shown in Table 1.

[0090] Example 3 Evaluation was performed in the same manner as in Example 1, except that the alcohol in Example 1 was changed to IPA. The results are shown in Table 1.

[0091] Example 4 Evaluation was performed in the same manner as in Example 1, except that the concentration of the aqueous solution of the PVA resin (a) in Example 1 was changed to 10% by mass. The results are shown in Table 1.

[0092] Example 5 In Example 1, at the start of mixing (A0), no methanol was added to the stirring tank, but 200 g of a 25% by mass aqueous solution of PVA resin (a) was added, and further, from the start of mixing, 1000 g of methanol was added dropwise at a dropping rate of 1000 g / hour, but the 25% by mass aqueous solution of PVA resin (a) was not added dropwise. The evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.

[0093] Example 6 The evaluation was carried out in the same manner as in Example 1, except that 42 g of methanol and 55 g of a 25% by mass aqueous solution of PVA resin (a) were added to the stirring tank at the start of mixing (A0), and 958 g of methanol and 145 g of a 25% by mass aqueous solution of PVA resin (a) were added dropwise at a rate of 958 g / hour and 145 g of the same, respectively, from the start of mixing. The results are shown in Table 1.

[0094] Comparative Example 1 The evaluation was carried out in the same manner as in Example 1, except that 1000 g of methanol was added to the stirring tank at the start of mixing (A0) and no dropwise addition of alcohol was carried out from the start of mixing. The results are shown in Table 1.

[0095] Comparative Example 2 Evaluation was performed in the same manner as in Comparative Example 1, except that the stirring speed was changed to 50 rpm. The results are shown in Table 1.

[0096] Comparative Example 3 The evaluation was carried out in the same manner as in Example 1, except that 400 g of methanol was added to the stirring tank at the start of mixing (A0), and 600 g of methanol was added dropwise at a rate of 600 g / hour from the start of mixing. The results are shown in Table 1.

[0097] Comparative Example 4 In Example 1, 1000 g of methanol was added to the stirring tank at the start of mixing (A0), and from the start of mixing, no dropwise addition of alcohol was performed, and a paddle impeller was used as the stirring impeller. The evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.

[0098] Comparative Example 5 The evaluation was carried out in the same manner as in Example 1, except that 1000 g of IPA was added to the stirring tank at the start of mixing (A0) and no alcohol was added dropwise from the start of mixing. The results are shown in Table 1.

[0099] Comparative Example 6 The evaluation was carried out in the same manner as in Example 1, except that 100 g of methanol was added dropwise at a rate of 100 g / hour. The results are shown in Table 1.

[0100] Comparative Example 7 In Example 1, 800 g of IPA was placed in the stirring tank at the start of mixing (A0), and further, from the start of mixing, 350 g of a 20 mass% aqueous solution of PVA-based resin (a) was dropped at 3.9 g / min (234 g / hr), and no alcohol was dropped. The evaluation was performed in the same manner as in Example 1. The results are shown in Table 1. In Comparative Example 7, the A time was 1.5 hours.

[0101] [Table 1]

[0102] [Table 2]

[0103] [Table 3]

[0104] In Examples 1 to 6, fine PVA-based resins with particle sizes of 10 mm or less were obtained, and the recovery rate was also high at 75% or more. On the other hand, in Comparative Examples 1 to 5 and 7, where the value calculated by formula (I) is less than 0.010 at A1, the precipitated PVA resin was in a lump form, although the recovery rate was high. In Comparative Example 6, where the value calculated by formula (I) is more than 0.75 at A60, the precipitated PVA resin had a small particle size, but the recovery rate was as low as 5%. [Industrial Applicability]

[0105] The PVA-based precipitation method of the present invention has a high recovery rate, and since the precipitated PVA-based resin is fine, a cutter pump or the like is not required during recovery, and recovery can be easily performed.

Claims

1. A method for precipitating a polyvinyl alcohol-based resin, comprising the steps of: The polyvinyl alcohol resin aqueous solution and the alcohol-based precipitating liquid are mixed under stirring, If the time from the start of mixing to the end of mixing is A time and A time is divided into 60 parts, the start of mixing is A0, the n / 60th hour is An, and the end of mixing is A60 (where 0<n<60), A method for precipitating a polyvinyl alcohol-based resin, wherein the value calculated by the following formula (I) is 0.010 to 20 for A1 and 0.05 to 0.75 for A60: (mass of polyvinyl alcohol resin+mass of water) / mass of alcohol...formula (I)

2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein in A2, the value calculated by the formula (I) is 0.020 to 16.

3. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein in A3, the value calculated by the formula (I) is 0.030 to 12.

4. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein in A20, the value calculated by the formula (I) is 0.040 to 3.

5. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the polyvinyl alcohol-based resin contains a 1,2-diol structural unit in a side chain.

6. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the particle size of the precipitated polyvinyl alcohol-based resin is 0.1 to 50 mm.

7. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein stirring is performed so that a value calculated by the following formula (II) is 100 or more. (d / D)×N...Formula (II) In the above formula (II), d is the blade diameter (m) of the stirring blade, D is the vessel diameter (m) of the stirring vessel, and N is the rotation speed (rpm) of the stirring blade.

8. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein an edged turbine blade is used as the stirring blade.

9. A method for recycling a polyvinyl alcohol-based resin, comprising recovering the polyvinyl alcohol-based resin precipitated by the method for precipitating a polyvinyl alcohol-based resin according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method of manufacturing recycled raw material from polyvinyl alcohol resin molded product

    JP2014218642A