Glass sheet comprising coating applied in at least one region of at least one side of glass sheet, composite material comprising the same, and paste for producing such glass sheet
A sol-gel coated borosilicate glass sheet with controlled Bi, ZnO, and alkali oxide content maintains mechanical strength and thermal resistance, addressing the strength reduction issues in laminated glass applications.
Patent Information
- Application Number
- JP2024054234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-11
AI Technical Summary
Existing coated borosilicate glass sheets used in laminates for vehicle windshields face issues with mechanical strength reduction due to high adhesive coatings, which cause differences in thermal expansion coefficients, leading to delamination and reduced bending strength.
A partially coated borosilicate glass sheet with a sol-gel coating containing SiO2, pigments, and additives, limited to less than 500 ppm Bi, ZnO, and alkali oxides, which is baked at lower temperatures to maintain mechanical strength and compatibility with polymer layers.
The sol-gel coating maintains or enhances the mechanical strength of the glass sheet, achieving bending strengths of at least 50% of the uncoated glass, with improved thermal and chemical resistance, suitable for laminated glass applications.
Smart Images

Figure 2024144381000004 
Figure 2024144381000005 
Figure 2024144381000006
Abstract
Description
[Technical field]
[0001] The present disclosure generally relates to glass panes, particularly partially coated glass panes, which may be used, for example, for vehicles, as well as composites containing such panes and pastes for producing such panes, wherein the panes are made of SiO 2 and B. 2 O 3 In particular, the present disclosure therefore also relates to glass sheets consisting of or comprising borosilicate glass. [Background technology]
[0002] Glass sheets made of or containing borosilicate glass, especially those that are at least partially coated, have been known for a long time and are used, for example, as oven viewing windows in oven doors.The advantage of borosilicate glass here is its heat resistance compared to conventional soda-lime glass, so that oven viewing windows, for example for pyrolysis ovens, often contain such borosilicate glass sheets.Such borosilicate glass sheets can also be used, for example, as cover plates for cookware, which can also be called cook plates or cooking surfaces.
[0003] However, borosilicate glass can also be advantageous for other applications, since such glass has inherent advantages over known soda-lime glass, for example with regard to scratch resistance or mechanical resistance in general, as well as chemical durability, and therefore such borosilicate glass sheets are increasingly being used in windshields as well.
[0004] In the exterior glazing of vehicles, for example, it is known to use borosilicate glasses, such as those sold under the trade name Borofloat®. Such glasses are, for example, very well suited for laminated glazing and are characterized by a very high transmittance in the visible light range. Furthermore, such borosilicate glasses have very good heat resistance, high chemical durability and good mechanical strength.
[0005] For example, International Patent Application No. WO2015 / 059406 A describes laminated glass sheets, one of which, for example the outer sheet, may comprise, for example, borosilicate glass.
[0006] International Patent Application No. 2017 / 157660 (WO2017 / 157660 A1) describes insulating glazing panes for head-up displays. Here too, one of the panes of insulating glazing may comprise borosilicate glass.
[0007] Colombian application CO2017 / 0005596 A1 also describes highly resistant automotive glass panes.
[0008] International Patent Application No. 2019 / 130285 (WO2019 / 130285 A1) describes a laminate that has high resistance to abrasion and environmental influences.
[0009] Finally, International Patent Application No. WO2018 / 122769 A1 describes a laminate having high breaking strength.
[0010] For the safety of the vehicle occupants, the windshield is formed as a laminated glass pane and usually has a coating in the edge region. This coating serves, on the one hand, for example, to optically hide adhesives or components, such as antennas, and on the other hand, to protect against UV rays. Usually, this frame is arranged between both glass panes of a composite. The composite further comprises a polymer layer between the two glass panes, i.e. a layer that contains or consists of a polymer, which bonds the glass panes to one another. The glass panes are superimposed on one another with a coating arranged between them, especially in at least one region in the edge region, and are bent in a hot forming process. Subsequently, a polymer layer is applied between the two panes, which bonds the bent glass panes to one another, so that finally a laminated glass pane (also simply called a "composite" in the scope of the present disclosure) is obtained.
[0011] Many requirements are therefore imposed on the glass sheets contained in such composites. Since the bending process is carried out thermally, the glass sheets and the coatings applied thereon must be able to withstand this temperature. The glass sheets and the coatings must be able to form a bond with the polymer layer in such a way that a stable composite is formed and no delamination occurs between the glass and the polymer. Finally, the coating must have a sufficient optical tightness so that the components arranged in the edge area of the windshield are not visible in an unobtrusive way. This prevents distraction to the driver and increases driving safety. Microcracks or other defects in the coating should also be avoided if possible or at least minimized.
[0012] However, in addition to the temperature resistance of glass and coating, the above-mentioned compatibility of glass or coating with polymeric material to form a composite, optical density, and minimization of possible defects, the mechanical strength of the coated glass plate, characterized for example by fracture strength, also plays a role. Here, it is known that coatings, especially high-adhesion coatings, can impair the strength of glass plate. Here, especially high-adhesion coatings, for example coatings based on glass, can decisively reduce mechanical strength, for example fracture strength or bending strength. This is true in principle for all glass substrates, but even more so when the substrate, i.e. here, the glass plate, has a small coefficient of expansion, as in the case of borosilicate glass plates. Because here, for example, when using known ceramic paints, differences in the coefficient of expansion between coating and substrate occur, which are considered to be the cause of the observed strength loss of coated glass plate.
[0013] So-called sol-gel coatings or layers on glass have also been known for a long time.
[0014] In their first commercial applications, such sol-gel layers were formed as thin oxide layers which served in particular for producing optically effective coating systems on glass (e.g. the commercial products Amiran®, Conturan®, and Mirogard®), and the potential of sol-gel materials as binders for particle-based or particle-based coatings has also become increasingly evident.
[0015] For example, DE 20 2008 003 804 U1 describes a sol-gel coating for glass composites. For example, the coating can be formed as a single layer based on a porous sol-gel, or the coating can be constructed as a multilayer system of layers with different refractive indices. The coating according to DE 20 2008 003 804 is pigment-free and clearly serves to improve the light flux through the composite system, and can be understood as an antireflection layer, especially in the form of a single layer. If the glass composite according to DE 20 2008 003 804 is a composite of two plates, a sol-gel layer is also arranged on the side of the plate facing outwards, i.e. on the side of the composite facing away from the further plate.
[0016] US2013 / 0266781 A1 describes a coating structure of a colored coating obtained with a sol-gel based binder. The coating structure includes two coatings, one of which, which usually gives color and is directly arranged on the substrate, is a colored coating with a sol-gel based binder. This at least one coating is made porous to the passage of fluids, so that a further colored coating with a silicone binder is applied on the at least one coating as a sealing layer. This results in a glass or glass article with a decorative coating system, for example for use as a cooking surface. Composites from multiple plates are not addressed.
[0017] US 2009 / 0233082 A2 describes a glass or glass-ceramic article with a decorative coating. The decorative coating comprises at least one decorative pigment and a sol-gel binder, and the ceramic structure of the decorative coating is obtained after curing and baking of the coating. The coating thus comprises a high proportion of pigment, in particular clearly more pigment than binder by weight. Composites are not described.
[0018] FR3084355 A1 describes an enamelled substrate, in which the enamel layer is formed porous. In addition to the porous enamel layer, the substrate can also have further layers, for example porous sol-gel coatings based on silicon, which are formed as transparent functional layers and therefore do not contain pigments.
[0019] US2015 / 0225285 A2 describes a method for printing on glass. In this case, the glass substrate is first coated with an adhesion promoter and then one or more layers are printed with ink. After this printing, the coating or coatings can be cured. Furthermore, it is also possible to apply further layers on this coating, for example laminating a film. Composite plates containing two glass plates are not described, nor are colored sol-gel-based coatings.
[0020] US 2010 / 0047556 A2 describes a decorative coating for glass or glass-ceramic articles, which comprises a solid lubricant in addition to platelet-shaped pigments, the pigment to lubricant weight ratio being between 10:1 and 1:1. The application of the article is particularly concerned with so-called cooktops. Insulating glass panes are not addressed.
[0021] US 2010 / 0028629 A2 also describes a glass or glass-ceramic article with a decorative coating. The coating comprises two coating layers, of which the layer applied to the substrate (also called sealing layer) comprises a solid lubricant in addition to platelet-shaped pigments, the pigment to lubricant weight ratio being between 10:1 and 1:1. The application of the article is in particular related to so-called cooktops. Insulating glass panes are not addressed.
[0022] Finally, EP3830046 A1 describes an enamelled substrate, in which the enamel layer is formed porous.In addition to the porous enamel layer, the substrate also has a further layer, for example a porous sol-gel coating based on silicon, which is formed as a transparent functional layer and therefore does not contain pigments.The sol-gel layer can be formed as a porous anti-reflective coating, in particular with a low refractive index of 1.3 or less.
[0023] The aforementioned sol-gel layers are either not intended for use in laminates, especially for placement as intermediate layers in laminates, or are applied without coloring. High strength composite plates are not addressed either.
[0024] Thus, there is a need for coated glass sheets that at least alleviate the above-mentioned shortcomings of the prior art. There is also a need for pastes for producing such glass sheets, and sheet composites that include such coated glass sheets. [Prior art documents] [Patent documents]
[0025] [Patent Document 1] International Patent Application No. 2015 / 059406 [Patent Document 2] International Patent Application No. 2017 / 157660 [Patent Document 3] Colombian Patent Publication No. 2017 / 0005596 [Patent Document 4] International Patent Application No. 2019 / 130285 [Patent Document 5] International Patent Application No. 2018 / 122769 [Patent Document 6] German Utility Model No. 20 2008 003 804 [Patent Document 7] US Patent Application Publication No. 2013 / 0266781 [Patent Document 8] US Patent Application Publication No. 2009 / 0233082 [Patent Document 9] French Patent Application Publication No. 3084355 [Patent Document 10] US Patent Application Publication No. 2015 / 0225285 [Patent Document 11] US Patent Application Publication No. 2010 / 0047556 [Patent Document 12] US Patent Application Publication No. 2010 / 0028629 [Patent Document 13] European Patent Application Publication No. 3830046 Summary of the Invention [Problem to be solved by the invention]
[0026] The object of the present invention is to provide a glass pane, in particular a partially coated glass pane for vehicles, a paste for producing such a glass pane, and a composite comprising such a glass pane, which at least partially overcomes or at least alleviates the above-mentioned disadvantages of the prior art. [Means for solving the problem]
[0027] Summary of the Invention The problem of the present invention is solved by the subject matter of the independent claims. Preferred and particular embodiments are evident from the description of the present disclosure, the drawings and the dependent claims.
[0028] Thus, the present disclosure generally relates to glass panes, and in particular to partially coated glass panes, such as partially coated glass panes for vehicles. The glass panes are generally made of SiO 2 and B. 2 O 3 The present invention relates to a glass comprising a glass material having a thickness of 100 nm to 150 nm, i.e. formed as a borosilicate glass sheet, and at least one coating applied to at least one region of at least one side of the glass sheet. The at least one coating comprises SiO 2At least one coating contains at least one binder and at least one pigment, and at least one additive advantageously formed as a filler. At least one coating contains less than 500 ppm Bi by weight, 2 O 3 , and / or contains less than 500 ppm ZnO.
[0029] This configuration has many advantages.
[0030] Advantageously, the glass sheet therefore has a flexural strength of at least 80 and at most 300 MPa, preferably at least 100 and at most 210 MPa, particularly preferably at least 140 MPa, in at least one region having at least one coating applied on at least one side of the glass sheet.
[0031] Generally, this strength value applies to the entire glass pane, i.e., it can be determined, for example, even for a completely uncoated glass pane, although it has been found that in the case of glass panes according to embodiments having a coating as described by the present disclosure, this very good strength is also obtained in the coated areas.
[0032] SiO 2 and B. 2 O 3 This very good strength of the coated glass sheets, i.e. the coated borosilicate glass sheets, is due to the fact that the glass contains SiO 2 With a binder containing, again, less than 500 ppm Bi by weight 2 O 3 and / or less than 500 ppm ZnO, and / or less than 500 ppm B by mass, respectively 2 O 3 and / or containing less than 500 ppm of alkaline oxides. This results advantageously from the special composition of the coating, which according to a preferred embodiment is configured as a sol-gel coating.
[0033] Thus, according to the present disclosure, it is possible to easily combine the advantages of glass-based coatings, i.e. coatings with inorganic amorphous (especially X-ray amorphous) binders, with good strength of the resulting coated glass panes. The good strength of the resulting coated glass panes, especially shown in bending strength, advantageously lying within the aforementioned limits, is especially due to the fact that at least one coating present is made of SiO 2 This is due to the fact that, despite the inclusion of a coating based on glass flux, it is not formed as a coating based on glass flux and can therefore be cured or baked, preferably at temperatures that are not much higher than those of coatings based on glass flux. For example, in the case of coatings according to the embodiments, temperatures of up to 400° C., for example about 380° C., are sufficient for baking. This is particularly advantageous in view of the differences in thermal expansion coefficients that may occur between the coating and the substrate, i.e. here the glass sheet, which may contribute to a decrease in strength. Although coatings based on glass flux do indeed offer the advantages of glass-based coatings with high thermal, mechanical and / or chemical resistance, depending on the exact composition of the glass flux used, they must be baked at high temperatures, during which not only does the glass flux itself melt, but also at least a part of the surface of the glass substrate melts, so that a so-called “melting reaction zone” is formed. Not only is the melting process more energy consuming than the curing / baking of at least one coating according to the present disclosure, but this melting of the surface of the glass sheet also reduces the strength of the coated glass sheet relative to its starting strength.
[0034] Thus, the low bake temperature of the coating according to the embodiments of the present disclosure is advantageous compared to the bake temperature of coatings based on glass fluxes, because the bending process typical for composites in which glass sheets according to the embodiments may be used is usually not subject to the bake temperature of the coating, but to the substrate and the T of the substrate. g This is because it depends only on the glass transformation temperature, the glass transition temperature.
[0035] Many glass fluxes, especially Bi, address the problem of high firing temperatures and / or have a thermal expansion coefficient well adapted to glasses with significantly lower expansion, such as borosilicate glasses. 2 O 3 Alternatively, glass fluxes based on ZnO do exist, but even in this case the inherent strength loss resulting from partial melting of the glass surface remains.
[0036] The problem is that the coating is SiO 2 The present invention can be addressed by at least one coating according to the present disclosure, which comprises a binder comprising, but is not a glass flux. According to an embodiment, the binder according to the present disclosure is in particular a sol-gel binder, in particular SiO 2 and thus the majority, i.e. more than 50% by weight, advantageously more than 90% by weight, of the binder is based on SiO 2 The at least one coating is generally made of ZnO and Bi, which are characteristic components of glass flux. 2 O 3 and less than 500 ppm by weight of each. Nevertheless, with such a coating it is possible to obtain the advantageous properties of glass-based coatings, in particular good thermal and chemical resistance, together with good mechanical strength of the coated glass.
[0037] The bending strength of the (coated) glass sheet is advantageously at least 50% of the bending strength of the uncoated glass sheet in the coated area. Since mechanical strength, for example bending strength, is a statistical value, it is to be understood here that the same sheet was not investigated before and after coating with respect to bending strength, but rather the above description relates to investigations carried out on uncoated and coated glass sheets of the same composition and composition. In the scope of this disclosure, bending strength is understood to mean the strength of the glass sheet, also called double ring bending tensile strength, each specified according to DIN 1288-5. In the scope of this disclosure, the arithmetic mean is respectively indicated as the strength value.
[0038] In general, SiO 2 It is advantageous to configure the binder as comprising. In this way, generally good chemical durability and heat resistance of the binder is possible. Generally such binders are or can contain silicones, polysiloxanes, polysilsesquioxanes or partial hydrolysates of siloxanes, and mixtures thereof. The binders mentioned are summarized in this document under the generic term sol-gel binders. If these binders or their precursor materials (precursors) contain organic components, this may remain in the resulting coating after curing and possibly thermal baking, but may be largely burned off depending on the exact composition of the precursor materials and the respective baking process.
[0039] The good chemical durability of such coatings according to embodiments of the present disclosure also results from the fact that at least one coating according to embodiments does not contain further components which are usual constituents of coatings based on glass fluxes for borosilicate glass sheets and which serve to achieve the lowest possible melting points (and correspondingly the lowest possible baking temperatures).
[0040] Thus, according to the present disclosure, at least one coating alternatively or additionally comprises less than 500 ppm of alkali oxides. By alkali oxides, in the present disclosure, is understood an oxide of an alkali metal. In particular, the coating according to the embodiment comprises less than 500 ppm of Na 2 O and / or K 2 O and / or Li 2 O, where references in ppm are generally always to mass within the scope of this disclosure.
[0041] Alternatively or additionally, at least one coating according to the present disclosure has less than 500 ppm B 2 O 3 Includes: B 2 O 3 is a component that is often used in glass fluxes for sheets made of or containing borosilicate glass, in particular to contribute to a lowering of the melting temperature of the glass flux and / or to the smallest possible thermal expansion of the resulting coating. The absence of this component therefore emphasizes the formation of at least one coating as a coating based on glass, but not on a glass flux.
[0042] According to a preferred embodiment of the present disclosure, at least one coating is formed as a sol-gel coating.Sol-gel binder is generally understood as a binder in which at least one component is obtained by hydrolysis-condensation reaction from organosilicon precursor, for example, compounds such as tetraethyl orthosilicate (TEOS), or by acid-catalyzed hydrolysis and condensation of close or similar compounds, where there are many variations in the preparation of such binders, and mixtures of different precursors are also possible, for example, addition of mostly inorganic, particle-based sols, or addition of so-called polysiloxanes and / or silicones, which are all incorporated into the broad concept of "sol-gel binder" within the scope of this disclosure.
[0043] SiO 2The advantage of a sol-gel binder consisting of or containing SiO 2 is not only the high flexibility in formulation, but also the good compatibility with glassy substrates, such as glasses and glass ceramics of various compositions. In particular for glass or glass ceramic substrates with a small thermal expansion coefficient, such a binder can be advantageous, since in this way not only is a good bond of the coating, for example at least one coating of a glass sheet according to the present disclosure, provided, but also the use of SiO 2 as a binder. 2 This also makes it possible to obtain a coating with a small linear thermal expansion coefficient.
[0044] It can therefore be particularly advantageous if the at least one coating comprises a sol-gel binder, since in this way it is ensured that a relatively low baking temperature, e.g. below 450° C. or even lower, e.g. below 400° C., is sufficient for baking the at least one coating.
[0045] In this way, it is easily possible for the glass pane to have a very high bending strength, which cannot be achieved, for example, with conventional glass-based, especially enamel layers, and in some cases even with silicone-based coatings. For this purpose, at least one coating containing a sol-gel binder and a SiO 2 and B. 2 O 3 As mentioned above, the glass sheet comprises or is a so-called borosilicate glass, in other words it is formed as a borosilicate glass sheet. This type of glass material (or glass for short) is a chemically very resistant material, is also mechanically resistant and has a good thermal resistance compared to conventional glasses, for example soda-lime glass, and a good mechanical strength even in the non-prestressed state. It has also been found that the scratch strength of such borosilicate glass is higher than that of soda-lime glass. With at least one coating according to the embodiment, the already good strength of the glass sheet is maintained or advantageously promoted, and in some cases can even be further improved.
[0046] In general, it is possible for a coating to comprise several binders, i.e. to be formed as a hybrid, for example. For example, coatings are known which, in addition to a sol-gel component, also comprise a component based on a glass flux or a component based on an organic polymer. This may be necessary, for example, when certain properties cannot be achieved with only one binder, but an organic component and an additional binder form are required, for example to adjust the sufficient sealing of the resulting coating.
[0047] However, this is not contemplated according to the preferred embodiment of the present disclosure, which instead contemplates that at least one coating comprises only one binder, advantageously one binder formed as a sol-gel binder.
[0048] According to an embodiment, the area coverage of at least one side of the glass plate with at least one coating is at least 10% and at most 80%, preferably at least 15% and at most 65% of the total surface area of the side of the plate on which at least one coating is applied.However, according to further embodiments, a full coverage with at least one coating or a coverage of more than 80%, for example 90% or 95%, is generally also possible.This is especially recommended for applications in which the glass plate and / or the composite produced therefrom is used as a cover plate, not as a viewing window.
[0049] A plate is generally understood within the scope of this disclosure to mean a plate-like shaped body. A glass plate (coated or uncoated) is a plate that contains or consists of glass. A shaped body is plate-like if its spatial dimension in one spatial direction of a Cartesian coordinate system is at least an order of magnitude smaller than its spatial dimension in both further spatial directions perpendicular to the first spatial direction of the Cartesian coordinate system. In other words, the thickness of the shaped body is at least an order of magnitude smaller than its length and width. Both main faces or main surfaces of the plate, i.e. the faces whose size is determined by the length and width, are simply referred to as sides for short within the scope of this disclosure.
[0050] According to a further embodiment, the visible transmittance τ in at least one area of the glass sheet on which at least one coating is arranged vis is at most 10%, preferably at most 7%, and particularly preferably at most 5%, very particularly preferably at most 1%. vis is at least 0.01%, preferably at least 0.05% and preferably at most 0.3%. These values relate here to the area where the at least one coating completely covers the glass pane.
[0051] At least one coating can be applied to the glass sheet over at least one area, i.e. "all over" with respect to the area, i.e. without any breaks in the coating, but can also be arranged, for example, in the form of a so-called dot pattern. Combinations of these variations are also possible. For example, a coating that is all over, i.e. without any breaks in the coating, arranged on the glass sheet, can also transition to a dot pattern in the edge area of the coating, usually towards the center of the glass sheet. This is, for example, the usual configuration of at least one coating, i.e. in this case for glass sheets used in vehicle windshields, arranged structured on the glass sheet.
[0052] According to a further embodiment, the glass pane is configured such that in at least one partial region of at least one side of the glass pane or in the entirety of said at least one region, a further coating, preferably a glass-based coating, in particular an enamel coating, is arranged on the glass pane.
[0053] Such a configuration may be advantageous when the advantages of sol-gel coating should be realized with at least one coating, and the advantages of enamel coating are also desired.Therefore, particularly for embodiments in which a particularly good scratch strength of the entire layer structure is necessary and / or desired, it may be advantageous to apply a further coating, for example an enamel coating, on at least one coating formed as a sol-gel layer in particular.In this case, the at least one coating applied first serves as an intermediate layer and separates the enamel coating from the glass substrate, so that the very good strength values for the glass plate are still retained.At the same time, the further coating serves as a cover layer in the area covering at least one coating applied first, so that the scratch strength and abrasion strength of the entire layer structure can be substantially improved, for example.
[0054] According to a further embodiment, the at least one coating comprises at least 15% by weight and at most 55% by weight, preferably at least 20% by weight, particularly preferably at least 25% by weight, of binder.This is advantageous, since in this way an optimal compromise is achieved between good mechanical resistance and good covering effect of the at least one coating and sufficient strength of the coated glass pane.
[0055] According to a further embodiment, the at least one coating comprises at least 15% by weight and at most 30% by weight of pigment, based on the sum of all pigments contained in the at least one coating. This is advantageous, since in this way a good covering effect of the at least one coating can be achieved, especially also in a single-layer structure, i.e. a structure in which only at least one coating is arranged at least partially on the glass sheet.
[0056] The remainder of the coating is generally a filler, e.g., SiO 2 or other fillers, such as those described within the scope of the present disclosure, provided that, in particular, SiO 2 The filler based on is difficult to detect because it bonds well to the matrix of the binder, especially to the matrix of the sol-gel binder.
[0057] In this case, the at least one coating may generally comprise only one pigment. Pigments are generally understood within the scope of this disclosure to mean pigments, especially ceramic pigments, which give a certain color and / or a certain optical impression, for example so-called "metallic" effects. The term pigment therefore generally includes so-called pure color pigments, especially so-called ceramic pigments, preferably oxide pigments, within the scope of this application. Mixed oxide pigments, for example of oxides with a spinel structure, may be particularly preferred. Furthermore, the term pigment within the scope of this disclosure also includes so-called effect pigments, for example based on mica, as well as other effect pigments, especially effect pigments that are present coated on platelet-shaped substrates made of oxide materials or on mica. In general, within the scope of this application, the statement that a coating, for example at least one coating according to an embodiment, or a paste, for example a paste according to an embodiment, comprises a pigment means that it comprises particulate pigments, i.e. it comprises particles, and these particles have the corresponding pigment composition. That is, within the scope of this disclosure, when a coating or paste is said to comprise a plurality of pigments, it is understood that the coating and / or paste comprises pigment particles of different compositions, i.e. corresponding to the composition of the pigments contained in the coating and / or paste.
[0058] At least one coating may contain only one pigment. However, it may also be possible and preferred for at least one coating to contain multiple pigments. For example, it may be envisaged that at least one coating contains a white pigment as well as a black pigment, so that in some cases batch-based variations in the color locus of the pigments used can be routinely compensated for. Advantageously, at least one coating may contain further pigments, for example effect pigments, because such effect pigments are often based on platelets and can advantageously affect the properties of the coating, for example its smoothness / surface condition and thus its mechanical strength, for example its scratch resistance and abrasion resistance.
[0059] According to an embodiment, the glass of the glass plate, i.e., the borosilicate glass contained in the glass plate according to the embodiment, is 2×10-6 / K~6×10 -6 / K, i.e., in this case, it is a glass with a relatively small thermal expansion compared to conventional soda-lime glass. In this way, it is also possible to construct the glass pane from one of the known low-expansion borosilicate glasses. This is therefore particularly advantageous, since this borosilicate glass already inherently has a fairly high glass strength. Furthermore, such glasses have fairly good heat resistance and are quite chemically resistant.
[0060] According to a further embodiment, the glass of the glass plate is at least 60% by weight of SiO 2 ~Up to 85% by mass SiO 2 and / or at least 7% by weight of B 2 O 3 ~Up to 26% by mass B 2 O 3 Such glasses are well meltable and have improved chemical durability, hardness and strength compared to, for example, conventional soda-lime glasses. They are therefore particularly well suited for use in mechanically stressed areas, in particular as, for example, vehicle visibility windows, for example windshields. Such glasses are therefore also advantageous, since they offer a good compromise between good mechanical resistance, chemical durability and heat resistance on the one hand and good meltability on the other hand, without the tendency to segregate and / or too high viscosity of the glass melt acting as a hindrance. Therefore, according to an embodiment of the present disclosure, glass panes made of such glasses, for example borosilicate glasses, having a low thermal expansion coefficient within the aforementioned limits and / or having a composition within the above-mentioned limits are particularly preferred.
[0061] According to a further embodiment, at least one coating has a molecular weight of at least 3×10 -6 / K and up to 10x10 -6 / K, preferably 9 × 10 -6 / K, particularly preferably less than 7.5×10 -6 / K, particularly preferably less than 6×10 -6 / K. In this case, this embodiment is advantageous in that the linear thermal expansion coefficient of the glass, in particular of the glass pane, is also limited and is less than 2×10 -6 / K~6×10 -6 In this way, the SiO 2 glass plate having sufficient bending strength is obtained. 2 Glass sheets with a colored coating comprising a sol-gel binder ...
[0062] In the context of this application, when a thermal expansion coefficient is mentioned, this is understood to be the linear thermal expansion coefficient α. Unless otherwise stated, this is indicated in the range from 20 to 300°C. α and α 20-300 are understood synonymously within the scope of the present invention. This can be determined in particular for vitreous materials in a manner conforming to ISO 7991. By the thermal expansion coefficient of a coating is meant the respective resulting thermal expansion coefficient of the corresponding coating, which is derived from the thermal expansion coefficients of the individual components of the coating, taking into account their proportion in the coating. If within the scope of the present application the thermal expansion coefficient of the glass pane (i.e. of the substrate) is specified, this always means the thermal expansion coefficient of the vitreous material (or glass) of the glass pane.
[0063] According to a further embodiment, the glass pane has a thickness of at least 1 mm and up to 12 mm. This represents a good compromise between sufficient strength and still low weight of the glass pane used, especially when the glass pane is specified for use in combination with further panes.
[0064] According to a further embodiment, at least one coating is microporous and / or has holes with a maximum lateral dimension, for example a diameter, of at most 1 μm. Surprisingly, it has been found that coatings based on enamels that allow a comparable strength of glass sheets coated with the same coverage as at least one coating have a significantly different porous structure. That is, it has been found that enamel layers that allow at least a somewhat comparable strength of partially coated glass sheets (but usually always lower than those with coatings according to embodiments) have a significantly higher porosity with a pore size of more than 1 μm as a maximum lateral dimension, and often with a maximum lateral dimension of several micrometers. That is, such coatings are macroporous. Such pores can be formed especially at the interface between the coating and the glass sheet, i.e., between the coating and the substrate. In contrast, the structure of the coating according to the embodiment is significantly different and has only a few small pores. Here, the maximum lateral dimension of the pores is understood to mean the maximum extent. Usually, the pores are formed in an ellipsoidal shape, often only slightly deviating from a spherical shape. Thus, the maximum lateral dimension may also be referred to approximately as the diameter of the hole.
[0065] According to yet a further embodiment, the glass sheet, in at least one area where at least one coating is disposed, has an optical density of at least 1 and at most 4.5, for example at most 3, for the aforementioned thickness of the coating. The optical density or color density is used to characterize the absorption behavior of a coating compared to "absolute white". The darker the color layer, the less light can be transmitted through it. The optical density is calculated according to the following formula:
number
[0066] where R is the diffuse reflectance grad. The optical density is determined with a densitometer, in particular in the context of the present disclosure, perpendicular to the maximum areal extent of the coating and thus of the coated surface of the coated glass pane. The higher the optical density, the lower the transmittance of the coating. This can be particularly advantageously achieved with a high pigment content in at least one coating and / or by the type and amount of pigment selected, in particular with a pigment content in the upper range of the aforementioned range of 0% to 30% by weight pigment.
[0067] The present disclosure also relates to a paste, in particular a paste for producing a coating that is arranged on a glass sheet according to the embodiments as at least one coating, suitable for producing a glass sheet according to the embodiments, i.e. arranged at least partially on at least one side of the glass sheet. The paste is preferably a SiO 2 At least one binder comprising SiO 2 , at least one pigment, at least one medium, and at least one additive advantageously formed as a filler. 2 The binder comprises at least one SiO 2 crosslinked by hydrolysis and condensation of at least one semi-organic silicon oxide precursor phase. 2 The paste is formed as a sol-gel binder containing a phase, where a semi-organic silicon oxide precursor phase is understood to mean a silicon compound in which an organic group, in particular an alkyl group, is bonded to the silicon atom directly or via an oxygen bridge atom. The paste contains less than 500 ppm of Bi 2 O 3 and / or less than 500 ppm ZnO. According to an embodiment, the binder further comprises less than 500 ppm B 2 O 3 and / or less than 500 ppm of alkali oxides, where what has been said above about the binder in relation to the glass panes generally applies correspondingly to the binder of the paste.
[0068] The medium may also be generally referred to as a dispersion medium. As previously mentioned, such pastes can be used to advantageously obtain glass sheets according to the embodiments.
[0069] According to an embodiment, the paste is generally made of SiO 2 The binder comprises at least one SiO 2 crosslinked by hydrolysis and condensation of at least one semi-organic silicon oxide precursor phase. 2 The semi-organic silicon oxide precursor phase is understood to mean a silicon compound in which an organic group, in particular an alkyl group, is bonded to the silicon atom directly or via an oxygen bridge atom. This is particularly advantageous, since in this way essentially pure SiO 2 The chemicals (advantageously, at least 90% by weight of the inorganic components of the binder) are 2 In spite of the limitation to the composition of the binder (which is understood to be formed by the reaction of the semi-organic silicon oxide precursor phase), there is a great flexibility in terms of the composition of the binder. That is, such semi-organic silicon oxide precursor phases are flexible to use and crosslink, and can be combined with additional SiO 2 Precursor materials, such as pre-condensed and dispersed SiO 2 Nanoparticles, such as those known under the commercial name "Levasil", or other nanoparticles, in particular SiO 2It can also be combined with a dispersion of nanoparticles, as will be further described below. It is also possible to use precursor phases in which the silicon atom has four oxygen bridge atoms, or in which at least one organic residue is directly bonded to the silicon atom. In this case, as mentioned above, alkyl groups are particularly preferred. In particular alkyl groups, especially methyl groups, bonded to the central silicon atom can be advantageous, since in this way the coating can provide a certain inherent tightness and durability against water and water vapor, as well as good compatibility with organic components, for example, of the laminated film. In this case, it is particularly important that in particular methyl groups are particularly resistant to high temperatures, and therefore can be preferably used. Alternatively, phenyl groups can be substituted, but they have a lower temperature stability and may possibly pose a health risk in the event of decomposition. In general, it is preferred when up to two organic groups are present per silicon atom in the precursor, in order to efficiently enable network formation. One organic group per silicon atom is preferred, for example methyl triethoxysilicate in the precursor / precursor phase.
[0070] According to an embodiment, the paste comprises at least 10% by weight and at most 40% by weight, preferably at least 15% by weight and at most 30% by weight, of additives, advantageously fillers, relative to the total weight of the paste and relative to the sum of the additives, advantageously fillers, contained in the paste.
[0071] In this way, a very favorable compromise is achieved between improving the paste properties and / or the properties of the resulting coating by adding fillers and adjusting the color locus of the resulting coating to be intense, as dark as possible and neutral. Too much filler can sometimes also have a negative effect on the covering action of the pigments used.
[0072] With respect to filler, it is understood here that this is a particulate material, i.e. that it comprises particles, which have a corresponding filler composition, i.e., within the scope of the present disclosure, when a coating or paste is said to comprise a plurality of fillers, it is understood that the coating and / or paste comprises filler particles of different composition, i.e., corresponding to the composition of the fillers contained in the coating / paste.
[0073] According to an embodiment, the paste has a linear thermal expansion coefficient of −10×10 -6 / K~+10×10 -6 / K, i.e. preferably a filler having a relatively small coefficient of linear thermal expansion. In particular, it is preferably pyrogenic silica, generally SiO 2 or graphite based on -10×10 -6 / K~+10×10 -6 / K, preferably -8 x 10 -6 / K~+5×10 -6 / K, and particularly preferably -6.5 × 10 -6 / K~+3×10 -6 Such a relatively small linear thermal expansion coefficient of 1 / K is achieved by the binder, i.e., SiO 2 In this way, good bonding of the filler into the coating can be ensured, and this can further improve the stability of the coating, i.e. here especially of at least one coating of the glass pane according to the present disclosure, for example with respect to scratch resistance and / or abrasion resistance.
[0074] Fillers as constituents of pastes, for example sol-gel pastes, have generally been known for a long time already. Such fillers can affect, in various ways, and in particular improve, the properties of the pastes containing them as well as the coatings obtained therefrom, for example by virtue of their ability to improve the cross-linking of the sol-gel matrix.
[0075] For example, the use of fillers which serve as rheological additives in the paste is also possible and can be easily incorporated into the coatings obtained therefrom and can also have further functions here, such as improving the wear of the coating. Particularly in the case of sol-gel pastes and the coatings obtained therefrom, the use of fillers as rheological additives is known.
[0076] As mentioned above, according to an embodiment, it is also possible for the paste to contain further additives, for example fillers. It is also possible that the paste contains two or three fillers, which, as mentioned above, advantageously have a rather small coefficient of linear thermal expansion, for example -10x10 -6 / K~+10×10 -6 / K, preferably -8 x 10 -6 / K~+5×10 -6 / K, and particularly preferably -6.5 × 10 -6 / K~+3×10 -6 It can also be advantageous if the filler has a linear thermal expansion coefficient of 1 / K.
[0077] As mentioned above, fillers with a thermal expansion coefficient in the above ranges can generally be particularly advantageous for forming at least one coating property and, correspondingly, for forming the properties of the glass pane, either as the only filler or even when several fillers are present. Moreover, such fillers, especially in the case of silica, can provide advantageous properties for the paste itself, for example by allowing or facilitating the adjustment of the viscosity, for example a viscosity suitable for application using a printing method, such as screen printing. Furthermore, the formation of the filler as a low-expansion filler can also be advantageous. However, it is not absolutely necessary that the filler has a very low linear thermal expansion coefficient. As mentioned above, the filler can be graphite, which in this case is advantageous because the binder itself has a fairly low thermal expansion coefficient and the material of the glass pane according to the embodiment itself has a linear thermal expansion coefficient of 2×10 -6 / K~6×10 -6This has the further advantage of compensating for the relatively high coefficient of thermal expansion of this material compared to amorphous silica, especially considering that the material will have a linear coefficient of thermal expansion in the range of 1 / K.
[0078] In general, as already mentioned above, fillers can perform very different functions in the paste and / or in the coating obtained therefrom.It has been found that it can be particularly advantageous for producing at least one coating of a glass sheet according to the embodiment of the present disclosure when the paste comprises two types of fillers.Of course, especially in the case of high-temperature stable fillers, the coating obtained can also comprise both of these fillers, but in individual cases, especially when the filler content is low, it may be difficult to detect them in the coating itself under some circumstances.
[0079] For example, in one embodiment, the filler can be silica, in particular pyrogenic silica. Such an embodiment is advantageous because pyrogenic silica, in other words chemically amorphous SiO 2 is not only a known material that is readily available, but can also show advantageous properties in the paste, for example as a rheological additive. In this way, it is not necessary to have to use, for example, organically modified rheological additives, which may possibly be difficult to remove again from the resulting coating and which may possibly lead to unsightly coloring or other defects of the coating when the glass sheet is subsequently used. Moreover, the pyrogenic silica remains in the coating and does not have to be removed from the glass sheet, as is the case with the glass sheet according to the present disclosure. 2 Good cross-linking of the coating, both within the coating itself and to the substrate, can also be promoted due to the good incorporation of the amorphous SiO into the sol-gel matrix based on amorphous SiO 2Pyrogenic silica as such only has a low coefficient of thermal expansion and can furthermore be in a number of variants, thus making it possible to specifically influence the properties of the resulting coating. Therefore, according to an embodiment, fillers formed as silica are particularly advantageous. In particular here, fillers are also present in the resulting coating, but in particular predominantly in the form of SiO 2 It turns out that in the case of a coating matrix formed from the filler, the filler is no longer detectable as such, but the influence of the filler is shown in the resulting advantageous properties of the coating thus obtained.
[0080] A further class of fillers, especially in the field of colored sol-gel coatings, are so-called "lubricants". In this case, "lubricants" is understood in the context of the present disclosure as a solid that has a "lubricating" effect similar to that of talc. This effect is brought about by the fact that the fillers formed as the lubricants themselves have a platelet-like structure. Advantageous known fillers used in sol-gel coatings are, for example, graphite or boron nitride. According to an embodiment, the paste preferably contains graphite as a filler. This is also sufficiently temperature-stable, so that it is also contained in the resulting coating. However, it is not easily detectable, especially due to the low atomic number of carbon, and therefore cannot be easily visualized, for example, in EDX analysis.
[0081] The advantageous effect of lubricants, such as graphite or boron nitride, which is manifested in particular in the resulting good properties of the coating, has not been fully understood by the inventors, but it has been found that such fillers having a platelet-like structure, in particular a graphite-like structure with respect to the crystalline structure of the fillers considered, can be advantageous for the formation of particularly durable sol-gel-based coatings.
[0082] However, such fillers also have some disadvantages.It has been previously known that such fillers can provide particularly desirable properties in the paste (and in the correspondingly obtained coating), especially in the case of sol-gel coatings, if a certain ratio of pigment to lubricant is used, which is between 10:1 and 1:1 by weight.
[0083] In the case of graphite as a filler, this can lead to some good properties of the resulting sol-gel coating, but also some undesirable properties. Graphite itself has a color and thus allows only relatively dark colors of the corresponding coating, but it is also difficult to achieve a really dark black color with such a relatively high content of graphite. Since the pigments used according to the prior art often also relate to effect pigments, the color range with graphite as lubricant was very limited up to now and often related to pastes producing light to dark gray coatings with a "metallic" effect. Furthermore, while a very high proportion of graphite was favorable for the formation of favorable mechanical properties of the layer, such as good adhesion strength, scratch and abrasion resistance, as well as good sealing, the layer was often also formed conductive, which was not desirable for certain applications.
[0084] Instead of using graphite as a lubricant, for example, boron nitride, which may also be referred to as "white graphite", can be used. However, this is associated with the formation of a rather white or light layer, which may be disadvantageous for mask coating, for example in the area of glass sheets envisaged for use as automotive sheets in sheet composites. Furthermore, boron nitride is expensive to produce and is therefore disadvantageous for energy efficiency and cost reasons.
[0085] Finally, it should be noted that it may be difficult to wet the coating with such fillers.While this may be advantageous for certain applications, there is a concern that if the proportion of fillers formed as lubricant is too high, it may be disadvantageous, especially with respect to the subsequent lamination of the glass sheet that is provided with the coating that contains fillers, as mentioned in the known prior art.Therefore, there is a particular need for a paste for producing a coating for glass sheets, which can be used, for example, in composites, and which also achieves dark colors, especially dark black.
[0086] Surprisingly, according to a particularly preferred embodiment, it has been found that a significantly smaller amount of filler than previously known can already be sufficient in the paste and in the correspondingly obtained at least one coating on a glass sheet according to the embodiment. According to this preferred embodiment, when a filler is present as a lubricant, the pigment to lubricant ratio is greater than 20:1, preferably greater than 30:1, and particularly preferably greater than 40:1, based on the total weight of the sum of the pigments contained in the paste or the resulting coating and the sum of the fillers formed as lubricant, respectively, based on the weight ratio of the respective components. In this way, not only is greater design freedom given to the resulting coating, for example when providing a specific color. Rather, in this way, unexpectedly, advantageous mechanical properties of the correspondingly produced coating, for example at least one coating on a glass sheet according to the embodiments of the present disclosure, as well as still sufficient scratch strength, can be obtained, while the disadvantages of known layers of the prior art can be avoided. In particular, the glass sheet containing at least one coating obtained in this way is well suited to be made into a solid composite with further glass sheets in a lamination process, for example meeting the requirements for vehicle sheets.
[0087] According to an embodiment, the paste comprises up to 50% by weight of a solvent, advantageously a high-boiling solvent having a boiling point of at least 130°C and preferably at most 330°C, for example at most 220°C.
[0088] In particular, the solvent can be or contain diethylene glycol monoethyl ether. Such a formulation is particularly advantageous for printing inks, since in this way a paste is obtained which can be easily printed, for example by screen printing, without the paste drying out on the sieve.
[0089] According to yet a further embodiment, the paste comprises a solution of cellulose, for example ethyl cellulose, advantageously with a content of 5% to 10% by weight relative to the total weight of the paste. The cellulose can for example be dissolved in a high boiling solvent, for example diethylene glycol monoethyl ether.
[0090] Such a paste configuration is not mentioned in the cited prior art documents: it was previously thought that cellulose, which is advantageous for adjusting the viscosity of the paste, which is particularly advantageous for screen printing, could not be successfully used in a paste based on sol-gel. 2 This is because the compounds are often acid-condensed, i.e. the pH value of such pastes is relatively low, in particular below 7, and thus in the acidic range, but since cellulose decomposes in such acidic solutions, only pastes with a pot life of a few days can be obtained in this way.
[0091] As already mentioned above, at least one coating is SiO 2 Generally, the formulation of the binder as a sol-gel binder comprising SiO 2Binders comprising, as mentioned above, can be obtained, for example, by hydrolysis-condensation reactions from organosilicon precursors or precursor compounds, for example by acid-catalyzed hydrolysis and condensation of compounds such as tetraethyl orthosilicate (TEOS) or close or similar compounds, where there are many variations in the preparation of such binders and mixtures of different precursors are also possible, for example the addition of mostly inorganic, particle-based sols or the addition of so-called polysiloxanes and / or silicones, which are all incorporated under the broad concept of "sol-gel binders" within the scope of this disclosure.
[0092] SiO 2 The advantage of a sol-gel binder consisting of or containing SiO 2 is not only the high flexibility in formulation, but also the good compatibility with glassy substrates, such as glasses and glass ceramics of various compositions. In particular for glass or glass ceramic substrates with a small thermal expansion coefficient, such a binder can be advantageous, since in this way not only is a good bond of the coating, for example at least one coating of a glass sheet according to the present disclosure, provided, but also the use of SiO 2 as a binder. 2 This also makes it possible to obtain a coating with a small linear thermal expansion coefficient.
[0093] Pastes with which a sol-gel based coating can be obtained are described, for example, in US 2010 / 0028629 A2. US 2010 / 0047556 A2 also refers to similarly constructed sol-gel pastes. Finally, US 2009 / 0233082 A2 also describes pastes with which a sol-gel based coating can be obtained.
[0094] However, the coatings mentioned in the aforementioned patent application are not suitable for the production of glass panes according to the embodiment. The pastes described therein are rather suitable for the production of glass-ceramic substrates which often have a very low expansion, preferably a linear thermal expansion coefficient of 2×10 -6 / K, i.e. LAS glass ceramics with low thermal expansion, such as those also used for cooktops. The special difficulties that arise when coating such substrates with low expansion lead to the pastes, and correspondingly the coatings obtained thereon, being constructed differently and having a different structure than those suitable for glass panes according to the embodiment, which should also be suitable for use as glass panes in vehicle glazing composites.
[0095] In particular, the layer systems referred to in the abovementioned prior art documents often comprise two layers which are applied in separate coating processes and have clear differences, especially with regard to the ratios of the individual components of the paste and of the correspondingly obtained coating.
[0096] According to an embodiment, the paste comprises at least 15% and at most 30% by weight of pigment, relative to the total weight of the paste and relative to the sum of the pigments contained in the paste. Advantageously, the paste comprises at least 20% by weight of pigment.
[0097] In other words, the pigment content of the paste and, correspondingly, the pigment content in the at least one coating that can be obtained using the paste according to the embodiment is clearly different from that of the known paste. The different composition of the paste and, correspondingly, of the at least one coating leads to a correspondingly different configuration of the coating. Thus, in this case, according to the embodiment, it is also possible that the glass pane according to the embodiment has only one coating, i.e., the at least one coating is the only coating.
[0098] According to an embodiment, the paste comprises at least 8% by weight and at most 20% by weight of a binder relative to the total weight of the paste. Advantageously, the paste comprises at least 8% by weight of a binder relative to the total weight of the paste, and at most 20% by weight of the SiO 2 of the paste. 2 The content is configured so that 8% to 20% by weight is provided by the organosilicon precursor.
[0099] In this way, sufficient adhesion strength of at least one coating produced with the paste and the glass plate can be ensured. In this way, sufficient scratch strength can also be achieved. Despite this rather high binder content compared to known pastes or coatings obtained from such known pastes, the strength of the glass plate according to the embodiment does not drop below a critical value. This is due to the use of particularly strongly crosslinking binders, i.e. polymerically crosslinked SiO 2 obtained from organosilicon precursor phases. 2 Because the framework is bonded to the nanoparticles, particularly high strength of the resulting coated glass sheets according to embodiments of the present disclosure may be achieved.
[0100] According to an embodiment, the paste comprises at least 10% by weight and at most 40% by weight of additives, preferably fillers, relative to the total weight of the paste and relative to the sum of the additives, preferably fillers, contained in the paste.
[0101] Thus, even in the paste, the content of additives, especially fillers, of the paste is relatively high, relative to the total weight of the pigments contained in the paste (correspondingly in at least one coating). According to an embodiment, at least one filler is formed as a lubricant, especially as graphite, and the pigment to lubricant ratio, relative to the total weight of the pigments contained in the at least one coating and the fillers formed as lubricant, is more than 20:1, preferably more than 30:1, and particularly preferably more than 40:1, based on the weight ratio of each component. According to this embodiment, the ratio of the pigments contained in the paste to the fillers formed as lubricant in the paste corresponds to the ratio that is also adjusted in at least one coating according to the embodiment.
[0102] According to yet a further embodiment, the paste comprises up to 50% by weight of a solvent, preferably a high-boiling solvent having a boiling point of at least 150° C. and preferably at most 330° C. In particular, the solvent can be or comprise diethylene glycol monoethyl ether. Such a formulation is particularly advantageous for printing inks, since in this way a paste is obtained which can be printed well, for example by means of screen printing, without the paste drying out on the sieve.
[0103] According to yet a further embodiment, the paste comprises cellulose, for example ethyl cellulose, advantageously in a content of 0.1% to 1% by weight relative to the total weight of the paste. The cellulose can for example be dissolved in a high boiling solvent, for example diethylene glycol monoethyl ether.
[0104] Such a composition of the paste is not mentioned in the cited prior art documents: it was previously thought that cellulose, which is advantageous for adjusting the viscosity of the paste, which is particularly advantageous for screen printing, could not be used well in a paste based on sol-gel. 2 The reason is that the compounds are usually acid-condensed. Admittedly, the pH value in the paste cannot be specified, because the paste contains many organic solvents and the concept of pH value is not applicable for such solutions. However, it was found that in the known pastes of the prior art, the cellulose decomposes, thus only a paste with a pot life of a few days is obtained. However, it was surprisingly found that cellulose can be used in the paste according to the present disclosure. The reasons for this are not entirely clear to the inventors. This may be due to the solution of cellulose in a suitable solvent, i.e. an ether, for example diethylene glycol monoethyl ether, and the relatively low total content of cellulose, up to 1% by weight in total.
[0105] In this case, the use of cellulose can be advantageous, because in this way the viscosity parameters of the paste can be adjusted and the printed image is better than that of the paste without cellulose. Simply put, cellulose-containing pastes have a rather "honey-like" viscosity behavior, whereas pastes whose viscosity is adjusted only with silica have a very high thixotropy, which can lead to excessively "pixelated" and not smooth printed images, which is undesirable, for example, in screen printing processes. This can be addressed by reducing the silica in the paste, but this can lead to an overall viscosity that is too low and the paint "dripping" through the sieve. However, the above disadvantages can surprisingly be easily avoided by adding cellulose within the aforementioned limits.
[0106] The present disclosure also relates to a composite material. The composite material comprises a glass sheet according to the embodiment as well as a further glass sheet, and advantageously at least one coating is arranged between both glass sheets of the composite material. In particular, a polymer layer can be arranged between both glass sheets of the composite material as usual, in particular in the form of a film, to form insulating glass that can be used, for example, as a windshield or other vehicle glazing. [Brief description of the drawings]
[0107] [Figure 1] 1 is a schematic diagram of a composite or insulating glass pane 10 according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic diagram of a composite or insulating glass pane 10 according to an embodiment of the present disclosure. [Diagram 3] 1 is a schematic diagram of a composite or insulating glass pane 10 according to an embodiment of the present disclosure. [Figure 4] 1 is a scanning electron micrograph of a plate according to an embodiment of the present disclosure. [Diagram 5] FIG. 2 is a diagram showing the bending strength of a glass plate. EXAMPLES
[0108] The invention is further explained below by means of examples. The compositions of the pastes according to the embodiments of the present disclosure from which the coatings according to the embodiments and the glass sheets according to the corresponding embodiments can be obtained are summarized in the following table.
[0109] SiO as a constituent of the binder of the paste and correspondingly the coating according to the embodiment 2 Exemplary compositions of sols based on the above are summarized in Table 1 below. This is the binder portion of the paste that includes or is formed by hydrolysis and condensation from semi-organosilicon compounds, as is evident from the descriptions in Table 1.
[0110] [Table 1]
[0111] As can be seen from Table 2 below, the binder, i.e. "semi-organic Si compound" or more precisely the binder produced from it, can have other components added to it, in addition to the components obtained from hydrolysis and condensation from at least one semi-organic silicon organic precursor phase, as exemplarily described above.The binder thus obtained as a whole is understood as a sol-gel binder within the scope of the present disclosure.Then, a paste is obtained with further components, such as pigments and / or fillers, and an exemplary composition is shown in the table below.
[0112] [Table 2]
[0113] The nanoparticle dispersion here is defined as a SiO 2 nanoparticle dispersion having an average particle size of less than 1 μm in terms of the volume-related equivalent diameter. 2A dispersion of nanoparticles, understood as particles, in diethylene glycol monoethyl ether, the proportion of nanoparticles in the dispersion being 37% by weight based on the weight of the dispersion here. Of course, it is also possible for the nanoparticles to be added in other forms, for example in the form of aqueous sols, such as those available under the trade name "Levasil". However, such sols contain a certain content of alkali oxides, in particular Na 2 Advantageously, therefore, the paste comprises SiO 2 in an organic solvent, advantageously a high boiling organic solvent, advantageously a high boiling organic solvent having a boiling point of at least 130° C. and preferably at most 330° C. 2 It is configured to contain a dispersion of nanoparticles.
[0114] Carbon black can also be added to the paste, acting as a pigment. Advantageously, according to an embodiment, lamp black, for example with CAS number 1333-86-4, can be used. Despite nominally having the same chemical composition as graphite, i.e. made of carbon, they are considered as pigments and do not act as lubricants within the meaning of the present disclosure due to their exact preparation and the different particle morphology obtained therefrom and the smaller (if any) degree of crystallinity compared to graphite and the different particle morphology associated therewith. The addition of carbon black can be advantageous, since in this way a particularly dense layer can be obtained, with a particularly black color impression. Depending on the exact type of carbon black, the properties of the paste and thus of the resulting coating are also very different; for example, it has been found that the above-mentioned paste 7, which contains carbon black of the type "Printex 95", is difficult to sieve, i.e. is not well printable.
[0115] The pastes according to the embodiments shown as numbers 1 to 5 in the above table were used to apply coatings onto glass plates by screen printing using a fine sieve (140 mesh) and a larger sieve (77 mesh), respectively. The paste containing carbon black was printed using a sieve with a 77 mesh.
[0116] These are heat treated, i.e. dried or baked, at 380°C for 1 hour.
[0117] Description of the drawings Figure 1 is a schematic and not to scale view of a composite or insulating glass pane 10 according to an embodiment of the present disclosure. The composite 10 comprises two panes 1, 2, where pane 1 is a glass pane for vehicles according to an embodiment of the present disclosure. Pane 2 is a further glass pane, which can be made, for example, of soda-lime glass or of the glass of the present disclosure of pane 1. Between both glass panes 1, 2 is arranged a polymer layer 3, as well as here a coating 11 in the edge region of the composite 10. This is arranged on one side (not shown) of the glass pane 1 and may comprise at least one coating, either alone or together with a further coating as an interlayer, each within the scope of the following description.
[0118] For the sake of better illustration, the coating 11 is shown here as thick, i.e. as thick as both plates 1, 2, but as mentioned above, this is only for the sake of better illustration. The coating 11 is usually significantly thinner than each of both plates 1, 2, and is usually thinner than the polymer layer 3. The polymer layer 3 may be a film.
[0119] As can be seen, the composite 10 is formed as a curved insulating glass sheet, for example so that it can be used as a windscreen. In general, however, it is also possible that the composite 10 does not include curved sheets 1, 2 and is formed flat, without being limited to the example shown in FIG. 1. It is also possible that the curvature of the composite 10 is formed inversely to the illustration shown in FIG. 1 in particular. Whereas in the example of FIG. 1 the glass sheet 1 is on the outside of the windscreen, it is also possible in general for the glass sheet 1 to be arranged on the inside of the windscreen. In either case, however, the coating 3 is arranged between both glass sheets 1, 2.
[0120] However, the arrangement as shown in FIG. 1 can be advantageous because the glass plate 1 contains SiO as a component of the vitreous material. 2 and B. 2 O 3 Since such borosilicate glass is more scratch resistant than, for example, soda-lime glass, it can be advantageous if the glass pane 1 is formed facing "out" in the composite 10 as shown in Figure 1, i.e. facing outwards when used as a windscreen. In this way, better protection against flying stones or similar mechanical loads is provided.
[0121] In order to clearly show the configuration of the glass sheet 1 according to the embodiment, this is shown in the form of a schematic and to-scale drawing in Figures 2 and 3, respectively. Figure 2 thus shows a side view, where the glass sheet 1 has not yet been bent. In general, it is also possible for the glass sheet to be bent, without being limited to the example shown in Figure 1 of the glass sheet 1. However, it can be advantageous if a flat, unbent sheet 1 is first used, which is subsequently bent, for example in a thermal manner. Here too, for better illustration, the thickness of the coating 11 is shown to be significantly larger than in reality.
[0122] The arrangement of plate 1 corresponds to that in Fig. 1 as previously described, except that in Fig. 2 the plate is not bent. As can be seen, the coating 11 can now be formed on the side 102 of the composite 10 facing the second plate 2. The polymer layer 3 arranged between plates 1 and 2 in the composite is not shown here. It is explicitly pointed out here that the polymer layer 3 can either be in direct contact with the side 102 of the plate or on a coating 11 arranged in an area (or areas) of plate 1 (or on side 102 of plate 1).
[0123] The coating 11 is here arranged in the edge region of the plate 1, respectively to the left and right of the illustration in Figure 2. Here, for example, the coating can be applied as a whole in the form of a "frame".
[0124] This is taught in Fig. 3, which shows a top view of the plate 1 according to an embodiment in a schematic and not to scale view. Here, the coating 11 is formed as a frame around the edge of the plate 1, the coating being first formed as a covering, i.e. as an uninterrupted layer, and transitioning towards the centre of the plate 1 via a grid or dot pattern 111 into an uncoated area, which is for example the visible area of a windscreen, in case the plate 1 is used in a composite 10. It will be appreciated that in general the frame is not formed uniformly as shown diagrammatically in Fig. 3, but can for example have protrusions, such as are typical in the region of the rear-view mirror of a windscreen.
[0125] Figure 4 is a scanning electron micrograph of a plate 1 according to an embodiment of the present disclosure with a coating 11 arranged on a side 102 of the plate 1. The coating comprises pigments, here only exemplary pigments 4 are shown, which are platelet-shaped pigments, i.e. so-called effect pigments. As can be seen from the diagram in Figure 4, the coating matrix 5, which may also be called binder 5, is in particular formed in particulate form. It is composed of SiO 2 or SiO 2 The coating contains less than 500 ppm Bi by weight. 2 O 3 and / or less than 500 ppm ZnO and / or less than 500 ppm B 2 O 3 and / or less than 500 ppm of alkali oxides. In particular, the binder 5 also contains SiO 2 , and less than 500 ppm Bi by mass 2 O 3 and / or less than 500 ppm ZnO and / or less than 500 ppm B 2 O 3 and / or less than 500 ppm of alkali oxides. The binder herein is formed as a sol-gel binder.
[0126] The coating 11 and / or the binder 5 may also contain pores 6. However, these are made relatively small so that the coating 11 is in particular made microporous or can be microporous and / or have pores with a maximum lateral dimension, e.g. diameter, of at most 1 μm. As can be seen from Figure 4, these are advantageously arranged at the interface between the plate 1 and the coating 11, i.e. on or near the side 102 of the plate 1. The scale of the figure is located below the scanning electron microscope view in the lower right region of Figure 4 and indicates a length of 2 μm.
[0127] The coating 11 here also contains at least one additive, which is preferably formed as a filler, although this additive is not visible in the scanning electron microscope view. Advantageously, the glass sheet 1 here has a flexural strength of at least 80 and at most 300 MPa, preferably at least 100 and at most 210 MPa, particularly preferably at least 140 MPa, in at least one region arranged on the side 102 of the glass sheet 1 and to which the coating 11 is applied.
[0128] The bending strength of various glass panes with various coatings or made of unprinted borosilicate glass as a reference is shown in FIG. 5. Unprinted borosilicate glass is shown at the far left of FIG. 5 with respect to the strength results, and in this so-called "box and whisker plot" the strengths obtained for such unprinted glass panes are shown. The strengths here average somewhat above 200 MPa. In contrast, the strength of glass panes with coatings based on conventional glass fluxes is reduced, based on the values for the samples plotted second from the left in FIG. 5. Strength values below 50 MPa are obtained here. That is to say, the strength is significantly reduced with such conventional coatings.
[0129] This is not the case for the coating 11 according to the embodiment shown in FIG. 5 under "Examples 1-4". Here too, a decrease in strength relative to the unprinted glass plate may occur (Examples 1 and 3), but values (average values) still exceeding 140 MPa, here even exceeding 150 MPa, are obtained. Example 2 has strength values that are comparable to the unprinted plates, but with somewhat higher scatter than these. Finally, as in Example 4, coatings according to embodiments are even possible in which the strength is improved by the coating relative to the unprinted glass plate (see Example 4). [Explanation of symbols]
[0130] 1, 2 Glass plate 3 Polymer Layer 10 Composite materials, insulating glass sheets 11 Coating 102 Side of board 1 111 Grid or dot pattern 4. Pigments 5. Binder 6 holes
Claims
1. SiO 2 and B 2 O 3 A glass pane, in particular a partially coated glass pane for a vehicle, comprising at least one coating applied to at least one region on at least one side of the glass pane, the at least one coating comprising SiO 2 At least one binder comprising At least one pigment, and The additive is preferably formed as at least one filler. and Advantageously, in at least one region having at least one coating applied on at least one side of the glass sheet, a bending strength of at least 80 and at most 300 MPa, preferably at least 100 and at most 210 MPa, particularly preferably at least 140 MPa, The at least one coating each contains less than 500 ppm Bi by weight. 2 O 3 and / or less than 500 ppm ZnO, and / or less than 500 ppm B 2 O 3 and / or containing less than 500 ppm of alkali oxides.
2. 10. The glass sheet of claim 1, wherein the at least one coating comprises only one binder.
3. 3. The glass sheet according to claim 1 or 2, wherein the binder is formulated as a sol-gel binder.
4. At least one of the following characteristics: a further coating, preferably a coating based on glass, in particular an enamel coating, is arranged on the glass pane in at least one partial region on at least one side of the glass pane or in the entire at least one region, the at least one coating comprises at least 15% by weight and at most 55% by weight, preferably at least 20% by weight and particularly preferably at least 25% by weight, of a binder; said at least one coating comprises at least 20% by weight and at most 30% by weight of pigment relative to the sum of all pigments contained in said at least one coating; The glass of the glass plate is 2×10 -6 / K~6×10 -6 / K, The glass of the glass plate contains at least 60% by weight of SiO 2 Up to 85% by mass of SiO 2 and / or at least 7% by weight of B 2 O 3 Up to 26% by mass of B 2 O 3 containing, said at least one coating having a surface roughness of at least 3×10 -6 / K and up to 10 x 10 -6 / K, preferably 9×10 -6 / K; the glass sheet has a thickness of at least 1 mm and at most 12 mm; 4. The glass sheet according to claim 1 , having
5. 5. A glass sheet according to claim 1, wherein the at least one coating is microporous and / or has holes with a maximum lateral dimension, e.g. a diameter, of at most 1 μm.
6. A paste for producing a coating on a glass plate, preferably on a glass plate according to any one of claims 1 to 5, SiO 2 At least one binder comprising at least one pigment, at least one medium; and additive, preferably in the form of at least one filler In the paste comprising the binder, each of the binders contains less than 500 ppm Bi by mass. 2 O 3 and / or less than 500 ppm ZnO, and / or less than 500 ppm B 2 O 3 and / or containing less than 500 ppm of alkali oxides.
7. The SiO 2 The binder comprises at least one SiO2 crosslinked by hydrolysis and condensation of at least one semi-organic silicon oxide precursor phase. 2 7. The paste according to claim 6, which is formed as a sol-gel binder containing a semi-organic silicon oxide precursor phase, by which is understood silicon compounds in which organic groups, in particular alkyl groups, are bonded directly to silicon atoms or via oxygen bridge atoms.
8. 8. The paste according to claim 6 or 7, which comprises at least one filler, which is or comprises silica, preferably pyrogenic silica, or the lubricant, graphite, and, if a filler is present as the lubricant, the pigment to lubricant ratio is greater than 20:1, preferably greater than 30:1, and particularly preferably greater than 40:1, based on the weight proportions of the respective components, based on the total weight of the sum of the pigments contained in the paste and the sum of the fillers formed as the lubricant, respectively.
9. At least one of the following characteristics: the paste comprises at least 15% and at most 30% by weight of pigment, preferably at least 20% by weight, relative to the total weight of the paste and relative to the sum of the pigments contained in the paste; the paste comprises at least 8% and at most 20% by weight of a binder relative to the total weight of the paste; the paste comprises at least 10% by weight and at most 40% by weight of additives, preferably fillers, relative to the total weight of the paste and relative to the sum of the additives, preferably fillers, contained in the paste; The paste has a linear thermal expansion coefficient of −10×10 -6 / K~+10x10 -6 / K, particularly preferably pyrogenic silica and / or graphite, the paste comprises up to 50% by weight of a solvent, advantageously a high-boiling solvent having a boiling point of at least 130° C. and preferably at most 330° C.; 9. The paste according to claim 6, wherein
10. 10. The paste according to claim 6, which comprises cellulose, preferably ethylcellulose, preferably in a content of 0.1% to 1% by weight relative to the total weight of the paste.
11. 6. A composite comprising a glass pane according to any one of claims 1 to 5 and a further glass pane, preferably with at least one coating arranged between the glass panes.
12. 10. A method for producing a glass sheet, preferably a glass sheet according to any one of claims 1 to 5, comprising applying a paste, preferably a paste according to any one of claims 6 to 10, to at least one region on at least one side of the glass sheet and baking the paste in such a way that at least one coating is present in at least one region.
13. 13. A glass pane produced or producible according to the method of claim 12 and / or using a paste according to any one of claims 6 to 10, preferably according to any one of claims 1 to 5.
Citation Information
Patent Citations
composite substrate element
DE202008003804U1
Enamelled substrate, illuminated glazed device comprising such a substrate, and production thereof
EP3830046A1
ENAMELED SUBSTRATE, AUTOMOTIVE LIGHTED WINDOW DEVICE WITH SUCH A SUBSTRATE AND ITS MANUFACTURE.
FR3084355A1
Top board lifting type furniture, and furniture system
JP2017000559A
Glass or glass-ceramic articles with decorative coating
US20090233082A1