Resin composition, molding, sheet, film, bottle, tube, container, multilayer laminate, and method for producing resin composition
By integrating carbon-14-containing polypropylene and sorbic acid into EVOH resin compositions, thermal stability is enhanced, addressing the weakness of conventional EVOH-polypropylene blends and enabling high-performance molded articles and multilayer structures.
Patent Information
- Application Number
- JP2024051185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
EVOH resin compositions containing polypropylene for modification exhibit poorer thermal stability compared to compositions consisting only of EVOH, necessitating further improvement.
Incorporating a polypropylene resin containing carbon-14 and sorbic acid into the EVOH resin composition, with specific mass ratios and content levels to enhance thermal stability.
The resulting resin composition demonstrates superior thermal stability, making it suitable for molded articles and multilayer structures due to the stronger bond energy of carbon-14 polypropylene and the thermal deterioration inhibiting effect of sorbic acid.
Smart Images

Figure 2024144336000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition containing an ethylene-vinyl alcohol copolymer and a polypropylene resin containing carbon 14. The present invention also relates to a molded article, a sheet, a film, a bottle, a tube, a container, a multilayer structure having a layer containing the resin composition, and a method for producing the resin composition. [Background technology]
[0002] Conventionally, ethylene-vinyl alcohol copolymer (hereinafter referred to as "EVOH") has been mainly used as a food packaging material because of its excellent gas barrier properties and transparency. Although the sheets, films, etc. used as the food packaging material can be produced using the above-mentioned EVOH alone, they are used in the form of a multilayer structure in which other thermoplastic resins are blended to improve the physical properties, etc., or layers made of polyolefin resins, etc. are laminated to impart other functions.
[0003] For example, in order to increase the flexibility of a film or the like made of EVOH, it has been proposed to incorporate two types of polypropylene with different physical properties in a specific ratio into an EVOH resin composition (see Patent Document 1 below). Furthermore, in order to improve the gas barrier properties of a film or the like made of EVOH, it has been proposed to disperse and incorporate EVOH in polypropylene as a layer of a specific shape (see Patent Document 2 below). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-34771 A [Patent Document 2] JP 2016-150949 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, such EVOH resin compositions that contain polypropylene for modification tend to have inferior thermal stability compared to resin compositions consisting of EVOH alone, and further improvements are therefore required.
[0006] Therefore, an object of the present invention is to provide an EVOH resin composition containing polypropylene, which has excellent thermal stability. [Means for solving the problem]
[0007] In view of the above circumstances, the present inventors have found that the above problems can be solved by using a polypropylene resin containing 14 carbon atoms instead of polypropylene and further containing sorbic acid.
[0008] That is, the present invention has the following aspects. [1] A resin composition containing EVOH (A), a polypropylene resin containing 14 carbon atoms (B), and sorbic acid (C). [2] The resin composition according to [1], wherein a mass ratio [(A) / (B)] of the EVOH (A) to the polypropylene resin containing 14 carbon atoms (B) is 10 / 90 to 99 / 1. [3] The resin composition according to [1] or [2], wherein the content of the EVOH (A) in the entire resin composition is 10 to 99 mass %. [4] The resin composition according to any one of [1] to [3], wherein the content of the polypropylene resin (B) containing 14 carbon atoms in the entire resin composition is 1 to 90 mass %. [5] The resin composition according to any one of [1] to [4], wherein the content of the sorbic acid (C) relative to the entire resin composition is 1 to 10,000 ppm by mass. [6] A molded article comprising the resin composition according to any one of [1] to [5]. [7] A sheet comprising the resin composition according to any one of [1] to [5]. [8] A film comprising the resin composition according to any one of [1] to [5]. [9] A bottle comprising the resin composition according to any one of [1] to [5].
[10] A tube comprising the resin composition according to any one of [1] to [5].
[11] A container comprising the resin composition according to any one of [1] to [5].
[12] A multilayer structure having a layer containing the resin composition according to any one of [1] to [5].
[13] A method for producing a resin composition, comprising the step of mixing EVOH (A), a carbon-14 containing polypropylene resin (B), and sorbic acid (C). Effect of the Invention
[0009] The resin composition of the present invention has excellent thermal stability and can therefore be suitably used as a raw material for molded articles and multilayer structures. The reason why the resin composition of the present invention has excellent thermal stability is believed to be that polypropylene resin containing carbon-14 has stronger bond energy due to the primary isotope effect compared to petroleum-derived polypropylene resin not containing carbon-14, which slows down decomposition and increases thermal stability, as well as a synergistic effect with sorbic acid, which has a thermal degradation inhibitory effect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in more detail below based on examples of the present invention, but the present invention is not limited to these embodiments.
[0011] In this specification, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "X and / or Y (X and Y are optional)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y. In the present specification, the upper limit or lower limit of a numerical range described in stages can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In addition, in the numerical range described in this specification, the upper limit or lower limit of the numerical range can be replaced with a value shown in the examples.
[0012] In this specification, the term "film" also includes the terms "tape" and "sheet." In this specification, the term "main component" means a component that has a significant effect on the properties of the target object, and the content of the component in the target object is usually 50 mass % or more, preferably 55 mass % or more, more preferably 60 mass % or more, and even more preferably 70 mass % or more, and may be 100 mass %.
[0013] A resin composition according to one embodiment of the present invention (hereinafter referred to as "the resin composition") contains EVOH (A), a polypropylene resin containing 14 carbon atoms (B), and sorbic acid (C). Each component will be described below.
[0014] <EVOH(A)> The EVOH (A) is a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.
[0015] The polymerization of ethylene and vinyl ester monomers can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, and generally, solution polymerization using methanol as a solvent is used. The saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method.
[0016] The EVOH (A) thus produced is mainly composed of structural units derived from ethylene and vinyl alcohol structural units, and usually contains a small amount of vinyl ester structural units which remain unsaponified.
[0017] As the vinyl ester monomer, vinyl acetate is typically used because of its good market availability and efficiency in treating impurities during production. Examples of vinyl ester monomers other than vinyl acetate include aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate. Usually, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These can be used alone or in combination of two or more kinds.
[0018] The ethylene content in the EVOH (A) can be controlled by the ethylene pressure when the vinyl ester monomer and ethylene are copolymerized, and is 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. If the content is too low, the gas barrier properties and melt moldability under high humidity conditions tend to decrease, and conversely, if the content is too high, the gas barrier properties tend to decrease. The ethylene content can be measured based on ISO14663.
[0019] The degree of saponification of the vinyl ester component in EVOH (A) can be controlled by the amount, temperature, time, etc. of the saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) used when saponifying the ethylene-vinyl ester copolymer, and is usually 90 to 100 mol%, preferably 95 to 100 mol%, particularly preferably 99 to 100 mol%. If the degree of saponification is too low, the gas barrier properties, thermal stability, moisture resistance, etc. tend to decrease. The degree of saponification of the EVOH (A) can be measured based on JIS K6726 (wherein the EVOH is used as a solution uniformly dissolved in a water / methanol solvent).
[0020] The melt flow rate (MFR) of the EVOH (A) (210°C, load 2160 g) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, the film formability tends to be unstable, and if it is too low, the viscosity tends to be too high, making melt extrusion difficult. The MFR is an index of the polymerization degree of the EVOH, and can be adjusted by the amount of polymerization initiator and the amount of solvent when copolymerizing ethylene and vinyl ester monomer.
[0021] Furthermore, EVOH (A) may further contain structural units derived from the comonomers shown below within a range that does not impair the effects of the present invention (for example, 10 mol % or less of EVOH). Examples of the comonomers include olefins such as propylene, 1-butene, and isobutene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 3-butene-1,2-diol, 4-penten-1-ol, and 5-hexene-1,2-diol, as well as their esterified and acylated derivatives; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyryloxy. -2-methylenepropane and other hydroxyalkylvinylidene diacetates; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, and other salts or mono- or dialkyl esters in which the alkyl group has 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its acid salts or its quaternary salts, etc. Acrylamides; methacrylamide, N-alkyl methacrylamides in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethyl methacrylamide, 2-methacrylamidopropanesulfonic acid or its salt, methacrylamidepropyldimethylamine or its acid salt or its quaternary salt; N-vinyl amides such as N-vinylpyrrolidone, N-vinylformamide, and N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; alkyl vinyl ethers in which the alkyl group has 1 to 18 carbon atoms, hydrochloride, etc. vinyl ethers such as alkoxyalkyl vinyl ether and alkoxyalkyl vinyl ether; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; and comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamido-2-methylpropanesulfonic acid.These can be used alone or in combination of two or more.
[0022] In particular, EVOH copolymerized with hydroxyl group-containing α-olefins, i.e., EVOH having a primary hydroxyl group in the side chain, is preferred because it has good secondary formability while retaining gas barrier properties, and among these, EVOH having a 1,2-diol structure in the side chain is preferred. In the case of EVOH having a primary hydroxyl group in the side chain, the content of structural units derived from a monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, and particularly preferably 1 to 10 mol %.
[0023] The EVOH (A) used in the present embodiment may be one that has been "post-modified" by, for example, urethanization, acetalization, cyanoethylation, or oxyalkylenation.
[0024] Furthermore, the EVOH (A) used in this embodiment may be a mixture of two or more types of EVOH (A), for example, EVOH (A) having a different ethylene content, a different degree of saponification, a different degree of polymerization, or a different copolymerization component.
[0025] The content of EVOH (A) in the present resin composition is usually 1 mass% or more, preferably 10 to 99 mass%, more preferably 30 to 95 mass%, and further preferably 50 to 90 mass%, based on the total mass of the resin composition. When such a value is within the above range, the effects of the present invention tend to be more effectively obtained. The "resin composition" in the "whole resin composition" that is the basis for the content of the EVOH (A) refers to the EVOH resin composition as a final product that contains the EVOH resin (A), the polypropylene resin (B) containing 14 carbon atoms, sorbic acid (C), various additives that are blended as necessary, etc. The same applies to the following explanations.
[0026] <Polypropylene resin containing carbon 14 (B)> The carbon-14-containing polypropylene resin (B) used in the resin composition means a polypropylene resin obtained by chemical or biological synthesis using renewable biomass resources as raw materials. The carbon-14-containing polypropylene resin (B) has the characteristic that even if it is incinerated, it does not increase the carbon dioxide concentration in the atmosphere due to the carbon-neutrality of biomass.
[0027] The polypropylene resin (B) containing carbon 14 is preferably a biopropylene derived from biopropanol obtained from a plant raw material. That is, the polypropylene resin (B) containing carbon 14 is preferably a plant-derived polypropylene resin.
[0028] In addition, polypropylene resin derived from plants (biomass resources) and polypropylene resin derived from petroleum do not differ in physical properties such as molecular weight and mechanical properties. Therefore, the bio-based content is generally used to distinguish between them. The bio-based content is defined as the carbon content of petroleum-derived polypropylene resin. 14 Since it does not contain C (radioactive carbon-14, half-life 5730 years), 14 The concentration of C is measured by accelerator mass spectrometry and used as an index of the content of plant-derived bio-polypropylene resin. Therefore, if a film is made using plant-derived polypropylene resin, the bio-based content of the film will be determined according to the content of plant-derived polypropylene resin. In other words, polypropylene resin (B), which contains carbon-14, can detect radioactive carbon ( 14 C) is meant to include
[0029] The biobased content can be determined, for example, by heating and stirring the resin composition in a water / methanol mixed solvent to dissolve the EVOH (A), and measuring the carbon content of the remaining polypropylene resin ( 14C) content can be determined by the following method. The sample to be measured is burned to generate carbon dioxide, which is purified in a vacuum line and reduced with hydrogen using iron as a catalyst to generate graphite. This graphite is then subjected to a tandem accelerator-based 14 Attach it to the C-AMS dedicated device (manufactured by NEC) 14 Counting C, 13 Concentration of C ( 13 C / 12 C). 14 Concentration of C ( 14 C / 12 C), and from this measurement, the carbon content of the sample relative to the standard modern carbon is 14 The C concentration is calculated and the biobased content is calculated in accordance with ASTM D6866. Furthermore, in order to distinguish between polypropylene resin derived from plants (biomass resources) and petroleum-derived polypropylene resin, the aforementioned bio-based content is used, and the measurement method is also as described above.
[0030] The carbon-14 content in the carbon-14-containing polypropylene resin (B) is not particularly limited, but the ratio of carbon-14 to the total carbon in the carbon-14-containing polypropylene resin (B) is usually 1.0×10 -14 It is equal to or greater than 1.0×10 -13 The upper limit is usually 1.2 × 10 -12 It is.
[0031] This resin composition contains polypropylene resin (B) containing carbon 14, and therefore has superior thermal stability compared to resin compositions containing conventional petroleum-derived polypropylene resins. The reason for this is presumed to be that polypropylene resin containing carbon 14 has stronger bond energy due to the primary isotope effect, which slows decomposition and increases thermal stability.
[0032] The carbon-14-containing polypropylene resin (B) used in the present resin composition usually has a bio-based content of 1 to 99%, preferably 5 to 95%, and particularly preferably 10 to 90%. By setting the bio-based content of the carbon-14-containing polypropylene resin (B) within the above range, a resin composition having better thermal stability can be obtained.
[0033] The type of "polypropylene" in the polypropylene resin (B) containing 14 carbon atoms is not particularly limited, and may be a homopolypropylene or a copolymer of propylene and a small amount of a comonomer. The form of the copolymer may be a block copolymer or a random copolymer. For example, a copolymer consisting of propylene and less than 50% by mass of other α-olefin monomers, or a copolymer consisting of 3% or less by mass of non-olefin monomers having functional groups may be used.
[0034] Examples of the other α-olefins include ethylene, α-olefins having 4 to 20 carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl- Examples thereof include 1-butene, 4-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc. These may be used alone or in combination of two or more kinds.
[0035] Examples of the non-olefin monomer include styrene monomers, diene monomers, cyclic monomers, oxygen atom-containing monomers, etc. These may be used alone or in combination of two or more kinds.
[0036] Examples of the styrene monomer include styrene, 4-methylstyrene, and 4-dimethylaminostyrene.
[0037] Examples of the diene monomer include 1,3-butadiene, 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, cyclohexadiene, and dicyclooctadiene.
[0038] Examples of the cyclic monomer include methylenenorbornene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornadiene, and cyclopentene.
[0039] Examples of the oxygen atom-containing monomer include hexenol, hexenoic acid, and methyl octenoate.
[0040] The other α-olefins and non-olefin monomers may be those made from renewable biomass resources or petroleum. When those made from renewable biomass resources are used, the bio-based content of the final product can be further increased. When those made from petroleum are used, a wide variety of them are available, so by using them to produce the polypropylene resin (B) containing carbon-14, the physical properties, etc. can be easily adjusted.
[0041] The polypropylene resin (B) containing 14 carbon atoms is obtained by homopolymerization of propylene or copolymerization of propylene and a comonomer, as described above, and the polymerization or copolymerization can be carried out by a conventional method using a metallocene catalyst or a Ziegler-Natta catalyst. Among them, it is preferable to use a metallocene catalyst.
[0042] The polypropylene resin (B) containing 14 carbon atoms may be used alone or in combination of two or more kinds. Among them, it is preferable to use homopolypropylene derived from biopropylene, or ethylene-propylene block copolymer, ethylene-propylene random copolymer, or impact copolymer derived from biopropylene in terms of moldability, handling, and thermal stability.
[0043] The melt flow rate (MFR) (230°C, load 2160 g) of the polypropylene resin (B) containing carbon 14 is usually 0.1 to 100 g / 10 min, preferably 0.5 to 90 g / 10 min, and particularly preferably 2 to 80 g / 10 min. If the MFR is too high, the film formability tends to be unstable, and if it is too low, the viscosity tends to be high, making melt extrusion difficult.
[0044] Commercially available polypropylene resin (B) containing carbon 14 that is preferably used in this embodiment includes HP640J manufactured by LyondellBasell.
[0045] The content of the polypropylene resin (B) containing carbon 14 in the resin composition is usually 0.5 mass% or more, preferably 1 to 90 mass%, more preferably 5 to 70 mass%, and particularly preferably 10 to 50 mass%, based on the total mass of the resin composition. By setting the content of the polypropylene resin (B) containing carbon 14 in the above range, a resin composition having better thermal stability can be obtained.
[0046] In the present resin composition, the mass ratio [(A) / (B)] of the EVOH (A) to the polypropylene resin (B) containing carbon 14 is usually 10 / 90 to 99 / 1, preferably 30 / 70 to 95 / 5, and more preferably 50 / 50 to 90 / 10. When the mass ratio of the EVOH (A) to the polypropylene resin (B) containing carbon 14 is within the above range, a resin composition having better thermal stability can be obtained.
[0047] In the present resin composition, the proportion of the total content of the EVOH (A) and the polypropylene resin (B) containing 14 carbon atoms in the entire resin composition is not particularly limited, but is usually 70 mass% or more, preferably 80 mass% or more, and more preferably 90 mass% or more.
[0048] <Sorbic acid (C)> The sorbic acid (C) used in the present resin composition is an unsaturated fatty acid having a conjugated double bond in its structure.
[0049] The content of the sorbic acid (C) is usually 1 to 10,000 ppm, preferably 10 to 5,000 ppm, more preferably 50 to 2,500 ppm, and even more preferably 100 to 1,500 ppm by mass based on the entire EVOH resin composition. By setting the content of the sorbic acid (C) within the above range, the thermal stability of the resin composition tends to be further improved. However, if the content of the sorbic acid (C) is too high, the amount of conjugated double bonds increases too much, and coloring tends to occur.
[0050] When the resin composition is in the form of a molded product such as pellets, the content of sorbic acid (C) in the resin composition can be quantified by the following method. That is, the molded product such as pellets is first crushed by any method (for example, freeze crushing) and dissolved in a lower alcohol solvent having 1 to 5 carbon atoms to obtain a sample. The sample is then measured by liquid chromatography mass spectrometry (LC / MS / MS) to quantitatively determine the content of sorbic acid (C).
[0051] Furthermore, in the case of a molded product in which the present resin composition is combined with other thermoplastic resins, for example a multilayer structure, the layer consisting of the present resin composition to be measured can be removed from the multilayer structure by any method and then quantified in the same manner as described above.
[0052] <Other ingredients> The resin composition may contain EVOH (A), resins other than the polypropylene resin (B) containing 14 carbon atoms (e.g., petroleum-derived polypropylene resins, other types of resins), and any additives other than sorbic acid (C) (hereinafter, these are referred to as "other components") according to various purposes within the scope of not significantly impairing the effects of the present invention. Only one type of other component may be used, or two or more types may be used in any combination and ratio.
[0053] Examples of the additives include antioxidants, ultraviolet absorbers, plasticizers, lubricants, fillers, and antistatic agents.
[0054] When the present resin composition contains the above-mentioned "other components", the total content thereof is usually 30 mass % or less, preferably 20 mass % or less, and more preferably 10 mass % or less, relative to the present resin composition.
[0055] [Method of producing resin composition] The resin composition can be produced by mixing the essential components EVOH (A), the polypropylene resin containing carbon 14 (B), and sorbic acid (C), as well as the other components as necessary. Examples of the mixing method include known methods such as a dry blend method, a melt mixing method in which a compound is obtained using a single-screw extruder or a twin-screw extruder, a solution mixing method, and an impregnation method, and these methods can be used in any combination.
[0056] [Resin composition] The resin composition obtained in this manner is less susceptible to decomposition at high temperatures and has excellent thermal stability compared to conventional resin compositions obtained by combining EVOH and petroleum-derived polypropylene.
[0057] The bio-based content of the resin composition can be determined, for example, by adding 14 carbon atoms ( 14 C) content can be determined by the following method. The sample to be measured is burned to generate carbon dioxide, which is purified in a vacuum line and reduced with hydrogen using iron as a catalyst to generate graphite. This graphite is then subjected to a tandem accelerator-based 14 Attach it to the C-AMS dedicated device (manufactured by NEC) 14 Counting C, 13 Concentration of C ( 13 C / 12 C). 14 Concentration of C ( 14 C / 12 C), and from this measurement, the carbon content of the sample relative to the standard modern carbon is 14 The C concentration is calculated and the biobased content is calculated in accordance with ASTM D6866.
[0058] The content of carbon-14 in the resin composition is not particularly limited, but the ratio of carbon-14 to the total carbon in the resin composition is usually 1.0×10 -16 It is equal to or greater than 1.0×10 -14 The upper limit is usually 1.2 × 10 -12 It is.
[0059] The biobased content of the present resin composition is usually 0.01 to 99.99%, preferably 0.1 to 99.9%, more preferably 1 to 99%, further preferably 1 to 90%, particularly preferably 10 to 90%, 2 to 70%, or 4 to 50%. By setting the biobased content of the resin composition within the above range, a resin composition having better thermal stability can be obtained.
[0060] The melt flow rate (MFR) of the present resin composition (210° C., load 2160 g) is usually from 0.1 to 100 g / 10 min, preferably from 0.5 to 90 g / 10 min, and particularly preferably from 2 to 80 g / 10 min.
[0061] The water content of the present resin composition is usually from 0.01 to 0.5% by mass, preferably from 0.02 to 0.35% by mass, and particularly preferably from 0.05 to 0.3% by mass.
[0062] The water content of the resin composition is measured and calculated by the following method. The mass (W1) of the resin composition before drying is weighed on an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and then cooled in a desiccator for 30 minutes, after which the mass (W2) is weighed and calculated using the following formula. Moisture content (mass%)=[(W1-W2) / W1]×100
[0063] The reduction temperature difference of the present resin composition is usually 10°C or more, preferably 11°C or more, more preferably 12°C or more, and further preferably 13°C or more. The temperature loss difference can be calculated by measuring the mass loss rate when the temperature is increased at 10°C / min in a nitrogen atmosphere using a thermogravimetric analyzer (Perkin Elmer, Pyris 1 TGA), and then subtracting the temperature at which the resin composition has lost 5% mass from the temperature at which the resin composition has lost 10% mass (temperature loss difference). The higher this value is, the slower the decomposition of the resin composition is, and the more excellent the thermal stability of the resin composition is.
[0064] The resin composition is prepared as a resin composition in various forms, such as pellets or powder, and is provided as a material for various molded bodies and multilayer structures. As described above, the resin composition has excellent thermal stability, so that a molded body using the resin composition or a multilayer structure having a layer using the resin composition is of excellent quality. In particular, in this embodiment, when the resin composition is provided as a material for melt molding, the effects of the present invention tend to be obtained more efficiently, which is preferable.
[0065] [Molded body] A molded article according to one embodiment of the present invention (hereinafter, referred to as the present molded article) is obtained by molding the present resin composition.
[0066] Examples of the shape of the present molded article include films, sheets, tapes, cups, trays, tubes, bottles, containers, pipes, filaments, irregular cross-section extrusions, various irregular shapes, and the like.
[0067] The method for molding the resin composition is not particularly limited, and any molding method applicable to general resin compositions can be used, such as extrusion molding, blow molding, injection molding, thermoforming, etc.
[0068] [Multilayer structure] A multilayer structure according to one embodiment of the present invention (hereinafter, referred to as "the present multilayer structure") has at least one layer containing the present resin composition. The present multilayer structure can be laminated with another substrate (hereinafter referred to as "substrate resin") mainly composed of a thermoplastic resin other than the present resin composition to impart further strength or other functions.
[0069] Examples of the base resin include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and side chain); and unsaturated carboxylic acid resins obtained by mixing these polyolefins. Examples of the polyolefin resin include polyolefin resins in the broad sense including modified olefin resins such as unsaturated carboxylic acid modified polyolefin resins graft-modified with an acid or an ester thereof, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, and aromatic or aliphatic polyketones.
[0070] Of these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred from the standpoint of economic efficiency and productivity, and polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.
[0071] The layer structure of the present multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, and b2 / b1 / a / b1 / a / b1 / b2, where a resin composition layer is a (a1, a2, . . .) and a base resin layer is b (b1, b2, . . .). In addition, a recycled layer containing a mixture of the present resin composition and base resin obtained by remelting and molding the ends and defective products generated during the manufacturing process of the multilayer structure may be provided. The total number of layers of the multilayer structure is usually 2 to 15, preferably 3 to 10. In the above layer structure, an adhesive resin layer containing an adhesive resin may be interposed between each layer as necessary.
[0072] The adhesive resin may be a known one, and may be appropriately selected according to the type of thermoplastic resin used in the base resin layer "b". A representative example is a modified polyolefin polymer containing a carboxy group obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin by addition reaction, graft reaction, or the like. Examples of the modified polyolefin polymer containing a carboxy group include maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-propylene (block and random) copolymer, maleic anhydride grafted ethylene-ethyl acrylate copolymer, maleic anhydride grafted ethylene-vinyl acetate copolymer, maleic anhydride modified polycyclic olefin resin, maleic anhydride grafted polyolefin resin, etc. One or a mixture of two or more selected from these may be used.
[0073] In the present multilayer structure, when an adhesive resin layer is used between the resin composition layer and the base resin layer, since the adhesive resin layers are located on both sides of the resin composition layer, it is preferable to use an adhesive resin with excellent hydrophobicity.
[0074] The base resin and adhesive resin may contain conventionally known plasticizers, fillers, clays (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, waxes, etc., within a range that does not impair the spirit of the present invention (for example, 30 mass % or less, preferably 10 mass % or less, based on the total resin).
[0075] The resin composition and the above-mentioned substrate resin can be laminated (including the case where an adhesive resin layer is interposed) by a known method. For example, a method of melt extrusion laminating a substrate resin onto a film, sheet, etc. of the resin composition, a method of melt extrusion laminating the resin composition onto a substrate resin layer, a method of co-extruding a resin composition and a substrate resin, a method of dry laminating a resin composition layer and a substrate resin layer using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the resin composition onto a substrate resin and then removing the solvent, etc. Among these, a method of co-extruding a resin composition and a substrate resin is preferred from the viewpoint of cost and environment.
[0076] The multilayer structure is subjected to a (heat) stretching treatment as necessary. The stretching treatment may be either uniaxial stretching or biaxial stretching, and in the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. As the stretching method, a method with a high stretch ratio among roll stretching, tenter stretching, tubular stretching, stretch blowing, vacuum pressure molding, etc. may be used. The stretching temperature is a temperature near the melting point of the multilayer structure, and is usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. If the stretching temperature is too low, the stretchability becomes poor, and if it is too high, it becomes difficult to maintain a stable stretched state.
[0077] In order to impart dimensional stability, heat setting may be performed after the stretching treatment. Heat setting can be performed by a known means, for example, the stretched film is heat-treated usually at 80 to 180°C, preferably 100 to 165°C, for about 2 to 600 seconds while being kept in a tensed state. When the multilayer stretched film obtained from the present resin composition is used as a shrink film, the above-mentioned heat setting may not be performed, and instead, in order to impart heat shrinkability, a treatment such as cooling and fixing by applying cold air to the stretched film may be performed.
[0078] In some cases, the multilayer structure can be used to obtain a cup- or tray-shaped multilayer container. In this case, a squeeze molding method is usually used, specifically vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. Furthermore, when a tube- or bottle-shaped multilayer container (laminate structure) is obtained from a multilayer parison (a hollow tubular preform before blowing), a blow molding method is used. Specifically, extrusion blow molding (double-head type, mold movement type, parison shift type, rotary type, accumulator type, horizontal parison type, etc.), cold parison type blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding in-line type biaxial stretch blow molding, etc.) can be used. The resulting laminate may be subjected to processes such as heat treatment, cooling, rolling, printing, dry lamination, solution or melt coating, bag making, deep drawing, box processing, tube processing, and splitting, as required.
[0079] The thickness of the present multilayer structure (including the stretched one), and further the thickness of the resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, cannot be generally stated depending on the layer structure, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., but the thickness of the multilayer structure (including the stretched one) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.
[0080] Furthermore, the thickness ratio of the resin composition layer to the base resin layer in the multilayer structure (resin composition layer / base resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, when there are multiple layers of each type. Furthermore, the thickness ratio of the resin composition layer to the adhesive resin layer in the multilayer structure (resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, when there are multiple layers of each type, when there are multiple layers of each type.
[0081] The thus obtained films, sheets, bags made of stretched films, and containers made of cups, trays, tubes, bottles, etc. are useful as various packaging materials and containers for general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc. EXAMPLES
[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. In addition, unless otherwise specified, "parts" and "%" below are based on mass. Prior to the examples, the following components were prepared:
[0083] [EVOH] EVOH (A1): Ethylene unit content 29 mol%, MFR (210°C, load 2160 g): 3.8 g / 10 min, saponification degree 99.9 mol% [Polypropylene resin] Polypropylene containing carbon-14 (B1): Polypropylene containing carbon-14 (LyondellBasell, HP640J), MFR (230°C, load 2160g) 3.2g / 10min, bio-based content 40% Petroleum-derived polypropylene (B'1): Polypropylene (Japan Polypropylene, FY6), MFR (230°C, load 2160g) 2.4g / 10min
[0084] <Example 1> 90 parts of EVOH (A1), 10 parts of polypropylene (B1) containing carbon 14, and a predetermined amount of sorbic acid (C) were mixed together by dry blending, and then fed to a twin-screw kneader at a rate of 8 kg / hour using a mass feeder, and then strand-cut with a drum pelletizer to prepare a pellet-shaped resin composition. The kneading conditions were as follows: [Mixing conditions] Twin screw extruder: diameter 20mm, L / D=48 (Toshiba Machine Co., Ltd.) ·Extruder setting temperature: C1 / C2 / C3 / C4 / C5 / C6 / H=170 / 200 / 210 / 210 / 210 / 210 / 210 Screw speed: 250 rpm - Take-off speed: 12m / min
[0085] <Examples 2 and 3, Comparative Examples 1 to 3> Resin compositions of Examples 2 and 3 and Comparative Examples 1 to 3 were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1 below.
[0086] The following thermal stability evaluation was carried out using the obtained resin compositions of Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1 below.
[0087] [Evaluation of Thermal Stability] [Decrease temperature difference] Using 5 mg of the pellet-shaped resin composition obtained, the mass loss rate was measured by a thermogravimetric analyzer (Perkin Elmer, Pyris 1 TGA) under a nitrogen atmosphere while increasing the temperature at 10°C / min. Then, the value (loss temperature difference) was calculated by subtracting the temperature at 5% mass loss from the temperature at 10% mass loss of the resin composition. The higher this value, the slower the decomposition of the resin composition is, and the more excellent the thermal stability of the resin composition is. [Thermal stability improvement rate] The thermal stability improvement rate was calculated from the following formula when the value of the decrease in temperature difference of the comparative example corresponding to each example (for example, the comparative example corresponding to Example 1 is Comparative Example 1) was set to 100. Thermal stability improvement rate (%) = (decrease in temperature difference of the embodiment / decrease in temperature difference of the comparative example corresponding to the embodiment × 100) - 100 (Thermal stability improvement rate (%) is rounded off to the nearest whole number.)
[0088] [Table 1]
[0089] From the results in Table 1, it can be seen that the resin compositions of Examples 1 and 2, which used polypropylene (B1) containing carbon 14 and sorbic acid (C), had improved thermal stability compared to Comparative Example 1, which used only bio-polypropylene (B1). This is thought to be because polypropylene containing carbon 14 decomposes more slowly due to stronger bond energy caused by the primary isotope effect, and the synergistic effect with sorbic acid significantly increases thermal stability. On the other hand, the resin composition of Comparative Example 2 uses petroleum-derived polypropylene (B'1) and therefore contains sorbic acid (C), but is inferior in thermal stability to that of Example 1. Moreover, it is apparent from the above Examples 1 to 3 and Comparative Examples 1 to 3 that the effect of the present invention of excellent thermal stability can be obtained in the same manner even if the blending ratio of each component is changed. Molded articles, sheets, films, bottles, tubes, containers, and multilayer structures having a layer containing the resin compositions of Examples 1 to 3 also have excellent thermal stability. [Industrial Applicability]
[0090] The present resin composition has superior thermal stability to resin compositions using petroleum-derived polypropylene, and therefore molded articles made of the present resin composition and multilayer structures having a layer containing the present resin composition are useful as materials for various packaging containers.
Claims
1. A resin composition comprising an ethylene-vinyl alcohol copolymer (A), a polypropylene resin containing 14 carbon atoms (B), and sorbic acid (C).
2. The mass ratio [(A) / (B)] of the ethylene-vinyl alcohol copolymer (A) to the polypropylene resin (B) containing 14 carbon atoms is 10 / 90 to 99 / 1. The resin composition according to claim 1.
3. The resin composition according to claim 1 or 2, wherein the content of the ethylene-vinyl alcohol copolymer (A) relative to the entire resin composition is 10 to 99 mass%.
4. The resin composition according to claim 1 or 2, wherein the content of the polypropylene resin (B) containing carbon 14 relative to the entire resin composition is 1 to 90 mass%.
5. The resin composition according to claim 1 or 2, wherein the content of the sorbic acid (C) relative to the entire resin composition is 1 to 10,000 ppm by mass.
6. A molded article comprising the resin composition according to claim 1 or 2.
7. A sheet comprising the resin composition according to claim 1 or 2.
8. A film comprising the resin composition according to claim 1 or 2.
9. A bottle comprising the resin composition according to claim 1 or 2.
10. A tube comprising the resin composition according to claim 1 or 2.
11. A container comprising the resin composition according to claim 1 or 2.
12. A multilayer structure having a layer comprising the resin composition according to claim 1 or 2.
13. A method for producing a resin composition, comprising the step of mixing an ethylene-vinyl alcohol copolymer (A), a carbon-14 containing polypropylene resin (B), and sorbic acid (C).
Citation Information
Patent Citations
Molding and method for producing the same
JP2016150949A
Ethylene-vinyl alcohol resin composition
JP2022034771A