Urethane foam molded body

The urethane foam molded article with aligned expanded graphite and magnetic particles addresses the challenge of achieving high thermal conductivity and flame retardancy, optimizing heat transfer and fire resistance.

JP2024144866APending Publication Date: 2024-10-15SUMITOMO RIKO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023057017
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing soundproofing materials face challenges in achieving high thermal conductivity and flame retardancy, with methods like using expanded graphite alone not sufficiently enhancing thermal conductivity, and the addition of magnetic particles impairing flame retardancy.

Method used

A urethane foam molded article with composite particles containing expanded graphite and magnetic particles aligned in a base material, where expanded graphite particles contribute to thermal conductivity and flame retardancy, and magnetic particles enhance orientation for improved heat transfer.

Benefits of technology

The article achieves excellent thermal conductivity and flame retardancy by aligning composite particles, ensuring each component's effect is maximized without interference, suitable for applications requiring both properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144866000001
    Figure 2024144866000001
Patent Text Reader

Abstract

To provide a urethane foam molded body with excellent thermal conductivity and flame retardancy.SOLUTION: A urethane foam molded body includes a substrate made of polyurethane foam and composite particles contained and oriented in the substrate. The composite particles include first composite particles containing expandable graphite particles and magnetic particles bonded to the surfaces of the expandable graphite particles with a binder, and second composite particles containing expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles with a binder. When the total mass of the expandable graphite particles and the expanded graphite particles in the substrate of the urethane foam molded body is defined as 100 mass%, the content of the expandable graphite particles is 20 mass% or more and 80 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a urethane foam molded article having high thermal conductivity. [Background technology]

[0002] In automobiles and other vehicles, measures are taken to reduce noise generated by engines, transmissions, etc., in order to reduce noise leaking outside the vehicle or into the passenger compartment. In electric vehicles (EVs) and hybrid electric vehicles (HEVs), the driving noise of the electric powertrain, which consists of inverters, motors, gearboxes, etc., is also a target for reduction. Soundproofing materials made of foams such as polyurethane foam are used as noise countermeasures. Foams have a low thermal conductivity because they have many cells (air bubbles) inside. For this reason, if they are placed around a noise source that generates heat, heat may accumulate and cause malfunctions.

[0003] From the viewpoint of improving the heat dissipation of a soundproofing material using a foam, for example, Patent Document 1 describes a polyurethane foam molded body in which composite particles, in which thermally conductive particles, magnetic particles, and insulating inorganic particles are combined, are oriented and arranged in a polyurethane foam, and a heat transfer path is formed in the orientation direction, thereby improving the heat dissipation. Expanded graphite and the like are described as thermally conductive particles. Patent Document 2 describes a polyurethane foam containing a thermally conductive filler. Expanded graphite, expanded graphite, and the like are described as thermally conductive fillers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 042611 [Patent Document 2] JP 2022-72896 A Summary of the Invention [Problem to be solved by the invention]

[0005] Soundproofing materials are required to have flame retardancy in addition to thermal conductivity depending on the application. For example, polyurethane foams that have been given flame retardancy have a dropping effect that drops fire seeds and suppresses the spread of fire even when exposed to flames. In the polyurethane foam molded body described in Patent Document 1, composite particles are used that are granulated by adhering magnetic particles to the surface of particles with relatively high thermal conductivity (thermally conductive particles) in order to orient the particles. If magnetic particles are mixed into polyurethane foam, the dropping effect may be impaired and the self-extinguishing property may decrease. Therefore, in consideration of flame retardancy, expanded graphite, which has a flame retardant effect and is inserted between layers of scaly graphite, is suitable as the thermally conductive particles. In this way, the flame retardancy of the polyurethane foam molded body is improved by using expanded graphite as the thermally conductive particles of the composite particles. However, in recent years, higher thermal conductivity is required for soundproofing materials. In this case, the thermal conductivity of expanded graphite is not sufficiently high, and there is a limit to the improvement of thermal conductivity by using expanded graphite alone.

[0006] In this regard, Patent Document 2 lists expanded graphite and expanded graphite as thermally conductive fillers. Expanded graphite is produced by heating and expanding expanded graphite, and then pulverizing it, and has a high purity because the interlayer material disappears. For this reason, the thermal conductivity of expanded graphite is higher than that of expanded graphite. However, as described in paragraph

[0006] , Patent Document 2 aims to perform foam molding without applying a magnetic field. Therefore, the thermally conductive filler in the polyurethane foam is not oriented, and even if expanded graphite or expanded graphite is used as a thermally conductive filler, they are merely dispersed alone. According to the study by the present inventor, it has been found that simply dispersing expanded graphite in polyurethane foam has little effect on improving thermal conductivity.

[0007] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a urethane foam molded product having excellent thermal conductivity and flame retardancy. [Means for solving the problem]

[0008] (1) In order to solve the above problems, the urethane foam molded product of the present disclosure comprises a substrate made of polyurethane foam and composite particles contained and oriented in the substrate, the composite particles comprising first composite particles having expanded graphite particles and magnetic particles bonded to surfaces of the expanded graphite particles with a binder, and second composite particles having expanded graphite particles and magnetic particles bonded to surfaces of the expanded graphite particles with a binder, and is characterized in that, when the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100 mass%, the content of the expanded graphite particles is 20 mass% or more and 80 mass% or less.

[0009] The urethane foam molded body of the present disclosure has at least two types of composite particles, a first and a second. In both composite particles, magnetic particles are bonded to the surface of a core particle by a binder. The core particles of the first composite particles are expanded graphite particles having a higher thermal conductivity than the expanded graphite particles, and mainly contribute to improving the thermal conductivity of the urethane foam molded body. The core particles of the second composite particles are expanded graphite particles that exhibit a flame retardant effect, and mainly contribute to improving the flame retardancy of the urethane foam molded body. These composite particles are oriented and arranged in a substrate made of polyurethane foam. The composite particles are aligned and oriented to form a heat transfer path in the substrate. This makes it easier for heat to be transferred to the composite particles, and the expanded graphite particles and the expanded graphite particles are more likely to exhibit their respective effects than in a form in which each is contained alone. In addition, both the expanded graphite particles and the expanded graphite particles are graphite-based materials, have thermal conductivity anisotropy, and have high affinity with polyurethane.

[0010] The urethane foam molded body of the present disclosure contains expanded graphite particles and expanded graphite particles, which have different functions, as separate, independent composite particles. This allows each particle to fully exert its effect without interfering with the other's function. As a result, the desired thermal conductivity and flame retardancy can be achieved. However, the urethane foam molded body of the present disclosure does not exclude a form that includes a composite particle in which magnetic particles are bonded to the surface of a particle in which expanded graphite particles and expanded graphite particles are integrated.

[0011] (2) In the above configuration, the average particle size of the expanded graphite particles may be from 100 μm to 3000 μm. This configuration reduces the effect on the moldability and brittleness of the urethane foam molded body, and allows the expanded graphite particles to exhibit the effect of improving thermal conductivity.

[0012] (3) In any of the above configurations, the purity of the expanded graphite particles may be 99% or more. With this configuration, the effect of improving thermal conductivity can be enhanced.

[0013] (4) In any of the above configurations, the average particle size of the expanded graphite particles may be 100 μm or more and 3000 μm or less. This configuration allows the flame retardant effect of the expanded graphite particles to be exhibited while minimizing the effect on the moldability and brittleness of the urethane foam molded body.

[0014] (5) In any of the above configurations, the content of the composite particles may be 5 volume % or more and 50 volume % or less, based on 100 volume % of the volume of the urethane foam molded body. This configuration is suitable for achieving both moldability of the urethane foam molded body and improvements in thermal conductivity and flame retardancy.

[0015] (6) In any of the above configurations, the binder constituting the first composite particles and the second composite particles may be a water-soluble polymer. This configuration has little effect on foam molding when producing a urethane foam molded product, and also has a small burden on the environment.

[0016] (7) In the above (6), the water-soluble polymer may be one or more selected from the group consisting of methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and starch. The water-soluble polymer of this configuration has good adhesiveness, is relatively inexpensive, and is easily available.

[0017] (8) In any of the above configurations, the content of the magnetic particles constituting the first composite particles and the second composite particles may be 20% by mass or more and 80% by mass or less, when the total mass of the expanded graphite particles and the expanded graphite particles in the base material is taken as 100% by mass. According to this configuration, the amount of magnetic particles is relatively small, which allows for cost reduction and weight reduction.

[0018] (9) In any of the above configurations, the magnetic particles constituting the first composite particle and the second composite particle may be one or more selected from iron particles and iron-based alloy particles. Iron particles and iron-based alloy particles have high saturation magnetization and are easily available as fine particles.

[0019] (10) In any of the above configurations, at least one of the first composite particles and the second composite particles may have the expanded graphite particles or insulating inorganic particles bonded to the surfaces of the expanded graphite particles with a binder.

[0020] In this configuration, the insulating inorganic particles may be directly attached to the surface of the expanded graphite particles or expanded graphite particles serving as the core, or may be indirectly attached via magnetic particles, that is, to the surface of the magnetic particles attached to each particle. As the magnetic particles, ferromagnetic materials such as stainless steel and iron are used. Therefore, composite particles in which the expanded graphite particles or the expanded graphite particles and the magnetic particles are composited have high electrical conductivity. When insulating inorganic particles are attached to the composite particles in this state, even if the composite particles are oriented in a state in which they are in contact with each other, the core particles and the magnetic particles (conductive particles) are unlikely to come into contact with each other between the adjacent composite particles. Therefore, the electrical resistance between the composite particles increases. In addition, the composite particles come into contact with each other via the insulating inorganic particles, so that the conduction between the composite particles can be cut off. As a result, the urethane foam molded body of the present disclosure can achieve electrical insulation. Thus, according to this configuration, in addition to high thermal conductivity and flame retardancy, electrical insulation can also be imparted. Therefore, the urethane foam molded body of this configuration is also suitable for applications requiring both heat dissipation and electrical insulation, such as heat dissipation members in electronic devices.

[0021] (11) In the above configuration (10), the insulating inorganic particles may be one or more selected from aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica. The insulating inorganic particles of this configuration have a relatively high thermal conductivity, so they are unlikely to inhibit thermal conductivity between composite particles. In addition, they are relatively inexpensive and easy to obtain. Effect of the Invention

[0022] In the urethane foam molded article of the present disclosure, the expanded graphite particles and the expanded graphite particles are arranged as separate composite particles oriented in the substrate, which results in the urethane foam molded article of the present disclosure having excellent thermal conductivity and flame retardancy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, embodiments of the urethane foam molded article of the present disclosure will be described. Note that the embodiments are not limited to the following embodiments, and various modifications and improvements that can be made by those skilled in the art can be made.

[0024] <Urethane foam molding> The urethane foam molded article of the present disclosure has a substrate made of polyurethane foam and composite particles contained and oriented in the substrate.

[0025] [Base material] The polyurethane foam of the base material is produced from urethane foam resin raw materials such as polyisocyanate components and polyol components. The urethane foam resin raw materials may be prepared from already known raw materials such as polyols and polyisocyanates. The polyol may be appropriately selected from polyhydric hydroxy compounds, polyether polyols, polyester polyols, polymer polyols, polyether polyamines, polyester polyamines, alkylene polyols, urea-dispersed polyols, melamine-modified polyols, polycarbonate polyols, acrylic polyols, polybutadiene polyols, phenol-modified polyols, and the like. The polyisocyanate may be appropriately selected from, for example, tolylene diisocyanate, phenylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, triphenylmethane triisocyanate, polymethylene polyphenyl isocyanate, naphthalene diisocyanate, and derivatives thereof (for example, prepolymers obtained by reaction with polyols, modified polyisocyanates), and the like.

[0026] The polyurethane foam resin raw material may further contain a catalyst, a blowing agent, a foam stabilizer, a plasticizer, a crosslinking agent, a chain extender, a flame retardant, an antistatic agent, a viscosity reducer, a stabilizer, a filler, a colorant, and the like. For example, the catalyst may be an amine catalyst such as tetraethylenediamine, triethylenediamine, or dimethylethanolamine, or an organometallic catalyst such as tin laurate or tin octanoate. The blowing agent is preferably water. Other than water, examples of the foam stabilizer include methylene chloride, fluorocarbons, and CO2 gas. The foam stabilizer may be a silicone foam stabilizer, and the crosslinking agent may be triethanolamine or diethanolamine.

[0027] The shape, size, etc. of the substrate are not particularly limited and may be appropriately determined depending on the application. The composite particles contained in the substrate may be arranged with a certain regularity. For example, they may be arranged in a straight line or a curved line between one end and the other end of the urethane foam molded body (the end does not have to be 180° opposite to the one end). They may also be arranged radially from the center toward the periphery.

[0028] [Composite particles] The composite particles oriented and contained in the substrate are particles in which magnetic particles or the like are bonded to the surface of a non-magnetic particle serving as a core by a binder, and have a first composite particle and a second composite particle. The first composite particle has an expanded graphite particle and a magnetic particle bonded to the surface of the expanded graphite particle by a binder. The second composite particle has an expanded graphite particle and a magnetic particle bonded to the surface of the expanded graphite particle by a binder. The non-magnetic particle serving as a core may be a single particle or a plurality of particles. For example, the expanded graphite particle constituting the first composite particle may be a single expanded graphite particle, or may be an aggregate particle in which a plurality of expanded graphite particles are integrated. The expanded graphite particle constituting the second composite particle may be a single expanded graphite particle, or may be an aggregate particle in which a plurality of expanded graphite particles are integrated. The composite particles may also include particles of a form other than the first composite particles and the second composite particles, such as a form in which magnetic particles are adhered to the surface of a particle in which an expanded graphite particle and an expanded graphite particle are integrated, or a form in which magnetic particles are adhered to the surface of another graphite particle or metal particle.

[0029] The content of the composite particles may be determined taking into consideration the thermal conductivity and flame retardancy, the effect on the foaming reaction of the polyurethane foam, moldability, etc. In order to achieve the desired thermal conductivity and flame retardancy, the content of the composite particles is desirably 5% by volume or more, where the volume of the urethane foam molded body is taken as 100% by volume. It is more preferable to make it 10% by volume or more. On the other hand, from the viewpoint of not inhibiting the foaming reaction, it is desirably the content of the composite particles is 50% by volume or less, and it is more preferable to make it 20% by volume or less.

[0030] In addition, when the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100% by mass, the content of the expanded graphite particles is set to 20% by mass or more and 80% by mass or less. If the content of the expanded graphite particles is less than 20% by mass, the effect of improving the thermal conductivity is small. 30% by mass or more is more preferable. On the other hand, if the content of the expanded graphite particles is more than 80% by mass, the flame retardancy decreases. 60% by mass or less is more preferable.

[0031] The expanded graphite particles constituting the first composite particles may be produced by heating and expanding expanded graphite, forming it into a sheet, and then pulverizing the sheet. The expanded graphite particles have a multi-layer structure in which multiple graphenes are stacked. From the viewpoint of enhancing the effect of improving thermal conductivity, it is desirable for the purity of the expanded graphite particles (the content of carbon components) to be 99% or more. It is desirable for the thermal conductivity of the expanded graphite particles to be 200 W / m·K or more.

[0032] The shape of the expanded graphite particles is not particularly limited, and may be flaky, fibrous, spherical, or the like. From the viewpoint of increasing thermal conductivity, the average particle size of the expanded graphite particles is desirably 100 μm or more, and more preferably 700 μm or more. On the other hand, if the expanded graphite particles are too large, there is a risk that the molded body will become brittle due to cracks originating from the expanded graphite particles. Therefore, the average particle size of the expanded graphite particles is desirably 3000 μm or less, and more preferably 2000 μm or less. Unless otherwise specified, the average particle size in this specification refers to the median diameter (D 50 For commercially available products, the catalog value may be used.

[0033] The expanded graphite particles constituting the second composite particles are obtained by inserting a substance that generates gas when heated between layers of scaly graphite by acid treatment or the like. When heat is applied to the expanded graphite particles, the generated gas expands the gap between the layers and forms a layer that is stable against heat and chemicals. This stable layer acts as a heat insulating layer and prevents the transfer of heat, thereby providing a flame retardant effect. The expanded graphite particles may be appropriately selected in consideration of the expansion start temperature, expansion coefficient, etc. The expansion start temperature must be higher than the heat generation temperature during molding of the urethane foam molded body, so expanded graphite particles with an expansion start temperature of 150°C or higher are suitable.

[0034] The shape of the expanded graphite particles is not particularly limited, and may be flaky, fibrous, spherical, or the like. Considering the dispersibility in polyurethane foam, the average particle size of the expanded graphite particles is desirably 100 μm or more. More preferably, it is 700 μm or more. On the other hand, as in the case of expanded graphite particles, if the expanded graphite particles are too large, cracks may occur starting from the expanded graphite particles, and the molded body may become brittle. Therefore, the average particle size of the expanded graphite particles is desirably 3000 μm or less. More preferably, it is 2000 μm or less. When the size of the expanded graphite particles and the size of the expanded graphite particles are approximately the same, there is an advantage that the composite particles can be granulated together.

[0035] In the first composite particle and the second composite particle, the magnetic particles attached to the surface of the expanded graphite particle or the expanded graphite particle (either or both of them may be collectively referred to as "core particle") serving as the core may be the same or different. The magnetic particles may be any particles capable of orienting the composite particles, and for example, ferromagnetic materials such as iron, nickel, cobalt, gadolinium, stainless steel, magnetite, maghemite, manganese zinc ferrite, barium ferrite, strontium ferrite, etc., antiferromagnetic materials such as MnO, Cr2O3, FeCl2, MnAs, and alloy particles using these are suitable. Among them, iron, nickel, cobalt, and their iron-based alloys (including stainless steel) are suitable from the viewpoints of being easily available as fine particles and having high saturation magnetization. In particular, iron is relatively inexpensive and easily available, so that the manufacturing cost can be reduced and it is suitable for mass production.

[0036] The magnetic particles may be directly attached to the surface of the core particle, or may be indirectly attached via other particles such as insulating inorganic particles described later. The magnetic particles may be attached only to a part of the surface of the core particle, or may be attached so as to cover the entire surface. The size of the magnetic particles may be appropriately determined in consideration of the size of the core particle, the orientation of the composite particles, and the thermal conductivity between the composite particles. For example, the particle diameter of the magnetic particles is preferably 1 / 10 or less of the particle diameter of the core particle. When the size of the magnetic particles is reduced, the saturation magnetization of the magnetic particles tends to decrease. Therefore, in order to orient the composite particles with a smaller amount of magnetic particles, it is desirable to set the average particle diameter of the magnetic particles to 100 nm or more. It is more preferable to set it to 1 μm or more, and even more preferable to set it to 5 μm or more.

[0037] The shape of the magnetic particles is not particularly limited. For example, when the shape of the magnetic particles is flat, the distance between adjacent core particles is shorter than when the shape of the magnetic particles is spherical. This improves the thermal conductivity between adjacent composite particles. As a result, the thermal conductivity of the urethane foam molding is improved. In addition, when the shape of the magnetic particles is flat, the magnetic particles and the core particles are in contact with each other on the surface. In other words, the contact area between the two particles is large. This improves the adhesive force between the magnetic particles and the core particles. Therefore, the magnetic particles are less likely to peel off. In addition, the thermal conductivity between the magnetic particles and the core particles is also improved. For these reasons, it is desirable to use flaky particles as the magnetic particles.

[0038] From the viewpoint of enabling the composite particles to be oriented even in a relatively weak magnetic field, the content of the magnetic particles is desirably 20% by mass or more, where the total mass of the expanded graphite particles and the expanded graphite particles in the substrate is taken as 100% by mass. From the viewpoint of cost reduction and weight reduction, the content of the magnetic particles is desirably 130% by mass or less. It is more preferable that the content is 100% by mass or less, and further 80% by mass or less. In the urethane foam molded product of the present disclosure, expanded graphite particles having high thermal conductivity are contained as the first composite particles, so that the thermal conductivity is not likely to decrease even if the content of the magnetic particles is reduced.

[0039] In the first composite particle and the second composite particle, the binder that bonds the core particle and the magnetic particle may be appropriately selected in consideration of the adhesiveness, the effect on the foam molding, etc. Water-soluble polymers are preferred because they have little effect on the foam molding and are environmentally friendly. Examples include methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, starch, etc. Among them, starch is preferred because it is relatively inexpensive, has high adhesion, and has excellent granulation properties. The binder of the first composite particle and the binder of the second composite particle may be the same or different.

[0040] The expanded graphite particles, the expanded graphite particles, and the magnetic particles are conductive. Therefore, the first composite particles and the second composite particles are aligned and oriented to form a conductive path in the substrate. For example, a composite particle can be formed by adhering insulating inorganic particles to the surface of a core particle in addition to magnetic particles with a binder. By doing so, even if the composite particles are oriented, the electrical resistance between adjacent composite particles can be increased or the electrical connection can be blocked. As a result, electrical insulation can be imparted to the urethane foam molded body. The urethane foam molded body of the present disclosure, in which at least one of the first composite particles and the second composite particles has insulating inorganic particles, is suitable for applications requiring electrical insulation, such as heat dissipation members in electronic devices.

[0041] The insulating inorganic particles may be particles of an inorganic material having insulating properties. In particular, from the viewpoint of not impeding the thermal conductivity between composite particles, it is preferable that the thermal conductivity of the insulating inorganic particles is relatively large. For example, it is preferable that the thermal conductivity of the insulating inorganic particles is 5 W / m·K or more. Examples of insulating inorganic materials having a thermal conductivity of 5 W / m·K or more include aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica. One of these can be used alone, or two or more can be used in combination. Among them, talc and mica are preferable because they are flaky and have excellent covering properties.

[0042] The insulating inorganic particles may be directly bonded to the surface of the core particle, or may be indirectly bonded via the magnetic particles. The insulating inorganic particles may be bonded to only a part of the surface of the core particle, or may be bonded so as to cover the entire surface. From the viewpoint of increasing the electrical resistance between the composite particles and improving the electrical insulation of the urethane foam molding, it is desirable that the insulating inorganic particles are disposed in the outermost layer of the composite particle. The binder that bonds the magnetic particles to the core particle and the binder that bonds the insulating inorganic particles may be the same or different.

[0043] The size of the insulating inorganic particles may be appropriately determined in consideration of the adhesiveness to the core particles and the magnetic particles, the electrical insulation between the composite particles, and the thermal conductivity. If the insulating inorganic particles are too large, the adhesiveness and the thermal conductivity between the composite particles are reduced. For example, the particle diameter of the insulating inorganic particles is preferably 1 / 100 to 1 / 10 of the particle diameter of the core particles. The shape of the insulating inorganic particles is not particularly limited. For example, when the insulating inorganic particles are flat, the distance between adjacent core particles can be shortened compared to when the insulating inorganic particles are spherical. Therefore, the thermal conductivity between adjacent composite particles is less likely to be hindered. In addition, the contact area is increased, so that the insulating inorganic particles are less likely to peel off.

[0044] The insulating inorganic particles may be simply dispersed in the substrate, not as a part of the composite particle, or may constitute the composite particle and further dispersed in the substrate. The insulating inorganic particles dispersed in the substrate may be the same as or different from the insulating inorganic particles added as constituent particles of the composite particle. The insulating inorganic particles dispersed in the substrate may be one type or two or more types. The insulating inorganic particles dispersed in the substrate are also preferably those having a relatively high thermal conductivity, and the above-mentioned aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, silica, etc. are suitable. When the insulating inorganic particles are dispersed in the substrate, the insulating inorganic particles enter between the composite particles, making it difficult for the composite particles to be conductive to each other. Therefore, the electrical insulation of the urethane foam molded body is improved. Furthermore, when the thermal conductivity of the insulating inorganic particles is relatively high, in addition to the heat transfer path by the composite particles, a heat transfer path by the insulating inorganic particles is also formed. This further improves the thermal conductivity of the urethane foam molded body. Furthermore, when the insulating inorganic particles have flame retardancy, the flame retardancy of the urethane foam molded article is improved.

[0045] <Method of manufacturing urethane foam molded body> The method for producing the urethane foam molded article of the present disclosure is not particularly limited. As a preferred embodiment of the production method, the method for producing the urethane foam molded article of the present disclosure includes a composite particle production step, a mixed raw material production step, and a foam molding step. Each step will be described below.

[0046] [Composite particle manufacturing process] This process is a process for producing composite particles by stirring a granulation raw material containing a powder of core particles, a powder of magnetic particles, a binder, and water. Regarding the composite particles, the first composite particles containing expanded graphite particles and the second composite particles containing expanded graphite particles may be produced together or separately. Since the expanded graphite powder and the expanded graphite powder have similar specific gravities and have no significant difference in granulation properties, the first composite particles and the second composite particles can be produced together, which improves productivity.

[0047] When two types of composite particles are produced together, both the expanded graphite powder and the expanded graphite powder may be stirred together with other raw materials such as water. In this case, the difference between the average particle size of the expanded graphite powder and the average particle size of the expanded graphite powder may be reduced in consideration of granulation properties. In addition, the amount of the expanded graphite powder may be 20% by mass or more and 80% by mass or less, where the total mass of the expanded graphite powder and the expanded graphite powder is 100% by mass. On the other hand, when two types of composite particles are produced separately, the expanded graphite powder may be stirred together with other raw materials such as water to produce the first composite particles, and the expanded graphite powder may be stirred together with other raw materials such as water to produce the second composite particles. The composite particles may be produced using a high-speed stirring mixer granulator or the like. The amounts of the magnetic particle powder, binder, and water to the core particle powder may be appropriately adjusted in consideration of granulation properties, magnetic field orientation of the composite particles, and the like.

[0048] Considering the magnetic field orientation of the composite particles, the amount of magnetic particle powder is preferably 20 parts by mass or more per 100 parts by mass of the core particle powder. On the other hand, considering the cost and weight reduction, it is preferable to set it to 130 parts by mass or less. It is more preferable to set it to 100 parts by mass or less, and even more preferable to set it to 80 parts by mass or less. The amount of binder is preferably 2% by mass or more, when the total mass of the powder to be bonded is 100% by mass, as a necessary and sufficient amount for bonding the particles. On the other hand, if the binder is excessive, there is a risk of the composite particles coagulating with each other. For this reason, the amount of binder is preferably 10% by mass or less. It is more preferable to set it to 5% by mass or less. The binder may be solid or liquid. When a water-soluble powder is used as the binder, it is recommended to add water after stirring the binder and other powder raw materials in advance. By doing so, the aggregation of the particles can be suppressed.

[0049] When insulating inorganic particles are added as constituent particles of the composite particles, the powder of insulating inorganic particles may be included in the granulation raw material. When insulating inorganic particles are arranged in the outermost layer of the composite particles, this process may be configured to include a first stirring process of stirring a first raw material having a powder of core particles, a powder of magnetic particles, a binder, and water, and a second stirring process of adding insulating inorganic particle powder to the stirred product of the first raw material and further stirring it.

[0050] [Mixed raw material manufacturing process] This step is a step of producing a mixed raw material by mixing the powder of the composite particles (including the first composite particles and the second composite particles) produced in the previous step with a urethane foam resin raw material.

[0051] As described above, the foamed urethane resin raw material may be prepared from raw materials such as polyol, polyisocyanate, catalyst, blowing agent, and foam stabilizer. In the urethane foam molded body of the present disclosure, insulating inorganic particles may be dispersed in the base material separately from the composite particles. When manufacturing a urethane foam molded body of this form, the composite particle powder and the insulating inorganic particle powder may be mixed with the foamed urethane resin raw material. The mixed raw material may be manufactured, for example, by mechanically stirring the composite particle powder and the foamed urethane resin raw material using a stirring blade or the like. In addition, the composite particle powder may be added to at least one of the two components (polyol raw material, polyisocyanate raw material) of the foamed urethane resin raw material to prepare two types of raw materials, and then the two raw materials may be mixed to manufacture the foamed urethane resin.

[0052] [Foam molding process] In this process, the mixed raw material produced in the previous process is injected into the cavity of a foaming mold, and foam-molded while applying a magnetic field so that the magnetic flux density in the cavity becomes approximately uniform.

[0053] The magnetic field may be formed in the direction in which the composite particles are oriented. For example, when the composite particles are oriented in a linear manner, it is desirable to form the magnetic field lines in the cavity of the foaming mold so that they are approximately parallel from one end to the other end of the cavity. In order to form such a magnetic field, for example, magnets may be placed near both sides of one end and the other end of the foaming mold so as to sandwich the foaming mold. The magnets may be permanent magnets or electromagnets. When an electromagnet is used, the magnetic field formation can be instantly switched on and off, and the strength of the magnetic field can be easily controlled. Therefore, it is easy to control the foaming molding. In addition, it is desirable that the magnetic field lines that constitute the magnetic field form a closed loop. In this way, leakage of the magnetic field lines is suppressed, and a stable magnetic field can be formed in the cavity.

[0054] In this process, the magnetic field is formed so that the magnetic flux density in the cavity is approximately uniform. For example, the difference in magnetic flux density in the cavity is preferably within ±10%. It is more preferable that it is within ±5%, and furthermore within ±3%. By forming a uniform magnetic field in the cavity of the foaming mold, uneven distribution of the composite particles can be suppressed, and a desired orientation state can be obtained. In addition, the foaming molding is preferably performed at a magnetic flux density of 150 mT or more and 350 mT or less. In this way, the composite particles in the mixed raw material can be reliably oriented. It is desirable to apply the magnetic field while the viscosity of the foamed urethane resin raw material is relatively low. If a magnetic field is applied when the foamed urethane resin raw material thickens and the foaming molding is completed to a certain extent, the composite particles are difficult to orient, and it is difficult to obtain the desired thermal conductivity. It is not necessary to apply the magnetic field for the entire time of foaming molding.

[0055] After the foam molding is completed in this step, the mold is removed to obtain the urethane foam molded article of the present disclosure. At this time, a skin layer is formed on at least one of one end and the other end of the urethane foam molded article depending on the foam molding method. The skin layer may be cut off depending on the application (or may not be cut off). EXAMPLES

[0056] Next, the present disclosure will be described more specifically with reference to examples.

[0057] <Production of composite particles> First, eight types of composite particles A to H were produced as follows (composite particle production process). For composite particles B to G, both expanded graphite powder and expanded graphite powder were stirred together to produce first and second types of composite particles at the same time.

[0058] [Composite particle A] The granulation raw material containing expanded graphite powder, stainless steel powder, starch powder, talc powder, and water was stirred to produce composite particle A as the second composite particle. First, the expanded graphite powder, stainless steel powder, and starch powder were charged into the container of a high-speed stirring type mixer granulator and mixed by impeller stirring, and water was further added and mixed for 1 minute. Next, talc powder was charged and mixed for another 4 minutes. The stirring speed was 400 rpm. The obtained powder was dried to obtain the powder of composite particle A. Details of the materials used are summarized in (a) to (d) below, and the blending amounts are shown in Table 1 below (the same applies to the following composite particles B to H).

[0059] [Composite particles B~G] Except for adding expanded graphite powder as a granulation raw material, composite particles B to G were produced by the same method as the manufacturing method of composite particle A. Composite particles B to G were produced by changing the blending ratio of expanded graphite powder and expanded graphite powder, and each of composite particles B to G includes both first composite particles and second composite particles.

[0060] [Composite particle H] Composite particles H were produced as first composite particles by the same method as the method for producing composite particles A, except that expanded graphite powder was used instead of expanded graphite powder.

[0061] (a) Nuclear particle Expanded graphite powder: "SYZR 502FP" manufactured by Shijiazhuang Aidi Trading Co., Ltd., particle size 300μm~: 80% or more. Expanded graphite powder: "AED-01" manufactured by Fuji Graphite Industries Co., Ltd., purity 99% or more, particle size 1000μm or more: 80% or more. (b) Magnetic particles Stainless steel powder: "AKT" manufactured by Mitsubishi Steel Corporation, average particle size 8.5 to 13.0 μm. (c) Binder Starch powder: "Instant Tender Gel C" manufactured by Nippon Corn Starch Co., Ltd. (d) Insulating inorganic particles Talc powder: "Microace (registered trademark) K-1" manufactured by Nippon Talc Co., Ltd., average particle size 8 μm.

[0062] [Table 1]

[0063] <Production of urethane foam molded body> The produced composite particles A to H were used to produce a urethane foam molded body. First, 100 parts by mass of polyether polyol (Sumika Covestro Urethane Co., Ltd.'s "SBU (registered trademark) Polyol 0248"), 2 parts by mass of diethylene glycol (Mitsubishi Chemical Co., Ltd.) as a chain extender, 2 parts by mass of water as a blowing agent, 1.5 parts by mass of tetraethylenediamine catalyst (Kao Corporation's "Kao Raiser (registered trademark) No. 31"), and 0.5 parts by mass of a silicone foam stabilizer (Dow Corning Toray Co., Ltd.'s "SZ-1333") were mixed to prepare a polyol raw material. In addition, a diphenylmethane diisocyanate (MDI) modified product was prepared as a polyisocyanate raw material. The MDI modified product was produced by mixing polyether polyol (same as above) and 4,4'-diphenylmethane diisocyanate ("Millionate MT" manufactured by Tosoh Corporation) so that the isocyanate (NCO) content was 70% by mass, and reacting for 180 minutes at 100°C under nitrogen purging. Next, 80 parts by mass of composite particles and 60 parts by mass of aluminum hydroxide powder ("SB93" manufactured by Nippon Light Metal Co., Ltd.) as insulating inorganic particles were added to 100 parts by mass of the polyol raw material and mixed to prepare a premix polyol. Next, 100 parts by mass of the premix polyol and 10 parts by mass of the polyisocyanate raw material (MDI modified product) were mixed to prepare a mixed raw material (mixed raw material production process).

[0064] The mixed raw material was then poured into an aluminum foaming mold (cavity was a rectangular parallelepiped with length 130 mm × width 130 mm × thickness 5 mm), and the foaming mold was sealed. The foaming mold was then placed in a magnetic induction foaming molding device to perform foaming molding. A uniform magnetic field was formed in the cavity of the foaming mold by magnetic lines of force that were approximately parallel from above to below. The magnetic flux density in the cavity was 200 mT, and the difference in magnetic flux density in the cavity was within ±3%. The foaming molding was performed with a magnetic field applied for the first 2 minutes, and without a magnetic field for the next 5 minutes (foaming molding process). After the foaming molding was completed, the mold was removed to obtain a urethane foam molding. The obtained urethane foam moldings are referred to as urethane foam moldings A to H according to the type of composite particles used. The content of the composite particles in the urethane foam moldings A to H is 10% by volume when the volume of the urethane foam molding is 100% by volume. The urethane foam moldings C to F are included in the concept of the urethane foam molding of the present disclosure.

[0065] <Evaluation of urethane foam molded products> The thermal conductivity and flame retardancy of the produced urethane foam molded articles were evaluated. The evaluation results of thermal conductivity and flame retardancy are summarized in Table 1. The evaluation methods are as follows.

[0066] [Thermal Conductivity] The thermal conductivity of the urethane foam molded body was measured using "HC-110" manufactured by Eiko Seiki Co., Ltd., which complies with the heat flow meter method of JIS A1412-2:1999.

[0067] [Flame retardant] A vertical flame test according to the UL94 standard was carried out. In the vertical flame test, the flame of a gas burner is applied to the bottom end of a sample held vertically for 10 seconds, and if all of the following five criteria are met, it is judged to be at the V-0 level: (1) The sample does not burn for longer than 10 seconds in either of the two flame applications. (2) The total burning time for each of the five samples, after two flame applications, does not exceed 50 seconds. (3) None of the samples burn up to the position of the fixing clamp. (4) None of the samples ignite the cotton placed below the sample or drip burning particles. (5) After the second flame application, the sample does not continue to glow red for longer than 30 seconds.

[0068] As shown in Table 1, the urethane foam moldings C to F have composite particles C to F containing both the first composite particles and the second composite particles, and the content of the expanded graphite particles is 20% by mass or more and 80% by mass or less when the total mass of the expanded graphite particles and the expanded graphite particles is 100% by mass. Therefore, the thermal conductivity of the urethane foam moldings C to F is 0.65 W / m·K or more, and the flame retardancy is V-0, and it was confirmed that the urethane foam moldings C to F satisfy both the thermal conductivity and the flame retardancy. In contrast, the urethane foam molding A using the composite particle A containing only the second composite particles and the urethane foam molding B containing a small amount of expanded graphite particles satisfied the flame retardancy but had poor thermal conductivity. In addition, the urethane foam molding H using the composite particle H containing only the first composite particles and the urethane foam molding G containing a large amount of expanded graphite particles satisfied the thermal conductivity but had poor flame retardancy. [Industrial Applicability]

[0069] The urethane foam molded article of the present disclosure is suitable as a soundproofing material for use in vehicle parts such as inverters, motors, and gear boxes of electric powertrains, cylinder heads and cylinder head covers of engines, and electronic devices such as personal computers.

Claims

1. The present invention has a substrate made of polyurethane foam and composite particles contained in the substrate in an oriented manner, The composite particles include A first composite particle having expanded graphite particles and magnetic particles bonded to the surface of the expanded graphite particles by a binder; second composite particles having expanded graphite particles and magnetic particles bonded to the surfaces of the expanded graphite particles by a binder; having A urethane foam molded article, characterized in that, when the total mass of the expanded graphite particles in the substrate and the expanded graphite particles is taken as 100 mass%, the content of the expanded graphite particles is 20 mass% or more and 80 mass% or less.

2. The urethane foam molded article according to claim 1, wherein the average particle size of the expanded graphite particles is from 100 μm to 3,000 μm.

3. 2. The urethane foam molded article according to claim 1, wherein the purity of the expanded graphite particles is 99% or more.

4. 2. The urethane foam molded article according to claim 1, wherein the average particle size of the expanded graphite particles is 100 μm or more and 3000 μm or less.

5. 2. The urethane foam molded article according to claim 1, wherein a content of the composite particles is 5 volume % or more and 50 volume % or less, where the volume of the urethane foam molded article is taken as 100 volume %.

6. The urethane foam molded article according to claim 1 , wherein the binder constituting the first composite particles and the second composite particles is a water-soluble polymer.

7. 7. The urethane foam molded article according to claim 6, wherein the water-soluble polymer is at least one selected from the group consisting of methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and starch.

8. 2. The urethane foam molded body according to claim 1, wherein a content of the magnetic particles constituting the first composite particles and the second composite particles is 20% by mass or more and 80% by mass or less, when a total mass of the expanded graphite particles and the expanded graphite particles in the base material is 100% by mass.

9. The urethane foam molded article according to claim 1 , wherein the magnetic particles constituting the first composite particles and the second composite particles include at least one type selected from the group consisting of iron particles and iron-based alloy particles.

10. 2. The urethane foam molded article according to claim 1, wherein at least one of the first composite particles and the second composite particles comprises the expanded graphite particles or insulating inorganic particles bonded to the surfaces of the expanded graphite particles with a binder.

11. The urethane foam molded article according to claim 10, wherein the insulating inorganic particles comprise at least one selected from the group consisting of aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, talc, calcium carbonate, clay, mica, and silica.

Citation Information

Patent Citations

  • Urethane foam molded body and method for producing the same

    JP2012051986A

  • Method for manufacturing urethane foam molding and apparatus for agitating foamed urethane resin ingredients used for the same

    JP2014188916A

  • Slurry dispersion and refractory material

    JP2022125931A

  • Polyurethane foam, polyol composition and method for producing polyurethane foam

    JP2023016623A

  • Urethane foam molding and method for manufacturing same

    WO2013042611A1