Conjugate fiber

The composite fiber, comprising a metal and ceramic sintered body, addresses the weakness of PZT fibers by enhancing strength and flexibility through co-sintering, achieving superior performance in vibration sensors and actuators.

JP2024144477AActive Publication Date: 2024-10-11MURATA MFG CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024117093
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Conventional lead zirconate titanate (PZT) fibers exhibit low tensile strength and are prone to delamination and breakage due to differences in thermal expansion coefficients, limiting their effectiveness in vibration sensors and actuators, particularly in applications requiring flexibility and durability.

Method used

A composite fiber composed of a metal sintered body and a ceramic sintered body, where the two are adjacent to each other, forming a fibrous structure through co-sintering, which enhances strength and flexibility by suppressing delamination and improving bonding at the interface.

Benefits of technology

The composite fiber achieves a tensile strength of 5 kgf/mm² or more, with a radius of curvature of 200 mm or less, providing improved durability and flexibility compared to conventional PZT fibers, suitable for use in vibration sensors and actuators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144477000008
    Figure 2024144477000008
  • Figure 2024144477000009
    Figure 2024144477000009
  • Figure 2024144477000010
    Figure 2024144477000010
Patent Text Reader

Abstract

To provide a conjugate fiber which can function as a piezoelectric material and is improved in strength as compared with a conventional PZT fiber.SOLUTION: There is provided a conjugate fiber composed of at least a metal sintered material and a ceramic sintered material, in which the metal sintered material and the ceramic sintered material are adjacent to each other in the conjugate fiber to form a fiber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite fiber, and more specifically to a composite fiber that may be composed of at least a metal sintered body and a ceramic sintered body. [Background technology]

[0002] Piezoelectric fibers using lead zirconate titanate fibers (PZT fibers) are known as vibration sensors and actuators that can be used in structures such as buildings, automobiles, ships, and aircraft (for example, Patent Documents 1 to 6). In addition, smart boards in which such PZT fibers are embedded in a structure to function as stress sensors, vibration sensors, and actuators are also known (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent application 2003-12829 [Patent Document 2] Patent application 2005-171752 [Patent Document 3] Patent application 2004-15489 [Patent Document 4] Patent application 2005-59552 [Patent Document 5] Patent application 2005-313715 [Patent Document 6] Patent application 2010-198092 Summary of the Invention [Problem to be solved by the invention]

[0004] The inventors of the present application realized that conventional lead zirconate titanate fibers (PZT fibers) had problems to be overcome and found it necessary to take measures to address these problems. Specifically, the inventors of the present application found the following problems:

[0005] For example, as shown in FIG. 11(A), a lead zirconate titanate fiber (PZT fiber) 100 described in Patent Document 1 and the like has a thin PZT layer 102 that can be formed by coating a metal wire 101 (a thin metal wire such as a titanium wire or a platinum wire) with lead zirconate titanate crystals (PZT crystals).

[0006] For example, PZT fiber can be manufactured by growing PZT crystals on the surface of a metal wire using hydrothermal synthesis. Alternatively, PZT fiber can be manufactured using extrusion molding. For example, as shown in Figure 13, in the extrusion molding method, PZT paste 105 (a mixture of PZT powder, binder, water, and in some cases organic solvents and various molding additives) is extruded simultaneously with metal wire 101 to produce a PZT fiber molded body with a metal core, and then this PZT fiber molded body is heated to remove the binder, and then sintered at a high temperature to produce a PZT fiber with a thin PZT layer formed on the surface of the metal wire.

[0007] In this way, the PZT fiber that can be manufactured by hydrothermal synthesis or extrusion molding has a structure in which the surface of the metal wire is simply coated with PZT crystals, and therefore the PZT thin layer 102 is easily cracked. For example, when used as a vibration sensor or actuator (particularly when used in the aircraft field), as shown in Figures 11(B) and (C), the PZT fiber 100 is partially embedded in a structure 202 made by laminating carbon fiber reinforced plastic (CFRP) prepregs 201 to reinforce it and used as a smart board 200 (see Figures 11(B) and (C)).

[0008] For example, when the smart board 200 is used as a vibration sensor or actuator, since the PZT fiber 100 is a piezoelectric material, when it detects vibration, it generates a potential and functions as a sensor, and conversely, when a potential is applied to the PZT fiber 100, the PZT fiber expands and contracts or vibrates according to the potential, and can function as an actuator. For example, as shown in FIG. 12(A), when the PZT fiber 100 extends along the axial direction indicated by the arrow by application of a potential, it can bend together with the structure 202 as shown in FIG. 12(B). In this way, in the smart board 200, a predetermined PZT fiber among the multiple PZT fibers 100 functions as a sensor to detect vibration, and another predetermined PZT fiber can operate as an actuator to suppress (damping) the vibration. Note that in FIG. 12, the portion below the dashed line of the PZT fiber 100 indicates that the PZT fiber 100 is embedded in the structure 202 (specifically, the CFRP prepreg 201) (see FIG. 11(C)).

[0009] When using a PZT fiber in a vibration sensor or actuator, the PZT fiber needs to have a certain degree of strength and flexibility. However, according to the contents of the Polymer Society, July issue (Vol. 57 No. 7, 2008), the strength (tensile strength or breaking elongation load) of a conventional PZT fiber is 4 kgf / mm 2 It was found that the fiber was easily broken, cut, and cracked, and that further improvement in strength was required.

[0010] 14, it was found that in a PZT fiber 300 in which a PZT film 302 is formed on a thin metal wire 301 such as platinum (Pt), delamination occurs between the PZT and the thin metal wire (Pt) due to the difference in thermal expansion coefficient, and the fiber is prone to cracking from the interface. This causes the fiber to have low physical strength.

[0011] The present invention has been made in view of the above problems. That is, a main object of the present invention is to provide a composite fiber that can function as a piezoelectric material and has improved strength compared to conventional PZT fibers. [Means for solving the problem]

[0012] The inventors of the present application attempted to solve the above problems by taking a new approach, rather than simply extending the conventional technology, and as a result, they came up with the invention of a composite fiber that achieves the above-mentioned main object.

[0013] The present invention provides a composite fiber that can be composed of at least a metal sintered body and a ceramic sintered body, in which the metal sintered body and the ceramic sintered body are adjacent to each other to form a fibrous body. Effect of the Invention

[0014] In the present invention, a composite fiber that can function as a piezoelectric material and has improved strength compared to conventional PZT fibers can be obtained. More specifically, delamination is significantly suppressed, and the tensile strength is 5 kgf / mm 2 More than 6kgf / mm 2 The above-mentioned composite fiber can be obtained. In addition, the composite fiber has flexibility, with a radius of curvature of 200 mm or less, preferably 10 mm or less, when bent. Note that the effects described in this specification are merely examples and are not limiting, and additional effects may be obtained. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram showing a composite fiber according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a cross section of adjacent metal sintered bodies and ceramic sintered bodies included in a composite fiber according to one embodiment of the present invention, in particular, a schematic cross-sectional view showing the interface between the metal sintered body and the ceramic sintered body. [Diagram 3] FIG. 3 is an electron microscope photograph showing the interface between a metal sintered body (Ni) composed of crystal grains and a ceramic sintered body (BT) also composed of crystal grains. [Figure 4] FIG. 4 is a schematic diagram showing a composite fiber according to another embodiment of the present invention. [Diagram 5]FIG. 5 is a schematic diagram showing a composite fiber according to another embodiment of the present invention. [Figure 6] FIG. 6(A) is a schematic perspective view showing a composite fiber according to another embodiment of the present invention, and FIG. 6(B) shows a cross section of the composite fiber of FIG. 6(A) taken along line YY'. [Figure 7] FIG. 7 is an electron microscope photograph showing a cross section of a composite fiber composed of a metal core (Ni), a first layer (Ni crystal grain layer), and a second layer (BaTiO3 crystal grain layer). [Figure 8] FIG. 8 is a schematic diagram showing an example of a method for producing a composite fiber. [Figure 9] FIG. 9 is an electron microscope photograph (5.0 kV, 2500x) showing a cross section of adjacent metal sintered body (Ni) and ceramic sintered body (BT) contained in the composite fiber produced in Example 1 of the present invention. [Figure 10] FIG. 10 is an electron microscope photograph (5.0 kV, 2500x) showing a cross section of adjacent metal sintered bodies and ceramic sintered bodies contained in the composite fiber produced in Comparative Example 1. [Figure 11] FIG. 11 is a schematic diagram showing a conventional PZT fiber and a smart board in which a PZT fiber is embedded in a structure. [Figure 12] FIG. 12 is a schematic diagram showing a conventional smart board used as a vibration sensor and an actuator. [Figure 13] FIG. 13 is a schematic diagram showing an example of a conventional method for producing a PZT fiber. [Figure 14] FIG. 14 is a schematic diagram showing a conventional PZT fiber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention relates to composite fibers, and more specifically, to composite fibers that can be composed or formed of at least a "metal sintered body" and a "ceramic sintered body", in which the metal sintered body and the ceramic sintered body are adjacent to each other to form a fibrous body (hereinafter, sometimes referred to as "the composite fiber of the present disclosure" or simply "composite fiber" or "fiber").

[0017] The composite fibers of the present disclosure generally have higher strength than piezoelectric fibers such as conventional PZT fibers. Conventional PZT fibers have a structure in which a "metal wire" is simply coated with "PZT crystals," and therefore have a strength of 4 kgf / mm 2 It has only about the same strength (tensile strength, breaking elongation load), and as described above, it causes delamination and easily breaks when used alone. When using such a PZT fiber in a vibration sensor or actuator, the PZT fiber must be reinforced with a structure such as a carbon fiber reinforced plastic (CFRP) prepreg, as shown in Figure 11(B).

[0018] However, as described in detail below, the composite fiber of the present disclosure has a structure in which the "metal sintered body" and the "ceramic sintered body" are adjacent to each other to form a fibrous body. 2 More than 6kgf / mm 2 It is possible to provide the above strength (tensile strength, breaking elongation load, etc.).

[0019] Furthermore, such an increase in strength enables the composite fiber to be made thinner, so that when bent, the composite fiber of the present disclosure has a smaller radius of curvature than conventional PZT fibers, and can exhibit flexibility such as a radius of curvature of, for example, 200 mm or less, preferably 10 mm or less.

[0020] Thus, the composite fiber of the present disclosure has superior properties such as strength and flexibility compared to conventional PZT fibers. Such properties are due to the structure in which a "metal sintered body" and a "ceramic sintered body" are adjacent to each other to form a "fibrous body," and in particular, the structure in which the "metal sintered body" and the "ceramic sintered body" are bonded to each other by co-sintering. Note that the present invention and its effects are not limited to a specific theory.

[0021] (Composite Fiber) The term "composite fiber" generally refers to a fiber that may be composed of two or more different materials, and in the present disclosure, the composite fiber refers to a fiber that comprises at least a "metal sintered body" and a "ceramic sintered body."

[0022] In the present disclosure, the term "fibrous body" (or "composite fiber" or "fiber") refers to an object or article having an elongated shape, and there is no particular limit to its length. In the present disclosure, there is no particular limit to the shape of the "fibrous body", particularly the cross-sectional shape, and the cross section may be, for example, circular, elliptical, rectangular, or irregular.

[0023] In the present disclosure, the term "metal sintered body" refers to a metal or alloy, preferably a metal element, formed by sintering at least the "metal component" described below. In other words, the "metal component" can be said to be a component that can constitute the "metal sintered body". Alternatively, the "metal component" can be said to be a component that can be included in the "metal sintered body".

[0024] In the present disclosure, the "metal component" is not particularly limited as long as it is a component (element) that can constitute a metal (preferably a simple metal), and is, for example, at least one selected from the group consisting of silver (Ag), palladium (Pd), copper (Cu), aluminum (Al), chromium (Cr), titanium (Ti), platinum (Pt), iron (Fe) and nickel (Ni) (hereinafter, sometimes referred to as "metal element"). In the composite fiber of the present disclosure, the metal component is preferably nickel or copper.

[0025] In the composite fiber of the present disclosure, the metal sintered body is preferably nickel (metal element) or copper (metal element), and more preferably has a structure in which particles or crystal grains of nickel metal (element) or copper metal (element) are bonded to each other.

[0026] In the present disclosure, the term "ceramic sintered body" refers to a ceramic, preferably a ceramic crystal, formed by firing at least the "ceramic components" described below. In other words, the "ceramic components" can be said to be components that can constitute the "ceramic sintered body". Alternatively, the "ceramic components" can be said to be components that can be included in the "ceramic sintered body".

[0027] In the present disclosure, the term "ceramic component" is not particularly limited as long as it is a component (element) that can constitute a ceramic (ceramic crystal, particularly a metal oxide), and examples thereof include lithium (Li), sodium (Na), potassium (K), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), yttrium (Y), zirconium (Zr), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), boron (B), aluminum (Al), silicon (Si), and the like. The ceramic component is preferably titanium, barium, and oxygen. The ceramic component in the composite fiber of the present disclosure is preferably titanium, barium, and oxygen. The ceramic component is preferably titanium, barium, and oxygen, or bismuth, sodium, titanium, and oxygen. The ceramic component may contain a glass component, such as at least one selected from the group consisting of soda-lime glass, potash glass, borate glass, borosilicate glass, barium borosilicate glass, zinc borate glass, barium borate glass, bismuth borosilicate glass, bismuth zinc borate glass, bismuth silicate glass, phosphate glass, aluminophosphate glass, and zinc phosphate glass.

[0028] In the composite fiber of the present disclosure, the ceramic sintered body preferably contains crystal grains or microcrystals, and in particular, barium titanate (BaTiO3) (BT) or bismuth sodium titanate ((Bi 1 / 2 Na 1 / 2 )TiO3)(BNT), or more preferably glass.

[0029] A composite fiber according to an embodiment of the present invention is, for example, a composite fiber 10 that can be composed of at least a metal sintered body 1 and a ceramic sintered body 2, as shown in Fig. 1(A). Fig. 1(B) shows a schematic cross section of the composite fiber 10 (a cross section perpendicular to the axial direction of the fiber), and Fig. 1(C) shows a schematic cross section along X-X' in Fig. 1(B) (a cross section in the axial direction of the fiber).

[0030] 1 shows a composite fiber 10 in which a metal sintered body 1 and a ceramic sintered body 2, each having a substantially circular cross section, are arranged substantially concentrically. The cross section of the composite fiber of the present disclosure is not limited to a circular or concentric shape.

[0031] The metal sintered body 1 and the ceramic sintered body 2 may be integrally formed or manufactured as described below in detail. For example, it is preferable to integrally form or manufacture the metal sintered body 1 and the ceramic sintered body 2 by co-sintering the above-mentioned metal component and ceramic component. More specifically, the metal sintered body 1 and the ceramic sintered body 2 can be integrally formed or manufactured by forming a paste containing the above-mentioned metal component (metal element) and a paste containing the above-mentioned ceramic component (ceramic element) into a desired shape and then firing them by co-sintering.

[0032] The means for forming into the desired shape is not limited to the method using a paste, and the metal sintered body and the ceramic sintered body can also be formed and manufactured by a chemical vapor deposition method such as thermal CVD of the metal component (metal element) and the ceramic component (ceramic element) or a physical vapor deposition method such as sputtering.

[0033] For example, as shown in Fig. 1, the composite fiber of the present disclosure is characterized in that the metal sintered body and the ceramic sintered body are adjacent to each other (contacting, facing, or bonded to each other) to form a fiber body. With such a configuration, the composite fiber of the present disclosure can provide improved strength and flexibility, and an effect of suppressing delamination, compared to conventional PZT fibers.

[0034] More specifically, in the composite fiber of the present disclosure, a metal sintered body 1 and a ceramic sintered body 2 are disposed adjacent to each other, as shown in Fig. 2. The metal sintered body 1 and the ceramic sintered body 2 may be configured to form an interface 3.

[0035] In the present disclosure, the term "interface" refers to the boundary between an adjacent "metal sintered body" and an adjacent "ceramic sintered body".

[0036] The interface that may be formed between the metal sintered body and the ceramic sintered body may be composed of crystal grains. In this disclosure, "crystal grains" refers to irregularly shaped microcrystals of about 1 / 20,000th of a millimeter to 1 / 10th of a millimeter.

[0037] The metal sintered body may be composed of crystal grains of a metal (or a metal component) (see FIG. 3). In other words, the metal sintered body may be a polycrystalline body of a metal (or a metal component). There is no particular limit to the size of the crystal grains in the metal sintered body (hereinafter, sometimes referred to as the "grain size" of the metal crystal grains). The size of the crystal grains in the metal sintered body is, for example, 0.1 μm to 10 μm. Here, the size of the crystal grains in the metal sintered body means the maximum dimension of the crystal grains or crystallites in a cross-sectional view.

[0038] The size of the crystal grains contained in the metal sintered body may depend on the metal component, and for example, the grain size of the powder of the metal component before sintering is preferably 0.05 μm to 5 μm.

[0039] The ceramic sintered body may be composed of crystal grains of ceramic (or ceramic components) (see FIG. 3). In other words, the ceramic sintered body may be a polycrystalline body of ceramic (or ceramic components). There is no particular limit to the size of the crystal grains in the ceramic sintered body (hereinafter, may be referred to as the "grain size" of the ceramic crystal grains). The size of the crystal grains in the ceramic sintered body is, for example, 0.1 μm to 10 μm. Here, the size of the crystal grains in the ceramic sintered body means the maximum dimension of the crystal grains or crystallites in a cross-sectional view.

[0040] The size of the crystal grains that can be contained in the ceramic sintered body may depend on the ceramic components. For example, the grain size of the powder of the ceramic components before sintering is preferably 0.05 μm to 5 μm.

[0041] 2, the metal sintered body 1 is preferably composed of crystal grains of a metal (or a metal component), and the ceramic sintered body 2 is preferably composed of crystal grains of a ceramic (or a ceramic component). It is more preferable that both the metal sintered body 1 and the ceramic sintered body 2 are formed by co-sintering (see FIG. 3). This is because co-sintering allows crystal grains or microcrystals to be formed by crystal growth in both the metal sintered body and the ceramic sintered body.

[0042] In the composite fiber of the present disclosure, an interface may be formed between crystal grains that may constitute a metal sintered body and crystal grains that may constitute a ceramic sintered body (see FIG. 3). The boundaries of crystal grains are also called grain boundaries, and such grain boundaries may form the interface between the metal sintered body and the ceramic sintered body. Alternatively, the metal sintered body and the ceramic sintered body may form an interface so as to share a part of the grain boundary or the outline of the crystal grain. In this case, it is preferable that the crystal grains that can constitute the metal sintered body are crystal grains that can be formed by crystal growth of a metal (or a metal component) (see FIG. 3). It is preferable that the crystal grains that can constitute the ceramic sintered body are crystal grains that can be formed by crystal growth of ceramic (or ceramic component) (see FIG. 3). More preferably, crystal growth proceeds during the firing or co-sintering process of the metal and / or ceramic. These crystal growths can be more appropriately controlled by the firing temperature, heating rate, holding time, cooling rate, atmosphere, pressure, sintering aids, added elements, and the like.

[0043] In the composite fiber of the present disclosure, the interface may have "surface roughness". In particular, in the composite fiber of the present disclosure, when the interface may be formed from crystal grains, it is preferable that the interface has "surface roughness" (see Figures 2 and 3). In other words, the interface may have irregularities, particularly fine irregularities based on crystal grains, and such an interface may be nonlinear rather than linear in cross-sectional view (see Figures 2 and 3). In other words, the interface may have a shape like a broken line in cross-sectional view (see Figures 2 and 3).

[0044] In addition, such an interface is characterized by having no gaps or voids in cross-sectional view. Conventionally, the boundary between the metal and the ceramic is linear and has gaps in cross-sectional view, which causes problems such as delamination and insufficient strength. However, the composite fiber of the present disclosure can solve the problems of delamination and insufficient strength by the surface roughness of the interface, and thus the fine irregularities.

[0045] In this disclosure, "surface roughness" refers to the degree of unevenness of an interface, and is therefore also called "surface roughness" or "surface roughness", or sometimes simply called "roughness". "Surface roughness" can be defined, for example, by measuring the "linear roughness" in a cross-sectional view of the interface from an electron microscope photograph or the like. In this disclosure, "surface roughness" is a term that can be used interchangeably with "linear roughness".

[0046] Specifically, the difference in interface structure can be determined by calculating the line roughness of the interface between a metal sintered body and a ceramic sintered body, and the line roughness of the interface between a metal body and a ceramic sintered body, respectively. For example, a cross section of a sample of the composite fiber of the present disclosure is polished and then observed with an SEM. Three fields of view in which the line roughness of the interface can be determined are randomly selected from the SEM image. The straight line connecting the two intersection points between the end face of the field image extracted using image analysis software and the interface of the metal sintered body and the ceramic sintered body is defined as the center line, and the distance between the actual boundary and the center line is measured at 30 equally spaced points along the center line. The line roughness can be evaluated based on the average value and standard deviation of these distances.

[0047] A specific value (measured value) of the line roughness is, for example, 15 nm or more and 1000 nm or less, preferably 75 nm or more and 300 nm or less, and more preferably 100 nm or more and 300 nm or less. The standard deviation (SD) of the distance between the boundary and the center line is, for example, 12 nm or more and 500 nm or less, and preferably 50 nm or more and 150 nm or less.

[0048] For example, as shown in Figures 2 and 3, when a crystal grain of a metal sintered body and a crystal grain of a ceramic sintered body can form an interface, the same linear roughness can also be confirmed in the depth direction when viewed in cross section, so the interface can have surface roughness or unevenness that extends two-dimensionally or three-dimensionally.

[0049] The interface having such surface roughness can improve the adhesion between the metal sintered body and the ceramic sintered body, suppress delamination, and obtain a composite fiber with improved fracture strength. Furthermore, the presence of such crystal grains can obtain a structure in which the residual stress caused by the thermal history during the process is uniformly relaxed.

[0050] Such a crystal grain may be composed of a plurality or a number of crystallites, or may be composed of a single crystallite.

[0051] The metallic and ceramic components may be distinct or may be at least partially intermixed with each other.

[0052] The region near the interface may also contain an amorphous portion, and therefore may be amorphous, crystalline, or may contain both amorphous and crystalline portions.

[0053] In this disclosure, "amorphous" (sometimes referred to as "amorphous" or "amorphous") means not in a crystalline state.

[0054] In the present disclosure, the term "region in the vicinity of the interface" specifically means a region adjacent to the interface, for example, a region within a range of 1500 nm, preferably 500 nm, from the interface.

[0055] The metal sintered body and the ceramic sintered body may contain impurities that originate or exist in the raw materials, sintering aids, components that may be contained in co-materials, etc. Such components may be present in an amount of less than 5%.

[0056] The presence or absence of crystal grains can be determined by observing the contrast difference due to differences in crystal orientation using a transmission electron microscope, scanning electron microscope, scanning ion microscope, or the like on an area including the target region. The crystallinity of the crystal grains can be evaluated by performing crystal structure analysis using X-ray diffraction or micro-X-ray diffraction over an area including the target region. Additionally, crystal structure analysis using X-ray diffraction or micro-X-ray diffraction can be used to determine whether a region of interest is crystalline, amorphous, or a mixture of both. Diffraction lines from crystalline materials can be detected as sharp peaks, while scattered light from amorphous materials can be detected as a halo (continuous).

[0057] In the composite fiber of the present disclosure, at least the metal sintered body and the ceramic sintered body are adjacent to each other, and the metal sintered body, which may be composed of crystal grains of a metal (or metal component), and the ceramic sintered body, which may be composed of crystal grains of a ceramic (or ceramic component), form an interface having surface roughness, particularly an interface having two-dimensional or three-dimensional unevenness formed by co-sintering, thereby making it possible to alleviate stress concentration that may occur between the metal sintered body and the ceramic sintered body. As a result, it is possible to suppress interlayer peeling that may occur between the metal sintered body and the ceramic sintered body, and to further improve the bonding strength between the metal sintered body and the ceramic sintered body.

[0058] This in turn makes it possible to improve (increase) the strength (breaking strength, particularly tensile strength or breaking elongation load) of the composite fiber. Furthermore, in the composite fiber of the present disclosure, the presence of an interface having complex irregularities that may be composed of such crystal grains makes it possible to suppress delamination, and by further improving the strength of the composite fiber, it becomes possible to reduce the diameter (size) of the composite fiber, which in turn makes it possible to improve the flexibility of the composite fiber of the present disclosure. Note that the mechanism by which the strength and flexibility of the composite fiber of the present disclosure are improved is not limited to the above theory.

[0059] In the composite fiber of the present disclosure, the tensile strength (breaking elongation load) of the entire fiber is, for example, 5 kgf / mm 2 More than 6kgf / mm 2 More preferably, 10kgf / mm 2More preferably, 14kgf / mm 2 or more than 20kgf / mm 2 More than 50kgf / mm 2 More than 400kgf / mm 2 or less, providing significantly improved strength over conventional PZT fibers.

[0060] In the composite fiber of the present disclosure, the tensile strength (breaking elongation load) preferably increases in the following order: ceramic sintered body<composite fiber<metal sintered body.

[0061] The composite fiber of the present disclosure has flexibility, for example, a radius of curvature of 200 mm or less, and can exhibit improved flexibility compared to conventional PZT fibers. Here, "radius of curvature" refers to the radius of curvature immediately before the composite fiber of the present disclosure breaks or breaks when the composite fiber is bent, for example, by hand. At the same time, the composite fiber of the present disclosure preferably maintains its electrical properties.

[0062] The fiber diameter of the composite fiber of the present disclosure is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less, and can achieve a smaller diameter (smaller size) than conventional PZT fibers. Here, the "fiber diameter" of the composite fiber of the present disclosure means the maximum dimension (e.g., diameter) in the cross section in the direction perpendicular to the axial direction of the fiber.

[0063] In the composite fiber of the present disclosure, the cross-sectional area ratio (metal / ceramic) of the metal sintered body to the ceramic sintered body is not particularly limited and is, for example, 1 / 99 to 99 / 1, and preferably 1 / 8 to 8 / 1. In the composite fiber of the present disclosure, the weight ratio of the metal sintered body to the ceramic sintered body (metal / ceramic) is not particularly limited and is, for example, 1 / 99 to 99 / 1, and preferably 1 / 8 to 8 / 1.

[0064] Here, in the composite fiber 10 according to one embodiment of the present invention shown in FIG. 1, the metal sintered body 1 is positioned at the "center" of the fiber 10 (in other words, the "center" of the fiber 10 is composed of the metal sintered body 1). Also, in the embodiment shown in FIG. 1, the ceramic sintered body 2 is positioned at the "outer portion" of the fiber 10 (in other words, the "outer portion" of the fiber 10 is composed of the ceramic sintered body 2). In such an embodiment, since the "center" of the composite fiber has metallic properties, the "center" can be electrically connected. Note that the composite fiber of the present disclosure is not limited to the embodiment shown in FIG. 1.

[0065] In the present disclosure, the "center" of a fiber means a portion that includes the geometric center of the fiber in a cross section perpendicular to the axial direction of the fiber. The term "outer portion" refers to the outermost portion of the fiber in a cross section perpendicular to the axial direction of the fiber. Between the "outer portion" and the "central portion" there may further be an "intermediate portion".

[0066] In the present disclosure, the "central portion", the "outer portion" and the "middle portion" may each independently be composed of a "metal sintered body" or a "ceramic sintered body". However, the "metal sintered body" and the "ceramic sintered body" are preferably positioned adjacent to each other according to the present disclosure.

[0067] According to another embodiment of the composite fiber of the present invention, the ceramic sintered body may be located in the center of the composite fiber, and the metal sintered body may be located on the outer part of the composite fiber. In such an embodiment, the outer part of the composite fiber may be electrically connected.

[0068] According to yet another embodiment of the composite fiber of the present invention, the core of the composite fiber may be made of a metal sintered body. In this case, at least a part of the outer part of the composite fiber may be made of a ceramic sintered body. In such an embodiment, the core of the composite fiber may be electrically connected to the outside.

[0069] In the present disclosure, "at least a portion of the outer portion" means at least a portion of the composite fiber in the axial direction and / or at least a portion of the composite fiber in the circumferential direction. The composite fiber of the present disclosure may be constituted or covered by the outer portion in a range of 0 to 100% (but not including 0%), preferably 50 to 100%, in any direction.

[0070] According to another embodiment of the composite fiber of the present invention, the central part of the composite fiber may be made of a ceramic sintered body. In this case, at least a part of the outer part of the composite fiber may be made of a metal sintered body. In such an embodiment, the outer part of the composite fiber may be electrically connected to the outside.

[0071] According to yet another embodiment of the composite fiber of the present invention, the central part of the composite fiber may be made of a metal sintered body. In this case, the outer part of the composite fiber may also be independently made of a metal sintered body, and the intermediate part that may be disposed between the central part and the outer part may be made of a ceramic sintered body. In such an embodiment, the central part and / or the outer part of the composite fiber may be electrically connected to the outside.

[0072] In any of the above embodiments, it is preferable that the metal sintered body and the ceramic sintered body are positioned adjacent to each other. As long as such a positional relationship is satisfied, the composite fiber of the present disclosure can have various types of multi-layer structures.

[0073] (electrode structure) As another embodiment, the composite fiber of the present disclosure may have an electrode structure as shown in Fig. 4. By having the composite fiber of the present disclosure have an electrode structure, the composite fiber of the present disclosure can be used as a material for electronic components, particularly as an electronic component element.

[0074] (a) For example, the composite fiber 20 shown in Fig. 4(a) has a substantially circular cross section, and has a structure in which a central portion 21 and an outer portion 22 are arranged substantially concentrically. Note that the cross-sectional shape of the composite fiber 20 is not limited to a circular or concentric shape. In the composite fiber 20, one of the central portion 21 and the outer portion 22 may be composed of one of the "metal sintered body" and the "ceramic sintered body", and the other of the central portion 21 and the outer portion 22 may be composed of the other of the "metal sintered body" and the "ceramic sintered body". In the composite fiber 20, the "metal sintered body" and the "ceramic sintered body" are preferably positioned adjacent to each other. Fiber diameter D shown in the cross-sectional view (axial cross-sectional view) of Figure 4(a) (bottom) showing the cross section at A-A' in Figure 4(a) (top) a (maximum dimension or maximum diameter) is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less.

[0075] (b) The composite fiber 30 shown in Fig. 4(b) has a structure in which an outer portion 32a having a substantially C-shaped (or substantially crescent-shaped) cross section and an outer portion 32b having a substantially inverted C-shaped (or substantially crescent-shaped) cross section (hereinafter, the outer portions 32a and 32b are collectively referred to as "outer portions 32") are arranged at a distance from each other around a center portion 31 having a substantially circular cross section. The cross-sectional shape of the composite fiber 30 is not limited to the shape shown in the figure. In the composite fiber 30, one of the central portion 31 and the outer portion 32 is composed of one of a "metal sintered body" and a "ceramic sintered body", and the other of the central portion 31 and the outer portion 32 is composed of the other of a "metal sintered body" and a "ceramic sintered body". In the composite fiber 30, the "metal sintered body" and the "ceramic sintered body" are preferably positioned adjacent to each other. The "metal sintered body" or the "ceramic sintered body" included in the outer portion 32 may be the same or different in the outer portions 32a and 32b. Fiber diameter D shown in the cross-sectional view (axial cross-sectional view) of Figure 4(b) (bottom) showing the cross section at B-B' in Figure 4(b) (top) b(maximum dimension or maximum diameter) is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less.

[0076] (c) 4(c) has a structure in which an outer portion 42 having a substantially C-shaped (or substantially crescent-shaped) cross section is disposed in a part of a central portion 41 having a substantially circular cross section. Note that the cross-sectional shape of the composite fiber 40 is not limited to the shape shown in the figure. In the composite fiber 40, one of the central portion 41 and the outer portion 42 is composed of one of the “metal sintered body” and the “ceramic sintered body”, and the other of the central portion 41 and the outer portion 42 is composed of the other of the “metal sintered body” and the “ceramic sintered body”. In the composite fiber 40, the “metal sintered body” and the “ceramic sintered body” are preferably positioned adjacent to each other. Fiber diameter D shown in the cross-sectional view (axial cross-sectional view) in Figure 4(c) (bottom) showing the cross section at C-C' in Figure 4(c) (top) c (maximum dimension or maximum diameter) is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less.

[0077] (d) 4(d) has a substantially circular cross section, and has a structure in which a central portion 51, an outer portion 52, and an intermediate portion 53 disposed between the central portion 51 and the outer portion 52 are arranged substantially concentrically. Note that the cross-sectional shape of the composite fiber 50 is not limited to a circular or concentric shape. In the composite fiber 50, the central portion 51 and the outer portion 52 are both made of one of the “metal sintered body” and the “ceramic sintered body”, and the middle portion 53 is made of the other of the “metal sintered body” and the “ceramic sintered body”. In the composite fiber 50, the “metal sintered body” and the “ceramic sintered body” are preferably positioned adjacent to each other. Fiber diameter D shown in the cross-sectional view (axial cross-sectional view) of Figure 4(d) (bottom) showing the cross section at D-D' in Figure 4(d) (top) d (maximum dimension or maximum diameter) is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less.

[0078] For example, in the above embodiments (a) and (c), it is preferable that the "center" of the fiber is made of a "metal sintered body" and the "outer" of the fiber is made of a "ceramic sintered body." With this configuration, the center of the fiber can function as an electrode.

[0079] For example, in the above embodiments (b) and (c), it is preferable that the "center" of the fiber is made of a "ceramic sintered body" and the "outer part" of the fiber is made of a "metal sintered body." With this configuration, the outer part of the fiber can function as an electrode.

[0080] For example, in the above embodiment (d), it is preferable that the "center" of the fiber is made of a "metal sintered body", the "outer part" of the fiber is also independently made of a "metal sintered body", and the "middle part" is made of a "ceramic sintered body". It is more preferable that the "metal sintered body" of the "center" and the "outer part" are the same. With such a configuration, the center and / or the outer part of the fiber can function as an electrode.

[0081] (Other embodiments) Other embodiments of the composite fiber of the present disclosure include, for example, a form in which a metal sintered body and a ceramic sintered body are adjacent to each other in the axial direction of the fiber as shown in FIG. 5(A), and a form in which a metal sintered body and a ceramic sintered body are adjacent to each other in a sandwich structure as shown in FIG. 5(B).

[0082] In the embodiment shown in Fig. 5(A), for example, it is preferable that a first end 61 in the axial direction of a composite fiber 60 is made of a "metal sintered body", a second end 62 on the opposite side facing the first end is also independently made of a "metal sintered body", and a connection part 63 that can be disposed between the first end 61 and the second end 62 is made of a "ceramic sintered body". By adopting such a configuration, both ends (61, 62) of the fiber can function as electrodes. Moreover, the first end portion 61 and the second end portion 62 may each be independently made of a "ceramic sintered body", and the connection portion 63 may be made of a "metal sintered body". Alternatively, in the above embodiment, the connection portion 63 may have a configuration in which the "metal sintered body" and the "ceramic sintered body" are alternately and continuously arranged.

[0083] In the embodiment shown in Fig. 5(B), for example, in a cross section in the axial direction or in a direction perpendicular to the axial direction of the composite fiber 70, the middle part (middle layer) 73 of the composite fiber is preferably made of a "metal sintered body", and the upper part (upper layer) 71 and the lower part (lower layer) 72 of the composite fiber 70 are each independently made of a "ceramic sintered body". With such a configuration, the middle part (middle layer) 73 of the fiber can function as an electrode. In the illustrated embodiment, the cross section of the fiber is substantially rectangular (quadrilateral), but is not limited to such a cross-sectional shape. Alternatively, the middle part (middle layer) 73 of the composite fiber 70 may be made of a "ceramic sintered body", and the upper part (upper layer) 71 and the lower part (lower layer) 72 of the composite fiber 70 may each be independently made of a "metal sintered body". By adopting such a configuration, the upper and lower parts (upper and lower layers) (71, 72) of the fiber can function as electrodes.

[0084] The conjugate fiber of the present disclosure is not limited to the above embodiment. A method for producing the conjugate fiber of the present disclosure will be briefly described below.

[0085] (Method of producing composite fiber of the present disclosure) In the composite fiber of the present disclosure, it is preferable that at least the "metal sintered body" and the "ceramic sintered body" are integrally formed or manufactured adjacent to each other, for example, by co-sintering. By forming the "metal sintered body" and the "ceramic sintered body" adjacent to each other integrally, it is possible to form an interface, particularly an interface having complex irregularities that may be constituted by the crystal grains of the metal component and the crystal grains of the ceramic component, and in particular an interface having the above-mentioned surface roughness.

[0086] There are no particular limitations on the method for producing the composite fiber of the present disclosure, and the composite fiber of the present disclosure can be produced as appropriate by applying a conventionally known ceramic firing technique or the like.

[0087] For example, a composite fiber in which a metal sintered body and a ceramic sintered body are integrally formed adjacent to each other can be produced by preparing a paste of raw materials containing the above-mentioned metal components (metal elements) together with sintering aids, co-materials, binder resins, solvents, dispersants, plasticizers, etc. as necessary, and a paste of raw materials containing the above-mentioned ceramic components (ceramic elements) together with sintering aids, co-materials, binder resins, solvents, dispersants, plasticizers, etc. as necessary, and then appropriately molding and co-firing the materials. At this time, each paste may be molded into a desired shape using, for example, a multiple nozzle (a composite spinning nozzle such as a double nozzle or triple nozzle) or a molding die.

[0088] When the paste for a metal sintered body and the paste for a ceramic sintered body are formed into fibers using a multiple nozzle, such as a double nozzle, other materials, such as a "metal not composed of crystalline grains" and / or a "ceramic not composed of crystalline grains", may be used as the core portion or core.

[0089] The "metal not composed of crystal grains" that can be used as the core portion in the composite fiber of the present disclosure means, for example, a metal or alloy that is formed or manufactured in advance separately from the above-mentioned "metal sintered body" and "ceramic sintered body". In other words, it means a metal or alloy that is formed or manufactured before the co-sintering of the above-mentioned "metal sintered body" and "ceramic sintered body". Therefore, a metal or alloy that can be formed or manufactured by sintering at the same time as the co-sintering of the above-mentioned "metal sintered body" and "ceramic sintered body" does not fall under the category of "metal not composed of crystal grains". As the "metal not composed of crystal grains" that can be used as the core portion, for example, a commercially available metal or alloy wire, particularly a metal or alloy wire manufactured by rolling, etc., may be used. More specifically, a nickel wire, a copper wire, etc. may be used.

[0090] The "ceramic not composed of crystal grains" that can be used as the core portion in the composite fiber of the present disclosure means, for example, a ceramic that is formed or manufactured in advance separately from the above-mentioned "metal sintered body" and "ceramic sintered body". In other words, it means a ceramic that is formed or manufactured before the co-sintering of the above-mentioned "metal sintered body" and "ceramic sintered body". Therefore, a ceramic that can be formed or manufactured by sintering at the same time as the co-sintering of the above-mentioned "metal sintered body" and "ceramic sintered body" does not fall under the category of "ceramic not composed of crystal grains". As the "ceramic not composed of crystal grains", for example, commercially available ceramic fibers, etc., may be used. More specifically, glass fibers, etc. may be used.

[0091] For example, as shown in FIG. 6(A), the composite fiber of the present disclosure may include a core portion (C), a first layer (11) covering the core portion (C), and a second layer (12) covering the first layer (11).

[0092] More specifically, as shown in FIG. 6(A), the composite fiber of the present disclosure includes a core portion (C), a first layer (11) covering the core portion (C), and a second layer (12) covering the first layer (11), wherein the core portion (C) includes a "metal not composed of crystal grains", the first layer (11) includes a "metal sintered body", specifically the metal sintered body composed of metal crystal grains, and the second layer (12) includes a "ceramic sintered body", specifically the ceramic sintered body composed of ceramic crystal grains. In such composite fibers, the first layer, which may be made of a "metal sintered body," and the second layer, which may be made of a "ceramic sintered body," may both be made of crystal grains, forming an interface having the above-mentioned surface roughness and bonding to each other, thereby improving the strength of the fiber. Furthermore, the strength of the fiber may be further improved by making the core portion (C) a "metal not made of crystal grains," more specifically, a metal wire. In this case, by making the first layer out of a "metal sintered body," the bonding force with the core portion (C) may be further improved, and the strength of the composite fiber may be significantly improved.

[0093] As an example, FIG. 7 shows a composite fiber that uses a nickel wire (metallic Ni core) as the core portion, has a first layer which is a nickel (Ni) crystal grain layer, and a second layer which is a barium titanate (BaTiO3) crystal grain layer (see Example 13).

[0094] For example, as shown in FIG. 6(A), the composite fiber of the present disclosure may include a core portion (C), a first layer (11) covering the core portion (C), and a second layer (12) covering the first layer (11), in which the core portion (C) includes a "ceramic not composed of crystal grains", the first layer (11) includes a "ceramic sintered body", specifically the ceramic sintered body composed of ceramic crystal grains, and the second layer (12) includes a "metal sintered body", specifically the metal sintered body composed of metal crystal grains. In such composite fibers, the first layer, which may be made of a "ceramic sintered body," and the second layer, which is made of a "metal sintered body," may both be made of crystal grains, forming an interface having the above-mentioned surface roughness and bonding to each other, thereby improving the strength of the fiber. Furthermore, the strength of the fiber may be further improved by including a "ceramic not made of crystal grains" in the core portion (C), more specifically, a ceramic fiber. In this case, by making the first layer out of a "ceramic sintered body," the bonding force with the core portion (C) may be further improved, and the strength of the composite fiber may be significantly improved.

[0095] Composite fibers with this structure can be manufactured, for example, by using a dual nozzle in a conventional device used in the extrusion molding method shown in Figure 13 to mold a paste for a sintered metal body and a paste for a sintered ceramic body into a concentric shape with a core portion (C) as a nucleus.

[0096] In the composite fiber of the present disclosure, for example, the second layer (12) shown in FIG. 6 may be a "grainless metal" and / or a "grainless ceramic".

[0097] When the second layer (12) is a "metal not composed of crystal grains", the second layer (12) may be a plated layer, a vapor-deposited film, or a sputtered film of a metal or alloy.

[0098] When the second layer (12) is a "ceramic not composed of crystal grains", the second layer (12) may be a ceramic coating layer, a vapor deposition film, or a sputtered film.

[0099] For example, as shown in FIG. 6(A), the composite fiber of the present disclosure includes a core portion (C), a first layer (11) covering the core portion (C), and a second layer (12) covering the first layer (11), in which the core portion (C) includes a "ceramic sintered body", specifically, the ceramic sintered body composed of ceramic crystal grains, the first layer (11) includes a "metal sintered body", specifically, a metal sintered body composed of metal crystal grains, and the second layer (12) includes a "metal not composed of crystal grains." In such composite fibers, the core portion, which may be made of a "ceramic sintered body," and the first layer, which may be made of a "metal sintered body," may both be made of crystal grains, forming an interface having the above-mentioned surface roughness and bonding to each other, thereby improving the strength of the fiber. Furthermore, the second layer (12) may contain a "metal not made of crystal grains," which may further improve the strength of the fiber. In this case, by making the first layer out of a "metal sintered body," the bonding force with the second layer (12) may be further improved, and the strength of the composite fiber may be significantly improved.

[0100] For example, as shown in FIG. 6(A), the composite fiber of the present disclosure includes a core portion (C), a first layer (11) covering the core portion (C), and a second layer (12) covering the first layer (11), in which the core portion (C) includes a "metal sintered body", specifically the metal sintered body composed of metal crystal grains, the first layer (11) includes a "ceramic sintered body", specifically the ceramic sintered body composed of ceramic crystal grains, and the second layer (12) includes a "ceramic not composed of crystal grains." In such composite fibers, the core portion, which may be made of a "metal sintered body," and the first layer, which may be made of a "ceramic sintered body," may both be made of crystal grains, forming an interface having the above-mentioned surface roughness and bonding to each other, thereby improving the strength of the fiber. Furthermore, the second layer (12) may contain a "ceramic not made of crystal grains," which may further improve the strength of the fiber. In this case, by making the first layer out of a "ceramic sintered body," the bonding force with the second layer (12) may be further improved, and the strength of the composite fiber may be significantly improved.

[0101] There is no particular limitation on the ratio of the thickness of the core portion (C), the first layer (11) and the second layer (12), and it may be appropriately determined according to the desired application. The total thickness or diameter (maximum dimension or maximum diameter) of the composite fiber is, for example, 500 μm or less, preferably 1 μm or more and 500 μm or less.

[0102] The composite fiber of the present disclosure can also be produced by a lamination technique such as a printing method such as a screen printing method, a green sheet method using a green sheet, or a combination method thereof. When using such a lamination technique, the composite fiber of the present disclosure may be produced by appropriately fiberizing the laminate before or after firing by cutting (see, for example, FIG. 8).

[0103] The method for producing the conjugate fiber of the present disclosure is not limited to the above. The conjugate fiber of the present disclosure will be described in more detail below with reference to examples. EXAMPLES

[0104] Examples 1 to 10 (1) Preparation of paste for sintered metal The paste for metal sintered body is composed of Ni powder, perovskite oxide containing Ba and Ti as co-materials, polycarboxylic acid dispersant, binder resin, and organic solvent. The average particle size of the Ni powder used is 0.2 μm. The average particle size of the perovskite oxide containing Ba and Ti is 30 nm. For example, a resin solution in which a resin is dissolved in butyl carbitol is used as the binder resin. For example, ethyl cellulose, cellulose acetate butyrate, etc. are used as the resin dissolved in butyl carbitol. In preparing the paste for metal sintered body, 50 parts by weight of Ni powder, 5 parts by weight of perovskite oxide containing Ba and Ti as co-materials, a resin solution in which 10 parts by weight of ethyl cellulose is dissolved in butyl carbitol, 1 part by weight of polycarboxylic acid dispersant, and the remainder butyl carbitol are mixed, and the paste for metal sintered body is prepared by a ball mill.

[0105] (2) Preparation of paste for sintered ceramics The paste for sintered ceramics is composed of perovskite oxide containing Ba and Ti, polyvinyl butyral binder resin, plasticizer, and organic solvent such as toluene. The perovskite oxide containing Ba and Ti has an average particle size of 100 nm. To prepare the paste for sintered ceramics, 90 parts by weight of perovskite oxide containing Ba and Ti, 10 parts by weight of polyvinyl butyral binder resin, plasticizer, and toluene were mixed and the paste for sintered ceramics was prepared by ball milling.

[0106] As shown in FIG. 8, the above-mentioned paste for sintered ceramic body was applied to a supporting base (not shown) and dried to produce a first green sheet 81 for sintered ceramic body (FIG. 8(A)). The paste for a sintered metal body was laminated on a first green sheet for a sintered ceramic body 81 by printing to form a printed layer for a sintered metal body 82 (FIG. 8(B)). In the same manner as in the case of the green sheet 81 for the first ceramic sintered body, a green sheet 83 for a second ceramic sintered body was prepared from the paste for the ceramic sintered body and peeled off from the supporting base. After that, the green sheet 83 for the second ceramic sintered body was laminated on a printing layer 82 for a metal sintered body and pressure-bonded to prepare a laminate 80 (FIG. 8(C)). Next, the laminate 80 was cut into strips, for example, along the dashed lines shown in FIG. 8(C), to produce a "composite fiber precursor." The thicknesses of the first green sheet 81 for sintered ceramic body, the printed layer 82 for sintered metal body, and the second green sheet 83 for sintered ceramic body were as shown in Table 1 below (unit: μm).

[0107] [Table 1]

[0108] (Firing process) The "composite fiber precursor" was fired under the following conditions to produce a composite fiber as a fibrous body in which a "metal sintered body" and a "ceramic sintered body" were adjacent to each other. Firing conditions After degreasing in a nitrogen atmosphere at 400°C for 10 hours, the specimen was placed in a nitrogen-hydrogen-water vapor mixed atmosphere at a top temperature of 1200°C and an oxygen partial pressure of 10 -9 ~10 -10 The mixture was fired under the condition of MPa.

[0109] Fig. 8(D) shows a schematic cross section (cross section in the axial direction) of the composite fiber produced in Example 1. More specifically, Fig. 8(D) shows a structure in which nickel metal (Ni) (92) (center of cross section) formed as a metal sintered body is sandwiched between barium titanate (BaTiO3) (BT) (91, 93) (upper and lower parts of cross section) formed as a ceramic sintered body, with the metal sintered body and the ceramic sintered body adjacent to each other.

[0110] (Cross-section observation) The cross section (cross section in the axial direction) of the composite fiber of Example 1 prepared above was observed using an electron microscope (JCM-5700, manufactured by JEOL Ltd.) The electron microscope photograph of the cross section of the composite fiber is shown in Figure 9 (5.0 kV, 2500x).

[0111] The electron microscope photograph in Figure 9 shows that the Ni thickness is 15.6 μm and the BaTiO3 (BT) thickness is 6.0 μm (Table 2). There was no peeling in the metal sintered body (Ni) and the ceramic sintered body (BaTiO3), and they were tightly bonded. Moreover, the Ni thickness and BaTiO3 thickness in Examples 2 to 10 are shown in Table 2 below (unit: μm).

[0112] [Table 2]

[0113] (Strength measurement) The tensile strength of the composite fibers produced in Examples 1 to 10 was measured using a strength tester (MST-1, manufactured by Shimadzu Corporation). The radius of curvature of the composite fibers produced in Examples 1 to 10 was also evaluated. Table 3 below shows the evaluation results of the tensile strength and radius of curvature of the composite fibers produced in Examples 1 to 10.

[0114] [Table 3]

[0115] In the composite fibers of Examples 1 to 10, the strength was 10 kgf / mm 2 It showed a tensile strength of or above and a radius of curvature of 15 mm or less.

[0116] Comparative Example 1 (composite fiber using nickel foil) (1) Preparation of nickel foil Instead of the paste for sintered metal, nickel foil with a thickness of 15 μm was purchased from Nilaco Corporation. (2) Preparation of paste for sintered ceramics A paste for sintered ceramic body was prepared in the same manner as in Examples 1 to 10.

[0117] As shown in FIG. 8, a paste for a sintered ceramic body was applied to a supporting base (not shown) and dried to produce a first green sheet 81 for a sintered ceramic body (FIG. 8(A)). Nickel foil was laminated on the first ceramic sintered body green sheet 81 as a substitute for the metal sintered body printing layer 82 (FIG. 8(B)). In the same manner as in the case of the green sheet 81 for the first ceramic sintered body, a green sheet 83 for a second ceramic sintered body was prepared from the paste for the ceramic sintered body and peeled off from the supporting base. After that, the green sheet 83 for the second ceramic sintered body was laminated on nickel foil and pressure-bonded to prepare a laminate 80 (FIG. 8(C)). Next, the laminate 80 was cut into strips, for example, along the dashed lines shown in FIG. 8(C), to produce a "composite fiber precursor." The thicknesses of the first sintered ceramic body green sheet 81, the nickel layer 82, and the second sintered ceramic body green sheet 83 were as shown in Table 4 below (unit: μm).

[0118] [Table 4]

[0119] (Firing process) The "composite fiber precursor" was fired under the following conditions to produce a composite fiber as a fibrous body consisting of a "nickel layer (metal foil layer)" and a "ceramic sintered body" adjacent to each other (i.e., a three-layered fibrous body consisting of a "ceramic sintered body (BT)", a "Ni layer (metal foil layer)", and a "ceramic sintered body (BT)" adjacent to each other). Firing conditions After degreasing in a nitrogen atmosphere at 400°C for 10 hours, the specimen was placed in a nitrogen-hydrogen-water vapor mixed atmosphere at a top temperature of 1200°C and an oxygen partial pressure of 10 -9 ~10 -10 The mixture was fired under the condition of MPa.

[0120] (Cross-section observation) The cross section (axial cross section) of the composite fiber prepared above was observed using an electron microscope (JCM-5700, manufactured by JEOL Ltd.) The electron microscope photograph of the cross section of the composite fiber is shown in Figure 10 (5.0 kV, 2500x magnification).

[0121] [Table 5]

[0122] As shown in Figure 10, the difference in thermal expansion coefficient caused stress in the BaTiO3 layer, resulting in the fracture of the BaTiO3 (BT) layer. The Ni-BaTiO3 (BT) layer also peeled off. This shows that the composite fiber of Comparative Example 1 does not physically function as a piezoelectric fiber.

[0123] (Strength measurement) The tensile strength of the composite fiber produced in Comparative Example 1 was measured using a strength tester (MST-1, manufactured by Shimadzu Corporation). The radius of curvature of the composite fiber produced in Comparative Example 1 was also evaluated. Table 6 below shows the evaluation results of the tensile strength and radius of curvature of the composite fiber of Comparative Example 1.

[0124] [Table 6]

[0125] The results shown in Table 6 reveal that the composite fiber of Comparative Example 1 has a tensile strength that is only about 60% of that of the composite fiber of Example 1.

[0126] Example 11 In the same manner as in Example 1, a composite fiber precursor having a circular cross section in which the paste for the metal sintered body and the paste for the ceramic sintered body were concentrically arranged through a double nozzle was produced using the paste for the metal sintered body and the paste for the ceramic sintered body (center: paste for the metal sintered body (Ni), outer part: paste for the ceramic sintered body (BT) with a cross-sectional area ratio (metal / ceramic): 1 / 1).

[0127] Next, the composite fiber precursor was fired under the same firing conditions as in Example 1 to produce a composite fiber having a circular cross section (fiber diameter: 90 μm) (center: metal sintered body (Ni), outer part: ceramic sintered body (BT)).

[0128] The strength of the composite fiber produced in Example 11 was measured in the same manner as in Example 1. The tensile strength of the composite fiber produced in Example 11 was 19.1 kgf / mm 2 It was. The radius of curvature of the composite fiber produced in Example 11 was 5 mm.

[0129] Example 12 A composite fiber precursor having a circular cross section in which the following pastes for a sintered metal body and pastes for a sintered ceramic body were concentrically arranged through a double nozzle was produced in the same manner as in Example 11, except that the following pastes for a sintered metal body and pastes for a sintered ceramic body were used (center: paste for a sintered metal body (Cu), outer part: paste for a sintered ceramic body (BNT), cross-sectional area ratio (metal (Cu) / ceramic (BNT)): 1 / 1).

[0130] (1) Preparation of paste for sintered metal The paste for metal sintered body is composed of Cu powder, a perovskite oxide containing Bi, Na, Ti as a co-material, a polycarboxylic acid dispersant, a binder resin, and an organic solvent. The average particle size of the Cu powder used is 0.2 μm. The average particle size of the perovskite oxide containing Bi, Na, Ti is 30 nm. As the binder resin, for example, a resin solution in which a resin is dissolved in butyl carbitol is used. As the resin dissolved in butyl carbitol, for example, ethyl cellulose, cellulose acetate butyrate, etc. are used. In preparing the paste for metal sintered body, 50 parts by weight of Cu powder, 5 parts by weight of a perovskite oxide containing Bi, Na, Ti as a co-material, a resin solution in which 10 parts by weight of ethyl cellulose is dissolved in butyl carbitol, 1 part by weight of a polycarboxylic acid dispersant, and the remainder butyl carbitol are mixed, and the paste for metal sintered body is prepared by a ball mill.

[0131] (2) Preparation of paste for sintered ceramics The paste for sintered ceramics is composed of perovskite oxides containing Bi, Na, and Ti, polyvinyl butyral binder resin, plasticizer, and organic solvent such as toluene. The perovskite oxides containing Bi, Na, and Ti have an average particle size of 100 nm. To prepare the paste for sintered ceramics, 90 parts by weight of perovskite oxides containing Bi, Na, and Ti, 10 parts by weight of polyvinyl butyral binder resin, plasticizer, and toluene were mixed, and the paste for sintered ceramics was prepared by ball milling.

[0132] Next, the composite fiber precursor was fired under the same firing conditions as in Example 1 to produce a composite fiber having a circular cross section (fiber diameter: 100 μm) (center: metal sintered body (Cu), outer part: ceramic sintered body (bismuth sodium titanate) (BNT)).

[0133] The strength of the composite fiber produced in Example 12 was measured in the same manner as in Example 1. The tensile strength of the composite fiber produced in Example 12 was 15.4 kgf / mm 2 It was. The radius of curvature of the composite fiber produced in Example 12 was 5 mm.

[0134] Example 13 Using the paste for metal sintered body (Ni) and paste for ceramic sintered body (BT) prepared in Example 1 and a nickel wire (diameter: 50 μm), the nickel wire (wire) was passed through a wire guide in the same manner as in the conventional method (see FIG. 13) (however, in this example, a double nozzle was used), and a composite fiber precursor having a circular cross section in which the paste for metal sintered body (Ni) and the paste for ceramic sintered body (BT) were concentrically arranged was produced (core part: Ni wire, first layer (inner part): paste for metal sintered body (Ni), second layer (outer part): paste for ceramic sintered body (BT), cross-sectional area ratio (Ni wire / Ni layer / BT layer): 0.70 / 0.30 / 1.0).

[0135] Next, the composite fiber precursor was fired under the same firing conditions as in Example 1 to produce a composite fiber having a circular cross section (fiber diameter: 88 μm) (core: metal Ni, first layer (inner part): metal sintered body (Ni), second layer (outer part): ceramic sintered body (BT)).

[0136] The strength of the composite fiber produced in Example 13 was measured in the same manner as in Example 1. The tensile strength of the composite fiber produced in Example 13 was 19.8 kgf / mm 2 It was. The radius of curvature of the composite fiber produced in Example 13 was 5 mm.

[0137] (Cross-section observation) The cross section (cross section perpendicular to the axial direction (axial cross section)) of the composite fiber produced in Example 13 was observed using an electron microscope (JCM-5700 manufactured by JEOL Ltd.). An electron microscope photograph of the cross section of the composite fiber is shown in Figure 7 (5.0 kV, 2500x magnification).

[0138] 7, it was found that there was no delamination or cracks at all in the composite fiber of Example 13. This shows that the composite fiber of Example 13 has high tensile strength and functions as a piezoelectric fiber.

[0139] Comparative Example 2 A composite fiber having a "Cu layer (metal foil layer)" and a "ceramic sintered body (BNT)" adjacent to each other, i.e., a three-layered fiber body having a "ceramic sintered body (BNT)", a "Cu layer (metal foil layer)", and a "ceramic sintered body (BNT)" adjacent to each other, was produced in the same manner as in Comparative Example 1, except that a 15 μm thick copper foil (manufactured by Nilaco) and the paste for sintered ceramic body prepared in Example 12 were used.

[0140] The strength of the composite fiber produced in Comparative Example 2 was measured in the same manner as in Example 1. The tensile strength of the composite fiber produced in Comparative Example 2 was 6.0 kgf / mm 2 It was. The radius of curvature of the composite fiber produced in Comparative Example 2 was 10 mm.

[0141] In the composite fiber produced in Comparative Example 2, as in the composite fiber produced in Comparative Example 1, stress was applied to the BNT layer due to the difference in thermal expansion coefficient, causing the BNT layer to break. In addition, peeling of the BMT layer also occurred. From these findings, it was found that the composite fiber of Comparative Example 2 did not function as a piezoelectric fiber.

[0142] (Determination of Line Roughness) The line roughness of the interface between the metal sintered body and the ceramic sintered body of the composite fiber produced in Example 3 and Comparative Example 1 was measured. The cross sections of the composite fibers prepared in Example 3 and Comparative Example 1 were polished and then observed with an SEM. The cross sections where the interface between the adjacent metal sintered body (Ni) and ceramic sintered body (BT) could be observed were observed with an SEM (15.0 kV, 5000x). Three fields of view where the interface could be identified were randomly extracted from the SEM images. Using image analysis software (Mitani Shoji Co., Ltd., WinROOF), the straight line connecting the two intersection points between the end face of the extracted field image and the interface between the metal sintered body and the ceramic sintered body was defined as the center line, and the distance between the actual boundary and the center line was measured at 30 points at equal intervals along the center line. The line roughness was evaluated based on the average value and standard deviation of these distances. The results are shown in Table 7 below.

[0143] [Table 7]

[0144] The conjugate fibers of the present disclosure are not limited to those illustrated in the above examples. [Industrial Applicability]

[0145] The composite fiber of the present disclosure can be used in sensors, particularly vibration sensors and actuators, used in structures such as buildings, automobiles, ships, and aircraft. The composite fiber of the present disclosure can also be used as an electronic component element. [Explanation of symbols]

[0146] 1. Metal sintered body 2. Sintered ceramics 3 Interface 10,20,30,40,50,60,70 Composite Fiber 11 1st layer 12 2nd layer C core part / core 21,31,41,51 Center 22,32,42,52 Outer part 53 Middle section 61 First end 62 Second end 63 Connection 71 Top 72 Lower 73 Chubu 80 Laminate 81 First ceramic sintered body green sheet 82 Printing layer for sintered metal bodies 83 Green sheet for second ceramic sintered body 90 Composite fiber (cross section) 91 Barium titanate (BaTiO3) (BT) 92 Nickel (Ni) 93 Barium titanate (BaTiO3) (BT) 100 PZT Fiber 101 Metal Wire / Thin Metal Wire 102 PZT thin layer / PZT film 103 Nozzle 104 Wire Guide 105 PZT paste 200 Smart Board 201 Carbon Fiber Reinforced Plastic (CFRP) Prepreg 202 Structure 300 PZT Fiber 301 Fine metal wire 302 PZT membrane

Claims

1. A composite fiber composed of at least a metal sintered body and a ceramic sintered body, the metal sintered body and the ceramic sintered body being adjacent to each other to form a fiber body, the metal sintered body and the ceramic sintered body form an interface, the interface has a surface roughness, the surface roughness is defined as a line roughness in a cross-sectional view of the interface, and the line roughness is 15 nm or more and 1000 nm or less; the metal sintered body is a simple metal sintered body, and the ceramic sintered body is a metal oxide ceramic sintered body, A composite fiber, wherein the metal sintered body is composed of metal crystal grains, and the ceramic sintered body is composed of ceramic crystal grains.

2. The composite fiber of claim 1 , wherein the interface is comprised of grains.

3. 3. The composite fiber according to claim 1, wherein an interface is formed between crystal grains constituting the metal sintered body and crystal grains constituting the ceramic sintered body.

4. The composite fiber according to any one of claims 1 to 3, wherein the crystal grains constituting the metal sintered body are crystal grains formed by crystal growth of a metal, and the crystal grains constituting the ceramic sintered body are crystal grains formed by crystal growth of a ceramic.

5. The composite fiber according to any one of claims 1 to 4, wherein the interface has no gaps in a cross-sectional view of the composite fiber.

6. The composite fiber according to any one of claims 1 to 5, wherein the metal sintered body is positioned at the center of the composite fiber.

7. The composite fiber according to any one of claims 1 to 5, wherein the ceramic sintered body is positioned at the center of the composite fiber.

8. The composite fiber according to any one of claims 1 to 5, wherein a central portion of the composite fiber is made of the metal sintered body, and at least a portion of an outer portion of the composite fiber is made of the ceramic sintered body.

9. The composite fiber according to any one of claims 1 to 5, wherein a central portion of the composite fiber is made of the ceramic sintered body, and at least a portion of an outer portion of the composite fiber is made of the metal sintered body.

10. A composite fiber according to any one of claims 1 to 5, wherein a central portion of the composite fiber is made of the metal sintered body, an outer portion of the composite fiber is also independently made of the metal sintered body, and an intermediate portion disposed between the central portion and the outer portion is made of the ceramic sintered body.

11. A composite fiber according to any one of claims 1 to 5, wherein a first end in the axial direction of the composite fiber is made of the metal sintered body, a second end opposite the first end is also independently made of the metal sintered body, and a connecting portion disposed between the first end and the second end is made of the ceramic sintered body.

12. A composite fiber according to any one of claims 1 to 5, wherein in a cross section in the axial direction or in a direction perpendicular to the axial direction of the composite fiber, a middle portion of the composite fiber is made of the metal sintered body, and an upper portion and a lower portion of the composite fiber are each independently made of the ceramic sintered body, or a middle portion of the composite fiber is made of the ceramic sintered body, and an upper portion and a lower portion of the composite fiber are each independently made of the metal sintered body.

13. The composite fiber according to any one of claims 1 to 4, wherein the composite fiber comprises a core portion, a first layer covering the core portion, and a second layer covering the first layer, the first layer comprising the metal sintered body composed of crystal grains of the metal, the second layer comprising the ceramic sintered body composed of crystal grains of the ceramic, and the core portion comprising a metal not composed of crystal grains.

14. The composite fiber according to any one of claims 1 to 4, wherein the composite fiber comprises a core portion, a first layer covering the core portion, and a second layer covering the first layer, the first layer comprising the ceramic sintered body composed of crystal grains of the ceramic, the second layer comprising the metal sintered body composed of crystal grains of the metal, and the core portion comprising a ceramic not composed of crystal grains.

15. The composite fiber according to any one of claims 1 to 4, wherein the composite fiber comprises a core portion, a first layer covering the core portion, and a second layer covering the first layer, the core portion comprising the ceramic sintered body composed of crystal grains of the ceramic, the first layer comprising the metal sintered body composed of crystal grains of the metal, and the second layer comprising a metal not composed of crystal grains.

16. The composite fiber according to any one of claims 1 to 4, wherein the composite fiber comprises a core portion, a first layer covering the core portion, and a second layer covering the first layer, the core portion comprising the metal sintered body composed of crystal grains of the metal, the first layer comprising the ceramic sintered body composed of crystal grains of the ceramic, and the second layer comprising a ceramic not composed of crystal grains.

17. The metal component constituting the metal sintered body is at least one selected from the group consisting of silver (Ag), palladium (Pd), copper (Cu), aluminum (Al), chromium (Cr), titanium (Ti), platinum (Pt), iron (Fe) and nickel (Ni). The composite fiber according to any one of claims 1 to 16.

18. The composite fiber according to any one of claims 1 to 17, wherein the metal sintered body is nickel metal alone or copper metal alone.

19. The ceramic component constituting the ceramic sintered body is oxygen (O) and at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), yttrium (Y), zirconium (Zr), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), aluminum (Al), indium (In), tin (Sn), antimony (Sb), barium (Ba), tantalum (Ta), tungsten (W), lead (Pb), bismuth (Bi), lanthanum (La), cesium (Ce), neodymium (Nd), samarium (Sm), gadolinium (Gd), dysprosium (Dy), holmium (Ho) and erbium (Er). The composite fiber according to any one of claims 1 to 18.

20. The composite fiber according to any one of claims 1 to 19, wherein the ceramic sintered body is barium titanate or bismuth sodium titanate.

21. The tensile strength of the composite fiber is 5 kgf / mm 2 Over 400kgf / mm 2 The conjugate fiber according to any one of claims 1 to 20, wherein:

22. The conjugate fiber according to any one of claims 1 to 21, having flexibility such that the radius of curvature is 3 mm or more and 200 mm or less.

23. The composite fiber according to any one of claims 1 to 22, wherein the fiber diameter of the composite fiber is 1 µm or more and 500 µm or less.

Citation Information

Patent Citations

  • Process for production of silicone carbide fiber reinforced steel comp osite material

    JP1977018409A

  • Manufacture of metallic fiber porous body

    JP1989215909A

  • Zirconic composite ceramic sintered compact and its production

    JP1996012425A

  • Multifunctional composite structure

    JP2005512311A

  • Metal and ceramic nanofiber

    JP2018104878A