Un-sintered stretched polytetrafluoroethylene composite film having dimensional stability
A novel method for forming ePTFE composite membranes by blending and stretching PTFE with thermoplastic polymers at controlled temperatures addresses the loss of crystallinity and stability issues, resulting in a dimensionally stable membrane with high mechanical properties.
Patent Information
- Application Number
- JP2024110197
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-10-04
AI Technical Summary
Existing ePTFE membranes and composite membranes lose crystallinity and dimensional stability when subjected to sintering processes, leading to reduced mechanical properties and dimensional changes at high temperatures.
A method of forming a biaxially expanded ePTFE composite membrane by blending fibrillable PTFE particles with thermoplastic polymer particles, stretching the blend in different directions at specific temperatures below the melting points of the components, without exposing it to temperatures above 327°C, resulting in a composite membrane with high geometric mean matrix modulus and tensile strength ratio.
The method produces a dimensionally stable ePTFE composite membrane with excellent mechanical properties, maintaining less than 1.5% dimensional change from 25°C to 200°C, and achieving a geometric mean matrix modulus/geometric mean matrix tensile strength ratio of at least 6.
Smart Images

Figure 2024144434000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to expanded polytetrafluoroethylene (ePTFE) composite membranes that are dimensionally stable without sintering, and more specifically to ePTFE composite membranes that include at least one thermoplastic polymer. Methods for producing such composite membranes are also provided. [Background technology]
[0002] ePTFE membranes and ePTFE composite membranes may be subjected to at least one sintering step to improve dimensional stability before use. Although it is known that sintering above the melting point of ePTFE improves the dimensional stability of ePTFE membranes, sintering adversely affects the membrane by decreasing crystallinity and increasing amorphous content. Membranes containing amorphous PTFE often exhibit a rigid amorphous phase with a transition temperature of about 120°C. Above this transition temperature, the mechanical properties of sintered ePTFE products may decrease. For example, sintering ePTFE membranes adversely affects the properties of the membrane, such as decreasing the average matrix modulus, dimensional stability over time, and decreasing crystallinity. It is desirable for those skilled in the art to produce dimensionally stable porous membranes derived from ePTFE without the need to sinter ePTFE and thereby lose crystallinity. Thus, there is a need to provide ePTFE membranes and ePTFE composite membranes that are dimensionally stable over time at high temperatures, exhibit high matrix modulus, and have a relatively high ratio of geometric mean matrix modulus / geometric mean matrix tensile strength. Summary of the Invention
[0003] One embodiment relates to a method of forming an unsintered biaxially expanded ePTFE composite membrane. The method includes providing a blend including a first plurality of fibrillizable polytetrafluoroethylene (PTFE) particles having a first melting point and a second plurality of thermoplastic polymer particles having a second melting point lower than the first melting point. The blend is then formed into a tape. The tape is then stretched in a first direction at a temperature lower than the first melting point and then stretched in a second direction different (e.g., perpendicular) to the first direction to form an ePTFE composite membrane. The stretching in the first direction can be performed at a temperature lower than the second melting point, such as about 170°C to about 300°C. The stretching in the second direction can be performed at a temperature higher than the second melting point and lower than the first melting point, such as about 280°C to 327°C. The blend includes 40% to 79.9% by weight of fibrillizable PTFE particles and 20.1% to 60% by weight of thermoplastic polymer. The ePTFE composite membrane can have a geometric mean matrix modulus / geometric mean matrix tensile strength ratio of at least about 6. Additionally, the method can be devoid of a heating step above 327°C.
[0004] Another embodiment relates to a method of forming an unsintered biaxially expanded ePTFE composite membrane. The method includes providing a blend including a first plurality of fibrillizable polytetrafluoroethylene (PTFE) particles having an average particle size of less than 1 μm and a second plurality of thermoplastic polymer particles having an average particle size of less than 1 μm. In an exemplary embodiment, the average particle size of the thermoplastic polymer particles is the same as or smaller than the average particle size of the fibrillizable PTFE particles. Additionally, the melting point of the thermoplastic polymer is lower than the melting point of the fibrillizable PTFE particles. The blend includes 40% to 79.9% by weight of the fibrillizable PTFE particles and 20.1% to 60% by weight of the thermoplastic polymer particles. The method also includes paste extruding the blend including a lubricant to form a calendered tape, drying the calendered tape to remove the lubricant and produce a dried calendered tape, and stretching the dried calendered tape in a first direction at a temperature below the melting point of the thermoplastic polymer to form a uniaxially expanded ePTFE composite membrane. The method also includes heating the uniaxially expanded porous ePTFE composite membrane to a temperature above the melting point of the thermoplastic polymer and below the melting point of the fibrillizable PTFE particles, and simultaneously or sequentially stretching the uniaxially expanded porous ePTFE composite membrane in a second direction, where the second direction is different from the first direction, to form a biaxially expanded ePTFE composite membrane. The temperature of the stretching step in the first direction can be about 170°C to about 300°C, and the temperature of the heating step can be about 280°C to about 300°C. The step of stretching the membrane in the second direction can be simultaneous with the step of heating. The method can be devoid of a heating step at a temperature equal to or greater than the melting point of the fibrillizable PTFE particles, such as above 327°C. Thermoplastic polymers can include poly(ethene-co-tetrafluoroethene) (ETFE), polyvinylidene difluoride (PVDF), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene propylene (FEP), perfluoroalkoxy (PFA), and combinations thereof.
[0005] Yet another embodiment relates to an unsintered biaxial ePTFE composite membrane having a plurality of nodes and fibrils. The ePTFE composite membrane comprises 40% to 79.9% by weight polytetrafluoroethylene (PTFE), 20.1% to 60% by weight thermoplastic polymer, and has a geometric mean matrix modulus / geometric mean matrix tensile strength ratio of at least about 6. The fibrils comprise primarily ePTFE, and the nodes comprise an amount of thermoplastic polymer greater than the amount of thermoplastic polymer originally present in the ePTFE composite membrane. The ePTFE composite membrane can exhibit a dimensional change of less than 1.5% when heated from 25° C. to 200° C. at a rate of 5° C. / min and held at 200° C. for 5 minutes, as measured by dynamic mechanical analysis (DMA). The fibrils can comprise at least about 85% or about 90% by weight of the ePTFE composite membrane. The nodes can comprise at least about 51% by weight of the thermoplastic polymer. Thermoplastic polymers can include poly(ethene-co-tetrafluoroethene) (ETFE), polyvinylidene difluoride (PVDF), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene propylene (FEP), perfluoroalkoxy (PFA), and combinations thereof. [Brief description of the drawings]
[0006] The accompanying drawings are included to provide a further understanding of the disclosure, and are incorporated in and constitute a part of this specification, illustrate embodiments and, together with the description, serve to explain the principles of the disclosure.
[0007] [Figure 1] FIG. 1 is a flow chart illustrating a method of forming a biaxially expanded polytetrafluoroethylene (ePTFE) composite membrane according to at least one embodiment.
[0008] [Diagram 2] FIG. 2 is a differential scanning calorimetry (DSC) graph of the poly(ethene-co-tetrafluoroethene) (ETFE) resin of Example 1 having a melting point of about 260° C. according to at least one embodiment.
[0009] [Diagram 3] FIG. 3 is a DSC graph of the PTFE / ETFE composite membrane of Example 7, which has a melting point of about 344° C., indicating that the PTFE composite membrane was not pre-sintered, according to at least one embodiment.
[0010] [Figure 4] FIG. 4 is a DSC graph of the FEP / PTFE composite membrane of Example 9, having a melting point of about 342° C. according to at least one embodiment.
[0011] [Diagram 5] FIG. 5 is a schematic diagram of the structure of an ePTFE composite membrane having fibrils formed primarily from ePTFE and nodes rich in thermoplastic polymer, according to at least one embodiment.
[0012] [Figure 6] 6 is a scanning electron micrograph (SEM) showing the structure of an ETFE / ePTFE composite membrane according to at least one embodiment; and
[0013] [Figure 7] FIG. 7 is a scanning electron micrograph (SEM) showing the structure of an ETFE / ePTFE composite membrane according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Those skilled in the art will readily appreciate that the various aspects of the present disclosure may be realized by any number of methods and devices configured to perform the intended functions. It should also be noted that the accompanying drawings referred to herein are not necessarily drawn to scale and may be exaggerated to illustrate the various aspects of the present disclosure, and in that regard, the drawings should not be construed as limiting. It should be understood that the terms "fibrillizable PTFE particles" and "fibrillizable PTFE" may be used interchangeably herein. Furthermore, the terms "thermoplastic polymer particles" and "thermoplastic polymer" may be used interchangeably herein. It should also be understood that the expanded composite membrane is porous.
[0015] Referring initially to Figure 1, a method 1000 for making an ePTFE composite membrane from PTFE particles and thermoplastic polymer particles, each having different melting points, is shown. The resulting ePTFE composite membrane has structural features of both PTFE and the thermoplastic polymer. The resulting ePTFE composite membrane exhibits excellent dimensional stability and mechanical properties. It should be understood that the term "thermoplastic polymer" is intended to include a single thermoplastic polymer or multiple thermoplastic polymers.
[0016] As shown in step 1010 of method 1000 of FIG. 1, thermoplastic polymer particles are provided. Fibrillizable PTFE particles useful for forming ePTFE composite membranes according to the present disclosure are disclosed, for example, in U.S. Pat. No. 3,953,566 to Gore (e.g., homopolymers) and U.S. Pat. No. 6,541,589 to Beyer (e.g., modified polymers). The polymers can be modified, for example, with perfluorobutyl ethylene (PFBE), poly(methyl vinyl ether) (PMVE), perfluoro(propyl vinyl ether) (PPVE), and the like. The PTFE particles can have an average particle size of less than 1.0 μm. The particle size of the PTFE can be about 0.1 μm, about 0.2 μm, about 0.3 μm, about 0.4 μm, about 0.5 μm, about 0.6 μm, about 0.7 μm, about 0.8 μm, about 0.9 μm, or about 1.0 μm. In some embodiments, the PTFE particle size is from about 0.1 μm to about 1.0 μm, from about 0.2 μm to about 0.9 μm, or from about 0.3 μm to about 0.8 μm.
[0017] As shown in step 1020 of the method 1000 of FIG. 1, thermoplastic polymer particles are provided. Suitable thermoplastic polymer particles include, but are not limited to, poly(ethene-co-tetrafluoroethene) (ETFE), polyvinylidene difluoride (PVDF), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene polyethylene (FEP), perfluoroalkoxy (PFA), and combinations thereof. The particle size of the thermoplastic polymer can be about the same size as the fibrillizable PTFE particles, or the particle size of the thermoplastic polymer can be smaller than the PTFE particles. The particle size of the thermoplastic polymer can be about 0.1 μm, about 0.2 μm, about 0.3 μm, about 0.4 μm, about 0.5 μm, about 0.6 μm, about 0.7 μm, about 0.8 μm, about 0.9 μm, or about 1.0 μm. In some embodiments, the particle size of the thermoplastic polymer is from about 0.1 μm to about 1.0 μm, from about 0.2 μm to about 0.9 μm, or from about 0.3 μm to about 0.8 μm.
[0018] As shown in step 1030 of method 1000 of FIG. 1, a composite resin is formed from the PTFE particles from step 1010 and the thermoplastic polymer particles from step 1020. The composite resin formation step 1030 includes blending the fibrillizable PTFE particles from step 1010 with the thermoplastic polymer particles from step 1020. In one embodiment, the PTFE particles can be polymerized in a suitable liquid (e.g., water) to form a first dispersion including the PTFE particles. The discreet thermoplastic polymer particles can be polymerized in a suitable liquid (e.g., water) to form a second dispersion including the thermoplastic polymer particles. Depending on the solids content of the dispersed particles in each dispersion, the two dispersions can be blended in a desired ratio (e.g., thermoplastic polymer particle dispersion / fibrillizable PTFE particle dispersion) to produce a desired weight percentage of each polymer in the blend. The blend may comprise about 40%, about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 77%, or 79.9% by weight of PTFE. In some embodiments, the PTFE content of the blend may be about 40% to 79.9%, about 50% to about 70%, or about 55% to about 65% by weight. In certain embodiments, the PTFE content of the blend may be as high as 75%, 76%, 77%, 78%, 79%, 79.5%, or 79.9% by weight. Additionally, the blend may comprise about 20.1%, about 23%, about 25%, about 30%, about 35%, about 45%, about 50%, about 55%, or about 60% by weight of thermoplastic polymer. In some embodiments, the thermoplastic polymer content of the blend can be about 23% to about 60%, about 30% to about 50%, or about 35% to about 45% by weight. In certain embodiments, the thermoplastic polymer content of the blend can be as low as 20.1%, 20.5%, 21%, 22%, 23%, or 24% by weight. In an exemplary embodiment, the blend comprises 40% to 79.9% ePTFE and 20.1% to 60% thermoplastic polymer by weight.
[0019] The resin formation step 1030 can include blending other ingredients and / or other steps to produce a blended dispersion having a desired weight fraction and other desired properties. For example, the resin formation step 1030 can include coagulating the blended dispersion, for example, by adding HNO3, which is then stirred. The resin formation step 1030 can also, or alternatively, dry the blended dispersion in a vacuum oven or by other suitable drying methods known in the art to produce a composite resin. Additionally, the resin formation step 1030 can include diluting the blended dispersion to a desired solids %. The solids % can be about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, or about 50% by weight. In some embodiments, the solids content is about 10% to about 50% by weight, about 15% to about 45% by weight, or about 20% to about 40% by weight. In some embodiments, the solids content is about 15% by weight.
[0020] As shown in step 1040 of method 1000 of FIG. 1, the composite resin is then molded into a tape. The molding step 1040 begins with cooling the composite resin prepared in the composite resin forming step 1030 to about 10° C. before mixing the composite resin with a suitable lubricant, such as light mineral oil, to form a lubricated mixture. Other suitable lubricants include aliphatic, aromatic, halogenated hydrocarbons, etc., selected according to flammability, evaporation rate, and economic considerations. It should be understood that the term "lubricant" as used herein is intended to describe a processing aid consisting of an incompressible fluid that is not a solvent for the polymer at process conditions. One particular example of a suitable lubricant is an isoparaffinic hydrocarbon, such as ISOPAR™ K SOLVENT (commercially available from Imperial Oil Chemical, Calgary, Canada).
[0021] The lubricated mixture can then be compressed to create pellets, which can be extruded through an extruder die to produce a wet tape. Non-limiting examples of methods for applying pressure (compression) include ram extrusion (e.g., when a lubricant is present, typically referred to as paste extrusion or pasting). The resulting wet tape can then be calendered, after which the calendered tape can be dried to remove the lubricant. Other known methods can be used to form the tape, such as extruding a tube followed by slitting the tube to the desired thickness. The thickness of the calendered tape can be about 0.10 mm, about 0.20 mm, about 0.30 mm, about 0.40 mm, about 0.50 mm, about 0.60 mm, about 0.70 mm, about 0.80 mm, about 0.90 mm, or about 1.0 mm. In some embodiments, the thickness of the calendered tape can be about 0.10 mm to about 1.0 mm, about 0.20 mm to about 0.60 mm, or about 0.30 mm to about 0.40 mm. The drying temperature is lower than the melting temperature of the thermoplastic polymer. The drying temperature can be about 145°C, about 150°C, about 155°C, about 160°C, about 165°C, about 170°C, or about 175°C. In some embodiments, the drying temperature is about 145°C to about 175°C, about 150°C to about 170°C, or about 155°C to about 165°C. In some embodiments, the drying temperature is about 160°C.
[0022] As shown in step 1050 of method 1000 of FIG. 1, the tape is then stretched in a first direction. The stretching step 1050 can be performed in a temperature controlled environment, such as two ovens in series or a single temperature adjustable oven. To stretch the tape in the first direction, the tape can be constrained, such as in a biaxial tenter frame. The constrained tape can then be heated to a first temperature, where the first temperature is below the melting point of the thermoplastic polymer. Suitable temperatures are specific to the thermoplastic polymer and are generally below the melting temperatures of both PTFE and the selected thermoplastic polymer. For PVDF, which has a melting temperature of 170°C, suitable temperatures include temperatures below about 170°C. In this example, the first temperature can be about 150°C, about 155°C, about 160°C, about 165°C, or about 170°C. In some embodiments involving PVDF, the first temperature can be from about 150°C to about 170°C, or from about 155°C to about 165°C. For PCTFE, which has a melting temperature of 200°C, suitable temperatures include temperatures less than about 200°C. In such embodiments, the first temperature can be about 180°C, about 185°C, about 190°C, about 195°C, or about 200°C. In some embodiments, the first temperature can be about 180°C to about 200°C, or about 185°C to about 195°C. For FEP, which has a melting temperature of 280°C, suitable temperatures include temperatures less than about 280°C. In such embodiments, the first temperature can be about 260°C, about 265°C, about 270°C, about 275°C, or about 280°C. In some embodiments, the first temperature can be about 260°C to about 280°C, or about 265°C to about 275°C. For PFA, which has a melting temperature of 310°C, suitable temperatures include temperatures less than about 310°C. In this example, the first temperature can be about 290°C, about 295°C, about 300°C, about 305°C, or about 310°C. In some embodiments, the first temperature is from about 290°C to about 310°C, or from about 295°C to about 305°C. For ETFE, which has a melting temperature of 260°C, suitable temperatures include temperatures less than about 260°C. In such embodiments, the first temperature can be about 240°C, about 245°C, about 250°C, about 255°C, or about 260°C.In some embodiments, the first temperature is from about 240° C. to about 260° C., from about 245° C. to about 255° C., or from about 249° C. to about 251° C. In other embodiments, suitable first temperatures can be less than about 290° C. for ETFE, less than about 170° C. for PVDF, less than about 200° C. for PCTFE, less than about 280° C. for FEP, or less than about 310° C. for PFA. In some embodiments, the constrained tape is heated to a first temperature of about 250° C.
[0023] As shown in steps 1060 and 1070 of method 1000 in FIG. 1, the uniaxially stretched porous membrane from step 1050, after heating in step 1060 (or simultaneously with heating step 1060), is further stretched in a second direction (i.e., orthogonal to the first direction) at a temperature below the melting temperature of PTFE but above the melting temperature of the thermoplastic polymer. In some embodiments, the second stretch in step 1070 is in a second direction different from the first direction. In further embodiments, the second direction is orthogonal to the first direction. In an exemplary embodiment, the composite membrane is heated to a temperature below the melting temperature of PTFE and above the melting temperature of the thermoplastic polymer and then stretched in a second direction. The heating step 1060 can be performed in a second oven different from the first oven of step 1050, or the heating can be performed in the oven utilized in step 1050.
[0024] The second temperature is higher than the first temperature of step 1050 (i.e., the temperature is higher than the melting temperature of the thermoplastic resin) but lower than the melting point of PTFE (i.e., less than about 340°C). The second temperature can be about 280°C, about 285°C, about 290°C, about 295°C, about 300°C, about 305°C, about 310°C, or about 315°C. In some embodiments, the second temperature is about 280°C to about 300°C, about 290°C to about 310°C, or about 295°C to about 305°C. In an exemplary embodiment, the second temperature is about 300°C. The heating step 1060 can be performed for about 30 seconds, about 60 seconds, about 90 seconds, or about 120 seconds. In certain embodiments, the heating step 1060 can be performed for about 60 seconds to about 90 seconds.
[0025] The first and second directions of stretching can correspond to (i) the machine direction (MD), also called the longitudinal direction or extrusion direction, or (ii) the transverse direction (TD), also called the cross direction, where TD is perpendicular to MD. In some embodiments, the first direction is oriented longitudinally and the second direction is transverse to the first stretching direction. In other embodiments, the first direction is oriented transversely and the second direction is longitudinal to the first stretching direction. To accommodate some standard equipment, it can be advantageous to stretch the tape in the machine direction before stretching in the transverse direction. Conversely, it is also conceivable to stretch the tape in the transverse direction before stretching in the machine direction.
[0026] The method 1000 of FIG. 1 also includes maintaining the tape at a temperature below 327° C. in all steps. The fibrillizable PTFE particles from step 1010 have an initial melting point of about 340° C. and a second melting point after sintering at 327° C. Thus, the method 1000 of FIG. 1 does not include heating the tape to a temperature of 340° C. or higher in any step. In some embodiments, the method 1000 is devoid of heating the tape above 327° C. or at the sintering temperature. In some embodiments, the method 1000 may be formed from the heating steps 1050 and 1070 without any additional heating. By maintaining the tape below the initial melting point of PTFE, the resulting ePTFE composite membrane 100 (FIG. 5) is unsintered.
[0027] Method 1000 shown in Figure 1 is provided as an example of various features of method 1000, and while combinations of these illustrated features are clearly within the scope of the present invention, the steps shown in method 1000 are not intended to suggest that the inventive concepts provided herein are limited from including fewer steps, additional steps, or alternatives to one or more steps shown in Figure 1. For example, in various embodiments, stretching steps 1050, 1070 and heating steps 1050, 1060 can occur simultaneously and / or in different orders.
[0028] A biaxially expanded ePTFE composite membrane 100 made according to the method 1000 of Figure 1 is shown generally in Figure 5. In particular, the ePTFE composite membrane 100 includes a microstructure including fibrils 110, nodes 120, and pores 130. The nodes 120 are masses of polymeric material and ePTFE, and the fibrils 110 are formed from the ePTFE and extend between and interconnect the nodes 120. The microstructure of the ePTFE composite membrane can be altered, for example, by changing the viscosity of the thermoplastic polymer, in which case the microstructure includes approximately parallel nodes (as shown in Figure 7).
[0029] The fibrils 110 are formed primarily from ePTFE, meaning that ePTFE constitutes a greater proportion (i.e., greater than 50%) of the weight of the fibrils 110. Thus, the weight ratio of ePTFE to thermoplastic polymer in the fibrils 110 is greater than 1:1. In some embodiments, the fibrils 110 can be formed from 51% ePTFE, about 55% ePTFE, about 60% ePTFE, about 65% ePTFE, about 70% ePTFE, about 75% ePTFE, about 80% ePTFE, about 85% ePTFE, about 90% ePTFE, or about 95% ePTFE by weight. In some embodiments, the fibrils 110 can be formed from at least about 90% ePTFE, or at least about 95% ePTFE, or more, by weight. In some embodiments, fibrils 110 are substantially formed from ePTFE or are completely formed from ePTFE. As used herein, the term "substantially formed" is intended to mean that the fibrils are completely (e.g., 100%) or nearly completely (e.g., 99%, 98%, 97%, 96%) formed from ePTFE. With respect to method 1000, a greater portion of the PTFE from providing step 1010 may be present in fibrils 110.
[0030] The nodes 120 can be rich in thermoplastic polymer, meaning that the thermoplastic polymer content at the nodes 120 is higher than the thermoplastic polymer content of the ePTFE composite membrane 100 as a whole. In some embodiments, the nodes 120 can have a thermoplastic polymer content that is greater than the thermoplastic polymer content provided in the composite resin (see step 1030 in FIG. 1 ). In other words, when an ePTFE composite membrane is formed having a thermoplastic polymer content of about 20% by weight, the thermoplastic polymer content of the nodes is greater than about 20% by weight, when a membrane is formed having a thermoplastic polymer content of about 30% by weight, the thermoplastic polymer content of the nodes is greater than about 30% by weight, etc.
[0031] In certain embodiments, node 120 may be formed primarily from thermoplastic polymer, meaning that the thermoplastic polymer constitutes a greater proportion (i.e., greater than 50%) of the mass of node 120. Thus, the mass ratio of thermoplastic polymer to ePTFE in node 120 is greater than 1:1. In some embodiments, node 120 may be formed from 51% by mass thermoplastic polymer, about 55% by mass thermoplastic polymer, about 60% by mass thermoplastic polymer, about 65% by mass thermoplastic polymer, about 70% by mass thermoplastic polymer, about 75% by mass thermoplastic polymer, or about 80% by mass thermoplastic polymer.
[0032] The porosity of the ePTFE composite membrane 100 can vary as a function of the distance between the nodes 120 (e.g., the size of the pores). As the distance between the nodes decreases, the porosity decreases, and vice versa. The porosity of the membrane 100 can also vary as a function of the size of each node 120. As the size of each node 120 increases, the porosity decreases, and vice versa. The porosity of the ePTFE composite membrane can be about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, about 95%, about 96%, about 97%, about 98%, or about 99%. In some embodiments, the porosity is about 10% to about 99%, about 40% to about 90%, or about 50% to about 80%.
[0033] The thickness of the ePTFE composite membrane 100 can also vary. The thickness of the ePTFE composite membrane 100 can be about 10 μm, about 15 μm, about 20 μm, about 30 μm, about 40 μm, about 50 μm, about 60 μm, about 70 μm, about 80 μm, about 90 μm, about 100 μm, about 110 μm, about 120 μm, about 130 μm, about 140 μm, or about 150 μm. In some embodiments, the thickness of the ePTFE composite membrane 100 is about 10 μm to about 150 μm, about 15 μm to about 120 μm, or about 20 μm to about 100 μm.
[0034] A scanning electron micrograph of an ePTFE / thermoplastic polymer composite membrane 200 made according to method 1000 of Figure 1 is shown in Figure 6. Similar to membrane 100 of Figure 5, membrane 200 of Figure 6 has fibrils 210, nodes 220 and pores 230. As noted above, ePTFE / thermoplastic polymer composite membranes can be constructed with thinner, substantially parallel nodes as shown in Figure 7, which shows membrane 300, fibrils 310, nodes 320 and pores 330.
[0035] The membranes 100, 200, 300 are dimensionally stable, exhibiting high matrix modulus and a relatively high ratio of geometric mean matrix modulus to geometric mean matrix tensile strength. The absolute dimensional change was measured by dynamic mechanical analysis (DMA), which is described in detail below under "Dimensional Stability Testing." In particular, the samples were heated at 5°C / min from 25°C to 200°C and then held at 200°C for 5 minutes. The absolute dimensional change of the ePTFE composite membrane can be about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.0%, about 1.25%, or about 1.5%. In some embodiments, the absolute dimensional change is about 0.1% to about 1.5%, about 0.2% to about 1.0%, or about 0.3% to about 0.9%. In some embodiments, the absolute dimensional change is less than 1.5%. The matrix modulus of the ePTFE composite membrane can be about 700 MPa, about 800 MPa, about 900 MPa, about 1000 MPa, about 1100 MPa, about 1200 MPa, about 1300 MPa, about 1400 MPa, about 1500 MPa, or about 1600 MPa. In some embodiments, the matrix modulus is about 700 MPa to about 1600 MPa, about 800 MPa to about 1500 MPa, or about 900 MPa to about 1400 MPa. The ratio of the geometric mean matrix modulus to the geometric mean matrix tensile strength of the ePTFE composite membrane can be about 6, about 8, about 10, about 12, about 14, or about 16. In some embodiments, the geometric mean matrix modulus is about 6 to about 16, about 8 to about 14, or about 10 to about 12. EXAMPLES
[0036] Test Method Although particular methods and apparatus are described below, it should be understood that other methods or apparatus, as determined to be suitable by those skilled in the art, may alternatively be utilized.
[0037] Non-contact thickness measurement
[0038] The non-contact thickness of the films was measured using a KEYENCE LS-7600 laser system (available from KEYENCE America).
[0039] Film density calculation
[0040] The samples were die cut to form rectangular sections measuring 9.05 cm by 5.08 cm. Each sample was weighed using an A&D Model HF400 balance. Using the thickness calculated by the KEYENCE laser, the density of the samples was calculated using the following formula:
number
[0041] Matrix Tensile Strength (MTS)
[0042] To determine the MTS, sample ePTFE composite membranes were cut in the longitudinal and transverse directions using an ASTM D412-Dog Bone Die Type F (DD412F). The tensile failure load was measured using an INSTRON® 5500R (Illinois Tool Works Inc., Norwood, MA) tensile tester equipped with flat-face grips and a "200 lb" (approximately 90.72 kg) load cell. The gauge length of the grips was set at 8.26 cm, and a strain rate of 0.847 cm / s or 14.3% / s was used. After placing the sample in the grips, the sample was shortened by 1.27 cm to obtain a baseline, and then tensile testing was performed at the strain rate described above. Two samples of each condition were tested separately, and the average of the maximum load (i.e., peak force) measurements was used to calculate the MTS. The longitudinal and transverse MTS were calculated using the following equations: MTS=(Maximum load / Cross-sectional area)*(Resin density / Membrane density).
[0043] The geometric mean of the MTS for each membrane was then calculated using the following formula: Geometric mean MTS = square root [(longitudinal MTS)*(transverse MTS)]
[0044] Matrix tensile stress at a specific strain
[0045] Matrix tensile stress = (load at specific strain / cross-sectional area)*(resin density / film density)
[0046] Matrix Modulus
[0047] From the same tensile tests described in Matrix Tensile Strength at Specific Strains, the raw data was imported into a data analysis program. Because it is difficult to fully load the samples into the grips, the zero strain point for each sample was calculated as the point where the load was two standard deviations above zero. Elastic modulus was taken from the 0 cm point to an additional 0.18 cm (or 0-3% strain based on the gauge length of the D412-F dogbone). Elastic modulus is the stress / strain gradient. Matrix elastic modulus in both the longitudinal and transverse directions was calculated using the following equations: Matrix tensile stress at 3% strain = (load at 3% strain / cross-sectional area) * (resin density / film density) Matrix modulus = (Matrix tensile stress at 3%) / (.03)
[0048] The geometric mean of the matrix modulus for each membrane was then calculated using the following formula: Geometric mean matrix modulus = square root [(longitudinal matrix modulus) * (transverse matrix modulus)]
[0049] The ratio of matrix modulus to matrix tensile strength was then calculated using the following formula: Ratio of matrix modulus to matrix tensile strength = geometric mean matrix modulus / geometric mean matrix tensile strength
[0050] Differential scanning calorimetry (DSC) measurement
[0051] DSC measurements were performed on a Q2000 machine (TA Instruments, New Castle, Delaware). DSC was used to identify the melting point of ETFE in Example 1, as shown in Figure 2, and the melting points of ePTFE composite membranes produced according to Examples 7 and 9, as shown in Figures 3 and 4, respectively. For the ePTFE composite membrane samples, the samples were not pre-sintered, given that the melting point of the resulting membrane measured by DSC was about 344°C. This provides an indication that the PTFE did not pre-sinter during stretching, as it experienced initial melting during DSC.
[0052] Dimensional Stability Test
[0053] Dynamic mechanical analysis (DMA) was performed using an RSA-G2 solids analyzer available from TA Instruments (New Castole, Delaware). ePTFE composite membrane samples were cut with a width of 13 mm in the machine direction and a gauge length of 15 mm. With a minimum load of 1 g to keep the sample taut, the samples were heated from 25° C. to 200° C. at 5° C. / min, then held at 200° C. for 5 minutes. The dimensional change of each sample was measured over a period of time, and the final absolute change in dimensions was reported (see Table 2).
[0054] Example 1
[0055] Ethylene-tetrafluoroethylene (ETFE) polymerization was carried out as follows: 23 kg of deionized (DI) water, 5 g of oxalic acid, 20 mL of chloroform, and 0.6 kg of non-telogenic perfluorinated dispersant were added to a 50 liter horizontal polymerization reactor equipped with a three-blade agitator. The reactor was repeatedly evacuated and pressurized to approximately 1 atmosphere (Atm) (approximately 101.325 kPa) with tetrafluoroethylene (TFEE) until the oxygen level dropped to below 20 ppm. The contents were briefly stirred at approximately 60 rpm between evacuation and purging cycles to ensure that the water was deoxygenated. The reactor was cooled to 20°C and stirred at 60 rpm. 1550 kPa of TFE was then added, followed by 550 kPa of ethylene. At this time, KMnO4 (0.6 g / L) in DI water solution was continuously injected at 40 g / min. Every time the pressure dropped by 200 kPa, 110 kPa of TFE and 90 kPa of ethylene were returned to the reactor to maintain a constant pressure. After 322 minutes, the reaction was stopped and the pressure was released. 44.64 kg of dispersion was produced, the solid content was 15.96 wt% solids, and the particle size of the raw dispersion was 220 nm. As shown in Figure 2, the resulting ETFE resin had a melting point of 260°C as measured by DSC.
[0056] Example 2
[0057] Polytetrafluoroethylene (PTFE) polymerization was carried out as follows: 1.5 kg of paraffin wax, 28 kg of deionized (DI) water, 18 g of non-telogenic perfluorinated dispersant, and 5 g of succinic acid dissolved in about 50 grams of DI water were added to a 50 liter horizontal polymerization reactor equipped with a three-blade agitator. The reactor and contents were heated above the melting point of the wax, about 60°C. The reactor was repeatedly evacuated and pressurized with TFE to about 1 atmosphere (about 101.325 kPa) or less until the oxygen level dropped to below 20 ppm. The contents were briefly stirred at about 60 rpm between evacuation and purging cycles to ensure that the water was deoxygenated. 8 mL of perfluorobutylethylene (PFBE) was added to the vacuum reaction as a comonomer precharge. The reactor was then heated to 83°C.
[0058] TFE was then added to the reactor until the pressure reached 2.8 MPA (approximately 3.0 kg), and KMnO4 (0.063 g / L) in a DI water solution was injected at 80 mL / min until approximately 2.0 kg of TFE had been added. This was accomplished in approximately 7 minutes. Approximately 100 g of the non-telogenic perfluorinated dispersant was added in 12 gram increments, with the first increment being added after approximately 1 kg of TFE had been added to the reactor, subsequent increments being added after each subsequent kg of TFE had been added, and the final increment being added after approximately 9 kg of TFE had been charged. The KMnO4 addition rate was reduced to 40 mL / min at the 2 kg TFE level and continued at this rate until approximately 3 kg TFE had been added. The KMnO4 addition rate was then further reduced to 20 mL / min until approximately 5 kg of TFE had been added. The KMnO4 addition was then reduced to 10 mL / min and continued at this rate until approximately 7 kg of TFE had been added to the reactor, at which point the KMnO4 addition was stopped. The resulting dispersion had an untreated dispersion particle size of 203 nm and a solids content of 35.0% solids by weight.
[0059] Example 3
[0060] Vinylidene difluoride (VDF) modified polychlorotrifluoroethylene (mPCTFE) polymerization was carried out as follows: 28 kg DI water, 5 g oxalic acid, 100 g ammonium bisulfite monohydrate and 0.5 kg non-telogenic perfluorinated dispersant were added to a 50 liter horizontal polymerization reactor equipped with a three-blade agitator. The reactor was repeatedly evacuated and pressurized to about 1 atmosphere (about 101.325 kPa) with vinylidene fluoride (VDF) until the oxygen level dropped to below 20 ppm. The contents were briefly stirred at about 60 rpm between evacuation and purging cycles to ensure that the water was deoxygenated. The reactor was then cooled to 60° C. and stirred at 60 rpm. 100 kPa of VDF was then added to the reactor, followed by 2.0 L of liquefied chlorotrifluoroethylene (CTFE) through a high pressure liquid pump to a final pressure in the reactor of 1400 kPa. Ammonium persulfate solution (5 g dissolved in 100 mL DI water) was added continuously to the reactor at a rate of 5 g / min. CTFE was added continuously to the reactor to maintain a pressure of 1400 kPa. For every 100 mL of liquefied CTFE added, 10 kPa of VDF was added to the reactor. After 300 minutes, the reaction was stopped (a total of 3.6 L of CTFE monomer and 360 kPa of VDF added) and the pressure in the reactor was released. A total of 37.74 kg of dispersion was produced with a solids content of 15.2 wt%. DSC analysis showed a melting point of 203°C. A skeletal density of 2.177 g / mL was determined using helium pycnometry. The mPCTFE dispersion was then co-coagulated with the PTFE dispersion produced in Example 2 using the general mixing method described in Example 4 to obtain a final composite resin that was 40 wt% PCTFE and 60 wt% PTFE.
[0061] Example 4
[0062] The mixing of ETFE and PTFE was carried out as follows. Based on the solids content of the two resins obtained from the polymerization described in Examples 1 and 2, respectively, the two dispersions were mixed in a ratio of 1 kg of 15.96 wt% solids ETFE dispersion / 0.684 kg of 35.0 wt% solids PTFE. This produced a dispersion with 23.7 wt% solids, containing 40 wt% ETFE and 60 wt% PTFE. This dispersion was then diluted to 15 wt% solids. To solidify the two materials, 1.0 L of 65 wt% HNO3 was added to 117 kg of the dispersion, which was stirred at 100 rpm. The stirring speed was increased to 420 rpm and stirred for an additional 12 minutes to produce an air-wet composite resin. The composite resin was then dried in a vacuum oven at 150°C for 28 hours to produce 17.7 kg of final resin containing 40 wt% ETFE thermoplastic and 60 wt% fibrillizable PTFE.
[0063] Example 5
[0064] Fluorinated ethylene propylene (FEP) polymerization was carried out as follows: 23 kg of DI water and 0.2 kg of non-telogenic perfluorinated dispersant were added to a 50 liter horizontal polymerization reactor equipped with a three-blade agitator. The reactor was repeatedly evacuated and pressurized to approximately 1 atm (approximately 101.325 kPa) with TFE until the oxygen level was reduced to below 20 ppm. The contents were briefly stirred at approximately 60 rpm between evacuation and purging cycles to ensure that the water was deoxygenated. The reactor was heated to 85° C. and stirred at 60 rpm. 3 kg of hexafluoropropylene (HFP) was then added to the reactor. TFE was then added to the reactor until the total pressure was 1100 kPa. At this time, 2.5 kg of a solution of ammonium persulfate in deionized water (1.13 g / L) was added to the reactor. The pressure was maintained at 1100 kPa by continuously adding TFE to the reactor as the TFE was consumed. The reaction was stopped after 105 minutes to give 35.65 kg of dispersion with 14.6 wt % solids. This resin is suitable for blending with PTFE according to the general blending process described in Example 4.
[0065] Example 6
[0066] ETFE / PTFE extrusion was carried out as follows: 3.17 kg of ETFE / PTFE resin blend prepared from Example 4 was cooled to 10° C., then mixed with 0.80 kg of ISOPAR™ K, an isoparaffinic hydrocarbon lubricant, and shaken in a drum tumbler for 10.5 minutes. The mixture was then compressed at 3.1 MPa in a 101 mm diameter tube to form pellets. The pellets were heated at 70° C. overnight in a concealed tube to prevent the ISOPAR™ K from evaporating. The pellets were then extruded at a rate of 0.76 mm / s through an extruder heated to 49° C. using a die measuring 229 mm wide by 0.46 mm thick. The resulting wet tape was then calendered to 0.30 mm, and then dried in a dryer at a temperature of 160° C. to remove all the ISOPAR™ K from the tape. The resulting dry tape had an areal weight of 420 g / m 2 It was.
[0067] Example 7
[0068] ETFE / PTFE stretching was performed as follows: A piece of the dried extrudate from Example 6 was then placed in a biaxial tenter frame equipped with two ovens to produce a biaxially stretched porous ETFE / PTFE membrane. The restrained tape was heated to 250°C for 120 seconds (i.e., below the melting point of ETFE) before stretching the tape 10:1 in the longitudinal direction at a rate of 50% / sec. The stretched ETFE / PTFE membrane was then heated in a second oven to 300°C (i.e., above the melting point of ETFE but below the melting point of PTFE) and stretched 10:1 in the transverse direction at a rate of 50% / sec. This biaxial stretching resulted in a mass per area of 6.2 g / m 2The resulting porous ETFE / PTFE membrane had a thickness of 18.85 micrometers and a MTS of 185 MPa in the longitudinal direction and 92 MPa in the transverse direction. As shown in Figure 3, the resulting membrane had a melting point of about 344°C as measured by DSC, indicating that the PTFE was initially melted during DSC and therefore was not pre-sintered during stretching. It should be understood that if the PTFE had been sintered, a melting point of 344°C would not have been indicated by DSC and the melting point of the PTFE would have been 327°C.
[0069] Comparative Example 1
[0070] PTFE extrusion was carried out as follows: PTFE resin prepared in Example 2 was solidified without blending with thermoplastic resin. 7.71 kg of this resin was added with 1.94 kg of ISOPAR™ K and mixed for 10.25 minutes. The mixture was then compressed at 3.1 MPa in a tube with a diameter of 101 mm to form pellets. The pellets were extruded at a speed of 12.2 mm / s at about 22°C using a die with a width of 229 mm and a thickness of 0.46 mm. The wet tape was calendered to 0.30 mm and then dried in a dryer to remove all the ISOPAR™ K from the tape. The resulting dry tape had an areal weight of 400 g / m 2 It was.
[0071] Comparative Example 2
[0072] PTFE stretching was performed as follows: A section of tape from Comparative Example 1 was placed in a biaxial tenter frame containing two ovens to produce a biaxially stretched membrane. After heating the restraining tape at 300°C, the tape was biaxially stretched 10:1 in both the longitudinal and transverse directions simultaneously at a rate of 700% / sec, and then sinter restrained at 365°C for 90 seconds. The resulting membrane had an area mass of 6.2 g / m2. 2 The thickness was 28.9 μm, and the MTS was 240 MPa in the longitudinal direction and 96 MPa in the transverse direction.
[0073] Comparative Example 3
[0074] Non-melt ETFE / PTFE blend stretching was performed as follows: A section of the tape prepared in Example 6 was placed in a biaxial tenter frame containing two ovens to produce a biaxially stretched membrane. After heating, the restrained tape was stretched 10:1 in the longitudinal direction at a rate of 250% / sec at 250°C (below the melting point of ETFE) and then stretched 10:1 in the transverse direction at a rate of 250% / sec at 250°C. This ETFE / PTFE composite membrane was not exposed to temperatures above the melting points of either ETFE or PTFE. The membrane had an areal weight of 6.81 g / m 2 The thickness was 120 μm.
[0075] Example 8
[0076] FEP / PTFE blend extrusion was carried out as follows: 13.22 kg of mixed resin was prepared according to the general mixing method described in Example 4. The mixed FEP / PTFE resin contained 40% by weight FEP (synthesized in Example 5) and 60% by weight PTFE (synthesized in Example 2). It was cooled to 10°C, after which it was mixed with 3.33 kg of ISOPAR™ K lubricant and shaken in a drum tumbler for 10.5 minutes. The mixture was then compressed at 3.1 MPa in a 101 mm diameter tube to form pellets. The pellets were heated overnight at 49°C in a concealed tube to prevent the ISOPAR™ K from evaporating. The pellets were extruded at a rate of 2.54 mm / s through an extruder heated to 49°C using a 229 mm wide x 0.46 mm thick die. The wet tape was then calendered to 0.25 mm and then dried in an oven at a temperature of 180° C. to remove all the ISOPAR™ K from the tape.
[0077] Example 9
[0078] Stretching of the FEP / PTFE blend was performed as follows: The dried tape from Example 8 was stretched in a 4:1 ratio in the longitudinal direction at a speed of 10 meters / min in an oven at a temperature of 200°C (below the melting point of FEP). This stretched tape was then stretched again in the same longitudinal direction through the same oven at 200°C, a 2:1 ratio, and a speed of 2.5 meters / min. Finally, the tape was sent to an oven at 300°C (higher than the melting point of FEP but below the melting point of PTFE) to produce a homogeneously molten uniaxially stretched tape. A portion of this tape was then placed in a tenter frame, heated to 300°C (higher than the melting point of FEP but below the melting point of PTFE), and stretched in the transverse direction at a speed of 100% / sec at a ratio of 10:1. The resulting membrane contained a melting point of about 342°C for PTFE as measured by DSC, indicating that the PTFE was initially melted during DSC and therefore was not pre-sintered during stretching (see FIG. 4).
[0079] Example 10
[0080] Stretching of the ETFE / PTFE blend was carried out as follows: A piece of the dried extrudate from Example 6 was placed in a biaxial tenter frame equipped with two ovens to produce a biaxially stretched porous membrane. After heating the restrained tape to 250°C (below the melting point of ETFE), the tape was stretched 10:1 in the longitudinal direction at a rate of 50% / sec. The stretched membrane was then heated in a second oven to 300°C (i.e., above the melting point of ETFE but below the melting point of PTFE) and stretched 5:1 in the transverse direction at a rate of 50% / sec. The resulting porous ETFE / PTFE composite membrane had an area mass of 13.6 g / m 2 , had a thickness of 67.8 micrometers, and had an MTS of 203 MPa in the longitudinal direction and 43 MPa in the transverse direction.
[0081] Example 11
[0082] Stretching of the ETFE / PTFE blend was carried out as follows: A piece of the dried extrudate from Example 6 was placed in a biaxial tenter frame equipped with two ovens to produce a biaxially stretched porous membrane. After heating the restrained tape to 250°C (i.e., below the melting point of ETFE), the tape was stretched 5:1 in the longitudinal direction at a rate of 50% / sec. This stretched membrane was then heated in a second oven to 300°C (i.e., above the melting point of ETFE and below the melting point of PTFE) and stretched 10:1 in the transverse direction at a rate of 50% / sec. This resulted in a mass per area of 13.6 g / m 2 produced a porous ETFE / PTFE composite membrane that was 67.8 micrometers thick and had an MTS of 108 MPa in the longitudinal direction and 107 MPa in the transverse direction.
[0083] Example 12
[0084] Stretching of the ETFE / PTFE blend was carried out as follows: A portion of the dried extrudate piece from Example 5 was placed in a biaxial tenter frame and biaxially stretched at 250°C (i.e., below the melting point of ETFE) at 10:1 and 250% / sec in the longitudinal direction followed by transverse stretching. No stretching was carried out at a temperature above the melting point of ETFE, 260°C. After the stretching operation, the membrane was heat treated at 300°C (i.e., above the melting point of ETFE but below the melting point of PTFE) for 60 seconds. This resulted in a mass per area of 6.7 g / m 2 An ETFE / PTFE composite membrane was produced having a thickness of 99 micrometers and an MTS of 164 MPa in the longitudinal direction and 96 MPa in the transverse direction.
[0085] Comparative Example 4
[0086] Stretching of the PTFE was performed as follows: A piece of the dried extrudate of Comparative Example 1 (PTFE-no thermoplastic) was placed in a biaxial tenter frame, heated to 300°C (i.e., below the melting point of PTFE) and then stretched 10:1 in the longitudinal direction. The sample was then transferred to a second oven, heated to 365°C (i.e., above the melting point of PTFE) and stretched 6:1 in the transverse direction. This resulted in a mass per area of 10.9 g / m2 This produced a porous ePTFE membrane having a thickness of 70.6 micrometers and an MTS of 251 MPa in the longitudinal direction and 192 MPa in the transverse direction. The ePTFE membrane was observed to be dimensionally stable and did not shrink on its own when removed from the tenter frame pins.
[0087] Comparative Example 5
[0088] The resin was made by blending 15 wt. % ETFE prepared according to Example 1 with 85 wt. % PTFE prepared according to Example 2. The resin was paste extruded into a flat tape 0.76 mm thick by 76 cm wide. The tape was then calendered between two metal nips to provide a tape with a thickness of 0.46 mm and an MTS of 30.6 MPa in the longitudinal direction and 15.0 MPa in the transverse direction. A piece of the dried extrudate was placed in a biaxial tenter frame and biaxially stretched 10:1 in both the machine and transverse directions at 250°C (i.e., below the melting point of ETFE). The sample was then transferred to a second oven and heated to 365°C (i.e., above the melting point of PTFE) for 60 seconds. This resulted in a 10.9 g / m 2 This produced an ETFE / PTFE composite membrane (15 wt % ETFE content) with a MTS of 283 MPa in the longitudinal direction and 175 MPa in the transverse direction, with a geometric mean MTS of 222 MPa. The matrix modulus in the longitudinal direction was 1738 MPa and the matrix modulus in the transverse direction was 1078 MPa, with a geometric mean of 1369 MPa.
[0089] Comparative Example 6
[0090] A piece of the dried extrudate from Example 6 was placed in a biaxial tenter frame containing two ovens to produce a biaxially stretched porous membrane. After heating the restrained tape at 250°C (i.e., below the melting point of ETFE), the tape was stretched 10:1 in the longitudinal direction and then 10:1 in the transverse direction. The ePTFE composite membrane was then sintered at 365°C (i.e., above the melting point of PTFE) for 60 seconds. This produced a 6.3 g / m 2produced a porous membrane with a MTS of 158 MPa in the longitudinal direction and 84 MPa in the transverse direction, with a geometric mean MTS of 108 MPa. The matrix modulus in the longitudinal direction was determined to be 1263 MPa and 337 MPa in the transverse direction, giving a geometric mean matrix modulus of 652 MPa.
[0091] Example 13
[0092] The above samples were evaluated for tensile strength and dimensional stability and the results are shown in Tables 1 and 2, respectively. [Table 1] [Table 2]
[0093] Examples 14-18
[0094] The thermoplastic resins prepared in Examples 1, 3, and 5 were used to produce various co-coagulated composite resins of thermoplastic resin and PTFE. These resins were then paste extruded in a manner similar to that of Examples 6 or 7, but at various conditions as would be accomplished by one skilled in the art of paste extrusion. Porous membranes were then stretched from these tapes by stretching in the MD direction at the specified stretch ratio below the melting point of the thermoplastic resin, and then stretching in the transverse direction above the melting point of the thermoplastic resin but below 327°C to provide the final properties in terms of geometric mean MTS, geometric mean matrix modulus, and ratio of matrix modulus to MTS as shown in Table 3. The composite resins of Examples 14-18 were stretched in the longitudinal direction below the melting point of the thermoplastic resin, and then stretched in the transverse direction above the melting point of the thermoplastic resin but below the melting point of PTFE. Comparative Examples 7-9, which did not contain a thermoplastic resin, required heat treatment at 365°C for 60 seconds to produce a dimensionally stable membrane. [Table 3]
[0095] The invention of this application has been described above both generally and with reference to specific embodiments. It will be apparent to those skilled in the art that various modifications and variations can be made in the embodiments without departing from the scope of the present disclosure. Thus, the embodiments are intended to cover the modifications and variations of the present invention provided they come within the scope of the appended claims and their equivalents.
Claims
1. providing a blend comprising a plurality of fibrillizable polytetrafluoroethylene (PTFE) particles having a first melting point and a plurality of thermoplastic polymer particles having a second melting point lower than the first melting point; forming the blend into a tape; stretching the tape in a first direction below the second melting point to form a stretched tape; and stretching the stretched tape in a second direction above the second melting point but below the first melting point to form an ePTFE composite membrane; A method of forming an expanded composite ePTFE membrane, wherein said expanding occurs at a temperature below said first melting point such that said ePTFE composite membrane is not sintered.
2. 2. The method of claim 1, wherein a plurality of said stretching steps are performed sequentially.
3. The method of claim 1 , wherein a plurality of said stretching steps are carried out simultaneously.
4. The method of claim 1 , wherein the thermoplastic polymer is a thermoplastic fluoropolymer.
5. The method of claim 4, wherein the thermoplastic fluoropolymer is selected from poly(ethene-co-tetrafluoroethene) (ETFE), polyvinylidene difluoride (PVDF), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene propylene (FEP), and combinations thereof.
6. The method of claim 1 , wherein the membrane has a ratio of geometric mean matrix modulus to geometric mean matrix tensile strength of about 6 or greater.
7. The method of claim 1 , wherein the blend comprises 40% to 79.9% by weight of fibrillizable polytetrafluoroethylene (PTFE) particles and 20.1% to 60% by weight of thermoplastic polymer particles.
8. The method of claim 1 , wherein the fibrillizable PTFE particles and the thermoplastic polymer particles each have an average particle size of less than 1 μm.
9. The method of claim 1 , wherein the ePTFE composite membrane has an absolute dimensional change of less than 1.5%.
10. a first plurality of particles comprising fibrillizable polytetrafluoroethylene (PTFE) particles having an average particle size of less than 1 μm; a second plurality of particles comprising thermoplastic polymer particles having an average particle size of less than 1 μm, the thermoplastic polymer particles having a melting point lower than the melting point of the fibrillizable PTFE particles; providing a blend comprising 40% to 79.9% by weight of fibrillizable PTFE particles and 20.1% to 60% by weight of thermoplastic polymer particles; paste extruding the blend in a lubricant to form a calendered tape; drying the calendered tape to remove the lubricant to produce a dry calendered tape; stretching the dried calendered tape in a first direction at a temperature below the melting point of the thermoplastic polymer to form a uniaxially expanded ePTFE composite membrane; heating the uniaxially expanded porous membrane to a temperature above the melting point of the thermoplastic polymer but below the melting point of the fibrillizable PTFE; and A method for forming an unsintered biaxially expanded composite ePTFE membrane, comprising stretching the uniaxially expanded porous membrane in a second direction different from the first direction to form a biaxially expanded ePTFE composite membrane.
11. The method of claim 10, wherein a plurality of said stretching steps are performed sequentially.
12. The method of claim 10, wherein a plurality of said stretching steps are performed simultaneously.
13. The method of claim 10, wherein the ePTFE composite membrane has an absolute dimensional change of less than 1.5%.
14. 11. The method of claim 10, wherein the membrane has a ratio of geometric mean matrix modulus to geometric mean matrix tensile strength of about 6 or greater.
15. 40% to 79.9% by weight of fibrillizable polytetrafluoroethylene (PTFE) particles; 20.1% to 60% by weight of thermoplastic polymer particles; a plurality of nodes interconnected by fibrils; and A ratio of geometric mean matrix elastic modulus to geometric mean matrix tensile strength of about 6 or greater. An unsintered biaxial ePTFE composite membrane comprising:
16. 16. The membrane of claim 15, wherein the fibrils comprise ePTFE and the nodes comprise a thermoplastic polymer content greater than the total thermoplastic polymer content of the ePTFE composite membrane.
17. 16. The membrane of claim 15, wherein said fibrils comprise greater than or equal to about 85% of said ePTFE.
18. The membrane of claim 15 , wherein the nodes comprise at least about 51% by weight of the thermoplastic polymer.
19. 16. The membrane of claim 15, wherein the ePTFE composite membrane exhibits a dimensional change of less than 1.5% when measured by dynamic mechanical analysis (DMA) upon heating from 25° C. to 200° C. at a rate of 5° C. / min and holding at 200° C. for 5 minutes.
20. 16. The membrane of claim 15, wherein the thermoplastic polymer is selected from the group consisting of poly(ethylene-co-tetrafluoroethene) (ETFE), polyvinylidene difluoride (PVDF), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene propylene (FEP), perfluoroalkoxy (PFA), and combinations thereof.
Citation Information
Patent Citations
JP1975010343A
Composition containing PTFE as main component, mixed powder, material for molding, filter medium for filter, air filter unit, and method for producing porous membrane
JP2016000817A
Porous polytetrafluoroethylene material and process for producing the same
WO1994003531A1