Concrete repair tape
The concrete repair tape addresses peeling issues in deteriorating structures by enhancing interfacial strength and tensile strength, offering superior adhesion and durability through a base material and adhesive layer design.
Patent Information
- Application Number
- JP2024040022
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-11
AI Technical Summary
Concrete structures are deteriorating due to corrosion and aging, leading to peeling issues, and existing repair methods like paint application are time-consuming and uneven, necessitating improved concrete peeling prevention performance.
A concrete repair tape with a base material and adhesive layer having an interfacial strength of 10 N/cm or more, tensile strength of 75 N/cm or more, and additional features such as an undercoat layer and surface modifications to enhance adhesion and durability.
The concrete repair tape provides excellent peeling prevention performance, ensuring structural integrity and longevity by improving adhesion and resistance to environmental factors.
Smart Images

Figure 2024144215000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a concrete repair tape. [Background technology]
[0002] Concrete structures are widely used for viaducts, tunnels, bridges, and other structures due to the need to improve their strength and durability. However, in recent years, concrete has been deteriorating due to corrosion of reinforcing bars caused by salt damage to concrete, neutralization due to exhaust gases, alkali-aggregate reactions, freezing of water that has penetrated into cracks, etc. As a result, pieces of concrete are peeling off from the surface of concrete structures, causing problems such as a decrease in the strength and aesthetics of the concrete structure itself, and the risk of accidents due to spalling. Traditionally, paint has been used to repair these defects, but applying paint takes time and can result in uneven work. Under these circumstances, and taking into consideration such issues, methods for preventing concrete spalling have been developed from various perspectives. For example, in the method for preventing concrete spalling described in Patent Document 1, a composite sheet having an adhesive layer and a sheet layer is placed on the surface of a concrete structure to prevent concrete from spalling from the concrete structure. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-178508 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, concrete structures have deteriorated further, and there is a risk that large pieces of concrete may peel off from the surface of the concrete structure. For this reason, there is a demand for a composite sheet having an adhesive layer and a sheet layer to have further improved concrete peeling prevention performance. Therefore, an object of the present invention is to provide a concrete repair tape that is excellent in preventing concrete peeling. [Means for solving the problem]
[0005] As a result of extensive research, the inventors discovered that the above problems can be solved by improving the interfacial strength and tensile breaking strength between the substrate and the adhesive layer in a concrete repair tape, and thus completed the present invention. The present invention provides the following [1] to [9]. [1] A substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate, The interfacial strength between the substrate and the pressure-sensitive adhesive layer is 10 N / cm or more; A concrete repair tape with a tensile breaking strength of 75N / cm or more. [2] The concrete repair tape described in [1] above, further comprising an undercoat layer on the surface of the substrate facing the adhesive layer. [3] The concrete repair tape according to [1] or [2] above, wherein the surface of the substrate on the side of the adhesive layer has been subjected to surface modification by corona treatment. [4] A concrete repair tape according to any one of [1] to [3] above, which has a gloss retention of 70% or more after a weather resistance test carried out in cycle A in accordance with JIS K 5600-7-7. [5] The concrete repair tape according to any one of the above [1] to [4], which has a tensile elongation of 100% or more. [6] The concrete repair tape according to any one of the above [1] to [5], wherein the pressure-sensitive adhesive layer has a thickness of 100 μm or more. [7] The concrete repair tape according to any one of the above [1] to [6], wherein the substrate is a fluororesin film. [8] The concrete repair tape according to any one of the above [1] to [7], further comprising a coating film provided on the surface of the substrate opposite to the surface on which the pressure-sensitive adhesive layer is formed. [9] The concrete repair tape according to the above [8], wherein the coating film is a coating film of a fluorine-based paint. Effect of the Invention
[0006] According to the present invention, a concrete repair tape having excellent concrete peeling prevention performance can be provided. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of the concrete repair tape of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of the concrete repair tape of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the configuration of the concrete repair tape of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Concrete repair tape] The concrete repair tape of the present invention comprises a substrate and an adhesive layer provided on one surface of the substrate, and has an interfacial strength between the substrate and the adhesive layer of 10 N / cm or more and a tensile breaking strength of 75 N / cm or more, which gives the concrete repair tape of the present invention excellent concrete peeling prevention performance.
[0009] (interface strength) The interfacial strength between the substrate and the adhesive layer in the concrete repair tape of the present invention is 10 N / cm or more. If the interfacial strength between the substrate and the adhesive layer is less than 10 N / cm, the concrete peeling prevention performance may be insufficient for use in an aged concrete structure. From this viewpoint, the interfacial strength between the substrate and the adhesive layer in the concrete repair tape of the present invention is preferably 11 N / cm or more, more preferably 12 N / cm or more, even more preferably 14 N / cm or more, even more preferably 16 N / cm or more, and particularly preferably 18 N / cm or more. The upper limit of the range of the interfacial strength between the substrate and the adhesive layer in the concrete repair tape of the present invention is not particularly limited, but is usually 100 N / cm, preferably 50 N / cm. The interfacial strength between the substrate and the adhesive layer in the concrete repair tape can be measured by the method described in the Examples below. The interfacial strength between the substrate and the adhesive layer in the concrete repair tape can be adjusted by providing an undercoat layer on the adhesive layer side of the substrate, modifying the surface of the substrate, or changing the material of the substrate.
[0010] (Tensile breaking strength) The tensile breaking strength of the concrete repair tape of the present invention is 75 N / cm or more. If the tensile breaking strength is less than 75 N / cm, the load resistance becomes insufficient, and spalling of concrete may not be sufficiently prevented. From this viewpoint, the tensile breaking strength of the concrete repair tape of the present invention is preferably 78 N / cm or more, more preferably 100 N / cm or more. The upper limit of the range of the tensile breaking strength of the concrete repair tape of the present invention is not particularly limited, but is usually 200 N / cm, preferably 150 N / cm. The tensile breaking strength of the concrete repair tape can be measured by the method described in the examples below. The tensile breaking strength of the concrete repair tape can be adjusted by the type and thickness of the substrate.
[0011] (Gloss retention) The gloss retention rate of the concrete repair tape of the present invention after the weather resistance test carried out in cycle A according to JIS K 5600-7-7 is preferably 70% or more. If the gloss retention rate of the concrete repair tape is 70% or more, the light resistance of the concrete repair tape is further improved. From this viewpoint, the gloss retention rate of the concrete repair tape of the present invention after the weather resistance test carried out in cycle A according to JIS K 5600-7-7 is more preferably 75% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more. The upper limit of the range of the gloss retention rate of the concrete repair tape of the present invention after the weather resistance test carried out in cycle A according to JIS K 5600-7-7 is not particularly limited, but is usually 100%. The gloss retention rate of the concrete repair tape can be measured by the method described in the examples described later. The gloss retention of the concrete repair tape of the present invention after a weather resistance test carried out in cycle A in accordance with JIS K 5600-7-7 can be adjusted by changing the type of substrate or by applying a paint to the surface of the substrate.
[0012] (Tensile elongation) The tensile elongation of the concrete repair tape of the present invention is preferably 100% or more. If the tensile elongation of the concrete repair tape is 100% or more, when concrete is deformed, it is possible to easily find the deformed part during inspection while preventing the concrete pieces from peeling off. From this viewpoint, the tensile elongation of the concrete repair tape of the present invention is more preferably 130% or more, more preferably 180% or more, and even more preferably 280% or more. The upper limit of the range of the tensile elongation of the concrete repair tape of the present invention is not particularly limited, but is usually 400%. The tensile elongation of the concrete repair tape can be measured by the method described in the examples below. The tensile elongation of the concrete repair tape can be adjusted depending on the type and thickness of the substrate.
[0013] (base material) The substrate in the concrete repair tape of the present invention is not particularly limited, but examples thereof include sheet-like materials such as resin films, nonwoven fabrics, and metal foils. Examples of the resin film include acrylic films, polyester films such as PET (polyethylene terephthalate) films, fluororesin films, polyvinyl chloride films, AES resin films, and ASA resin films. The nonwoven fabric is made of synthetic resin fibers, such as polyamide, polyester, polyacrylic, polyolefin, or polyurethane. Examples of metal foils include metal foils of iron and its alloys, metal foils of metals having a lower electric potential than iron, such as chromium, zinc, titanium, aluminum, and magnesium, and metal foils of metals having a higher electric potential than iron, such as gold, silver, copper, tin, nickel, and cobalt. These sheet-like materials can be used alone or in combination of two or more. From the viewpoint of protecting the pressure-sensitive adhesive layer, the substrate is preferably a resin film, more preferably a PET film or a fluororesin film. In addition, in the case of a resin film, the interfacial strength can be easily increased by modifying the surface of the substrate by corona treatment or by providing an undercoat layer.
[0014] The thickness of the substrate is not particularly limited, but is preferably 10 to 500 μm, more preferably 30 to 400 μm, and further preferably 40 to 300 μm. When the substrate has a thickness of 10 μm or more, it can function as a support. When the substrate has a thickness of 500 μm or less, it is easy to increase the adhesion to concrete structures.
[0015] The surface of the substrate on the side of the adhesive layer may be surface-modified by corona treatment. This can further increase the interfacial strength between the substrate and the adhesive layer in the concrete repair tape. The treatment intensity when carrying out the corona treatment is, for example, 0.05 to 0.5 kW, and the conveying speed is, for example, 0.5 to 20 m / min.
[0016] (Undercoat layer) The concrete repair tape of the present invention preferably further comprises an undercoat layer on the adhesive layer side of the substrate, which can further improve the interfacial strength between the substrate and the adhesive layer. Examples of the polymer constituting the undercoat layer include aminoethylated acrylic polymer, polyethyleneimine, polyurethane water dispersion, isocyanate-based compounds, modified polybutadiene, and organic titanate-based compounds. Aminoethylated acrylic polymer is a primary amino group-containing acrylic polymer with polyethyleneimine grafted to the side chain. Commercially available aminoethylated acrylic polymers include "Polyment NK-350" manufactured by Nippon Shokubai Co., Ltd. Polyethyleneimine is a water-soluble polymer obtained by polymerizing ethyleneimine. Commercially available polyethyleneimine products include "Epomin P-1000" and "Epomin P-3000" manufactured by Nippon Shokubai Co., Ltd. Polyurethane water dispersions are self-dispersing polyurethane resins that have been given a small amount of hydrophilic groups or hydrophilic segments, or hydrophobic polyurethane resins that have been forcibly emulsified with a surfactant. Commercially available polyurethane water dispersions include "Superflex Series" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Of these polymers, aminoethylated acrylic polymers and polyethyleneimines are preferred from the viewpoint of the interfacial strength between the substrate and the pressure-sensitive adhesive layer. The undercoat can be formed by applying an undercoat paint containing the above-mentioned polymer to a substrate, and drying it as necessary.
[0017] <Amount of application> The coating weight (wet) of the undercoat layer is preferably 2 g / m 2 The coating amount (wet) is 2g / m 2 More than 20g / m 2 By setting the coating amount (wet) of the undercoat layer to 4 g / m or less, the interfacial strength between the substrate and the pressure-sensitive adhesive layer can be further improved. From this viewpoint, the coating amount (wet) of the undercoat layer is more preferably 4 g / m or less. 2 More than 15g / m 2 More preferably, it is 7 g / m or less. 2 More than 12g / m2 The following is the result.
[0018] (Adhesive layer) <Adhesive> The adhesive layer is preferably formed of an adhesive. The type of adhesive is not particularly limited, but examples thereof include acrylic adhesives, rubber adhesives, urethane adhesives, and silicone adhesives. These may be used alone or in combination. Among these, the pressure-sensitive adhesive layer is preferably formed from an acrylic pressure-sensitive adhesive.
[0019] (Acrylic adhesive) The acrylic pressure-sensitive adhesive is a pressure-sensitive adhesive containing an acrylic polymer obtained by polymerizing a polymerizable monomer including a (meth)acrylic acid alkyl ester monomer (A). In this specification, the term "(meth)acrylic acid alkyl ester" refers to a concept including both acrylic acid alkyl ester and methacrylic acid alkyl ester, and the same applies to other similar terms. In addition, the term "polymerizable monomer" refers to a concept that can include not only a compound having no repeating unit, but also a monomer itself having a repeating unit, such as the olefin polymer (C) described later, as long as it is a compound that copolymerizes with the (meth)acrylic acid alkyl ester monomer (A).
[0020] ((Meth)acrylic acid alkyl ester monomer (A)) The (meth)acrylic acid alkyl ester monomer (A) is an ester of (meth)acrylic acid and an aliphatic alcohol, and is preferably an alkyl ester derived from an aliphatic alcohol in which the carbon number of the alkyl group of the aliphatic alcohol is preferably 2 to 14, more preferably 4 to 10. When the carbon number of the alkyl group is within this range, the adhesive strength is easily increased, and the storage modulus at 23°C of the adhesive described below is easily adjusted to a predetermined range.
[0021] Specific examples of the (meth)acrylic acid alkyl ester monomer (A) include ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, and tetradecyl (meth)acrylate. Among these, n-butyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate are preferred, with 2-ethylhexyl (meth)acrylate being more preferred. The (meth)acrylic acid alkyl ester monomers may be used alone or in combination of two or more kinds.
[0022] The constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) constitutes the main component in the adhesive layer, and its content is generally 30% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more based on the total amount of the adhesive layer. In this way, by increasing the content of the (meth)acrylic acid alkyl ester monomer (A), it is possible to impart the desired adhesive strength to the adhesive layer. In addition, the content of the constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) is, for example, 97% by mass or less, preferably 95% by mass or less, more preferably 90% by mass or less in order to contain a certain amount or more of other components. The content of the constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) in the pressure-sensitive adhesive layer is substantially the same as the content of the (meth)acrylic acid alkyl ester monomer (A) in the pressure-sensitive adhesive composition described below, and can be expressed interchangeably. The same applies to components other than the component (A), such as the components (B) and (C) described below.
[0023] (Polar Group-Containing Vinyl Monomer (B)) The polymerizable monomer preferably contains a polar group-containing vinyl monomer (B) in addition to the (meth)acrylic acid alkyl ester monomer (A). The polar group-containing vinyl monomer (B) has a polar group and a vinyl group. By using the polar group-containing monomer (B), the adhesive strength to the adherend is easily improved. Examples of the polar group-containing vinyl monomer (B) include carboxylic acid vinyl esters such as vinyl acetate, carboxylic acids containing a vinyl group such as (meth)acrylic acid and itaconic acid, and their anhydrides, vinyl monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyoxyethylene (meth)acrylate, and polyoxypropylene (meth)acrylate, and nitrogen-containing vinyl monomers such as (meth)acrylonitrile, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinyllaurolactam, (meth)acryloylmorpholine, (meth)acrylamide, dimethyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and dimethylaminomethyl(meth)acrylate. Among these, (meth)acrylic acid, carboxylic acids containing a vinyl group such as itaconic acid, and their anhydrides and nitrogen-containing vinyl monomers are preferred, and (meth)acrylic acid (particularly acrylic acid), (meth)acryloylmorpholine, and dimethyl(meth)acrylamide are more preferred. These polar group-containing vinyl monomers (B) may be used alone or in combination of two or more.
[0024] When the polar group-containing vinyl monomer (B) is used, the content of the structural unit derived from the polar group-containing vinyl monomer (B) in the adhesive layer is preferably 1 to 15 parts by mass, more preferably 2 to 12 parts by mass, and even more preferably 3 to 10 parts by mass, per 100 parts by mass of the structural unit derived from the (meth)acrylic acid alkyl ester monomer (A). By setting the content of the polar group-containing vinyl monomer (B) within such a range, the adhesive strength of the concrete repair tape is easily improved.
[0025] (Olefin polymer (C)) The polymerizable monomer preferably further contains an olefin polymer (C) having a polymerizable bond at one end. By using such an olefin polymer (C), the adhesive strength of the concrete repair tape can be easily improved. The polymerizable bond means an unsaturated carbon-carbon bond capable of polymerizing with a polymerizable monomer, and examples thereof include an unsaturated double bond, and preferably a (meth)acryloyl group. The olefin polymer (C) may be a polyolefin having a (meth)acryloyl group at one end. The polyolefin is a polymer of an aliphatic hydrocarbon compound having a double bond, such as ethylene, propylene, butane, butadiene, isoprene, or the like, or a hydrogenated product thereof.
[0026] Examples of polyolefins having a (meth)acryloyl group at one end include polyethylene having a (meth)acryloyl group at one end, which is prepared by reacting polyethylene having an epoxy group at one end with (meth)acrylic acid. In addition, examples include polybutadiene having a (meth)acryloyl group at one end or a hydrogenated product thereof, and examples of commercially available products thereof include "L-1253" manufactured by Kuraray Co., Ltd.
[0027] The number average molecular weight of the olefin polymer (C) is preferably 500 to 20000, more preferably 1000 to 10000. The number average molecular weight may be measured by gel permeation chromatography (GPC) and calculated using a calibration curve of standard polystyrene. In addition, the content of the structural unit derived from the olefin polymer (C) in the pressure-sensitive adhesive layer is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 4 to 12 parts by mass, per 100 parts by mass of the structural unit derived from the (meth)acrylic acid alkyl ester monomer (A).
[0028] (Crosslinking agent (D)) The polymerizable monomer preferably further contains a crosslinking agent. Examples of the crosslinking agent include a polyfunctional monomer having two or more vinyl groups, and preferably a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups. The use of a polyfunctional monomer makes it easier to adjust the adhesive strength of the adhesive layer to an appropriate range. The polyfunctional (meth)acrylate is not particularly limited, and examples thereof include bifunctional alkyl (meth)acrylates such as hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, proxied trimethylolpropane triacrylate, proxied glyceryl triacrylate, neopentyl glycol adipate diacrylate, and the like, as well as polymers such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and liquid hydrogenated 1,2-polybutadiene di(meth)acrylate. Among these polyfunctional (meth)acrylates, polymers are preferred, and liquid hydrogenated 1,2-polybutadiene diacrylate is more preferred. Commercially available liquid hydrogenated 1,2-polybutadiene diacrylates include "TEAI-1000" manufactured by Nippon Soda Co., Ltd. In addition, bifunctional alkyl (meth)acrylates are also preferred, and commercially available products include A-HD-N of the NK Ester series manufactured by Shin-Nakamura Chemical Co., Ltd. The content of the structural unit derived from the crosslinking agent in the pressure-sensitive adhesive layer is preferably 0.005 to 0.1 parts by mass, more preferably 0.01 to 0.09 parts by mass, and even more preferably 0.02 to 0.08 parts by mass, per 100 parts by mass of the structural unit derived from the (meth)acrylic acid alkyl ester monomer (A).
[0029] (tackifier resin) The acrylic adhesive may contain a tackifier resin from the viewpoint of improving adhesive strength. As the tackifier resin, a tackifier resin having low polymerization inhibition properties, such as hydrogenated terpene resin, hydrogenated rosin, disproportionated rosin resin, petroleum resin, etc., is preferable. Among these, hydrogenated tackifier resins are preferable because tackifier resins having many double bonds inhibit polymerization reactions, and hydrogenated petroleum resins are particularly preferable. From the viewpoint of improving the cohesive strength and adhesive strength of the adhesive, the softening point of the tackifier resin may be about 95° C. or higher, but preferably includes one that is 120° C. or higher, and for example, one that is 95° C. or higher and lower than 120° C. may be used in combination with one that is 120° C. or higher and 150° C. or lower. The softening point may be measured by the ring and ball method specified in JIS K2207. The content of the tackifier resin in the acrylic adhesive is preferably 5 to 40 parts by mass, more preferably 7 to 35 parts by mass, and even more preferably 10 to 25 parts by mass, per 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0030] (fine particles) The acrylic adhesive may contain fine particles, which can improve the adhesive strength. Examples of the fine particles include inorganic hollow particles such as glass balloons, shirasu balloons, and fly ash balloons; organic hollow particles made of polymethyl methacrylate, acrylonitrile-vinylidene chloride copolymers, polystyrene, and phenolic resins; inorganic fine particles such as glass beads, silica beads, and synthetic mica; and organic fine particles such as ethyl polyacrylate, polyurethane, polyethylene, and polypropylene. The content of the fine particles in the acrylic pressure-sensitive adhesive is preferably 0.1 to 15 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.7 to 7 parts by mass, based on 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0031] (Other Ingredients) The acrylic adhesive used in the adhesive layer may contain, in addition to the components described above, various additives conventionally used in adhesives, such as plasticizers, softeners, pigments, dyes, polymerization initiators, flame retardants, and thickeners.
[0032] (Method of manufacturing acrylic adhesive and adhesive layer) The acrylic adhesive can be obtained by irradiating a pressure-sensitive adhesive composition containing the above-mentioned polymerizable monomer, and optionally a sacrificial anticorrosive metal and a conductive material with light to polymerize the polymerizable monomer. The pressure-sensitive adhesive composition may also contain at least one of the above-mentioned tackifier resin, fine particles, and other components as required. More specifically, first, the polymerizable monomer, the sacrificial corrosion protection metal and conductive material which are blended as necessary, and further the tackifier resin, fine particles, and other components which are blended as necessary are placed in a reaction vessel such as a glass vessel and mixed to obtain a pressure-sensitive adhesive composition. Next, in order to remove dissolved oxygen in the pressure-sensitive adhesive composition, an inert gas such as nitrogen gas is generally supplied to purge the oxygen. Then, the pressure-sensitive adhesive composition is applied onto a release sheet, or onto a support such as a resin film, woven fabric, or nonwoven fabric, and then irradiated with light to polymerize the polymerizable monomer, thereby obtaining a pressure-sensitive adhesive layer. The steps from coating or impregnation with the pressure-sensitive adhesive composition to the step of irradiating with light are preferably carried out in an inert gas atmosphere or in a state in which oxygen is blocked by a film or the like. In the present production method, the pressure-sensitive adhesive composition obtained by mixing the components may be pre-polymerized before being applied to a release sheet, a support or the like in order to increase the viscosity.
[0033] (Rubber adhesive) Next, the rubber-based adhesive used in the adhesive layer will be described. The rubber-based adhesive contains a rubber component and a tackifier resin, and it is preferable to use a styrene-isoprene block copolymer as the rubber component. The styrene-isoprene block copolymer has a diblock ratio of preferably 25 to 70% by mass, more preferably 30 to 65% by mass, and even more preferably 45 to 60% by weight. Here, the diblock refers to a diblock consisting of styrene and isoprene. By setting the diblock ratio within the above range, it becomes easier to increase the adhesive strength. In addition to the diblock, the styrene-isoprene block copolymer also contains one having three or more blocks, such as a triblock consisting of a styrene, isoprene, and styrene block.
[0034] The amount of styrene in the styrene-isoprene block copolymer is not particularly limited, but is preferably 14 to 24% by mass, and more preferably 15 to 18% by mass. If the amount of styrene is 14% by mass or more, the adhesive tends to have high cohesiveness. If the amount of styrene is 24% by mass or less, the cohesive strength becomes moderate and adhesive strength is easily expressed. The molecular weight of the styrene-isoprene block copolymer is not particularly limited, but the mass average molecular weight is preferably 100,000 to 400,000, and more preferably 150,000 to 250,000. The mass average molecular weight here refers to the molecular weight measured in terms of polystyrene by a GPC (gel permeation chromatography) method.
[0035] The tackifier resin used in the rubber-based adhesive can be any of various types, but is preferably a petroleum-based resin, a terpene resin, or a coumarone resin. The tackifier resin may be used alone or in combination of two or more types, but it is preferable to use a petroleum-based resin in combination with at least one selected from a terpene resin and a coumarone resin. Such a combination of tackifier resins makes it easier to improve the adhesive strength. Examples of the petroleum resin include aliphatic petroleum resin (C5 petroleum resin), alicyclic petroleum resin, aromatic petroleum resin, etc., and from the viewpoint of compatibility with the styrene-isoprene block copolymer, aliphatic petroleum resin is preferred. In addition, it is preferable to use a petroleum resin having a softening point of about 90 to 120°C. The terpene resin may have a softening point of about 80 to 120° C., but from the viewpoint of ensuring adhesive strength, it is preferable that the softening point is less than 100° C. The coumarone resin used has a softening point of preferably 110 to 130° C., more preferably 115 to 125° C., in order to ensure cohesive strength.
[0036] The amount of the tackifier resin is preferably 60 to 250 parts by mass, more preferably 100 to 200 parts by mass, and even more preferably 110 to 180 parts by mass, per 100 parts by mass of the rubber component. By setting the amount of the tackifier resin within the above range, it is possible to improve the cohesive force and impart appropriate adhesive strength. When a petroleum-based resin is used in combination with at least one selected from a terpene resin and a coumarone resin, the amount of the petroleum-based resin is preferably 50 to 200 parts by mass, more preferably 60 to 150 parts by mass, and more preferably 60 to 110 parts by mass, relative to 100 parts by mass of the rubber component. On the other hand, the amount of the terpene resin is preferably 10 to 70 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 30 to 50 parts by mass, relative to 100 parts by mass of the rubber component. Furthermore, the amount of the coumarone resin is preferably 10 to 60 parts by mass, more preferably 15 to 50 parts by mass, and even more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the rubber component. The rubber-based adhesive may contain the above-mentioned fine particles, like the acrylic-based adhesive, and may also contain a sacrificial corrosion protection metal, a conductive material, a softener, an antioxidant, a filler, etc., as necessary.
[0037] (Urethane adhesive) The urethane-based adhesive is not particularly limited, and examples thereof include urethane resins obtained by reacting at least a polyol with a polyisocyanate compound. Examples of the polyol include polyether polyol, polyester polyol, polycarbonate polyol, polycaprolactone polyol, etc. Examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, hexamethylene diisocyanate, etc. These urethane adhesives may be used alone or in combination of two or more. In addition, as the urethane-based adhesive, a urethane resin obtained by reacting a polyurethane polyol with a polyfunctional isocyanate-based curing agent may be used. The polyurethane polyol may be a reaction product of the above-mentioned polyol with a polyisocyanate compound, or a reaction product of a polyol with a polyisocyanate compound and a chain extender such as a diamine. As the polyfunctional isocyanate-based curing agent, any compound having two or more isocyanate groups may be used, and the above-mentioned isocyanate compounds may be used. The urethane-based adhesive may contain the above-mentioned fine particles in addition to the urethane resin, and may also contain a tackifier resin, a sacrificial corrosion-protective metal, a conductive material, a softener, an antioxidant, a filler, etc., as necessary.
[0038] (Silicone adhesive) Examples of silicone-based adhesives include silicone-based adhesives of addition reaction type, peroxide curing type, or condensation reaction type. Among them, addition reaction type silicone-based adhesives are preferably used from the viewpoint of being curable at low temperature in a short time. The addition reaction type silicone-based adhesive is cured when the adhesive layer is formed. When an addition reaction type silicone-based adhesive is used as the silicone-based adhesive, the silicone-based adhesive may contain a catalyst such as a platinum catalyst. The silicone-based adhesive may contain fine particles, and may also contain a crosslinking agent and various additives for controlling adhesive strength.
[0039] (Thickness) The thickness of the adhesive layer is preferably 100 μm or more. By making the thickness 100 μm or more, the adhesive strength of the concrete repair tape can be further improved. From this viewpoint, the thickness of the adhesive layer is more preferably 250 μm or more, even more preferably 300 μm or more, and even more preferably 500 μm or more. In addition, the upper limit of the thickness of the adhesive layer is not particularly limited, but from the viewpoint of the deterioration of workability due to the weight increase while obtaining the effect of improving the adhesive strength of the concrete repair tape according to the thickness, it is, for example, 2000 μm, and 1200 μm or less is preferable.
[0040] (mesh) From the viewpoint of production cost, it is preferable that the adhesive layer does not include a mesh. Furthermore, in many conventional concrete repair tapes, a mesh is provided and the adhesive layer is impregnated with the mesh to ensure strength. The concrete repair tape of the present invention has excellent concrete peeling prevention performance even if the adhesive layer does not include a mesh. The mesh is generally formed by arranging warp threads and weft threads so that they cross each other, and has openings between the warp threads and weft threads, into which the pressure-sensitive adhesive layer fits.
[0041] (Paint film) The concrete repair tape of the present invention preferably further comprises a coating film provided on the surface of the substrate opposite to the surface of the adhesive layer. This can further improve the weather resistance of the concrete repair tape of the present invention. Examples of paints for forming the coating film include fluorine-based paints and silicon-based paints. Among these paints, fluorine-based paints are preferred from the viewpoint of weather resistance. The coating film can be formed by applying the above-mentioned paint to the substrate and drying it as necessary.
[0042] From the viewpoint of weather resistance of the concrete repair tape of the present invention, the thickness of the coating film (dry) is preferably 25 μm or more, more preferably 30 μm or more, and further preferably 35 μm or more. The upper limit of the range of the coating film thickness is usually 60 μm.
[0043] (Composition of concrete repair tape) 1, concrete repair tape 10 is preferably a single-sided adhesive tape having a substrate 12 and an adhesive layer 11 provided on one side of substrate 12. This allows adhesive layer 11 to be protected by substrate 12. The concrete repair tape in each drawing is used by being attached to a concrete structure with surface 11A of adhesive layer 11 as the adhesive surface.
[0044] In order to improve the interfacial strength between the substrate 12 and the adhesive layer 11, the concrete repair tape 10 may further include an undercoat layer 13 on the adhesive layer side of the substrate 12, as shown in FIG. 2.
[0045] In order to improve weather resistance, a coating film 14 may be further formed on the surface of the substrate 12 opposite to the surface on which the pressure-sensitive adhesive layer is formed, as shown in Fig. 3. In this case, the undercoat layer may be omitted.
[0046] (Method of using the concrete repair tape of the present invention) The concrete repair tape of the present invention may be applied directly to a concrete structure, but it is preferable to coat the surface of the concrete structure with a primer paint, and then apply the concrete repair tape of the present invention onto the primer layer formed by the primer paint while the primer paint applied to the concrete structure is still wet.
[0047] The primer coating preferably contains an epoxy resin. Since the epoxy resin has excellent adhesion to concrete structures, it can provide high-level concrete spalling prevention performance. Here, the epoxy resin is preferably a resin having at least two epoxy groups in one molecule, and is obtained by reacting, for example, a polyhydric alcohol or a polyhydric phenol with a halohydrin. Specific examples include bisphenol A type epoxy resin, halogenated bisphenol A type epoxy resin, novolac type epoxy resin, polyglycol type epoxy resin, bisphenol F type epoxy resin, epoxidized oil, 1,6-hexanediol diglycidyl ether, and neopentyl glycol diglycidyl ether, as well as modified epoxy resins such as amine-modified epoxy resin, isocyanate-modified epoxy resin, acrylic-modified epoxy resin, urethane-modified epoxy resin, and polyester-modified epoxy resin, which are modified products of such epoxy resins. These epoxy resins may be used alone or in combination of two or more.
[0048] The above primer coating may contain other components, such as other resins, curing agents, pigments, thickeners, rust inhibitors, dispersants, defoamers, leveling agents, anti-settling agents, anti-sagging agents, curing accelerators, anti-algae agents, anti-mold agents, preservatives, ultraviolet absorbers, and light stabilizers, as necessary.
[0049] The means for applying the primer coating is not particularly limited, and known coating means such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, and spray coating (e.g., aerosol spray coating, air spray coating, airless spray coating, etc.) can be used.
[0050] The concrete repair tape of the present invention is preferably used by being applied to damaged areas of existing concrete, and may be used as a repair tape that suppresses deterioration of the damaged areas by being applied to the damaged areas. In particular, the concrete repair tape of the present invention is preferably used for preventing spalling, and may be applied to damaged areas that are at risk of spalling to prevent the damaged areas from spalling. In addition, the concrete repair tape can be used as an emergency repair tape. For example, when inspecting existing concrete, if damaged areas that require repair are found, the tape can be applied to the damaged areas as an emergency repair until the concrete can be re-poured. EXAMPLES
[0051] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0052] [Evaluation method]
[0053] In the examples and comparative examples, the concrete repair tapes were evaluated by the following evaluation methods. <Thickness> The measurement was performed using a dial gauge.
[0054] <Interfacial strength between substrate and adhesive layer> Each of the concrete repair tapes of the examples and comparative examples was laminated to a PET film / thickness of 50 μm (used as the evaluation film) coated with NK350, heated at 100° C. for 10 minutes, and then cut to a width of 24 mm to prepare a test specimen. The obtained test specimen was subjected to a tensile test using a tensile tester (RTG1310, manufactured by AND Co.) under conditions of 23° C., 50% humidity, and a speed of 200 mm / min, with the substrate on one side and the adhesive layer and evaluation film on the other side, and a tensile test was performed to measure the interfacial strength between the substrate and the adhesive layer.
[0055] <Tensile strength and elongation at break> Each of the concrete repair tapes of the examples and the comparative examples was cut to a width of 24 mm to prepare a test piece. The obtained test pieces were subjected to a tensile test using a tensile tester (RTG1310, manufactured by AND Co.) under the conditions of 23°C, 50% humidity, 5 mm sample chuck distance, and 300 mm / min speed, to measure the tensile breaking strength and tensile breaking elongation.
[0056] <Gloss retention> The gloss retention was measured as follows in accordance with JIS K 5600-4-7. The concrete repair tapes of the examples and comparative examples were subjected to a weather resistance test in cycle A according to JIS K 5600-7-7. The gloss of the surface of the concrete repair tape after the test was measured. The gloss retention rate was calculated by the following formula using the gloss value of the concrete repair tape after the test (gloss value after the test) and the gloss value of the concrete repair tape before the test (gloss value before the test). Gloss retention (%) = 100 x (gloss value after test) / (gloss value before test) The gloss value is a gloss value under a geometric condition of 60°, and is a value measured using a haze meter (manufactured by Horiba Ltd., product name: "IG-340").
[0057] <Load resistance test> A primer paint (manufactured by Dai Nippon Toryo Co., Ltd., product name "Regiguard HG Primer") was roller-painted onto the concrete substrate. After the primer coating was applied to the concrete substrate, a concrete repair tape was placed on the primer layer formed from the primer coating, and the primer layer and the concrete repair tape were then dried for 168 hours at a temperature of 23°C and a relative humidity of 50%. After drying, the concrete substrate on which the concrete repair sheet was placed was subjected to a spalling prevention performance test in accordance with the Metropolitan Expressway Company, Bridge Structure Design Guidelines, Concrete Piece Spalling Prevention Edition, August 2006 edition, and the punching load (kN) per φ10 cm was measured. Evaluation was based on the following criteria. ○··Push-out load per φ10cm is 1.5kN or more × Push-out load per φ10cm is less than 1.5kN
[0058] [Substrate treatment] (Corona treatment) A corona discharge device (manufactured by Kasuga Denki Co., Ltd.) was used to carry out a corona treatment on the surface of the substrate under the conditions shown in Table 1.
[0059] (Undercoat layer) Using a Mayer bar coater, a primer layer was formed on the surface of the substrate using the paint and Mayer bar shown in Table 1.
[0060] (Paint film) A coating material described below was applied to the surface of the substrate opposite to the surface that had been subjected to the corona treatment or the surface on which the undercoat layer had been formed, and then dried to form a coating film. The thickness of the dried coating film was 40 μm.
[0061] [Examples 1 to 14, Comparative Examples 1 to 4] A pressure-sensitive adhesive composition was prepared according to the formulation shown in Table 1. The pressure-sensitive adhesive composition was purged with nitrogen to remove dissolved oxygen. The pressure-sensitive adhesive composition was then applied onto a release-treated PET film, which was then covered with another release-treated PET film. In this state, the ultraviolet irradiation intensity was 5 mW / cm. 2 The lamp intensity of the chemical lamp was adjusted so that the adhesive composition was cured by irradiating the adhesive composition with ultraviolet light for 5 minutes. Next, one side of the release-treated PET film was peeled off, and the substrate described in Table 1 was laminated on the adhesive surface. For substrates that had been corona-treated, the corona-treated surface of the substrate was laminated. When a primer layer was formed on the substrate, the primer layer surface was laminated. When a primer layer was further formed on the corona-treated surface of the substrate, the primer layer surface was laminated. When neither the corona treatment nor the primer layer was formed on the substrate, the surface opposite to the surface on which the coating film of the substrate was formed was laminated. A concrete repair tape was obtained by the above procedure. The results are shown in Tables 1 to 3.
[0062] [Table 1]
[0063] [Table 2]
[0064] [Table 3]
[0065] The components in Table 1 are as follows. Olefin polymer: Product name "L-1253", manufactured by Kuraray Co., Ltd., hydrogenated polybutadiene having a (meth)acryloyl group at one end Tackifying resin 1: Product name "Alcon P140", manufactured by Arakawa Chemical Industries, Ltd., hydrogenated petroleum resin, softening point 140°C Tackifier resin 2: Product name "Alcon P100", manufactured by Arakawa Chemical Industries, Ltd., hydrogenated petroleum resin, softening point 100°C Thickener: Product name "AEROSIL 200", manufactured by Nippon Aerosil Co., Ltd., fumed silica Microparticles: Manufactured by 3M Company, product name "Glass Bubbles K25" Crosslinking agent: Shin-Nakamura Chemical Co., Ltd., NK Ester A-HD-N, bifunctional alkyl acrylate Polymerization initiator: 2,2-dimethoxy-2-phenylacetophenone Substrate 1: Polyethylene terephthalate (PET), manufactured by Toray Industries, Inc., product name "Lumirror T60" Substrate 2: Fluorine resin film, manufactured by AGC Inc., product name "Aflex 250NJ" Substrate 3: Acrylic film, manufactured by Mitsubishi Chemical Corporation, product name "Acryplene MBS121E" Coating: Fluorine-based paint, manufactured by Dai Nippon Paint Co., Ltd., product name "V-Flon #100H Smile Topcoat IG" Polymer 1: Aminoethylated acrylic polymer, manufactured by Nippon Shokubai Co., Ltd., product name "Polyment NK-350" Polymer 2: Polyethyleneimine, product name "Epomin P-1000" manufactured by Nippon Shokubai Co., Ltd. Polymer 3: Polyethyleneimine, product name "Epomin P-3000" manufactured by Nippon Shokubai Co., Ltd.
[0066] The concrete repair tapes of Examples 1 to 14 had an interface strength between the substrate and the adhesive layer of 10 N / cm or more, and a tensile strength at break of 75 N / cm or more. Therefore, it is clear that the concrete repair tapes of Examples 1 to 14 had good results in the load resistance test and were excellent in concrete peeling prevention performance. On the other hand, the concrete repair tapes of Comparative Examples 1 and 2 had an interfacial strength between the substrate and the adhesive layer of less than 10 N / cm, and the concrete repair tapes of Comparative Examples 3 and 4 had a tensile breaking strength of less than 75 N / cm. Therefore, it is clear that the concrete repair tapes of Comparative Examples 1 to 4 had poor results in the load resistance test and were inferior in concrete peeling prevention performance to the concrete repair tapes of Examples 1 to 14. [Explanation of symbols]
[0067] 10 Concrete repair tape 11 Adhesive layer 12 Base material 13 Undercoat layer 14 Coating
Claims
1. A substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate, The interfacial strength between the substrate and the pressure-sensitive adhesive layer is 10 N / cm or more; A concrete repair tape having a tensile breaking strength of 75 N / cm or more.
2. The concrete repair tape according to claim 1 , further comprising an undercoat layer on the surface of the substrate facing the adhesive layer.
3. 2. The concrete repair tape according to claim 1, wherein the surface of the substrate on which the adhesive layer is formed has been subjected to surface modification by corona treatment.
4. 4. The concrete repair tape according to claim 1, which has a gloss retention of 70% or more after a weather resistance test carried out in cycle A in accordance with JIS K 5600-7-7.
5. The concrete repair tape according to any one of claims 1 to 3, which has a tensile elongation of 100% or more.
6. The concrete repair tape according to any one of claims 1 to 3, wherein the adhesive layer has a thickness of 100 µm or more.
7. 4. The concrete repair tape according to claim 1, wherein the substrate is a fluororesin film.
8. The concrete repair tape according to any one of claims 1 to 3, further comprising a coating film provided on a surface of the substrate opposite to the surface on which the pressure-sensitive adhesive layer is formed.
9. 9. The concrete repair tape according to claim 8, wherein the coating is a coating of a fluorine-based paint.
Citation Information
Patent Citations
Concrete peeling prevention method
JP2019178508A
Cited By
DRIVE UNIT FOR A MUSCLE-POWERED VEHICLE
DE102025131017A1