Recycled polypropylene-based resin foam sheet, and method for producing the same
The formulation of a recycled polypropylene resin foam sheet with targeted mechanical properties addresses the brittleness and strength issues of recycled materials, achieving enhanced mechanical strength and reduced environmental impact.
Patent Information
- Application Number
- JP2023057025
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polypropylene resin foam sheets made from recycled materials suffer from reduced mechanical strength and increased brittleness due to resin deterioration from heat, leading to brittle molded bodies and environmental concerns from plastic waste.
A recycled polypropylene resin foam sheet is formulated with specific mechanical properties, including a tensile fracture energy of 3000 to 6000 J/g, weight average molecular weight of 200,000 to 500,000, and a content of recycled polypropylene resin of 10% to 100% by mass, combined with optional additives to enhance strength and flexibility.
The solution provides a recycled polypropylene resin foam sheet with excellent mechanical strength, reduced environmental impact, and improved moldability, maintaining flexibility and strength even under stretching conditions.
Smart Images

Figure 2024144871000002 
Figure 2024144871000003 
Figure 2024144871000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a recycled polypropylene resin foam sheet and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art Polypropylene-based resin foam sheets have been widely used as transport containers and protective materials due to their excellent moldability and strength. On the other hand, in recent years, environmental problems associated with the manufacture and disposal of plastic products have been attracting attention, such as the depletion of petroleum resources due to plastic production, and the problem of global warming due to the increase in CO2 concentration that occurs when waste plastic is incinerated. In order to alleviate these problems as much as possible, various attempts have been made to recycle materials, which effectively utilize waste plastic as recycled resin.
[0003] Patent Document 1 discloses that a polypropylene-based resin foamed sheet having excellent thermoformability and an apparent density of 150 to 750 g / L is provided at low cost. In Patent Document 1, a low-cost low-melt tension type polypropylene-based resin having no long chain branches is mixed with a high-melt tension type polypropylene-based resin having long chain branches to reduce the amount of expensive resin used, thereby reducing the production cost. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-356573 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, Patent Document 1 does not consider the use of recycled polypropylene to produce a polypropylene resin foam sheet in order to reduce costs. Generally, when a foamed sheet is thermoformed into a molded article and then reused as a recycled plastic, the resin component has already been deteriorated by heat, so that the mechanical strength of the resulting foamed sheet is reduced and the molded article is likely to become brittle.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a recycled polypropylene-based resin foamed sheet that uses recycled polypropylene-based resin and thus has excellent mechanical strength while reducing the environmental impact, and a method for producing the same. [Means for solving the problem]
[0007] The present invention has the following aspects. [1] Contains recycled polypropylene-based resin; A recycled polypropylene resin foam sheet having a tensile breaking energy of 3000 to 6000 J / g in a tensile test measured by the following measurement method. <Method for measuring tensile fracture energy> The recycled polypropylene resin foam sheet is cut into dumbbell-shaped No. 1 shapes as specified in JIS K6251:2010 in both the MD and TD directions, and measurements are performed with a gripping distance of 80 mm and a test speed of 200 mm / min. The tensile modulus (MPa) is obtained using data processing on a universal testing machine, and the tensile breaking stress (MPa) and tensile breaking elongation (%) are calculated. Next, the tensile breaking energy (J / g) is calculated for each of the MD and TD directions from the obtained graphs of tensile breaking stress and tensile breaking elongation and the apparent density of the test piece. The average value of the tensile breaking energy values in the MD and TD directions is calculated and used as the tensile breaking energy. [2] The weight average molecular weight of the recycled polypropylene resin is 200,000 to 500,000; The recycled polypropylene-based resin foam sheet according to [1], wherein the average tensile stress at break in the MD direction and the average tensile stress at break in the TD direction are 0.5 to 20 MPa, and the average tensile elongation at break in the MD direction and the average tensile elongation at break in the TD direction are 5 to 400%, in a tensile test of the recycled polypropylene-based resin foam sheet measured by the following measuring method. <Method of measuring tensile breaking stress and tensile breaking elongation> The recycled polypropylene resin foam sheet is cut into dumbbell-shaped No. 1 shapes as specified in JIS K6251:2010 in the MD and TD directions, and measurements are taken with a gripper interval of 80 mm and a test speed of 200 mm / min. The tensile modulus (MPa) is obtained using universal testing machine data processing, and the tensile breaking stress (MPa) and tensile breaking elongation (%) are calculated. The average tensile breaking stress (MPa) and the average tensile breaking elongation (%) are calculated from the values in the MD and TD directions, respectively. [3] The apparent density of the recycled polypropylene resin foam sheet is 0.05 to 1.0 g / cm 3 The thickness is 0.5 to 5.0 mm, and the basis weight is 200 to 600 g / m 2 The recycled polypropylene resin foam sheet according to [1] or [2], [4] The recycled polypropylene-based resin foam sheet according to any one of [1] to [3], wherein the recycled polypropylene-based resin content is 10 mass% or more based on the total mass of all resin components in the recycled polypropylene-based resin foam sheet. [5] The recycled polypropylene-based resin foam sheet according to any one of [1] to [4], wherein the recycled polypropylene-based resin has a tensile yield stress of 10 to 50 MPa and a nominal tensile break strain of 50 to 500% in a tensile test measured by the following measurement method. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are taken with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing. [6] The tensile yield stress of the recycled polypropylene-based resin in a tensile test measured by the following measurement method is 5 to 20 times the average value of the tensile break stress in the MD direction and the tensile break stress in the TD direction in a tensile test of the recycled polypropylene-based resin foam sheet; The recycled polypropylene-based resin foam sheet according to any one of [1] to [5], wherein the recycled polypropylene-based resin has a nominal tensile break strain in a tensile test measured by the following measurement method, which is 1.1 to 20 times the average value of the tensile break elongation in the MD direction and the tensile break elongation in the TD direction in a tensile test of the recycled polypropylene-based resin foam sheet. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are taken with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing. [7] Contains recycled polypropylene-based resins; The recycled polypropylene-based resin foam sheet has a tensile yield stress of 10 to 50 MPa in a tensile test measured by the following measurement method, and a nominal tensile break strain of 50 to 500% in a tensile test measured by the following measurement method. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are taken with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing. [8] The recycled polypropylene-based resin foam sheet according to [7], further comprising a polypropylene-based resin having a branched structure other than the recycled polypropylene-based resin. [9] A method for producing a recycled polypropylene-based resin foam sheet according to any one of [1] to [8], The recycled polypropylene resin is a resin obtained from a molded body containing a polypropylene resin. A method for producing recycled polypropylene resin foam sheets. Effect of the Invention
[0008] According to the present invention, it is possible to provide a recycled polypropylene-based resin foam sheet that uses recycled polypropylene-based resin and has excellent mechanical strength while reducing the environmental impact, and a method for producing the same. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing a method for measuring an average bubble diameter. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a foam sheet manufacturing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following definitions of terms apply throughout the specification and claims. A numerical range expressed by "to" means that the numerical values before and after the "to" are the lower and upper limits of the numerical range. The number average molecular weight (hereinafter also referred to as Mn), weight average molecular weight (hereinafter also referred to as Mw), and Z average molecular weight (hereinafter also referred to as Mz) refer to polystyrene (PS) equivalent weight average molecular weights measured using gel permeation chromatography (GPC). Polydispersity (hereinafter, also referred to as Mw / Mn) is the weight average molecular weight (Mw) divided by the number average molecular weight (Mn).
[0011] <Recycled polypropylene resin foam sheet> The recycled polypropylene resin foam sheet of the present invention (hereinafter, simply referred to as "foam sheet") is produced by foaming a resin composition containing recycled polypropylene resin. The resin composition contains recycled polypropylene resin and a foaming agent.
[0012] The tensile breaking energy of the recycled polypropylene resin foam sheet, measured by the following measurement method, is preferably from 3,000 to 6,000 J / g, and more preferably from 3,500 to 5,000 J / g. When the tensile breaking energy is equal to or greater than the lower limit, the brittleness of the foamed sheet containing the recycled polypropylene-based resin is easily improved. When the tensile breaking energy is equal to or less than the upper limit, the foamed sheet is easily able to maintain its mechanical strength even when stretched, and the mechanical strength of the molded article is also easily improved. <Method for measuring tensile fracture energy> The recycled polypropylene resin foam sheet is cut into dumbbell-shaped No. 1 shapes as specified in JIS K6251:2010 in both the MD and TD directions, and measurements are performed with a gripping distance of 80 mm and a test speed of 200 mm / min. The tensile modulus (MPa) is obtained using data processing on a universal testing machine, and the tensile breaking stress (MPa) and tensile breaking elongation (%) are calculated. Next, the tensile breaking energy (J / g) is calculated for each of the MD and TD directions from the obtained graphs of tensile breaking stress and tensile breaking elongation and the apparent density of the test piece. The average value of the tensile breaking energy values in the MD and TD directions is calculated and used as the tensile breaking energy.
[0013] The tensile breaking energy in the MD direction of the recycled polypropylene resin foam sheet, measured by the above-mentioned measuring method, is preferably from 2000 to 7000 J / g, and more preferably from 3000 to 6000 J / g. When the tensile fracture energy in the MD direction is within the above range, the brittleness of the foamed sheet containing the recycled polypropylene-based resin is easily improved, and the mechanical strength is easily maintained even when the foamed sheet is stretched, and the mechanical strength of the molded body is also easily improved.
[0014] The tensile breaking energy in the TD direction of the recycled polypropylene resin foam sheet, measured by the above-mentioned measuring method, is preferably from 3,000 to 6,000 J / g, and more preferably from 4,000 to 5,000 J / g. When the tensile fracture energy in the TD direction is within the above range, the brittleness of the foamed sheet containing the recycled polypropylene-based resin is easily improved, and the mechanical strength is easily maintained even when the foamed sheet is stretched, and the mechanical strength of the molded body is also easily improved.
[0015] In the recycled polypropylene resin foam sheet, the difference between the tensile breaking energy in the MD direction and the tensile breaking energy in the TD direction measured by the above-mentioned measuring method is preferably from 100 to 2000 J / g, more preferably from 300 to 1500 J / g. When the difference between the tensile fracture energy in the MD direction and the tensile fracture energy in the TD direction is within the above range, the anisotropy of the foamed sheet is reduced, and deformation and distortion of the foamed sheet and molded article during use are easily improved.
[0016] The tensile breaking energy in the MD direction and the tensile breaking energy in the TD direction of the recycled polypropylene resin foam sheet measured by the above-mentioned measuring method can be adjusted by the type, composition, and combination of the recycled polypropylene resin and other resins constituting the recycled polypropylene resin foam sheet, as well as the manufacturing conditions.
[0017] In the recycled polypropylene resin foam sheet, the average value of the tensile breaking stress in the MD direction and the tensile breaking stress in the TD direction, measured by the same method as the measuring method described in the above <Method for measuring tensile breaking energy>, is preferably 0.5 to 20 MPa, more preferably 1 to 15 MPa, and even more preferably 2 to 10 MPa. When the average tensile breaking stress is equal to or greater than the lower limit, the mechanical strength of the foamed sheet containing the recycled polypropylene-based resin is easily ensured. When the average tensile breaking stress is equal to or less than the upper limit, the foamed sheet is easily able to maintain its flexibility even when stretched, and the brittleness of the molded product is easily improved.
[0018] The tensile breaking stress in the MD direction of the recycled polypropylene resin foam sheet, measured by the same method as the above-mentioned measuring method, is preferably 0.5 to 20 MPa, more preferably 1 to 15 MPa, and further preferably 2 to 10 MPa. When the tensile breaking stress in the MD direction is within the above range, the mechanical strength of the foamed sheet containing the recycled polypropylene-based resin is easily ensured, and the flexibility of the foamed sheet is easily maintained even when the foamed sheet is stretched, which makes it easier to improve the brittleness of the molded body.
[0019] The tensile breaking stress in the TD direction of the recycled polypropylene resin foam sheet, measured by the same method as the above-mentioned measuring method, is preferably 0.5 to 15 MPa, more preferably 1 to 10 MPa, and even more preferably 2 to 5 MPa. When the tensile breaking stress in the TD direction is within the above range, the mechanical strength of the foamed sheet containing the recycled polypropylene-based resin is easily ensured, and the flexibility of the foamed sheet is easily maintained even when the foamed sheet is stretched, which makes it easier to improve the brittleness of the molded body.
[0020] The tensile stress at break in the MD direction and the tensile stress at break in the TD direction of the recycled polypropylene-based resin foam sheet measured by the above-mentioned measuring method can be adjusted by the manufacturing method of the recycled polypropylene-based resin foam sheet, and the type, composition, and combination of the recycled polypropylene-based resin and other resins constituting the recycled polypropylene-based resin foam sheet, as well as the manufacturing conditions.
[0021] In the recycled polypropylene resin foam sheet, the average value of the tensile breaking elongation in the MD direction and the tensile breaking elongation in the TD direction, measured by the same method as the measuring method described in the above <Method for measuring tensile breaking energy>, is preferably 5 to 400%, more preferably 8 to 300%, and even more preferably 10 to 200%. When the average tensile elongation at break is equal to or greater than the lower limit, the brittleness of the foamed sheet containing the recycled polypropylene resin is easily improved. When the average tensile elongation at break is equal to or less than the upper limit, the foamed sheet is easily able to maintain its mechanical strength even when stretched, and the mechanical strength of the molded article is also easily improved.
[0022] The tensile elongation at break in the MD direction of the recycled polypropylene resin foam sheet, measured by the same method as the above-mentioned measuring method, is preferably from 1 to 100%, more preferably from 5 to 50%, and even more preferably from 10 to 30%. When the tensile elongation at break in the MD direction is within the above range, the brittleness of the foamed sheet containing the recycled polypropylene-based resin is easily improved, and the mechanical strength is easily maintained even when the foamed sheet is stretched, and the mechanical strength of the molded body is also easily improved.
[0023] The tensile elongation at break in the TD direction of the recycled polypropylene resin foam sheet, measured by the same method as the above-mentioned measuring method, is preferably from 5 to 500%, more preferably from 10 to 400%, and even more preferably from 20 to 300%. When the tensile elongation at break in the TD direction is within the above range, the brittleness of the foamed sheet containing the recycled polypropylene-based resin is easily improved, and the mechanical strength is easily maintained even when the foamed sheet is stretched, and the mechanical strength of the molded body is also easily improved.
[0024] In the recycled polypropylene resin foam sheet, the difference between the tensile elongation at break in the MD direction and the tensile elongation at break in the TD direction, measured by the same method as the above-mentioned measuring method, is preferably 1 to 300%, more preferably 3 to 250%, even more preferably 5 to 100%, particularly preferably 5 to 50%, and most preferably 5 to 30%. When the difference between the tensile elongation at break in the MD direction and the tensile elongation at break in the TD direction is within the above range, the anisotropy of the foamed sheet is reduced, and deformation and distortion of the foamed sheet and molded article during use is easily improved.
[0025] The tensile elongation at break in the MD direction and the tensile elongation at break in the TD direction of the recycled polypropylene-based resin foam sheet measured by the above-mentioned measuring method can be adjusted by the manufacturing method of the recycled polypropylene-based resin foam sheet, and the types, compositions, and combinations of the recycled polypropylene-based resin and other resins that constitute the recycled polypropylene-based resin foam sheet, as well as the manufacturing conditions.
[0026] The density (apparent density) of the foamed sheet is, for example, 0.05 to 1.0 g / cm 3 is preferable, and 0.1 to 0.5 g / cm 3 More preferably, 0.15 to 0.3 g / cm 3 When the content is equal to or more than the above lower limit, moldability and strength are easily ensured, and when the content is equal to or less than the above upper limit, the heat insulating property and light weight of the molded product are easily ensured. In this specification, the apparent density can be measured by the method described in the Examples.
[0027] The thickness of the foamed sheet 1 is, for example, preferably 0.5 to 5.0 mm, more preferably 1.0 to 3.0 mm. If the thickness of the foamed sheet is equal to or greater than the lower limit, sufficient strength is easily obtained. If the thickness is equal to or less than the upper limit, molding is easy. In this specification, the thickness can be measured by the method described in the examples.
[0028] The basis weight of the foam sheet is, for example, 200 to 600 g / m 2 is preferable, and 300 to 500 g / m 2 More preferably, 350 to 480 g / m 2 When the content is equal to or more than the above lower limit, moldability is easily ensured, and when the content is equal to or less than the above upper limit, the light weight of the molded product is easily ensured. In this specification, the basis weight can be measured by the method described in the examples.
[0029] The open cell ratio of the foamed sheet is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less. When the open cell ratio is equal to or less than the above upper limit, moldability and mechanical strength are easily ensured. In this specification, the open cell ratio can be measured by the method described in the Examples.
[0030] The average cell diameter of the entire foamed sheet is preferably 0.3 to 3 mm, more preferably 0.5 to 1.5 mm, and even more preferably 0.6 to 1.0 mm. When the average cell diameter of the entire foamed sheet is within the above range, the mechanical strength is easily improved. In this specification, the average cell diameter can be measured by the method described in the Examples.
[0031] The apparent density, thickness, basis weight, open cell ratio, and average cell diameter of the recycled polypropylene-based resin foam sheet can be adjusted by the production conditions of the recycled polypropylene-based resin foam sheet, as well as the types, compositions, foaming agents, optional components, and combinations of these of the recycled polypropylene-based resin and other resins that constitute the recycled polypropylene-based resin foam sheet, and the production conditions.
[0032] <Recycled polypropylene resin> The recycled polypropylene resin is a resin obtained from a molded body obtained by thermoforming a polypropylene resin. The recycled polypropylene resin can be obtained by pulverizing the molded body into a powder. The recycled polypropylene resin may be either a recycled polypropylene resin having a linear structure or a recycled polypropylene resin having a branched structure, and from the viewpoint of ease of foaming when made into a foamed sheet and reduction in production costs, a recycled polypropylene resin having a branched structure is preferred. When used in combination with a resin having a branched structure other than the recycled polypropylene resin, the recycled polypropylene resin may be a recycled polypropylene resin having a linear structure.
[0033] The recycled polypropylene-based resin may be a homopolymer of propylene or a copolymer of propylene and a polymerizable vinyl monomer. These polypropylene-based resins may be used alone or in combination of two or more. Among them, polypropylene homopolymer is preferred. When the recycled polypropylene-based resin is a copolymer, the content of structural units derived from propylene is preferably 80% by mass or more, and more preferably 90% by mass or more, relative to 100% by mass of the copolymer.
[0034] The weight average molecular weight of the recycled polypropylene resin is preferably 200,000 to 500,000, more preferably 250,000 to 450,000, and even more preferably 300,000 to 400,000. When the weight average molecular weight of the recycled polypropylene resin is equal to or greater than the lower limit, the mechanical strength of the foamed sheet is easily improved. When the weight average molecular weight of the recycled polypropylene resin is equal to or less than the upper limit, the handleability of the resin composition during the production of the foamed sheet is easily improved. The weight average molecular weight of the recycled polypropylene resin can be measured by the method described in the Examples.
[0035] The polydispersity of the recycled polypropylene resin is preferably 3-8, more preferably 4-8, and further preferably 4-7. When the polydispersity of the recycled polypropylene resin is equal to or higher than the lower limit, the mechanical strength of the foamed sheet is easily improved. When the polydispersity of the recycled polypropylene resin is equal to or lower than the upper limit, the handleability of the resin composition when producing a foamed sheet is easily improved.
[0036] The content of the recycled polypropylene resin is preferably 10% by mass or more, more preferably 10 to 100% by mass, even more preferably 20 to 90% by mass, and particularly preferably 30 to 80% by mass, relative to 100% by mass of the resin components constituting the recycled polypropylene resin foam sheet. When the content of the recycled polypropylene resin is equal to or more than the lower limit, the environmental impact is easily reduced. When the content of the recycled polypropylene resin is equal to or less than the upper limit, the foamed sheet is easily foamed.
[0037] The recycled polypropylene resin has a tensile yield stress in a tensile test measured by the following measurement method of preferably 10 to 50 MPa, more preferably 15 to 45 MPa, and even more preferably 20 to 40 MPa. When the tensile yield stress is within the above range, the mechanical strength is easily improved. <Method of measuring tensile yield stress> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are taken with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) is calculated using universal testing machine data processing.
[0038] The nominal tensile strain at break of the recycled polypropylene resin in a tensile test measured by the following measurement method is preferably from 50 to 500%, more preferably from 75 to 450%, and even more preferably from 80 to 400%. When the nominal tensile strain at break is within the above range, brittleness is easily improved. <Method of measuring nominal tensile breaking strain> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are taken with a gripping distance of 115 mm and a test speed of 1 mm / min. The nominal tensile fracture strain (%) is calculated using universal testing machine data processing.
[0039] The tensile yield stress of the recycled polypropylene resin in the tensile test measured by the above-mentioned measuring method is preferably 5 to 20 times, more preferably 6 to 15 times, and even more preferably 7 to 10 times the average value of the tensile breaking stress in the MD direction and the tensile breaking stress in the TD direction in the tensile test of the recycled polypropylene resin foam sheet. When the ratio of the tensile yield stress to the average value of the tensile breaking stress is within the above range, the mechanical strength is easily improved.
[0040] <Other resins> The foam sheet may contain other resins besides the recycled polypropylene-based resin. The other resins are thermoplastic resins, such as polyolefin-based resins such as polyethylene and polypropylene, polyester-based resins, polyimide-based resins, polystyrene-based resins, polyphenylene ether-based resins, polyamide-based resins, polyarylate-based resins, polyphenylsulfone-based resins, polysulfone-based resins, polyethersulfone-based resins, etc. The other resins may be recycled resins derived from recycled raw materials.
[0041] As a polypropylene resin other than the recycled polypropylene resin, a high melt tension polypropylene (HMS-PP) resin is preferable. A high melt tension polypropylene resin is a polypropylene resin in which a high molecular weight component or a component having a branched structure is mixed into the polypropylene resin, or a long-chain branched component is copolymerized with the polypropylene, thereby increasing the tension in the molten state. High melt tension polypropylene resins are commercially available, and examples of such resins include "WB140HMS" manufactured by Borealis, and "MFX8" and "MFX6" manufactured by Japan Polypropylene Corporation.
[0042] The content of the polypropylene-based resin including the recycled polypropylene-based resin relative to the total mass of the resin contained in the foam sheet is preferably 95 mass% or more, more preferably 98 mass% or more, even more preferably 99 mass% or more, and particularly preferably 100 mass%.
[0043] The content of polypropylene-based resins other than recycled polypropylene-based resins relative to the total mass of resins contained in the foamed sheet is preferably 90 mass% or less, more preferably 80 mass% or less, further preferably 10 to 80 mass%, and particularly preferably 20 to 70 mass%. When the content of the polypropylene resin other than the recycled polypropylene resin is equal to or more than the lower limit, the foam sheet is easily foamed. When the content of the recycled polypropylene resin is equal to or less than the upper limit, the environmental load is easily reduced.
[0044] The melting point of the resin component including the recycled polypropylene resin constituting the foamed sheet is preferably 150° C. or higher and 170° C. or lower, more preferably 155° C. or higher and 165° C. or lower. When the melting point of the resin component is equal to or higher than the lower limit, the heat resistance of the foamed sheet is more easily improved. When the melting point of the resin component is equal to or lower than the upper limit, the thermoformability is more easily improved. The melting point of the resin component is measured by the method described in JIS K7121:1987 "Method of measuring transition temperature of plastics."
[0045] <Optional ingredients> The foamed sheet may contain additives such as surfactants, cell regulators, crosslinking agents, fillers, flame retardants, flame retardant assistants, lubricants (hydrocarbons, fatty acids, fatty acid amides, esters, alcohols, metal soaps, silicone oils, waxes such as low molecular weight polyethylene, etc.), spreading agents (liquid paraffin, polyethylene glycol, polybutene, etc.), colorants, heat stabilizers, ultraviolet absorbers, antioxidants, etc. Optional components include a cell regulator, a stabilizer, a flame retardant, an antistatic agent, a colorant, and the like. These may be appropriately selected from additives known in the art for use in recycled polypropylene-based resin foam sheets.
[0046] Examples of the foam regulator include inorganic powders such as talc, silica, mica, and the like, fluorine-based resin powders such as polytetrafluoroethylene, acid salts of polycarboxylic acids, and mixtures of polycarboxylic acids and sodium carbonate or sodium bicarbonate, etc. The foam regulator may be used alone or in combination of two or more kinds. The content of the cell regulator is preferably, for example, 0.01 to 5.0 parts by mass per 100 parts by mass of the total amount of resins contained in the foamed sheet (the total amount of recycled polypropylene resin and other resins).
[0047] The above-mentioned optional components may each be used alone or in combination of two or more. The total amount of optional components contained in the foamed sheet is preferably 0.01 to 5.0 parts by mass per 100 parts by mass of the total mass of the resins contained in the foamed sheet.
[0048] The foamed sheet of the present invention has excellent impact resistance. The impact absorption energy of the foamed sheet is preferably at least 0.36 J, and more preferably at least 0.40 J. When the impact absorption energy is within the above range, the foamed sheet has excellent impact resistance. The impact absorption energy can be measured by the method described in the Examples. Impact absorption energy per basis weight (impact absorption energy / basis weight) is 0.00095J / (g / m 2 The greater the value of impact absorption energy / basis weight, the better the impact resistance. The impact absorption energy per basis weight can be measured by the method described in the Examples.
[0049] <Manufacturing method of recycled polypropylene resin foam sheet> The foamed sheet of the present invention is produced in accordance with a conventionally known production method. Examples of methods for producing a foamed sheet include a method in which a resin composition is prepared, extruded into a sheet shape, and foamed (primary foaming) (extrusion foaming method). An example of a method for producing a foamed sheet will be described with reference to FIG. The foamed sheet manufacturing apparatus 200 in FIG. 2 is an apparatus for obtaining a foamed sheet by extrusion foam molding, and includes an extruder 202, a foaming agent supply source 208, a circular die 210, a mandrel 220, and two winders 240. The extruder 202 is a so-called tandem type extruder, and is configured such that an extruder A 202a and an extruder B 202b are connected by a pipe 206. The first extrusion section 202a includes a hopper 204, and a foaming agent supply source 208 is connected to the extruder A 202a. A circular die 210 is connected to the extruder B 202b, and a mandrel 220 is provided downstream of the circular die 210. The mandrel 220 includes a cutter 222.
[0050] First, the raw materials constituting the resin composition are fed from a hopper 204 into the extruder A 202a. The raw materials fed from the hopper 204 include the resin constituting the foamed sheet, and additives that are mixed as necessary.
[0051] In the extruder A202a, the raw materials are mixed while being heated to a given temperature to form a resin melt, and a foaming agent is supplied from a foaming agent supply source 208 to the extruder A202a, and the foaming agent is mixed into the resin melt to form a resin composition. The heating temperature is appropriately determined in consideration of the type of resin, etc., so long as the resin melts and the additives are not denatured.
[0052] The resin composition is supplied from the extruder A 202a through a pipe 206 to the extruder B 202b, further mixed, cooled to a given temperature, and then supplied to the circular die 210. The temperature of the resin composition when extruded from the circular die 210 is 140 to 190°C, and more preferably 150 to 190°C. The resin composition is extruded through the circular die 210, and the foaming agent foams to form a cylindrical foamed sheet 101a. The foamed sheet 101a extruded from the circular die 210 is blown with cooling air 211 and then supplied to a mandrel 220. The cooling rate of the foamed sheet 101a can be adjusted by combining the temperature, amount, and blowing position of the cooling air 211. The cylindrical foamed sheet 101a is heated to an arbitrary temperature by the mandrel 220, sized, and cut into two pieces by the cutter 222 to become the foamed sheet 101. The foamed sheet 101 is stretched around a guide roll 242 and a guide roll 244, respectively, and taken up by the winder 240 to become the foamed sheet roll 102. The foaming ratio of the foamed sheet is, for example, 2 to 20 times. The foamed sheet may be produced by a method other than extrusion foam molding.
[0053] <Foaming agent> As the foaming agent, a known foaming agent can be used. Examples of the foaming agent include inorganic decomposable foaming agents such as sodium bicarbonate-citric acid foaming agents, ammonium carbonate, sodium bicarbonate, ammonium bicarbonate, ammonium nitrite, calcium azide, sodium azide, and sodium borohydride; azo compounds such as azodicarbonamide, azobissulfuramide, azobisisobutyronitrile, and diazoaminobenzene; nitroso compounds such as N,N'-dinitrosopentanemethylenetetramine and N,N'-dimethyl-N,N'-dinitrosoterephthalamide; benzenesulfonyl hydrazide, p-toluenesulfonyl hydrazide, p,p'-oxybisbenzenesulfonylsemicarbazide, p-toluenesulfonylsemicarbazide, trihydrazinotriazine, and barium azodicarboxylate. Examples of the gaseous foaming agent include air, nitrogen, carbon dioxide, propane, neopentane, methyl ether, dichlorofluoromethane, n-butane, and isobutane. In this case, gas means a gas at room temperature (15°C to 25°C). On the other hand, examples of volatile blowing agents include ether, petroleum ether, acetone, pentane, hexane, isohexane, heptane, isoheptane, benzene, toluene, etc. The blowing agent may be used alone or in combination of two or more kinds.
[0054] The content of the foaming agent in the resin composition is appropriately determined taking into consideration the type of foaming agent, specific gravity, etc., and is, for example, preferably 0.5 to 20 parts by mass, more preferably 0.8 to 5.5 parts by mass, per 100 parts by mass of the resin.
[0055] The step of extruding and foaming the resin composition can be carried out by using a known method. For example, when the raw materials (resin, optional components, foaming agent) constituting the resin composition are fed to an extruder equipped with a die (flat die or circular die), they are melt-mixed while being transported toward the die to become a resin composition. The resin composition is extruded from the die, and the foaming agent foams to become a foamed sheet. The raw materials constituting the resin composition, except for the foaming agent, may be mixed in advance by a dry blending method, a full compounding method or the like, and the resulting mixture may be supplied to the extruder. The apparent density and open cell ratio of the foamed sheet can be adjusted by the amounts of foaming agent and cell regulator, the resin temperature during extrusion, etc. The resin temperature during extrusion can be set within a range in which the resin melts and the optional components are not denatured.
[0056] <Resin molded body> The resin molded article of the present embodiment is obtained by molding the foamed sheet of the present embodiment. Examples of the resin molded article include containers such as food trays and industrial part transport trays, cushioning materials, packaging materials, heat insulating materials, industrial parts for electrical appliances or automobiles, and building materials. The resin molded article of this embodiment has excellent impact resistance and is therefore suitable for use as, for example, carrier trays, in-vehicle components for automobiles and the like, building components, and the like.
[0057] The foamed sheet can be formed by any known thermoforming method, for example, by a method including the following steps. (1) a heating step in which the foam sheet is heated to soften it to a state in which it can be thermoformed; (2) a molding step in which the softened foam sheet is deformed to conform to the surface shape of a mold to form a product shape; and (3) A trimming process in which unnecessary portions of the foam sheet that has formed the product shape are cut off to obtain the desired resin molded product from the foam sheet.
[0058] The heating step (1) can be carried out, for example, by a method in which the foamed sheet is passed through a heating furnace equipped with a radiant heater or the like for a certain period of time. The molding step (2) can be carried out by contacting the heated and softened foamed sheet with the surface of a mold to cool it. As the mold, a general mold such as a vacuum mold, a pressure mold, a vacuum pressure mold, or a match mold mold can be used. When forming a relatively large resin molded body, a pair of male and female molds is preferred, and it is preferable to use a plug-assisted vacuum mold or a match mold mold. In deep drawing, the foamed sheet may be cooled rapidly during molding, causing breakage or thinning, so it is preferable to adjust the temperature as necessary. The trimming step (3) can be carried out by a general method using a Thompson blade or a puncher (punch).
[0059] ≪Applications≫ The molded article of the present embodiment can be used as a cushioning material, packaging material, structural member, heat insulating material, etc., used in industrial members such as food containers, electrical products, or automobiles. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The raw materials used in the examples and comparative examples are shown below. <Recycled polypropylene resin> · Recycled PP (A): Recycled polypropylene resin, weight average molecular weight 390,000, tensile yield stress 27 MPa, nominal tensile break strain 334%. · Recycled PP (B): Recycled polypropylene resin, weight average molecular weight 360,000, tensile yield stress 35 MPa, nominal tensile break strain 93%. Recycled PP (C): Recycled polypropylene resin, weight average molecular weight 400,000, tensile yield stress 20 MPa, nominal tensile break strain 20%. Other resins WB140HMS: Polypropylene resin, manufactured by Borealis. · MFX6: Polypropylene resin, manufactured by Japan Polypropylene Corporation.
[0061] The weight average molecular weight (Mw) of the above recycled polypropylene resin was measured by the following method. A solution was prepared by adding 6 mL of o-dichlorobenzene to a container containing 6 mg of sample and sealing it. The solution was prepared by dissolving the sample by heating at 160°C for 1 hour using a DF-8321 manufactured by Tosoh Corporation. This solution was used as the measurement sample and measured using a chromatograph under the following measurement conditions. The weight average molecular weight (Mw) of the sample was obtained from the calibration curve of standard polystyrene that had been measured and prepared in advance. Equipment used: Tosoh Corporation "HLC-8321GPC / HT" Sample column: Tosoh Corporation TSKgel GMHHR-H(20)HT2 (7.8mm ID x 30cm) x 3 Sample guard column: TSKgel guardcolumn HHR(30)HT2 (7.5mm ID x 7.5cm) x 1, manufactured by Tosoh Corporation Reference column: Tosoh Corporation TSKgel GMHHR-H(S)HT (7.8 mm ID x 30 cm) x 2 Reference guard column: TSKgel guardcolumn HHR(S)HT (7.5mm ID x 7.5cm) x 1, manufactured by Tosoh Corporation Mobile phase: o-dichlorobenzene Sample flow rate: 1.0mL / min Reference flow rate: 0.5mL / min Detector: RI Sample concentration: 0.1wt% Injection volume: 300μL Measurement time: 34 min (Temperature settings for each part of the device) Solvent stocker: 40℃ Column oven (column temperature): 160℃ Sample table: 160℃ Injection valve: 160℃ Detector: 160℃ The standard polystyrene samples used for the calibration curve were "High polymer kit" and "oligomer kit" manufactured by Tosoh Corporation, with weight average molecular weights of 8,420,000, 5,480,000, 2,110,000, 1,090,000, 706,000, 427,000, 190,000, 96,400, 37,900, 17,400, 5,060, 2,550, 1,013, and 589. The above-mentioned standard polystyrene for the calibration curve was grouped into A (8,420,000, 1,090,000, 190,000, 17,400, 1,013), B (5,480,000, 706,000, 96,400, 5,060, 589) and C (2,110,000, 427,000, 37,900, 2,550), and then 10 mg of A was weighed out and dissolved in 30 mL of o-dichlorobenzene, and 10 mg of B and C were also weighed out and dissolved in 100 mL of o-dichlorobenzene. The standard polystyrene calibration curve was obtained by injecting 300 μL of each of A, B and C solutions and creating a calibration curve (cubic equation) from the retention time obtained after measurement. The weight average molecular weight was calculated using the calibration curve.
[0062] The tensile yield stress and nominal tensile strain at break were measured by the following method. <Method of measuring tensile yield stress and nominal tensile breaking strain> The tensile yield stress and nominal tensile break strain were measured in accordance with JIS K7151-1:2014 and JIS K7161-2:2014. The test pieces were molded into test piece 1A type under conditions of 200 ° C. using a compression molding machine. The number of test pieces was 5. The test pieces were conditioned for 16 hours under the standard atmosphere of JIS K 7100:1999 symbol "23 / 50", class 2, and then used for measurement. The measurement was performed under the same environment, with a gripper interval of 115 mm and a test speed of 1 mm / min. From the obtained graph, the load region where the slope was maximum was set, and the tensile modulus of elasticity was obtained by the universal testing machine data processing. The intersection point of the straight line of this modulus of elasticity and the stroke was set as the origin of elongation, and the tensile yield stress and tensile break nominal strain were automatically calculated. The above measurements were carried out using Shimadzu Corporation's "Autograph AG-X plus 100kN" universal testing machine and Shimadzu Corporation's "TRAPEZIUM X" universal testing machine data processing.
[0063] [Example 1] A composition obtained by mixing 0.025 parts by weight of Fine Cell Master PO217K (trade name, master batch of sodium bicarbonate and citric acid, manufactured by Dainichi Seika Chemicals Co., Ltd.) as a bubble nucleating agent with 100 parts by weight of the resin composition with the raw materials and blending amounts shown in Table 1 was fed to a twin-screw extruder with a diameter of φ75 mm, and after heating and melting, 0.85 wt% of carbon dioxide was injected as a foaming agent from the middle and melt-kneaded. The molten mixture was then uniformly cooled to 173°C suitable for foaming, and extrusion foamed into the air from an annular die with an outlet diameter of φ125 mm. The extruded foam was taken, and the inner surface was cooled in the process of passing it along a mandrel with a diameter of φ339 mm whose inside was cooled to about 15°C, and air was blown on the mandrel to cool the outer surface. The cooled cylindrical foam was cut open with a cutter in the extrusion direction at one point on its circumference to produce a band-shaped foam sheet.
[0064] [Example 2, Comparative Examples 1 and 2] A foamed sheet was obtained in the same manner as in Example 1, except that the raw materials and their amounts were changed as shown in Table 1.
[0065] The thickness, basis weight, apparent density, open cell ratio, average cell diameter, tensile breaking stress, tensile breaking elongation, tensile modulus, tensile breaking energy, and impact absorption energy of the obtained foamed sheet were measured by the following methods. The obtained results are shown in Table 1.
[0066] <Thickness> Twenty-one arbitrary positions in the width direction (direction perpendicular to the extrusion flow direction) were used as measurement points. These measurement points were measured with a thickness measuring device (manufactured by Techlock Corporation, model: SM-125) to the nearest 0.01 mm. The arithmetic mean of these measurements was used as the thickness.
[0067] <Basic weight> Excluding 20 mm from both ends in the width direction (direction perpendicular to the extrusion flow direction), ten pieces of 10 cm x 10 cm were cut out at equal intervals in the width direction, and the mass (g) of each piece was measured to the nearest 0.001 g. The average mass (g) of each piece was calculated using the formula: 2 The converted value is expressed as the mass per unit weight (g / m 2 ) was decided.
[0068] <Apparent density> 50cm to avoid changing the bubble structure. 3 The sheet was cut out to prepare a test piece, the mass and volume of the test piece were measured, and the overall apparent density was calculated using the following formula: The test piece was cut out from a sheet that was 72 hours or more old (maximum 90 days) after production, and left for 24 hours in an atmospheric condition of 23°C±2°C and 50RH%±5RH%. Apparent density (g / cm 3 ) = mass of test piece (g) ÷ volume of test piece (cm 3 )
[0069] <Open cell ratio> From the foam sheet, several sheet-like samples measuring 25 mm in length and 25 mm in width were cut out. The cut out samples were stacked together so that there were no gaps, resulting in a thickness of 25 mm, which was used as a test piece. The apparent volume (cm 3 The apparent volume (cm 3 ) was obtained by measuring the outer dimensions of the test piece to 1 / 100 mm. A "Digimatic Caliper" caliper made by Mitutoyo Corporation was used for the measurement. Next, the volume (cm) of the test piece was measured using a Tokyo Science Co., Ltd. "1000" air comparison specific gravity meter by the 1-1 / 2-1 atmospheric pressure method. 3 ) was sought. The open cell ratio (%) was calculated using the following formula. The open cell ratio was calculated as the average value of five test pieces. The test pieces were conditioned in a JIS K7100:1999, symbol 23 / 50, class 2 environment for 16 hours before use in the measurement. The measurement was carried out in the same environment. The air comparison specific gravity meter was used with a standard ball (large 28.96 cm 3 Small 8.58cm 3 ) was used for correction. Open cell rate (%) = (apparent volume - volume measured with an air comparison type specific gravity meter) / apparent volume x 100
[0070] <Average bubble diameter> Sample 1 for cross-sectional observation was cut out from the center of the width direction of the foamed sheet. The cross section of the sample was photographed at 50x magnification using a scanning electron microscope "TM3030Plus" manufactured by Hitachi High-Technologies Corporation. One of the cross sections to be observed was a cross section (hereinafter referred to as "MD cross section") obtained by cutting the sample in a plane (arrow 1 in Figure 1) parallel to the extrusion direction (MD) and perpendicular to the surface of the foamed sheet. The other cross section to be observed was a cross section (hereinafter referred to as "TD cross section") obtained by cutting the sample in a plane (arrow 2 in Figure 1) perpendicular to the extrusion direction. Microscopic images were taken using a scanning electron microscope, with two fields of view for each of the MD and TD cross sections, for a total of four fields of view. The captured image was printed on a sheet of A4 paper, and three straight lines were drawn at arbitrary positions on the printed image connecting both ends of the image so that they were parallel to the extrusion direction (MD direction) and width direction (TD direction), and three straight lines were drawn at arbitrary positions connecting the back and front surfaces of the sheet so that they were parallel to the thickness direction (VD direction) perpendicular to each direction. In addition, we tried to avoid contacting any bubble with any point of contact for any line, and counted the number of bubbles that the line passed through. If any bubble was contacted only at a point of contact, the bubble was also included in the count. The length of the drawn straight line and the scale bar on the image were measured, and the image magnification was calculated from the measured length of the scale bar and the displayed value of the scale bar, and the average chord length was calculated using the following formula. Average chord length t (mm) = measured value of straight line / (number of bubbles x image magnification) The bubble diameter in each direction was then calculated using the following formula. Bubble diameter D(mm)=t / 0.616 Furthermore, the cube root of the product was taken as the average bubble diameter. Average bubble diameter (mm) = (D MD ×D TD ×D VD )1 / 3 D MD : Bubble diameter in MD direction (mm) D TD : bubble diameter in TD direction (mm) D VD : Bubble diameter in VD direction (mm)
[0071] <Tensile stress at break, tensile elongation at break and tensile modulus of elasticity> The tensile stress at break, tensile elongation at break and tensile modulus of elasticity were measured according to JIS K6251:2010. Test pieces were cut from the foamed sheet in the extrusion direction (MD) and the direction perpendicular to the extrusion direction (TD) in a dumbbell shape No. 1 as specified in JIS K6251:2010. The number of test pieces was 5 for each direction. The test pieces were conditioned for 16 hours in a standard atmosphere of JIS K 7100:1999 code "23 / 50", class 2, and then used for measurement. The measurement was performed under the same environment, with a gripper interval of 80 mm and a test speed of 200 mm / min. From the obtained graph, the load region where the slope was maximum was set, and the tensile modulus of elasticity was obtained by the universal testing machine data processing. The intersection point of the straight line of this modulus of elasticity and the stroke was set as the origin of elongation, and the tensile stress at break and the tensile elongation at break were automatically calculated. The above measurements were carried out using Shimadzu Corporation's "Autograph AG-X plus 100kN" universal testing machine and Shimadzu Corporation's "TRAPEZIUM X" universal testing machine data processing.
[0072] <Tensile breaking energy> The tensile breaking energy (J / g) in the MD and TD directions was calculated from the graphs of tensile breaking stress and tensile breaking elongation obtained by the above measurement method and the apparent density of the test piece. Furthermore, the overall average value was calculated from these values.
[0073] <Impact energy absorption> The impact absorption energy was measured using a film impact tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd., product name "No. 181 Film Impact Tester"). An evaluation sample of 100 mm x 90 mm was taken from the foam sheet, and the impact absorption energy (unit: J) of the sample was determined in an environment adjusted to a temperature of 22°C and a relative humidity of 40%, with an impact ball size of 6.35 mmR and a pendulum angle of 90 degrees. Specifically, the sample for which the impact absorption energy is to be calculated is set between the evaluation sample and the sample holder, the pointer is placed on the 1.5 J line, and the pendulum is dropped by tilting the pendulum stopper handle. The sample breaks and the pendulum pushes the pointer, and the scale indicated is read. The above operation is performed five times on each side of the foam sheet, and the average value is calculated. In addition, the impact absorption energy per basis weight (unit: J / (g / m 2 )) was sought.
[0074] [Table 1]
[0075] Examples 1 and 2 to which the present invention was applied were excellent in the evaluation of mechanical strength. Comparative Examples 1 and 2, which had a tensile fracture energy of less than 3000 J / g, were inferior to Examples 1 and 2 in the evaluation of mechanical strength. [Explanation of symbols]
[0076] 1. Foam sheet (sample for cross-sectional observation)
Claims
1. Contains recycled polypropylene resin, A recycled polypropylene-based resin foam sheet having a tensile breaking energy of 3000 to 6000 J / g in a tensile test measured by the following measurement method. <Method for measuring tensile fracture energy> The recycled polypropylene resin foam sheet was cut into a dumbbell shape No. 1 as specified in JIS K6251:2010 in the MD and TD directions, respectively, and measured with a gripping tool interval of 80 mm and a test speed of 200 mm / min. The tensile modulus (MPa) was obtained using universal testing machine data processing, and the tensile breaking stress (MPa) and tensile breaking elongation (%) were calculated. Next, the tensile breaking energy (J / g) is calculated for each of the MD and TD directions from the obtained graphs of tensile breaking stress and tensile breaking elongation and the apparent density of the test piece. The average value of the tensile breaking energy values in the MD and TD directions is calculated to be the tensile breaking energy.
2. The weight average molecular weight of the recycled polypropylene resin is 200,000 to 500,000; The recycled polypropylene-based resin foam sheet according to claim 1, wherein the average tensile stress at break in the MD direction and the average tensile stress at break in the TD direction are 0.5 to 20 MPa, and the average tensile elongation at break in the MD direction and the average tensile elongation at break in the TD direction are 5 to 400%, in a tensile test of the recycled polypropylene-based resin foam sheet measured by the following measurement method. <Method of measuring tensile stress at break and tensile elongation at break> The recycled polypropylene resin foam sheet is cut into a dumbbell shape No. 1 as specified in JIS K6251:2010 in the MD direction and the TD direction, and measured with a gripper interval of 80 mm and a test speed of 200 mm / min. The tensile modulus (MPa) is obtained by data processing of a universal testing machine, and the tensile breaking stress (MPa) and the tensile breaking elongation (%) are calculated. The average value of the tensile breaking stress (MPa) and the average value of the tensile breaking elongation (%) are calculated from the values in the MD direction and the TD direction, respectively.
3. The apparent density of the recycled polypropylene resin foam sheet is 0.05 to 1.0 g / cm 3 The thickness is 0.5 to 5.0 mm, and the basis weight is 200 to 600 g / m 2 The recycled polypropylene resin foam sheet according to claim 1,
4. The recycled polypropylene-based resin foam sheet according to claim 1, wherein the content of the recycled polypropylene-based resin is 10% by mass or more based on the total mass of all resin components in the recycled polypropylene-based resin foam sheet.
5. The recycled polypropylene resin foam sheet according to claim 1, wherein the recycled polypropylene resin has a tensile yield stress of 10 to 50 MPa and a nominal tensile break strain of 50 to 500% in a tensile test measured by the following measurement method. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are performed with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing.
6. The recycled polypropylene-based resin has a tensile yield stress in a tensile test measured by the following measurement method, which is 5 to 20 times the average value of the tensile break stress in the MD direction and the tensile break stress in the TD direction in a tensile test of the recycled polypropylene-based resin foamed sheet, The recycled polypropylene-based resin foam sheet according to claim 1, wherein the nominal tensile break strain of the recycled polypropylene-based resin in a tensile test measured by the following measurement method is 1.1 to 20 times the average value of the tensile break elongation in the MD direction and the tensile break elongation in the TD direction in a tensile test of the recycled polypropylene-based resin foam sheet. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are performed with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing.
7. Contains recycled polypropylene resin, The recycled polypropylene resin has a tensile yield stress of 10 to 50 MPa in a tensile test measured by the following measurement method, and a nominal tensile break strain of 50 to 500% in a tensile test measured by the following measurement method. <Method for measuring tensile yield stress and nominal tensile break strain of recycled polypropylene resin> Recycled polypropylene resin is molded into test piece type 1A in accordance with JIS K7161-1:2014 and JIS K7161-2:2014, and measurements are performed with a gripping distance of 115 mm and a test speed of 1 mm / min. The tensile yield stress (MPa) and nominal tensile break strain (%) are calculated using universal testing machine data processing.
8. The recycled polypropylene-based resin foam sheet according to claim 7, further comprising a polypropylene-based resin having a branched structure other than the recycled polypropylene-based resin.
9. A method for producing the recycled polypropylene-based resin foam sheet according to any one of claims 1 to 8, The recycled polypropylene resin is a resin obtained from a molded body containing a polypropylene resin. A method for producing recycled polypropylene resin foam sheets.