Manufacturing method for polishing pad

By employing a disposable intaglio plate made of low-cost general-purpose plastic and a mold release agent, the resin peeling issue is resolved, allowing for cost-effective and efficient manufacturing of polishing pads.

JP2024144269APending Publication Date: 2024-10-11FUJIBO HLDG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024046141
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing polishing pad manufacturing methods using intaglio plates face challenges with resin peeling difficulties and high costs due to the use of expensive materials like photosensitive resin and silicone rubber, which are not suitable for mass production.

Method used

The method involves using a disposable intaglio plate made of general-purpose plastic, such as polyolefins or polystyrene, with low surface free energy, and applying a mold release agent to facilitate easy peeling of the resin, which is then cured and separated from the intaglio to form a polishing layer.

Benefits of technology

This approach reduces production costs and enables easy separation of the resin, preventing damage to the polishing layer, making it suitable for mass production and efficient polishing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144269000001_ABST
    Figure 2024144269000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a polishing pad that is configured so that resin can be easily peeled off at low cost, when transferring an uneven pattern to the resin using an engraved plate.SOLUTION: A manufacturing method for a polishing pad, which can be manufactured at low cost by using a general-purpose plastic as a disposable engraved plate and is configured so that resin forming a polishing layer can be easily peeled off by using polyolefin and polystyrene which are low in surface free energy, manufactures a polishing pad formed by curing the resin and having a polishing layer including abrasive grain, which comprises a step of preparing a plastic engraved plate on which an uneven pattern is formed by vacuum molding or injection molding; a step of flowing a resin material including abrasive grain into the plastic engraved plate; a step of curing the resin; and a step of obtaining the polishing layer, by peeling off the cured resin from the plastic engraved plate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing pad. In particular, the polishing pad of the present invention is used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc., and is particularly suitable for lapping and polishing sapphire, SiC, etc. [Background technology]

[0002] Polishing pads are used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, sapphire, and SiC. There are various types of polishing pads, including nonwoven fabric polishing pads, foamed or nonfoamed polyurethane polishing pads, fixed abrasive polishing pads, and polishing pads using a resin layer with a concave-convex pattern as the polishing surface.

[0003] Among these, polishing pads using a resin layer having a concave-convex pattern as a polishing surface have the advantage that the grooves forming the concave-convex pattern affect the fluidity of the slurry, resulting in uniform polishing of the workpiece. Methods for manufacturing such polishing pads include a method of forming grooves by cutting the surface of a flat base material, a method of forming a concave-convex pattern on a substrate by applying a screen printing method, and a method of manufacturing a mold having a concave-convex pattern and using the mold to perform molding.

[0004] For example, Patent Document 1 discloses a polishing pad on which a concave-convex pattern is formed by transferring from a plate having a concave-convex pattern made of photosensitive resin, while Patent Document 2 discloses a polishing pad on which a concave-convex pattern is formed using a molding die made of silicone rubber or the like onto which a plate having a concave-convex pattern made of photosensitive resin is transferred. However, the method of transferring a concave-convex pattern to a resin using an intaglio plate as in Patent Documents 1 and 2 has a problem in that the cured resin is difficult to peel off from the intaglio plate, and the convex parts of the resin fall off. In addition, the photosensitive resin, silicone rubber, etc. used in the intaglio plate are expensive and have poor durability when used repeatedly, making them unsuitable for mass production. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2019-178248 [Patent Document 2] Patent Publication 2019-178258 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems, and provides a method for manufacturing a polishing pad that is inexpensive and allows the resin to be easily peeled off when a concave-convex pattern is transferred to the resin using an intaglio printing plate. [Means for solving the problem]

[0007] As a result of investigations, the inventors have found a method for producing a polishing pad that can be produced inexpensively by using a general-purpose plastic as a disposable intaglio plate, and that can be easily peeled off from the resin that forms the polishing layer by using a polyolefin or polystyrene that has low surface free energy. [1] A method for producing a polishing pad having a polishing layer containing abrasive grains, the method comprising: A step of preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum forming or injection molding; pouring the resin raw material containing abrasive grains into the plastic intaglio plate; curing the resin; peeling the cured resin from the plastic intaglio to obtain the polishing layer. A method for manufacturing a polishing pad. [2] The method for manufacturing a polishing pad described in [1], wherein the temperature of the plastic intaglio is 130°C or lower in the step of hardening the resin. [3] The method for manufacturing a polishing pad described in [1], wherein the plastic intaglio plate is composed of polyethylene, polypropylene, polystyrene, and polyvinyl chloride. [4] The method for producing a polishing pad described in [1], further comprising a step of applying a release agent to the plastic intaglio plate, the release agent being a silicone-based release agent or a fluorine-based release agent. [5] The method for producing a polishing pad described in [1], wherein the resin is a UV-curable resin composition. [6] A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to any one of [1] to [5], comprising the steps of: A polishing method in which polishing is carried out by fixed abrasive polishing. Effect of the Invention

[0008] Using general-purpose plastic as a disposable intaglio plate makes it possible to produce it inexpensively, and using polyolefins or polystyrene, which have low surface free energy, makes it easy to peel it off from the resin that forms the polishing layer. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a process diagram of a method for producing a polishing layer 11 of a polishing pad of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of another embodiment of the polishing layer 11 of the polishing pad of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.

[0011] <<Polishing pad manufacturing method>> A first embodiment of the method for producing a polishing pad of the present invention will be described with reference to the flow chart of FIG. The first aspect is as follows: The polishing pad comprises a polishing layer, and the polishing layer comprises a polishing surface for polishing an object to be polished. A method for manufacturing a polishing pad having a polishing layer 11 formed by curing a resin 50, comprising the steps of: A step (Step 1) of preparing a plastic intaglio plate 72 having a concave-convex pattern formed by vacuum molding or injection molding; A step (Step 2) of applying a release agent 8 to the plastic intaglio plate 72; A step of pouring the resin raw material 50 into the plastic intaglio plate 72 (Step 3); A step of curing the resin 50 (Step 4); and a step (Step 5) of peeling off the cured resin (50) from the plastic intaglio (72) to obtain the polishing layer (11). In this specification, for the sake of convenience, both the resin raw material before being poured into a mold (that is, the resin before being cured) and the cured resin will be represented by the reference numeral 50.

[0012] (Step 1) First, a mold for forming the concave-convex pattern is prepared. There are no particular limitations on the mold as long as it can form a concave-convex pattern in a plastic material by vacuum molding or injection molding, and examples of the mold include a wooden mold, a resin mold, and a metal mold. Since the plastic intaglio plate 72 on which the concave-convex pattern is formed does not require very high durability, a mold that can be repeatedly manufactured is preferable.

[0013] Next, a plastic material for the plastic intaglio 72 is prepared. The plastic material is not particularly limited as long as it is a plastic that is inexpensive and has a low surface free energy, and examples of the plastic material include polyolefin resins (polyethylene, polypropylene), polystyrene, polyvinyl chloride, etc. The surface free energy of the material used for the intaglio 72 of the present invention is preferably 50 mN / m or less, more preferably 40 mN / m or less. If the surface free energy is 50 mN / m or less, the polishing layer 11 can be easily peeled off from the intaglio 72, so that the falling off and damage of the convex portion 51 during the peeling of the intaglio 72 and the polishing layer 11 can be suppressed. The surface free energy can be calculated by measuring the contact angle with water and methylene iodide using a contact angle meter. As the material for the intaglio 72, polypropylene (surface free energy: 29.8 mN / m) and polyethylene (surface free energy: 35.6 mN / m) are preferable because they are easily available, inexpensive, and have a low surface free energy. Examples of polypropylene that can be used include products manufactured by OJK under the trade name "Ellon" and products manufactured by Sanvic under the trade name "Hyperal." Examples of polyethylene that can be used include products manufactured by Resonac under the trade name "EL-N-AN."

[0014] The shape of the plastic material is not particularly limited as long as it is a shape that allows the production of a plastic intaglio plate 72 having a concave-convex pattern by vacuum molding or injection molding, but a film or sheet shape is preferred because it is easy to mold. The thickness of the film or sheet-like plastic material is not particularly limited as long as it is a thickness that allows the production of a plastic intaglio plate 72 with an uneven pattern formed thereon by vacuum molding or injection molding, but from the viewpoint of maintaining the strength as a plate and making it easy to mold, a thickness of 0.1 mm to 5 mm is preferable. In the case of vacuum molding, a film or sheet-like plastic material is heated and softened, placed in a mold with a concave-convex pattern, and the space between the plastic material and the mold is evacuated, so that the plastic material adheres to the mold. Once molding is complete, it is cooled and removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. Vacuum molding conditions vary depending on the plastic material, its thickness, etc. In the case of injection molding, a heated and melted plastic material is injected into a mold in which a concave-convex pattern has been formed, cooled and solidified, and then removed from the mold to obtain a plastic intaglio plate 72 with a concave-convex pattern. The conditions for injection molding vary depending on the plastic material, the thickness of the intaglio plate 72 made of the plastic material, etc. The strength of the plastic intaglio plate 72 on which the concave-convex pattern has been formed by vacuum molding or injection molding is not particularly limited, so long as the concave-convex pattern can be accurately transferred from the plastic intaglio plate 72 to obtain an abrasive layer 11 on which the concave-convex pattern has been formed in Step 4. However, in order to prevent cracking or breaking due to impact, it is preferable that the strength of the plastic intaglio plate 72 be 0.5 J / m or more at 0°C in a DuPont impact test.

[0015] (Step 2) Next, a release agent 8 is applied to the obtained plastic intaglio 72. The release agent 8 facilitates the release of the hardened resin from the plastic intaglio. There are no particular limitations on the type of release agent, and examples of the release agent include silicone-based release agents and fluorine-based release agents, with fluorine-based release agents being preferred. The method of applying the release agent 8 is not particularly limited as long as it is possible to peel off the hardened resin from the plastic intaglio plate. Examples of the method include a spray method and an electrostatic application method, with the spray method being preferred.

[0016] (Step 3) The resin material 50 is poured into the plastic intaglio plate 72 on which the mold release agent 8 has been applied. In the present invention, the resin raw material 50 contains abrasive grains. That is, the polishing pad 1 obtained by the manufacturing method of the present invention is a polishing pad for a fixed abrasive polishing method, and it is preferable to prepare the resin raw material 50 by mixing abrasive grains with a liquid resin before pouring the resin raw material 50 into the plastic intaglio plate 72. The amount of abrasive grains relative to the resin is not particularly limited, and may be the same as in the past. For example, the abrasive grains may be contained in a ratio of 1% by mass or more and 20% by mass or less, preferably 5% by mass or more and 10% by mass or less, relative to the entire resin raw material 50. The type of abrasive grains is not particularly limited, and examples of usable abrasive grains include diamond, cerium oxide, silicon carbide, silicon oxide, zirconium oxide, iron oxide, manganese oxide, magnesium oxide, zinc oxide, titanium oxide, aluminum oxide, zirconium silicate, boron nitride, silicon nitride, barium sulfate, calcium carbonate, etc. The grain size of the abrasive grains is preferably 1 to 100 μm. There are no particular limitations on the method for pouring the resin raw material 50 into the plastic intaglio 72, so long as the resin raw material 50 is filled (pouring) into the recesses of the plastic intaglio 72. Examples of such a method include a gravity casting method in which the resin raw material is poured into the recesses under its own weight at room temperature and normal pressure, and a vacuum casting method in which the plastic intaglio 72 and resin 50 are placed in a vacuum container, the pressure is reduced, and the resin raw material is poured into the recesses at atmospheric pressure.

[0017] The resin 50 is not particularly limited as long as a polishing pad using the resin layer 11 having a concave-convex pattern as a polishing surface can be obtained, but a curable resin composition is preferred. The curable resin composition is not particularly limited, and examples thereof include a thermosetting resin, a UV-curable resin, a photocurable resin composition containing a photopolymerization initiator and a polymerizable compound, a thermosetting resin composition containing a thermal polymerization initiator and a polymerizable compound, a curable resin composition containing a two-liquid mixed curable resin, etc. Furthermore, the curable resin composition may contain a crosslinking agent having two or more polymerizable functional groups, etc., as necessary.

[0018] The thermosetting resin is not particularly limited, but examples thereof include phenol resin, epoxy resin, acrylic resin, urethane resin, and formaldehyde resin.

[0019] The UV-curable resin is not particularly limited, but for example, a prepolymer having a number average molecular weight of about 1,000 to 10,000 is preferable. Examples of the material include isocyanurate-based resins, acrylic (methacrylic) ester resins and their urethane-modified resins, thiokol-based resins, etc., and a reactive diluent or organic solvent can be used appropriately depending on the application.

[0020] Examples of photopolymerization initiators include benzophenone compounds, acetophenone compounds, and thioxanthones. Examples of thermal polymerization initiators include azo compounds such as 2,2'-azobisbutyronitrile, and peroxides such as methyl ethyl ketone peroxide and benzoyl peroxide (BPO).

[0021] Specific examples of the resin include unsaturated carboxylic acids having a polymerizable unsaturated group, such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid; unsaturated carboxylic acid esters having a polymerizable unsaturated group, such as (meth)acrylate, epoxy (meth)acrylate (vinyl ester), urethane (meth)acrylate, and polyester (meth)acrylate; polyesters having unsaturated groups; polyethers having a polymerizable unsaturated group; polyamides having a polymerizable unsaturated group; urethanes having a polymerizable unsaturated group; aromatic compounds having a polymerizable unsaturated group, such as styrene, and vinyl ester resins.

[0022] The two-liquid mixed curable resin is not particularly limited, but examples thereof include prepolymers having different physical properties, such as epoxy resins, unsaturated polyester resins, and polyamide resins.

[0023] Among these, those that harden at room temperature are preferable from the viewpoint of the heat resistance of the plastic intaglio plate 72. Examples include a curable resin composition containing a polymerization initiator that acts at room temperature, a UV-curable resin and a photocurable resin composition that harden when irradiated with light, and a mixed type curable resin composition that hardens by mixing two liquids. In terms of polishing (lapping) performance, vinyl ester resin or unsaturated polyester resin, which has high heat resistance (high deformation temperature), is preferred.

[0024] A step of embedding a sheet-like fiber material 6 in the resin 50 before the resin 50 hardens may be further included. By embedding the fiber material 6 inside the resin 50, the strength of the protrusions 51 is increased, and a polishing layer 11 is obtained that can prevent the polishing pad protrusions 51 from falling off during production (when peeling off from the plastic intaglio 72) and during polishing.

[0025] Furthermore, the method may further include a step of bonding a substrate to the surface of the resin 50 opposite to the surface in contact with the plastic intaglio 72 before curing the resin 50. By using a substrate, the resin 50 is cured in a state in which the resin 50 is sandwiched between the substrate and the plastic intaglio 72. This tends to improve the uniformity of the thickness of the obtained cured product, and to further improve the flatness of the back surface (the surface opposite to the surface in contact with the plastic intaglio 72) of the obtained cured product.

[0026] (Step 4) The process of curing the resin raw material 50 will now be described. The method for curing the resin raw material 50 is not particularly limited as long as it is a method suitable for each resin raw material 50, but depending on the properties of the resin, examples include a photocuring method in which ultraviolet rays or the like are irradiated, a thermal curing method in which heat is applied (including a method in which the material is left at room temperature), or a method in which the material is mixed and left as in a two-liquid mixture type. The light to be irradiated is not particularly limited as long as it can cure the resin raw material 50, and examples thereof include ultraviolet light. Examples of light sources that emit such light include high-pressure mercury lamps, UV-LED lamps, and black light fluorescent lamps (BLB), among which BLB is preferred. The direction of light irradiation may be either the direction of irradiation from the lower surface 72A side of the plastic intaglio 72 or the direction of irradiation from the upper surface 50A side of the resin raw material 50. In particular, when the plastic intaglio 72 is used, even if irradiation is performed from the lower surface 72A side, the transparency of the plastic intaglio 72 allows light sufficient to cure the convex portions 51 to pass through, and the convex portions 51 are sufficiently cured. This was not possible with the conventional molding die made of silicone rubber or the like. The wavelength of the ultraviolet irradiation is preferably 200 nm to 400 nm, and the irradiation time is preferably 3 minutes to 30 minutes.

[0027] (Step 5) The hardened resin 50 is peeled off from the plastic intaglio 72 to obtain the polishing layer 11. The peeling method is not particularly limited, and may be a method of holding an edge of the hardened resin and peeling it off from the intaglio 72. The polishing layer 11 obtained has a concave-convex pattern transferred from the plastic intaglio 72, and the surfaces of the convex parts 51 of the concave-convex pattern become the polishing surface for polishing an object to be polished. In addition, the plastic intaglio 72 may be peeled off from the hardened resin 50. Since the plastic intaglio 72 used in the method for manufacturing an abrasive pad of the present invention is disposable, it is acceptable for the plastic intaglio 72 to be deformed or damaged when peeled off from the hardened resin 50, and damage or deformation of the abrasive layer 11, or defects such as the falling off of the convex portions 51 of the resin 50 can be suppressed. The peeled polishing layer 11 can be cut to a predetermined size so as to be provided for a polishing pad. If necessary, a cushion layer may be attached to the surface opposite to the concave-convex pattern to form a polishing pad.

[0028] The bending strength of the obtained abrasive layer 11 is 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and further preferably 50 to 800 MPa. The bending strength is obtained by measurement performed in accordance with JIS K7203. When the bending strength is within the above range, damage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the plastic intaglio 72.

[0029] FIG. 2 shows a polishing layer 11 having a different shape from that shown in FIG. 1. The polishing layer 11 is different from the polishing layer 11 shown in FIG. 2 in that it has a recess 53 on the opposite side to the protrusion 51. Providing the recess 53 can achieve further weight reduction and cost reduction. The recess 53 can be provided by intentionally reducing the amount of resin at the location where the protrusion 51 is to be formed in the above-mentioned Step 3, or by pressing a mold corresponding to the recess 53 from above after the step 3. The shape of the recess 52 is not particularly limited, and may be a shape having corners (for example, a truncated pyramid) as shown in FIG. 2, or a shape having a curved surface (for example, a dome shape).

[0030] (polishing method) The polishing pad 1 obtained by the manufacturing method of the present invention is preferably used in fixed abrasive polishing, which is a method in which abrasive grains are embedded in the polishing layer of the polishing pad 1 to perform polishing. Fixed abrasive polishing is more efficient and reduces waste during polishing than free abrasive polishing. Therefore, the polishing pad 1 of the present invention can be used when it is desired to reduce waste during polishing and to be more efficient. EXAMPLES

[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0032] In each of the examples and comparative examples, unless otherwise specified, "parts" means "parts by mass".

[0033] (polishing pad manufacturing)

[0034] (Manufacture of polishing pad 1) A polypropylene resin sheet was vacuum molded to produce a plastic intaglio plate 72 having a plurality of recesses in the shape of a truncated quadrangular pyramid with a height of 0.85 mm and a base of 1.5 mm on each side. Next, 90 parts of unsaturated polyester resin (product name: Rigolac, manufactured by Resonac Co., Ltd.) was poured into this plastic intaglio plate 72. Before hardening, a mesh fabric made of polypropylene with a fiber diameter of 150 μm, mesh opening of 30 μm, and thickness of 300 μm was sunk into the resin 50 from above as a fiber material, so that the fiber material penetrated into the base 52. After the resin 50 was cured at room temperature (25° C.) for 30 minutes, the plastic intaglio 72 was removed by peeling the resin 50 from the plastic intaglio 72, and the polishing pad 1 was produced.

[0035] (Manufacture of polishing pad 2) Polishing pad 2 was manufactured in the same manner as polishing pad 1, except that the polishing pad material was made of vinyl ester resin (product name: Lipoxy, manufactured by Resonac Co., Ltd.) instead of unsaturated polyester resin, and the mesh fabric material was made of polyethylene fiber instead of polypropylene fiber.

[0036] (Manufacture of polishing pad 3) Polishing pad 3 was manufactured in the same manner as polishing pad 1, except that the material of the polishing pad was a UV-curable resin (product name: SR368D NS (tris(2-hydroxyethyl)isocyanurate acrylate), manufactured by Arkema) containing 12 mass% abrasive grains (product name: SQDP, manufactured by Surface Phase, particle size 4 μm) instead of unsaturated polyester resin, and the resin was cured by exposure to ultraviolet light without allowing any fibrous material to penetrate.

[0037] Furthermore, in manufacturing polishing pads 2 and 3, it was confirmed that polishing pads similar to polishing pad 1 can be manufactured using a plastic intaglio plate made of polypropylene resin, even if the material of the polishing pad, the material of the mesh fabric, the presence or absence of abrasive grains, etc. are changed.

[0038] (When peeled off from the intaglio plate) A peeling experiment was carried out on the resin 50 from the plastic intaglio 72 using a peeling roller. As the peeling roller, for example, a combination of an adhesive tape and a rod-shaped peeling roller as described in JP-A-9-114384 is used. When a peeling experiment was carried out under conditions that allowed the intaglio to be peeled off from the resin 50 using the plastic intaglio 72 according to the above embodiment and using silicone rubber as the intaglio instead of plastic, a large force was required for peeling when the silicone rubber intaglio was used, and the protrusions 51 of the peeled resin 50 were found to have fallen off or been damaged, whereas the polishing pads 1 to 3 obtained using the plastic intaglio 72 made of polypropylene resin did not find any fall-off or damage to the protrusions 51 during peeling. [Industrial Applicability]

[0039] The method for producing a polishing pad of the present invention is a method for producing a polishing pad that is inexpensive and facilitates peeling of the resin from the intaglio plate, and therefore has industrial applicability as a method for producing polishing pads used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc.

[0040] 11 Polishing layer 50 Resin raw materials 50A Top surface of resin raw material 51 Convex 52 Base 53 Recess 71 Plastic Materials 72 Plastic Intaglio 72A Plastic Intaglio Underside 8. Release Agent

Claims

1. A method for producing a polishing pad having a polishing layer formed by curing a resin and containing abrasive grains, comprising the steps of: A step of preparing a plastic intaglio plate having a concave-convex pattern formed by vacuum forming or injection molding; pouring a resin material containing abrasive grains into the plastic intaglio plate; curing the resin; peeling the cured resin from the plastic intaglio to obtain the polishing layer. A method for manufacturing a polishing pad.

2. The method for producing a polishing pad according to claim 1 , wherein the temperature of the plastic intaglio is 130° C. or less in the step of curing the resin.

3. The method for producing a polishing pad according to claim 1 , wherein the plastic intaglio is made of a resin selected from polyethylene, polypropylene, polystyrene, and polyvinyl chloride.

4. The method for producing a polishing pad according to claim 1 , further comprising a step of applying a release agent to the plastic intaglio plate, the release agent being a silicone-based release agent or a fluorine-based release agent.

5. The method for producing a polishing pad according to claim 1 , wherein the resin is a UV-curable resin composition.

6. A method for polishing an object to be polished using a polishing pad obtained by the method for producing a polishing pad according to any one of claims 1 to 5, comprising the steps of: A polishing method in which polishing is carried out by fixed abrasive polishing.

Citation Information

Patent Citations

  • Polishing pad and method for manufacturing the same

    JP2019178248A

  • Polishing pad and method for manufacturing the same

    JP2019178258A