Catalyst support carbon material and method for manufacturing catalyst support carbon material
An elongated graphene-containing mesoporous carbon structure addresses gas permeability and explosion risks in catalyst carriers, enhancing performance and safety in catalyst carrier applications.
Patent Information
- Application Number
- JP2024045333
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing carbon materials for catalyst carriers, such as those described in Patent Document 1, suffer from poor gas permeability and the risk of large-scale explosions during the phase separation reaction of silver acetylide, necessitating robust reactors.
A carbon material for catalyst carriers is developed with an elongated mesoporous structure containing graphene, featuring specific dimensions and pore characteristics, and a production method involving controlled heating to reduce the risk of explosions and enhance gas permeability.
The new carbon material exhibits improved gas permeability and electrical conductivity, with reduced explosion risk, enabling efficient gas movement and increased catalyst support area.
Smart Images

Figure 2024144257000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon material for a catalyst support and a method for producing the same. [Background technology]
[0002] As this type of carbon material for a catalyst support and a manufacturing method thereof, for example, there are the carbon material and the manufacturing method described in Patent Document 1. The carbon material described in Patent Document 1 is a carbon dendritic nanostructure (called mesoporous carbon nano dendrite). The carbon material is obtained by synthesizing silver acetylide and then via a phase separation reaction. First, silver acetylide is generated as a precipitate by blowing acetylene gas into an aqueous ammonia solution of silver nitrate while irradiating the solution with ultrasonic waves. After separating water from the silver acetylide precipitate, heat treatment is performed at a temperature of 60°C to 80°C in a vacuum atmosphere for 12 hours or more. This causes segregation of silver acetylide, and a metal-encapsulated dendritic nanostructure containing metallic silver particles is formed. If the precipitate is completely dried, it becomes unstable and may exhibit an explosive reaction due to frictional stimuli, etc.
[0003] Next, the silver acetylide precipitate is heated to a temperature of 160°C to 200°C. The silver acetylide undergoes an explosive phase separation reaction at around 150°C, causing the encapsulated silver to erupt, resulting in a carbon dendritic nanostructure with numerous eruptions (mesopores) on its surface and inside. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6198810 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the carbon material described in Patent Document 1 is a dendritic nanostructure, and therefore gases and the like tend to remain in the pores. For this reason, there is a demand for a carbon material for a catalyst support that is excellent in permeability to gases and the like.
[0006] Furthermore, in the case of the production method described in Patent Document 1, the scale of an explosion that occurs when a phase separation reaction of silver acetylide occurs is large, which requires a reaction apparatus with high strength or increases the size of the reaction apparatus. [Means for solving the problem]
[0007] A carbon material for a catalyst support that solves the above-mentioned problems is a carbon material for a catalyst support consisting of an elongated carbon mesoporous structure containing graphene, in which the carbon mesoporous structure has a major axis of 50 nm or more and 200 nm or less and a minor axis of 30 nm or more and 100 nm or less, a pore diameter determined by analyzing a nitrogen adsorption isotherm by the Dollimore-Heal method of 1 nm or more and 20 nm or less, and an integrated pore volume of 1.5 cc / g or more and 2.5 cc / g or less.
[0008] According to this configuration, the carbon material for the catalyst support is made of an elongated, so-called bean-shaped, mesoporous carbon structure containing graphene. The major axis of this mesoporous carbon structure is 50 nm or more and 200 nm or less, and the minor axis is 30 nm or more and 100 nm or less. Therefore, compared with conventional dendritic mesoporous carbon structures, gases and the like present in the pores can move to the outside more easily. Therefore, the residence time of gases and the like in the pores can be shortened.
[0009] According to the above-mentioned configuration, the pore diameter is 1 nm or more and 20 nm or less, and the cumulative pore volume is 1.5 cc / g or more and 2.5 cc / g or less. Since the cumulative pore volume is larger than that of the conventional material, the permeability of gases and the like is increased. Therefore, it is possible to provide a carbon material for a catalyst carrier that has high electrical conductivity and excellent permeability of gases and the like.
[0010] A method for producing a carbon material for a catalyst support that solves the above-mentioned problems includes the steps of preparing a solution containing silver or a silver salt, blowing acetylene gas into the solution to produce dendritic carbon nanostructures made of silver acetylide and consisting of branched rod-shaped or ring-shaped bodies, heating the dendritic carbon nanostructures in a water bath at a temperature of 80°C or higher to break the dendritic carbon nanostructures into elongated shapes and generate ion pairs between silver cluster cations and carbon cluster anions, and expanding the elongated carbon nanostructures by heat generation associated with charge recombination of the ion pairs to produce a carbon mesoporous structure containing silver, and subjecting the carbon mesoporous structure to a heat treatment at a temperature of 1600°C to 2000°C under a reduced pressure atmosphere or an inert gas atmosphere for 0.5 hours or more and 2.0 hours or less.
[0011] According to this configuration, the dendritic carbon nanostructure is heated in a water bath at a temperature of 80° C. or higher, and the water of crystallization that stabilizes the shape of the carbon nanostructure is evaporated. As the water of crystallization evaporates, an external force acts on the dendritic carbon nanostructure, and the carbon nanostructure is broken into elongated shapes.
[0012] In addition, by heating as described above, the silver ions constituting the carbon nanostructure grow into silver cluster cations, and the carbon ions grow into carbon cluster anions covering the silver cluster cations. This generates ion pairs of silver cluster cations and carbon cluster anions. The elongated carbon nanostructure expands due to heat generated by charge recombination of these ion pairs, generating a carbon mesoporous structure containing silver. In detail, when the ion pairs recombine, the positive and negative charges approach each other to become neutral charges. At this time, heat of about 2000°C is generated locally with the movement of electrons and holes. This heat causes carbon to turn into graphene, and a carbon mesoporous structure containing silver is generated.
[0013] Here, the silver ions and carbon ions become silver cluster cations and carbon cluster anions, and the number of pairs of positive and negative charges decreases, so the risk of explosion is reduced. In the state of silver cluster cations and carbon cluster anions, silver acetylide does not explode on a large scale unless the temperature is 200°C or higher. This makes silver acetylide easy to handle at room temperature. However, although silver acetylide becomes easy to handle at room temperature, it is necessary to be careful when attempting to produce the above carbon mesoporous structure of about 100g or more, as a chain reaction of charge recombination occurs when heated to about 300°C, which may cause a large explosion.
[0014] The carbon mesoporous structure produced as described above has low crystallinity of graphene. According to the above configuration, by subjecting the carbon mesoporous structure to the heat treatment as described above, the crystallinity of graphene is increased. In addition, the encapsulated silver is sublimated and removed.
[0015] Therefore, a carbon material for a catalyst support, which is made of an elongated mesoporous carbon structure containing graphene, can be easily produced. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is an SEM image of a carbon material for a catalyst support according to one embodiment. [Diagram 2] FIG. 2 is another SEM image of the carbon material for a catalyst support according to one embodiment. [Diagram 3] FIG. 3 is a TEM image of a carbon material for a catalyst support according to one embodiment. [Figure 4] FIG. 4 is another TEM image of the carbon material for a catalyst support according to one embodiment. [Diagram 5] FIG. 5 is a flow chart showing a manufacturing procedure of a carbon material for a catalyst support according to one embodiment. [Figure 6] Figure 6 shows an SEM image of mesoporous carbon nanodendrites as a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, one embodiment of a carbon material for a catalyst support and a method for producing a carbon material for a catalyst support will be described with reference to FIGS. As shown in Figures 1 to 4, the carbon material for catalyst support (hereinafter referred to as carbon material) is composed of an elongated carbon mesoporous structure containing graphene. The inventors of the present application have named the carbon material Graphene Walled Carbon Nano-Sponge.
[0018] The carbon mesoporous structure has a major axis of 50 nm or more and 200 nm or less and a minor axis of 30 nm or more and 100 nm or less. The carbon mesoporous structure is in the shape of a bean. The pore diameter of the carbon mesoporous structure is 1 nm or more and 20 nm or less. The cumulative pore volume of the carbon material is 1.5 cc / g or more and 2.5 cc / g or less. The pore diameter and cumulative pore volume were determined by analyzing the nitrogen adsorption isotherm by the Dollimore-Heal method.
[0019] The BET specific surface area of the carbon mesoporous structure is 1500-1800m 2 It is preferable that the molecular weight is 1 / g. The volume of micropores with pore diameters of 2 nm or less in the carbon mesoporous structure is preferably 0.80 cc / g or more and 0.95 cc / g or less.
[0020] As shown in Figures 3 and 4, the carbon mesoporous structure is preferably composed mainly of graphene bilayer films, and includes graphene trilayer films and graphene quadruple layer films.
[0021] The carbon material of the present embodiment can be applied to, for example, a catalyst layer constituting a single cell of a polymer electrolyte fuel cell. In this case, catalytic metal particles such as platinum having a diameter of several nm are supported in a highly dispersed state within the pores.
[0022] Next, a manufacturing procedure for the carbon material of this embodiment will be described with reference to FIG. As shown in FIG. 5, the method for producing a carbon material includes a solution preparation step, a carbon nanostructure formation step, a carbon mesoporous structure formation step, a drying treatment step, and a heat treatment step.
[0023] <Solution preparation process> The solution preparation step is a step of preparing a solution containing silver or a silver salt. In this embodiment, an aqueous ammonia solution of silver nitrate is prepared as the solution.
[0024] <Carbon nanostructure production process> The carbon nanostructure producing step is a step of producing dendritic carbon nanostructures made of silver acetylide and consisting of branched rod-shaped or ring-shaped bodies by blowing acetylene gas into the above solution.
[0025] <Mesoporous carbon structure production process> The carbon mesoporous structure generating step is a step of generating a carbon mesoporous structure encapsulating silver by heating the dendritic carbon nanostructure in a water bath at a temperature of 80° C. or higher. In this embodiment, the carbon nanostructure is heated in a water bath at a temperature of 100° C.
[0026] Specifically, the water of crystallization that stabilizes the shape of the dendritic carbon nanostructures is evaporated by heating the dendritic carbon nanostructures in a water bath at a temperature of 80° C. or higher. As the water of crystallization evaporates, an external force acts on the dendritic carbon nanostructures, causing the carbon nanostructures to break into elongated shapes.
[0027] In addition, by heating as described above, the silver ions constituting the carbon nanostructure grow into silver cluster cations, and the carbon ions grow into carbon cluster anions covering the silver cluster cations. This generates ion pairs of silver cluster cations and carbon cluster anions. The elongated carbon nanostructure expands due to heat generated by charge recombination of these ion pairs, generating a carbon mesoporous structure containing silver. In detail, when the ion pairs recombine, the positive and negative charges approach each other to become neutral charges. At this time, heat of about 2000°C is generated locally with the movement of electrons and holes. This heat causes carbon to turn into graphene, and a carbon mesoporous structure containing silver is generated.
[0028] Here, the silver ions and carbon ions become silver cluster cations and carbon cluster anions, and the number of pairs of positive and negative charges decreases, so the risk of explosion is reduced. In the state of silver cluster cations and carbon cluster anions, silver acetylide does not explode on a large scale unless the temperature is 200°C or higher. This makes silver acetylide easy to handle at room temperature. However, although silver acetylide becomes easy to handle at room temperature, it is necessary to be careful when attempting to produce the above carbon mesoporous structure of about 100g or more, as a chain reaction of charge recombination occurs when heated to about 300°C, which may cause a large explosion.
[0029] <Drying process> The drying step is a step of drying the above-mentioned mesoporous carbon structure. <Heat treatment process> The heat treatment step is a step in which the mesoporous carbon structure is heat treated in a reduced pressure atmosphere or an inert gas atmosphere at a temperature of 1600° C. to 2000° C. for 0.5 hours or more and 2.0 hours or less.
[0030] The carbon mesoporous structure after the drying process has low crystallinity of graphene. Therefore, by subjecting the carbon mesoporous structure to the heat treatment as described above, the crystallinity of graphene is increased and the encapsulated silver is sublimated and removed.
[0031] In this embodiment, the heat treatment is performed at a temperature of 1800°C using an electric furnace. As a result, mainly a graphene bilayer film is obtained. Note that, by increasing the heat treatment temperature above 1800°C, the ratio of graphene triple layer film and graphene quadruple layer in the carbon mesoporous structure increases. The larger the ratio of graphene triple layer and graphene quadruple layer, the smaller the BET specific surface area of the carbon mesoporous structure. On the other hand, the larger the ratio of graphene triple layer and graphene quadruple layer, the higher the electrical conductivity of the carbon mesoporous structure.
[0032] By carrying out each of the above steps in order, a carbon material can be obtained. Next, the operation of this embodiment will be described. The carbon material is made of an elongated, so-called bean-shaped, mesoporous carbon structure containing graphene. The long diameter of this mesoporous carbon structure is 50 nm or more and 200 nm or less, and the short diameter is 30 nm or more and 100 nm or less. Therefore, gas and the like present in the pores can move to the outside more easily than in the conventional dendritic mesoporous carbon structure shown in FIG. 6. Therefore, the residence time of gas, ions, and the like in the pores can be shortened (above, effect 1).
[0033] In addition, the pore diameter is 1 nm or more and 20 nm or less, and the cumulative pore volume is 1.5 cc / g or more and 2.5 cc / g or less. Since the cumulative pore volume is larger than that of conventional materials, the permeability of gases, ions, etc. is increased (above, effect 2).
[0034] Next, the effects of this embodiment will be described. (1) Because of the above-mentioned effects 1 and 2, it is possible to provide a carbon material for a catalyst carrier that is excellent in electrical conductivity and permeability to gases, ions, etc.
[0035] (2) The volume of micropores with pore diameters of 2 nm or less in the carbon mesoporous structure is 0.80 cc / g or more and 0.95 cc / g or less. Therefore, when the carbon material is applied to the catalyst layer that constitutes the unit cell of a polymer electrolyte fuel cell, the pores with diameters of 2 nm or less effectively function as pools that temporarily store protons. This allows the protons to efficiently come into contact with or be close to the catalyst.
[0036] (3) BET specific surface area is 1500-1800m 2 / g, the area on which the catalyst is supported can be increased, and therefore a larger amount of catalytic metal particles can be supported.
[0037] (4) The carbon mesoporous structure is mainly composed of a graphene bilayer film, and therefore has a larger BET specific surface area than a carbon mesoporous structure mainly composed of a graphene triple layer film, which allows the catalyst to be supported on a larger area, thereby enabling a larger amount of catalyst to be supported.
[0038] (5) The method for producing a carbon material includes a solution preparation step, a carbon nanostructure formation step, a carbon mesoporous structure formation step, and a heat treatment step. According to this configuration, it is possible to easily produce a carbon material for a catalyst support, which is made of an elongated carbon mesoporous structure containing graphene.
[0039] <Example of change> This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that there is no technical contradiction.
[0040] The heating temperature in the carbon mesoporous structure production process is not limited to 100°C, but may be any temperature above 80°C. The BET specific surface area of the carbon mesoporous structure is 1500m 2 / g or greater than 1800 m2 / g.
[0041] <Additional Notes> The above embodiment includes the configurations described in the following supplementary notes. [Appendix 1] A carbon material for a catalyst support, comprising an elongated carbon mesoporous structure containing graphene, The carbon mesoporous structure has a major axis of 50 nm or more and 200 nm or less and a minor axis of 30 nm or more and 100 nm or less, The pore diameter obtained by analyzing the nitrogen adsorption isotherm using the Dollimore-Heal method is 1 nm or more and 20 nm or less, and the cumulative pore volume is 1.5 cc / g or more and 2.5 cc / g or less. Carbon material for catalyst supports.
[0042] [Appendix 2] The carbon mesoporous structure has a micropore volume of pores having a diameter of 2 nm or less of 0.80 cc / g or more and 0.95 cc / g or less. Attachment 1: A carbon material for a catalyst support.
[0043] [Appendix 3] The BET specific surface area of the carbon mesoporous structure is 1500 to 1800 m 2 / g, 3. A carbon material for a catalyst support according to claim 1 or 2.
[0044] [Appendix 4] The carbon mesoporous structure is mainly composed of a graphene bilayer film. The carbon material for a catalyst support according to any one of claims 1 to 3.
Claims
1. A carbon material for a catalyst support, comprising an elongated carbon mesoporous structure containing graphene, The carbon mesoporous structure has a major axis of 50 nm or more and 200 nm or less and a minor axis of 30 nm or more and 100 nm or less, The pore diameter determined by analyzing the nitrogen adsorption isotherm by the Dollimore-Heal method is 1 nm or more and 20 nm or less, and the cumulative pore volume is 1.5 cc / g or more and 2.5 cc / g or less. Carbon material for catalyst supports.
2. The carbon mesoporous structure has a micropore volume of pores having a diameter of 2 nm or less of 0.80 cc / g or more and 0.95 cc / g or less. The carbon material for a catalyst support according to claim 1 .
3. The BET specific surface area of the carbon mesoporous structure is 1500 to 1800 m 2 / g, The carbon material for a catalyst support according to claim 1 .
4. The carbon mesoporous structure is mainly composed of a graphene bilayer film. The carbon material for a catalyst support according to any one of claims 1 to 3.
5. Providing a solution containing silver or a silver salt; A step of blowing acetylene gas into the solution to produce a dendritic carbon nanostructure made of silver acetylide and having rod-shaped or ring-shaped bodies branched therefrom; a step of heating the dendritic carbon nanostructure in a water bath at a temperature of 80° C. or higher to break the dendritic carbon nanostructure into elongated shapes and generate ion pairs of silver cluster cations and carbon cluster anions, and expanding the elongated carbon nanostructures by heat generation associated with charge recombination of the ion pairs to generate a carbon mesoporous structure containing silver; and subjecting the carbon mesoporous structure to a heat treatment at a temperature of 1600° C. to 2000° C. for 0.5 hours or more and 2.0 hours or less under a reduced pressure atmosphere or an inert gas atmosphere. A method for producing a carbon material for a catalyst support.
Citation Information
Patent Citations
Falling device for bagform weir