Manufacturing method for polishing pad

By employing a disposable intaglio plate of polyolefin or polystyrene with a mold release agent, the method addresses the challenges of resin peeling and cost in polishing pad manufacturing, enabling efficient and cost-effective production of high-quality polishing pads with a concavo-convex pattern.

JP2024144268APending Publication Date: 2024-10-11FUJIBO HLDG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024046140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for manufacturing polishing pads with concavo-convex patterns face challenges such as difficulty in peeling off the resin from intaglio plates, high costs due to expensive materials like photosensitive resin and silicone rubber, and poor durability, making them unsuitable for mass production.

Method used

The method involves using a disposable intaglio plate made of general-purpose plastic, specifically polyolefin or polystyrene with low surface free energy, and applying a mold release agent to facilitate easy peeling of the resin, which is then cured and separated from the intaglio to form a polishing layer.

Benefits of technology

This approach allows for cost-effective production of polishing pads with a concavo-convex pattern, ensuring easy separation of the resin and preventing damage to the convex parts, suitable for mass production and high-quality polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144268000001_ABST
    Figure 2024144268000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a polishing pad that is configured so that resin can be easily peeled off at low cost, when transferring an uneven pattern to the resin using an engraved plate.SOLUTION: A manufacturing method for a polishing pad, which can be manufactured at low cost by using a general-purpose plastic as a disposable engraved plate and is configured so that resin forming a polishing layer can be easily peeled off by using polyolefin and polystyrene which are low in surface free energy, manufactures a polishing pad formed by curing the resin and having a polishing layer not including abrasive grain, which comprises a step of preparing a plastic engraved plate on which an uneven pattern is formed by vacuum molding or injection molding; a step of flowing a resin material not including abrasive grain into the plastic engraved plate; a step of curing the resin; and a step of obtaining the polishing layer, by peeling off the cured resin from the plastic engraved plate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polishing pad. In particular, the polishing pad of the present invention is used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc., and is particularly suitable for lapping and polishing sapphire, SiC, etc. [Background technology]

[0002] Polishing pads are used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, sapphire, and SiC. Various types of polishing pads are known, including polishing pads made of nonwoven fabric, polishing pads made of foamed or non-foamed polyurethane, polishing pads with fixed abrasive grains, and polishing pads using a resin layer with a concave-convex pattern as the polishing surface.

[0003] Among these, the polishing pad using a resin layer having a concave-convex pattern as the polishing surface has the advantage that the grooves forming the concave-convex pattern affect the fluidity of the slurry, and as a result, the object to be polished can be polished uniformly. The manufacturing method of such a polishing pad includes a method of cutting the surface of a flat base material to form grooves, a method of forming a concave-convex pattern on a substrate by applying a screen printing method, and a method of making a mold having a concave-convex pattern and using the mold to mold.

[0004] For example, Patent Document 1 discloses a polishing pad on which a concave-convex pattern is formed by transferring it from a plate having a concave-convex pattern made of photosensitive resin, and Patent Document 2 discloses a polishing pad on which a concave-convex pattern is formed using a molding die made of silicone rubber or the like onto which a plate having a concave-convex pattern made of photosensitive resin is transferred. However, the methods of transferring a concave-convex pattern to a resin using an intaglio plate as in Patent Documents 1 and 2 have the problem that the cured resin is difficult to peel off from the intaglio plate, causing the convex portions of the resin to fall off. Furthermore, the photosensitive resins and silicone rubbers used in the intaglio plate are expensive and have poor durability when used repeatedly, making them unsuitable for mass production. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2019-178248 [Patent Document 2] Patent Publication No. 2019-178258 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems, and provides a method for manufacturing a polishing pad that is inexpensive and allows the resin to be easily peeled off when a concave-convex pattern is transferred to the resin using an intaglio printing plate. [Means for solving the problem]

[0007] As a result of investigations, the inventors have discovered a method for manufacturing a polishing pad that can be manufactured inexpensively by using a general-purpose plastic as a disposable intaglio plate, and that can be easily peeled from the resin that forms the polishing layer by using a polyolefin or polystyrene that has low surface free energy. [1] A method for manufacturing a polishing pad having a polishing layer formed by curing a resin and not containing abrasive grains, comprising: A step of preparing a plastic intaglio plate having a concave-convex pattern formed thereon by vacuum forming or injection molding; pouring the resin raw material containing no abrasive grains into the plastic intaglio; curing the resin; peeling the cured resin from the plastic intaglio to obtain the polishing layer. A method for manufacturing a polishing pad. [2] The method for manufacturing a polishing pad according to [1], wherein the temperature of the plastic intaglio is 130°C or less in the step of curing the resin. [3] The method for manufacturing a polishing pad described in [1], wherein the plastic intaglio is made of polyethylene, polypropylene, polystyrene, and polyvinyl chloride. [4] The method for manufacturing a polishing pad according to [1], further comprising a step of applying a release agent to the plastic intaglio plate, wherein the release agent is a silicone-based release agent or a fluorine-based release agent. [5] The method for producing a polishing pad according to [1], wherein the resin is a thermosetting resin composition. [6] A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to any one of [1] to [5], A polishing method in which polishing is carried out by loose abrasive polishing. [Effects of the Invention]

[0008] Using general-purpose plastic as a disposable intaglio plate allows for inexpensive production, and using polyolefins or polystyrene, which have low surface free energy, makes it easy to peel off the resin that forms the polishing layer. [Brief explanation of the drawings]

[0009] [Figure 1] FIG. 1 is a process diagram of a method for producing a polishing layer 11 of a polishing pad of the present invention. [Figure 2] FIG. 2 is a cross-sectional view of another embodiment of the polishing layer 11 of the polishing pad of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0010] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the ``present embodiment''), but the present invention is not limited to this and various modifications are possible within the scope of the gist of the present invention.

[0011] <<Polishing pad manufacturing method>> A first embodiment of the method for producing a polishing pad of the present invention will be described with reference to the flowchart of FIG. The first aspect is as follows: The polishing pad comprises a polishing layer, and the polishing layer comprises a polishing surface for polishing an object to be polished. A method for manufacturing a polishing pad having a polishing layer 11 formed by curing a resin 50, comprising: Step 1: preparing a plastic intaglio plate 72 on which a concave-convex pattern is formed by vacuum molding or injection molding; a step (Step 2) of applying a release agent 8 to the plastic intaglio 72; A step (Step 3) of pouring the resin raw material 50 into the plastic intaglio 72; A step (Step 4) of curing the resin 50; The method for manufacturing a polishing pad further comprises a step (Step 5) of peeling off the cured resin (50) from the plastic intaglio (72) to obtain the polishing layer (11). In this specification, for convenience, the resin raw material before being poured into a mold (that is, the resin before being hardened) and the hardened resin will both be represented by the reference numeral 50.

[0012] (Step 1) First, a mold for forming the concave-convex pattern is prepared. There are no particular limitations on the mold, as long as it can form a concave-convex pattern in a plastic material by vacuum forming or injection molding, and examples of the mold include a wooden mold, a resin mold, and a metal mold. Since the plastic intaglio plate 72 with the concave-convex pattern formed on it does not require very high durability, a mold that can be repeatedly manufactured is preferred.

[0013] Next, a plastic material for the plastic intaglio 72 is prepared. The plastic material is not particularly limited as long as it is inexpensive and has low surface free energy, but examples include polyolefin resins (polyethylene, polypropylene), polystyrene, and polyvinyl chloride. The surface free energy of the material used for the intaglio 72 of the present invention is preferably 50 mN / m or less, more preferably 40 mN / m or less. A surface free energy of 50 mN / m or less facilitates the peeling of the polishing layer 11 from the intaglio 72, thereby preventing the protrusions 51 from falling off or being damaged during the peeling of the intaglio 72 and the polishing layer 11. The surface free energy can be calculated by measuring the contact angles with water and methylene iodide using a contact angle meter. Polypropylene (surface free energy: 29.8 mN / m) and polyethylene (surface free energy: 35.6 mN / m) are preferred materials for the intaglio 72 because they are readily available, inexpensive, and have low surface free energy. Examples of polypropylene that can be used include "Elon" manufactured by OJK Corporation and "Hyperl" manufactured by Sanvic, and examples of polyethylene that can be used include "EL-N-AN" manufactured by Resonac.

[0014] The shape of the plastic material is not particularly limited as long as it is a shape that allows the production of a plastic intaglio plate 72 with a concave-convex pattern by vacuum molding or injection molding, but a film or sheet shape is preferred because it is easy to mold. The thickness of the film or sheet-like plastic material is not particularly limited as long as it is thick enough to produce a plastic intaglio plate 72 with a concave-convex pattern by vacuum forming or injection molding, but a thickness of 0.1 mm to 5 mm is preferable from the viewpoint of maintaining the strength of the plate and making it easy to form. In the case of vacuum forming, a film or sheet of plastic material is heated and softened, placed in a mold with a concave-convex pattern, and the space between the plastic material and the mold is evacuated, causing the plastic material to adhere to the mold. Once molding is complete, the plastic is cooled and removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. Vacuum forming conditions vary depending on the plastic material, its thickness, etc. In the case of injection molding, a heated and melted plastic material is injected into a mold in which a concave-convex pattern has been formed, cooled and solidified, and then removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. The conditions for injection molding vary depending on the plastic material, the thickness of the intaglio plate 72 made of the plastic material, etc. The strength of the plastic intaglio 72 on which the concave-convex pattern has been formed by vacuum molding or injection molding is not particularly limited, as long as the concave-convex pattern can be accurately transferred from the plastic intaglio 72 in Step 4 to obtain a polishing layer 11 on which the concave-convex pattern has been formed. However, in order to prevent cracking or breaking due to impact, it is preferable that the strength of the plastic intaglio 72 be 0.5 J / m or more at 0°C in a DuPont impact test.

[0015] (Step 2) Next, a release agent 8 is applied to the obtained plastic intaglio 72. The release agent 8 facilitates the separation of the cured resin from the plastic intaglio. There are no particular limitations on the type of release agent, and examples include silicone-based release agents and fluorine-based release agents, with fluorine-based release agents being preferred. The method for applying the release agent 8 is not particularly limited as long as it can peel off the hardened resin from the plastic intaglio plate. Examples include spraying and electrostatic application, with the spraying method being preferred.

[0016] (Step 3) The resin material 50 is poured into the plastic intaglio plate 72 to which the mold release agent 8 has been applied. The method for pouring the resin raw material 50 into the plastic intaglio 72 is not particularly limited as long as the resin raw material 50 is filled (poured) into the recesses of the plastic intaglio 72. Examples include gravity casting, in which the resin raw material is poured into the recesses under its own weight at room temperature and normal pressure, and vacuum casting, in which the plastic intaglio 72 and resin 50 are placed in a vacuum container, the pressure is reduced, and the resin raw material is poured into the recesses at atmospheric pressure.

[0017] The resin 50 is not particularly limited as long as a polishing pad using the resin layer 11 having a concave-convex pattern as the polishing surface can be obtained, but a curable resin composition is preferred. The curable resin composition is not particularly limited, and examples thereof include thermosetting resins, UV-curable resins, photocurable resin compositions containing a photopolymerization initiator and a polymerizable compound, thermosetting resin compositions containing a thermal polymerization initiator and a polymerizable compound, and curable resin compositions containing a two-component mixed curable resin. Furthermore, the curable resin composition may contain a crosslinking agent having two or more polymerizable functional groups, etc., as necessary.

[0018] The thermosetting resin is not particularly limited, but examples thereof include phenol resin, epoxy resin, acrylic resin, urethane resin, and formaldehyde resin.

[0019] The UV-curable resin is not particularly limited, but for example, a prepolymer having a number-average molecular weight of about 1,000 to 10,000 is preferable, and examples of the material include isocyanurate resins, acrylic (methacrylic) ester resins and their urethane-modified resins, and thiokol resins, and a reactive diluent or organic solvent can be used as appropriate depending on the application.

[0020] Examples of photopolymerization initiators include benzophenone compounds, acetophenone compounds, and thioxanthone compounds. Examples of thermal polymerization initiators include azo compounds such as 2,2'-azobisbutyronitrile, and peroxides such as methyl ethyl ketone peroxide and benzoyl peroxide (BPO).

[0021] Specific examples of the resin include unsaturated carboxylic acids having a polymerizable unsaturated group, such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid; unsaturated carboxylic acid esters having a polymerizable unsaturated group, such as (meth)acrylate, epoxy (meth)acrylate (vinyl ester resin), urethane (meth)acrylate, and polyester (meth)acrylate; polyesters having an unsaturated group; polyethers having a polymerizable unsaturated group; polyamides having a polymerizable unsaturated group; urethanes having a polymerizable unsaturated group; and aromatic compounds having a polymerizable unsaturated group, such as styrene.

[0022] The two-component mixed curable resin is not particularly limited, but examples thereof include prepolymers with different physical properties, such as epoxy resin, unsaturated polyester resin, and polyamide resin.

[0023] Among these, those that cure at room temperature are preferred in terms of the heat resistance of the plastic intaglio 72. Examples include curable resin compositions containing a polymerization initiator that works at room temperature, UV-curable resins and photocurable resin compositions that cure upon exposure to light, and mixed curable resin compositions that cure by mixing two liquids. In terms of polishing (lapping) performance, vinyl ester resin or unsaturated polyester resin, which has high heat resistance (high deformation temperature), is preferred.

[0024] A step of embedding a sheet-like fiber material 6 in the resin 50 before the resin 50 hardens may be further included. By embedding the fiber material 6 inside the resin 50, the strength of the convex portions 51 is increased, and a polishing layer 11 is obtained that can prevent the polishing pad convex portions 51 from falling off during manufacturing (when peeling from the plastic intaglio 72) and during polishing.

[0025] Furthermore, the method may further include a step of bonding a substrate to the surface of resin 50 opposite to the surface that contacts plastic intaglio 72 before curing resin 50. By using a substrate, resin 50 is cured while sandwiched between the substrate and plastic intaglio 72. This tends to improve the uniformity of the thickness of the obtained cured product and further improve the flatness of the back surface of the obtained cured product (the surface opposite to the surface that contacts plastic intaglio 72).

[0026] (Step 4) The process of curing the resin raw material 50 will now be described. The method for curing the resin raw material 50 is not particularly limited as long as it is a method suitable for each resin raw material 50, but depending on the properties of the resin, examples include a photo-curing method in which ultraviolet rays or the like are irradiated, a thermal curing method in which heat is applied (including a method in which the material is left at room temperature), or a method in which the material is mixed and left as in a two-liquid mixture. The light to be irradiated is not particularly limited as long as it can cure the resin raw material 50, but examples include ultraviolet light. Light sources that emit such light include high-pressure mercury lamps, UV-LED lamps, and black light fluorescent lamps (BLBs), with BLBs being preferred. The light may be irradiated from either the lower surface 72A of the plastic intaglio 72 or the upper surface 50A of the resin raw material 50. In particular, when using a plastic intaglio 72, even when irradiated from the lower surface 72A, its transparency allows sufficient light to pass through to cure the convex portions 51, resulting in sufficient curing of the convex portions 51. This was not possible with conventional molding dies made of silicone rubber or the like. The wavelength of the ultraviolet light irradiation is preferably 200 nm to 400 nm, and the irradiation time is preferably 3 to 30 minutes.

[0027] (Step 5) The cured resin 50 is peeled off from the plastic intaglio 72 to obtain the polishing layer 11. The peeling method is not particularly limited, and may involve holding the edge of the cured resin and peeling it off from the intaglio 72. The resulting polishing layer 11 has a concave-convex pattern transferred from the plastic intaglio 72, and the surfaces of the convex portions 51 of the concave-convex pattern become the polishing surface for polishing the object to be polished. In addition, the plastic intaglio 72 may be peeled off from the hardened resin 50. Since the plastic intaglio 72 used in the method for manufacturing a polishing pad of the present invention is disposable, it is acceptable for the plastic intaglio 72 to be deformed or damaged when peeled off from the hardened resin 50, and damage such as damage or deformation of the polishing layer 11 and falling off of the convex portions 51 of the resin 50 can be suppressed. The peeled polishing layer 11 can be cut to a predetermined size so as to be provided in a polishing pad. If necessary, a cushion layer may be attached to the surface opposite to the uneven pattern surface to form a polishing pad.

[0028] The resulting abrasive layer 11 has a bending strength of 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and even more preferably 50 to 800 MPa. The bending strength is obtained by measurement performed in accordance with JIS K7203. When the bending strength is within the above range, breakage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the plastic intaglio 72.

[0029] FIG. 2 shows an enlarged view of a polishing layer 11 having a different shape from that shown in FIG. 1. The polishing layer 11 differs from the polishing layer 11 shown in FIG. 1 in that it includes a recess 53 on the opposite side of the protrusion 51. The provision of the recess 53 enables further weight reduction and cost reduction. The recess 53 can be formed by intentionally reducing the amount of resin in the area where the protrusion 51 is to be formed in Step 3, or by pressing a mold corresponding to the recess 53 from above after Step 3. The shape of the recess 53 is not particularly limited, and may be a shape with corners (for example, a truncated pyramid) as shown in FIG. 2, or a shape with curved surfaces (for example, a dome shape).

[0030] (polishing method) The polishing method using the polishing pad 1 obtained by the manufacturing method of the present invention is preferably used in free abrasive polishing. Here, free abrasive polishing is a polishing method using a slurry in which abrasive grains are not fixed but mixed with a liquid. That is, it is a method of polishing using a slurry containing abrasive grains (abrasive grain-containing solution). Therefore, the polishing layer of the polishing pad 1 does not contain abrasive grains. Compared to fixed abrasives, there are fewer problems such as scratching, and when scratching is kept as low as possible, for example, when performing final finishing, by using the polishing pad 1 obtained by the manufacturing method of the present invention, it is possible to minimize the occurrence of scratches on the object being polished at low cost. [Example]

[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0032] In each example and comparative example, unless otherwise specified, "parts" means "parts by mass".

[0033] (polishing pad manufacturing)

[0034] (Manufacture of polishing pad 1) A polypropylene resin sheet was vacuum-formed to produce a plastic intaglio plate 72 having a plurality of recesses in the shape of a truncated quadrangular pyramid with a height of 0.85 mm and a base of 1.5 mm square. Next, 90 parts of unsaturated polyester resin (product name: Rigolac, manufactured by Resonac Co., Ltd.) was poured into this plastic intaglio 72. Before curing, a mesh fabric made of polypropylene as a fiber material with a fiber diameter of 150 μm, a mesh size of 30 μm, and a thickness of 300 μm was sunk into the resin 50 from above, so that the fiber material penetrated into the base 52. After the resin 50 was cured at room temperature (25° C.) for 30 minutes, the resin 50 was peeled off from the plastic intaglio 72 to remove the plastic intaglio 72, thereby producing the polishing pad 1.

[0035] (Manufacture of polishing pad 2) Polishing pad 2 was manufactured in the same manner as polishing pad 1, except that the polishing pad material was made of vinyl ester resin (product name: Lipoxy, manufactured by Resonac Co., Ltd.) instead of unsaturated polyester resin, and the mesh fabric material was made of polyethylene fiber instead of polypropylene fiber.

[0036] Furthermore, in manufacturing polishing pad 2, it was confirmed that even if the material of the polishing pad and the material of the mesh fabric were changed, a polishing pad similar to polishing pad 1 could be manufactured using a plastic intaglio made of polypropylene resin.

[0037] Furthermore, a polishing pad 1 without a mesh fabric was also manufactured by the same manufacturing method (polishing pad 3), and a polishing pad 2 without a mesh fabric was also manufactured by the same manufacturing method (polishing pad 4).

[0038] (When peeling from the intaglio plate) A peeling experiment was conducted using a peeling roller to peel the resin 50 from the plastic intaglio 72. Examples of the peeling roller include a combination of adhesive tape and a rod-shaped peeling roller, as described in JP-A-9-114384. Peeling experiments were conducted under conditions that allowed peeling of the intaglio from the resin 50, using the plastic intaglio 72 of the above example and using silicone rubber instead of plastic as the intaglio. The results showed that the silicone rubber intaglio required a large force to peel, and that the convex portions 51 of the peeled resin 50 fell off or were damaged. In contrast, the polishing pads 1 to 4 obtained using the plastic intaglio 72 made of polypropylene resin did not suffer from any dropout or damage to the convex portions 51 during peeling. [Industrial Applicability]

[0039] The method for manufacturing a polishing pad of the present invention is an inexpensive method for manufacturing a polishing pad that facilitates resin peeling from an intaglio plate, and therefore has industrial applicability as a method for manufacturing polishing pads used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc.

[0040] 11 Polishing layer 50 Resin raw materials 50A Top surface of resin raw material 51 Convex part 52 Base 53 Recess 71 Plastic Materials 72 Plastic Intaglio 72A Plastic Intaglio Underside 8. Release Agent

Claims

1. A method for producing a polishing pad having a polishing layer formed by curing a resin and not containing abrasive grains, comprising the steps of: A step of preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum forming or injection molding; pouring the resin raw material not containing abrasive grains into the plastic intaglio plate; curing the resin; peeling the cured resin from the plastic intaglio to obtain the polishing layer. A method for manufacturing a polishing pad.

2. The method for producing a polishing pad according to claim 1 , wherein the temperature of the plastic intaglio is 130° C. or less in the step of curing the resin.

3. The method for producing a polishing pad according to claim 1 , wherein the plastic intaglio is made of a resin selected from polyethylene, polypropylene, polystyrene, and polyvinyl chloride.

4. The method for producing a polishing pad according to claim 1 , further comprising a step of applying a release agent to the plastic intaglio plate, the release agent being a silicone-based release agent or a fluorine-based release agent.

5. The method for producing a polishing pad according to claim 1 , wherein the resin is a thermosetting resin composition.

6. A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to any one of claims 1 to 5, comprising the steps of: A polishing method in which polishing is carried out by loose abrasive polishing.

Citation Information

Patent Citations

  • Polishing pad and method for manufacturing the same

    JP2019178248A

  • Polishing pad and method for manufacturing the same

    JP2019178258A