Epihalohydrin-based rubber and rubber composition
Epihalohydrin rubber with a specified molecular weight range and alkylene oxide ratio, combined with a decomposition process, addresses the issues of viscosity increase and bleed-out, maintaining processability and physical properties in rubber compositions.
Patent Information
- Application Number
- JP2023057531
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Epihalohydrin rubbers experience increased viscosity when processed with fillers, leading to bleed-out and deterioration of physical properties due to the use of plasticizers, which compromises handleability and processability.
Utilizing epihalohydrin rubber with a weight average molecular weight (Mw) of 30,000 to 200,000, incorporating a molar ratio of alkylene oxide to epihalohydrin ranging from 0:100 to 90:10, and employing a decomposition process with an oxidizing agent to achieve a balanced molecular weight distribution.
The solution maintains handleability and processability while preventing bleed-out, ensuring good compression set properties and normal physical properties without compromising on rubber composition performance.
Smart Images

Figure 2024145254000001 
Figure 2024145254000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an epihalohydrin rubber and a rubber composition, more specifically to an epihalohydrin rubber that does not bleed out, maintains handleability and processability during measurement and processing, and has a balance of rubber properties. [Background technology]
[0002] Epihalohydrin rubbers, including epichlorohydrin rubber, have excellent heat resistance, oil resistance, fuel resistance, ozone resistance, low temperature properties, semi-conductive properties, and the like, and are therefore widely used as rubber parts for automobiles and rubber components for electrical and electronic equipment.
[0003] When epihalohydrin rubber is processed into a compound, the viscosity increases in the presence of a filler such as carbon black. Normally, a plasticizer or softener is used to lower the viscosity of the compound and make it flexible. Although this improves processability, it causes problems such as bleeding out on the surface of the rubber composition and deterioration of rubber physical properties such as compression set and normal physical properties.
[0004] Patent Document 1 discloses a rubber composition that uses a low-molecular-weight epichlorohydrin polymer instead of a plasticizer, but all of the examples shown contain 30 parts by weight of calcium carbonate as a filler per 100 parts by weight of the epichlorohydrin rubber alone or a blend with an NBR copolymer, and it is difficult to say that the low-molecular-weight epichlorohydrin polymer alone is effective in achieving a good balance between the processability and normal physical properties of the rubber composition. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-087892 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an epihalohydrin rubber which does not bleed out, maintains easy handling and processability during measurement and processing, and has a good balance of rubber physical properties. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above object, the present inventors have found that the above object can be achieved by using an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000. The present invention has been completed based on these findings.
[0008] That is, the present invention provides an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000.
[0009] The epihalohydrin rubber contains at least one structural unit derived from a compound selected from alkylene oxide and epihalohydrin, and the molar ratio of alkylene oxide:epihalohydrin is preferably in the range of 0:100 to 90:10.
[0010] Furthermore, the epihalohydrin rubber is preferably a decomposition product of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000.
[0011] The present invention also provides a rubber composition comprising 100 parts by mass of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 and 10 to 150 parts by mass of an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000.
[0012] The present invention also provides a method for producing an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000, which comprises reacting an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 in the presence of an oxidizing agent.
[0013] The oxidizing agent is preferably at least one selected from the group consisting of organic peroxides and inorganic peroxides. Effect of the Invention
[0014] The epihalohydrin rubber and rubber composition of the present invention do not bleed out, and exhibit good compression set and normal state physical properties while maintaining handleability and processability during measurement and processing.
[0015] In the rest of this specification, for ease of understanding, an epihalohydrin-based rubber having a weight average molecular weight (Mw) of 30,000 to 200,000 will be referred to as "epihalohydrin-based rubber I," and an epihalohydrin-based rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 will be referred to as "epihalohydrin-based rubber II." BEST MODE FOR CARRYING OUT THEINVENTION
[0016] The rubber composition of the present invention contains at least epihalohydrin rubber I having a weight average molecular weight (Mw) of 30,000 to 200,000 as measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and converted into polystyrene.
[0017] Epihalohydrin Rubber I The weight average molecular weight (Mw) of the epihalohydrin rubber I of the present invention is not particularly limited, but is more preferably 30,000 or more, and particularly preferably 40,000 or more, and the upper limit is preferably 200,000 or less, more preferably 150,000 or less, and particularly preferably 100,000 or less. The weight average molecular weight (Mw) of the epihalohydrin rubber I of the present invention is measured using gel permeation chromatography (GPC) and a differential refractometer (RI detector), using tetrahydrofuran (THF) as a solvent, and is measured in terms of polystyrene.
[0018] A specific method for measuring the weight average molecular weight (Mw) of the epihalohydrin rubber I of the present invention is shown to be performed using a GPC apparatus RID-6A (differential refractometer (RI detector)) manufactured by Shimadzu Corporation and Shodex columns KF-806L, KF-803L, and KF-801, with a flow rate of 1.0 mL / min, a concentration of 10 mg epihalohydrin rubber I / tetrahydrofuran (THF) 8 ml, an injection amount of 50 μL, and a column temperature of 40° C.
[0019] As for the epihalohydrin rubber I of the present invention, the lower limit of the proportion of molecular weight of 10,000 or less measured by gel permeation chromatography (GPC) is preferably 1% or more, more preferably 5% or more, particularly preferably 7% or more, and the upper limit is preferably less than 50%, preferably 40% or less, and preferably 30% or less. The proportion of molecular weight of 10,000 or less is based on a graph obtained from gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and a differential refractometer (RI detector) for detection, and the horizontal axis of the graph is the logarithm of the molecular weight, and the vertical axis is the integral distribution value. That is, the proportion of molecular weight of 10,000 or less in the epihalohydrin rubber I measured by GPC is the ratio of the peak area of the molecular weight component of 10,000 or less to the peak area of the entire molecular weight distribution of the epihalohydrin rubber I determined based on a calibration curve obtained by measuring the molecular weight of polystyrene. By making the proportion of epihalohydrin rubber I having a molecular weight of 10,000 or less 10% or more, handleability during metering and processing is not impaired and viscosity can be sufficiently reduced. If the proportion of epihalohydrin rubber I having a molecular weight of 10,000 or less exceeds 50%, compatibility during kneading is poor in the production of a rubber composition described below, causing bleed-out and deteriorating processability and normal physical properties of the rubber.
[0020] The epihalohydrin rubber I of the present invention may be in a solid state at room temperature (23°C), for example. In the case of a solid state (waxy state), the rubber composition can be easily handled during measurement in the production thereof, and the amount of filler that deteriorates processability can be reduced, resulting in good processability and normal physical properties of the resulting rubber composition. Furthermore, the occurrence of bleeding out onto the rubber surface is suppressed compared to when a plasticizer or a liquid epihalohydrin rubber is used.
[0021] The epihalohydrin rubber I of the present invention contains at least one structural unit derived from a compound selected from an alkylene oxide and an epihalohydrin.
[0022] Specific examples of alkylene oxides in the epihalohydrin rubber I of the present invention include ethylene oxide, propylene oxide, butylene oxide, pentylene oxide, hexylene oxide, etc., with ethylene oxide and propylene oxide being more preferred, and ethylene oxide being even more preferred.
[0023] In the epihalohydrin rubber I of the present invention, the alkylene oxide may be used alone or in combination of two or more kinds.
[0024] Specific examples of epihalohydrin in the epihalohydrin rubber I of the present invention include epichlorohydrin, epibromohydrin, epiiodohydrin, epifluorohydrin, etc., with epichlorohydrin and epibromohydrin being more preferred, and epichlorohydrin being even more preferred.
[0025] In the epihalohydrin rubber I of the present invention, the epihalohydrin may be used alone or in combination of two or more kinds.
[0026] In the epihalohydrin rubber I of the present invention, the molar ratio of alkylene oxide:epihalohydrin is in the range of 0:100 to 90:10, more preferably 0:100 to 80:20, and further preferably 0:100 to 70:30.
[0027] Manufacturing method of epihalohydrin rubber I The epihalohydrin rubber I of the present invention may be obtained by polymerization of alkylene oxide and / or epihalohydrin as raw materials, or may be obtained by decomposition of epihalohydrin rubber II having a weight average molecular weight (Mw) of 600,000 to 3,000,000. However, it is more preferable that it is a decomposition product of epihalohydrin rubber II, since it is easy to adjust the molecular weight to a desired value and the production equipment is simple.
[0028] The method for producing the epihalohydrin rubber I of the present invention by polymerization is not particularly limited, but a catalyst capable of ring-opening polymerization of an oxirane compound is used, and the polymerization temperature is, for example, in the range of -20 to 100°C. This polymerization may be either solution polymerization or slurry polymerization. Examples of the catalyst include a catalyst system in which organoaluminum is the main component and water, a phosphorus oxo acid compound, acetylacetone, or the like is reacted therewith, a catalyst system in which organozinc is the main component and water is reacted therewith, a metal halide catalyst system, and an organotin-phosphate ester condensate catalyst system (for example, the organotin-phosphate ester condensate catalyst system described in U.S. Pat. No. 3,773,694). When copolymerizing by such a method, it is preferable to copolymerize these components substantially randomly. Regardless of the production method, the method for controlling the molecular weight is well known, and the epihalohydrin rubber I of the present invention can be produced by mixing low molecular weight and non-low molecular weight components in an appropriate ratio.
[0029] In order to obtain the epihalohydrin rubber I of the present invention by decomposition, for example, the epihalohydrin rubber II is reacted in the presence of an oxidizing agent.
[0030] In the production of the epihalohydrin rubber I of the present invention, the epihalohydrin rubber II (starting material) used to obtain a decomposition product includes an epihalohydrin-alkylene oxide copolymer, an epihalohydrin homopolymer, etc., and as commercially available products, for example, Epichromer C (epichlorohydrin-ethylene oxide copolymer, structural units based on epichlorohydrin: 50 mol%, structural units based on ethylene oxide: 50 mol%) and Epichromer H (epichlorohydrin homopolymer) manufactured by Osaka Soda Co., Ltd. are preferably used, and these may be used alone or in combination of two or more types.
[0031] In the production of the epihalohydrin rubber I of the present invention, the oxidizing agent used in obtaining the decomposition product may be an organic peroxide or an inorganic peroxide, or a gas such as air or oxygen. From the viewpoint of handling, however, an organic peroxide is preferred. These may be used alone or in combination of two or more. When a peroxide is used, it is sufficient to add it to the reaction system and carry out the decomposition reaction, and when a gas is used, it is sufficient to carry out the decomposition reaction in the reaction system under a gas atmosphere. When the reaction system is carried out under a gas atmosphere, the gas concentration in the reaction system may be appropriately selected, and specifically, it may be 1% to 100%.
[0032] Examples of organic peroxides that may be used in the production of the epihalohydrin rubber I of the present invention include tert-butyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, tert-butylcumyl peroxide, 1,1-tert-butylperoxycyclohexane, 2,5-dimethyl-2,5-ditert-butylperoxyhexane, 2,5-dimethyl-2,5-ditert-dibutylperoxyhexyne-3, 1,3-bistert-butylperoxyisopropylbenzene, Examples of the peroxyalkylene include 2,5-dimethyl-2,5-dibenzoylperoxyhexane, 1,1-bistert-butylperoxy-3,3,5-trimethylcyclohexane, n-butyl-4,4-bistert-butylperoxyvalerate, benzoyl peroxide, tert-butylperoxyisobutyrate, tert-butylperoxy2-ethylhexanoate, tert-butylperoxybenzoate, tert-butylperoxyisopropylcarbonate, tert-butylperoxyallyl monocarbonate, p-methylbenzoyl peroxide, and 1,4-bis[(tert-butylperoxy)isopropyl]benzene. Among these, dicumyl peroxide, 1,3-bistert-butylperoxyisopropylbenzene, and 2,5-dimethyl-2,5-ditert-butylperoxyhexane are preferred, and 1,3-bistert-butylperoxyisopropylbenzene and 2,5-dimethyl-2,5-ditert-butylperoxyhexane are more preferred.
[0033] Examples of inorganic peroxides that can be used in the production of the epihalohydrin rubber I of the present invention include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate.
[0034] The amount of the oxidizing agent used in the production of the epihalohydrin rubber I of the present invention is 0.1 to 10 parts by mass relative to 100 parts by mass of the epihalohydrin rubber II (starting material). It is preferably 0.2 to 8 parts by mass, and more preferably 0.5 to 5 parts by mass. If the amount of the oxidizing agent used exceeds 10 parts by mass, decomposition of the epihalohydrin rubber II proceeds too much, which is not preferable from the viewpoint of not being able to obtain a desired molecular weight, and if it is less than 0.1 part by mass, it is not preferable because the molecular weight of the obtained epihalohydrin rubber II does not decrease.
[0035] In the production method of the present invention by decomposition of epihalohydrin rubber I, the reaction temperature is, for example, in the range of 25 to 300° C., and the reaction time is 1 to 60 minutes. The reaction temperature and reaction time can be appropriately changed depending on the half-life temperature of the peroxide used.
[0036] In the method for producing the epihalohydrin rubber I of the present invention by decomposition, the conditions are not limited, but the process may be carried out under a pressure of from normal pressure to 100 MPa, and is preferably carried out under normal pressure. A solvent may be used as necessary, but it is more preferable not to use a solvent.
[0037] In the method of producing the epihalohydrin rubber I of the present invention by decomposition, examples of suitable experimental equipment for use in the decomposition reaction include a gear oven, a constant temperature dryer, and an electric furnace, and any of them may be used. The epihalohydrin rubber I of the present invention can be easily produced by appropriately adjusting the reaction temperature and reaction time in accordance with the desired molecular weight.
[0038] Rubber composition The rubber composition containing the epihalohydrin rubber I of the present invention contains 100 parts by mass of the epihalohydrin rubber II having a weight average molecular weight (Mw) of 600,000 to 3,000,000 and 10 to 150 parts by mass of the epihalohydrin rubber I having a weight average molecular weight (Mw) of 30,000 to 200,000.
[0039] The epihalohydrin rubber II used in the rubber composition of the present invention can be one or more of these homopolymers or copolymers, such as epichlorohydrin homopolymer, epichlorohydrin-ethylene oxide copolymer, epichlorohydrin-propylene oxide copolymer, epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer, epichlorohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether quaternary copolymer, etc. Examples of commercially available products of these homopolymers or copolymers include Epichromer H, Epichromer C, Epichromer CG series, Epichromer D, Epichromer DG, and Epione series manufactured by Osaka Soda Co., Ltd.
[0040] A specific example of a method for measuring the weight average molecular weight (Mw) of the epihalohydrin rubber II used in the rubber composition of the present invention is to use a GPC apparatus RID-6A (differential refractometer (RI detector)) manufactured by Shimadzu Corporation and Shodex columns KD-807, KD-806M, and KD-803, with a flow rate of 1.0 mL / min, a concentration of 10 mg epihalohydrin rubber II / 8 mL of dimethylformamide (DMF), an injection amount of 50 μL, and a column temperature of 60° C.
[0041] In the rubber composition of the present invention, the epihalohydrin rubber I is 10 to 150 parts by mass, preferably 10 to 140 parts by mass, and more preferably 20 to 120 parts by mass, per 100 parts by mass of the epihalohydrin rubber II. If the amount is less than 10 parts by mass, the viscosity reducing effect is limited, and if the amount exceeds 150 parts by mass, compression set and tensile properties are deteriorated, which is not preferable.
[0042] The rubber composition of the present invention may further contain additives other than those mentioned above, such as additives such as lubricants, antioxidants, acid acceptors, fillers, antioxidants, ultraviolet absorbers and light stabilizers, reinforcing agents, plasticizers, processing aids, flame retardants, crosslinking accelerators, crosslinking retarders, crosslinking agents, mastication accelerators, etc., as long as the effects of the present invention are not impaired. Furthermore, it is also possible to blend rubbers, resins, etc., as is commonly done in the art, as long as the characteristics of the present invention are not lost.
[0043] Specific examples of the lubricant include paraffin and hydrocarbon resins such as paraffin wax and hydrocarbon wax; fatty acids such as stearic acid and palmitic acid; fatty acid amides such as stearamide and oleyl amide; fatty acid esters such as n-butyl stearate; sorbitan fatty acid esters; fatty alcohols; and the like, which may be used alone or in combination of two or more. When a lubricant is contained, the content thereof is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0044] Examples of the antiaging agent include known amine-based antiaging agents, phenol-based antiaging agents, benzimidazole-based antiaging agents, dithiocarbamate-based antiaging agents, thiourea-based antiaging agents, organic thioacid-based antiaging agents, and phosphorous-based antiaging agents. These may be used alone or in combination of two or more. Preferred are amine-based antiaging agents, phenol-based antiaging agents, benzimidazole-based antiaging agents, and dithiocarbamate-based antiaging agents, and more preferred are dithiocarbamate-based antiaging agents. When an antiaging agent is contained, the content is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the total of the epihalohydrin-based rubber I and the epihalohydrin-based rubber II.
[0045] As the acid acceptor, a known acid acceptor can be used depending on the crosslinking agent, and a metal compound and / or an inorganic microporous crystal is used.
[0046] Examples of the metal compounds include oxides, hydroxides, carbonates, carboxylates, silicates, borates, and phosphites of metals in Group II (Groups 2 and 12) of the periodic table, and oxides, basic carbonates, basic carboxylates, basic phosphites, basic sulfites, and tribasic sulfates of non-lead metals in Group IV (Groups 4 and 14) of the periodic table.
[0047] Specific examples of the metal compound include magnesium oxide, magnesium hydroxide, barium hydroxide, magnesium carbonate, barium carbonate, sodium carbonate, quicklime, slaked lime, calcium carbonate, calcium silicate, calcium stearate, zinc stearate, calcium phthalate, calcium phosphite, zinc oxide, tin stearate, basic tin phosphite, etc. Particularly preferred acid acceptors include magnesium oxide, calcium carbonate, slaked lime, and quicklime.
[0048] Inorganic microporous crystals refer to crystalline porous bodies, and are clearly distinguishable from amorphous porous bodies such as silica gel and alumina. Examples of such inorganic microporous crystals include zeolites, alumina phosphate-type molecular sieves, layered silicates, hydrotalcites, and alkali metal titanates. Particularly preferred acid acceptors include hydrotalcites.
[0049] When the acid acceptor is contained, the content thereof is preferably from 0.5 to 10 parts by mass, and more preferably from 1 to 8 parts by mass, per 100 parts by mass in total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0050] As the filler, a known filler can be used, and specific examples thereof include calcium carbonate, talc, silica, clay, carbon fiber, glass fiber, carbon black, titanium oxide, magnesium oxide, hydrotalcite, magnesium hydroxide, antimony oxide, zinc oxide, etc. Among these, carbon black, magnesium oxide, and silica are preferred, and carbon black and magnesium oxide are more preferred. When a filler is contained, the content thereof is preferably 1 to 200 parts by mass, more preferably 5 to 100 parts by mass, relative to 100 parts by mass in total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0051] The crosslinking accelerator may be, for example, a tertiary amine. Specific examples of the tertiary amine include aliphatic tertiary amines, dithiocarbamic acid salts, and diazabicycloalkene compounds. Among these, diazabicycloalkene compounds are preferred from the viewpoints of normal physical properties and heat resistance.
[0052] Specific examples of aliphatic tertiary amines include trimethylamine, triethylamine, tripropylamine, triallylamine, triisopropylamine, tri-n-butylamine, tri-t-butylamine, tri-sec-butylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, triundecylamine, and tridodecylamine.
[0053] Specific examples of dithiocarbamate include zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc dipentyldithiocarbamate, zinc dihexyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc dibenzyldithiocarbamate, copper dipropyldithiocarbamate, copper diisopropyldithiocarbamate, copper dibutyldithiocarbamate, sodium diethyldithiocarbamate, sodium diisopropyldithiocarbamate, sodium dibutyldithiocarbamate, ferric dimethyldithiocarbamate, and ferric diethyldithiocarbamate.
[0054] Specific examples of the diazabicycloalkene compound include 1,8-diazabicyclo(5.4.0)undecene-7 (DBU), 1,5-diazabicyclo(4.3.0)nonene-5, 1,4-diazabicyclo(2.2.2)octane, and their p-toluenesulfonate salts, phenol salts, phenol resin salts, orthophthalate salts, formate salts, octylate salts, naphthoate salts, etc. Among these, from the viewpoints of normal state physical properties and handling, 1,8-diazabicyclo(5.4.0)undecene-7, naphthoate salts and phenol resin salts of 1,8-diazabicyclo(5.4.0)undecene-7 are preferred.
[0055] When the crosslinking accelerator is contained, the content thereof is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass in total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0056] Examples of the crosslinking retarder include N-cyclohexylthiophthalimide, phthalic anhydride, an organic zinc compound, acidic silica, etc. When the crosslinking retarder is contained, the content thereof is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, per 100 parts by mass in total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0057] Examples of the crosslinking agent include polyamine-based crosslinking agents, thiourea-based crosslinking agents, thiadiazole-based crosslinking agents, mercaptotriazine-based crosslinking agents, pyrazine-based crosslinking agents, quinoxaline-based crosslinking agents, and bisphenol-based crosslinking agents.
[0058] Examples of polyamine crosslinking agents include ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, p-phenylenediamine, cumenediamine, N,N'-dicinnamylidene-1,6-hexanediamine, ethylenediamine carbamate, and hexamethylenediamine carbamate.
[0059] Examples of the thiourea-based crosslinking agent include ethylene thiourea, 1,3-diethyl thiourea, 1,3-dibutyl thiourea, and trimethyl thiourea.
[0060] Examples of the thiadiazole crosslinking agent include 2,5-dimercapto-1,3,4-thiadiazole, and 2-mercapto-1,3,4-thiadiazole-5-thiobenzoate.
[0061] Examples of mercaptotriazine crosslinking agents include 2,4,6-trimercapto-1,3,5-triazine, 2-methoxy-4,6-dimercaptotriazine, 2-hexylamino-4,6-dimercaptotriazine, 2-diethylamino-4,6-dimercaptotriazine, 2-cyclohexaneamino-4,6-dimercaptotriazine, 2-dibutylamino-4,6-dimercaptotriazine, 2-anilino-4,6-dimercaptotriazine, and 2-phenylamino-4,6-dimercaptotriazine.
[0062] Examples of pyrazine-based crosslinking agents include 2,3-dimercaptopyrazine derivatives, and examples of 2,3-dimercaptopyrazine derivatives include pyrazine-2,3-dithiocarbonate, 5-methyl-2,3-dimercaptopyrazine, 5-ethylpyrazine-2,3-dithiocarbonate, 5,6-dimethyl-2,3-dimercaptopyrazine, and 5,6-dimethylpyrazine-2,3-dithiocarbonate.
[0063] Examples of quinoxaline-based crosslinking agents include 2,3-dimercaptoquinoxaline derivatives, and examples of 2,3-dimercaptoquinoxaline derivatives include quinoxaline-2,3-dithiocarbonate, 6-methylquinoxaline-2,3-dithiocarbonate, 6-ethyl-2,3-dimercaptoquinoxaline, 6-isopropylquinoxaline-2,3-dithiocarbonate, and 5,8-dimethylquinoxaline-2,3-dithiocarbonate.
[0064] Examples of bisphenol-based crosslinking agents include 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfone (bisphenol S), 1,1-cyclohexylidene-bis(4-hydroxybenzene), 2-chloro-1,4-cyclohexylene-bis(4-hydroxybenzene), 2,2-isopropylidene-bis(4-hydroxybenzene) (bisphenol A), hexafluoroisopropylidene-bis(4-hydroxybenzene) (bisphenol AF), and 2-fluoro-1,4-phenylene-bis(4-hydroxybenzene).
[0065] When a crosslinking agent is contained, the content thereof is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass in total of the epihalohydrin rubber I and the epihalohydrin rubber II.
[0066] Method for producing rubber composition The rubber composition of the present invention can be produced by any means conventionally used in the field of rubber processing, such as a mixing roll, a Banbury mixer, or various kneaders.
[0067] The manufacturing procedure can be the usual procedure used in the field of rubber processing. For example, the rubber components alone are first mixed, then compounding ingredients other than the crosslinking agent and crosslinking accelerator are added to prepare kneaded compound A, and then kneaded compound B is performed, in which the crosslinking agent and crosslinking accelerator are added.
[0068] The rubber composition of the present invention thus obtained has excellent roll processability during processing. When the rubber composition of the present invention is formed into a sheet (uncrosslinked sheet) having a thickness of about 2 to 2.5 mm, the scorch time t5 (JIS K6300) at a temperature of 125°C is 60 minutes or less, preferably 5 minutes or more and 60 minutes or less, more preferably 5.5 minutes or more and 60 minutes or less, and even more preferably 6 minutes or more and 55 minutes or less. If the scorch time t5 is too long, the crosslinking speed is slow, and it takes time to completely crosslink, and good crosslinking properties and adhesiveness may not be obtained. The scorch time t5 can be adjusted to a desired value by adjusting the type and content of the crosslinking agent and crosslinking accelerator.
[0069] The rubber composition of the present invention can be made into a cross-linked rubber by heating it usually at 100 to 250° C. The cross-linking time varies depending on the temperature, but is usually carried out for 0.5 to 300 minutes.
[0070] A general crosslinking molding method may be any of a method of integrally performing crosslinking and molding, a method of heating a previously molded crosslinkable rubber composition again to form a crosslinked product, and a method of processing a previously heated crosslinked rubber product for molding. Specific methods for crosslinking molding include compression molding using a mold, injection molding, heating using a steam can, air bath, infrared rays, or microwaves, and other methods.
[0071] The cross-linked rubber product thus obtained is obtained by using the above-mentioned rubber composition of the present invention, and therefore has excellent roll processability during processing, and also has excellent normal physical properties when cross-linked.
[0072] The cross-linked rubber product of the present invention has good processability, normal physical properties, and is inhibited from bleeding out, and is therefore suitably used for development, charging, and transfer rolls in laser printers and copiers, as well as automotive hose materials, tube materials, mounting materials, and seal materials.
[0073] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. Tests and evaluations of physical properties and characteristics were carried out as follows. EXAMPLES
[0074] (Mooney Viscosity (ML 1+4 , 100℃) The rubber composition was measured for Mooney viscosity (ML) at a measurement temperature of 100°C using a Mooney Viscometer AM-3 manufactured by Toyo Seiki Co., Ltd. in accordance with the Mooney viscosity test of the uncrosslinked rubber physical test method of JIS K6300. 1+4 ) was measured.
[0075] (Scorch Time t5) The rubber composition was kneaded with a kneader and an open roll to prepare an uncrosslinked rubber sheet having a thickness of 2 to 2.5 mm, and the scorch time t5 (the time from the start of measurement until the Mooney viscosity increases by 5 points compared to the minimum value (Vm) of the Mooney viscosity) was measured at 125°C using a Mooney Viscometer AM-3 manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K6300. If the scorch time t5 is 5 minutes or more, good processing stability and fluidity during molding can be obtained. On the other hand, if the scorch time t5 is shorter than 5 minutes, hardening due to crosslinking begins during processing, so fluidity during molding cannot be obtained, and a crosslinked product with good appearance may not be obtained.
[0076] (Compression set) The rubber composition was pressed in a mold for preparing test pieces at 170°C for 20 minutes, and then heated in an air oven at 150°C for 2 hours to obtain a cylindrical cross-linked rubber product with a diameter of about 29 mm and a height of about 12.5 mm. Using the obtained cross-linked rubber product, testing was carried out under the conditions of 125°C and 72 hours in accordance with the method described in JIS K6262.
[0077] (Normal physical properties) The crosslinked product was subjected to a tensile test and a hardness test using a precision universal testing machine (Shimadzu Corporation: Autograph AGS-5kNX). The tensile test was performed according to the method described in JIS K6251, and the hardness test was performed according to the method described in JIS K6253.
[0078] (bleed out) The bleeding out on the rubber surface was evaluated visually using a crosslinked rubber sheet having a thickness of 2 mm.
[0079] First, in order to evaluate the epihalohydrin rubber I itself, epihalohydrin rubbers I-1, I-2, and I-3 were produced in Production Examples 1 to 3 described below, and the processability of the rubber compositions made without any filler was evaluated. (Raw materials used) <Epihalohydrin Rubber I-1; Production Example 1> Epihalohydrin rubber II: Epichromer C (Osaka Soda Co., Ltd., epichlorohydrin-ethylene oxide copolymer, epichlorohydrin-based structural units: 50 mol%, ethylene oxide-based structural units: 50 mol%) <Epihalohydrin Rubber I-2; Production Example 2> Epihalohydrin rubber II: Epichromer H (Osaka Soda Co., Ltd., epichlorohydrin homopolymer) Organic peroxide: Perbutyl P (NOF Corporation, 1,3-bis tert-butylperoxyisopropylbenzene) *Common to Production Examples 1 and 2 <Epihalohydrin Rubber I-3; Production Example 3> Epichlorohydrin (Osaka Soda Co., Ltd.) Ethylene oxide (Osaka Soda Co., Ltd.) Ethylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Antimony pentachloride (Sigma-Aldrich) Methylene chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0080] [Production Example 1] One part by mass of organic peroxide (Perbutyl P) was added to 100 parts by mass of epihalohydrin rubber II (Epichromer C), and the mixture was heated at 180°C for 15 minutes in a Gear Aging Tester (Mize Co., Ltd.) to quantitatively obtain a waxy yellow-brown solid (epihalohydrin rubber I-1). Gel permeation chromatography (GPC) was performed on epihalohydrin rubber I-1 using tetrahydrofuran (THF) as a solvent and measured in terms of polystyrene. The weight average molecular weight (Mw) was 60,000, and the proportion of molecular weights below 10,000 was 16%.
[0081] [Production Example 2] As epihalohydrin rubber II, epichromer C was changed to epichromer H, and heat treatment was carried out under the same conditions as in Production Example 1 to quantitatively obtain a waxy yellow-brown solid (epihalohydrin rubber I-2). When epihalohydrin rubber I-2 was subjected to gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and measured in terms of polystyrene, the weight average molecular weight (Mw) of epihalohydrin rubber I-2 was 60,000, and the proportion of molecular weights of 10,000 or less was 14%.
[0082] [Production Example 3] 0.12 g of ethylene glycol was added to 300 g of epichlorohydrin dried over molecular sieves, and 0.15 g of antimony pentachloride was dissolved in 12 ml of methylene chloride, and the mixture was added dropwise over 1 hour while maintaining the reaction temperature at 35 to 45°C. After 5 hours of reaction, 1 g of water was added to terminate the polymerization, and the unreacted monomer was distilled off under reduced pressure to obtain 112 g (37% yield) of a viscous liquid yellow polymer (epihalohydrin rubber I-3). Gel permeation chromatography (GPC) was performed on epihalohydrin rubber I-3 using tetrahydrofuran (THF) as a solvent, and the weight average molecular weight (Mw) of epihalohydrin rubber I-3 was 20,000, and the proportion of molecular weights of 10,000 or less was 51%.
[0083] Using the epihalohydrin rubbers I-1, I-2, and I-3 obtained in Production Examples 1 to 3, each rubber composition described in Reference Example 1, Examples 1 to 4, and Comparative Example 1 was prepared based on the formulation table in Table 1 without adding other compounding materials. The kneading conditions for Reference Example 1 were as follows: 60cc internal kneading mixer (Labo Plastomill, roller mixer: Toyo Seiki Co., Ltd.), temperature 100°C, filling rate 75%, rotation speed 40 rpm, and 3 minutes from feeding epihalohydrin rubber II (Epichromer C) to discharging. For Examples 1 to 4 and Comparative Example 1, the kneading work was performed under the same conditions as Reference Example 1, except that the epihalohydrin rubbers I-1, I-2, and I-3 were each fed after 1 minute had elapsed since feeding epihalohydrin rubber II (Epichromer C), and were discharged after a total of 3 minutes had elapsed. The dispersibility of the epihalohydrin rubber II (Epichromer C) and the epihalohydrin rubbers I-1, I-2, and I-3, and the Mooney viscosity of each of the resulting rubber compositions were measured. The results are shown in Table 1. The evaluation criteria for dispersibility were as follows: <Evaluation criteria for dispersibility> ○: Dispersed torque ×: Not dispersed and no torque applied
[0084] [Table 1]
[0085] In Examples 1 to 4 using solid epihalohydrin rubber I-1 and epihalohydrin rubber I-2, it was found that the Mooney viscosity decreased and processability improved in proportion to the increase in the compounding amount up to 30 parts by mass relative to 100 parts by mass of epihalohydrin rubber II (Epichromer C). On the other hand, in Comparative Example 1 using viscous liquid epihalohydrin rubber I-3, the rubber was in a finely crushed state, the dispersibility was poor, and no torque was applied to allow sufficient dispersion. Therefore, the Mooney viscosity could not be measured.
[0086] Since improved processability was confirmed for solid epihalohydrin-based rubber I (epihalohydrin-based rubber I-1 and epihalohydrin-based rubber I-2), rubber compositions with practical blends including fillers, etc. were prepared and the rubber properties and the presence or absence of bleed-out on the rubber surface were confirmed.
[0087] (Raw materials used) Compound A Epihalohydrin rubber I-1 (weight average molecular weight (Mw): 60,000, proportion of molecular weights below 10,000: 16%) Epihalohydrin rubber II: Epichromer C (Osaka Soda Co., Ltd., epichlorohydrin-ethylene oxide copolymer, epichlorohydrin-based structural units: 50 mol%, ethylene oxide-based structural units: 50 mol%) Lubricant: Splendor R-300V (Kao Corporation, sorbitan monostearate) Anti-aging agent: Nocrac NBC (Ouchi Shinko Chemical Co., Ltd., nickel dibutylcarbamate) Carbon black (filler): Seast SO (manufactured by Tokai Carbon Co., Ltd., classification according to ASTM D1765: N550) Acid acceptor: MgO#150 (Kyowa Chemical Industry Co., Ltd., magnesium oxide), Stabiace HT-1 (Sakai Chemical Industry Co., Ltd., hydrotalcite) Crosslinking accelerator: P-152 (Osaka Soda Co., Ltd., phenolic resin salt of DBU) B Compound Crosslinking agent: DAISONET XL-21S (Osaka Soda Co., Ltd., quinoxaline-based crosslinking agent) · Crosslinking retarder: Retarder CTP (Ouchi Shinko Chemical Co., Ltd., N-cyclohexylthiophthalimide)
[0088] Based on the recipe in Table 2, each compounding ingredient was kneaded in a kneader (temperature 100°C), pressure pressed at a temperature of 170°C for 15 minutes, and hot air crosslinked at 150°C for 2 hours to obtain sheets of the crosslinked rubber of Reference Example 2 and Examples 5 to 6. Processability (Mooney viscosity; ML 1+4 The results of the compression set test (CS), minimum Mooney viscosity (Vm), scorch time (t5), normal physical properties (tensile stress (M100), tensile strength (Tb), elongation (Eb), and hardness (Hs) are shown in Table 2.
[0089] [Table 2]
[0090] The results in Table 2 show that, compared with Reference Example 2 in which the solid epihalohydrin rubber I-1 was not compounded, Examples 5 and 6 had lower Mooney viscosities and improved processability. The same tendency was observed for Vm, and it was found that in Examples 5 and 6, Vm could be reduced to about half that of Reference Example 2, which did not contain the epihalohydrin rubber I-1, and that the materials had good processability. It was confirmed that the normal physical properties were excellent when compared with Reference Example 2 in which the epihalohydrin rubber I-1 was not compounded. In the compression set test, Example 6 gave results equivalent to those of Reference Example 2. No bleeding out was observed on the sheet surfaces of the cross-linked rubbers obtained in Reference Example 2 and Examples 5 to 6, and it was revealed that the rubber compositions using epihalohydrin rubber I improve the processability of the rubber while maintaining the normal physical properties and causing no bleeding out.
[0091] Variations of the invention according to the present disclosure are described below. [Appendix 1] Epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000. [Appendix 2] The epihalohydrin-based rubber according to Appendix 1, characterized in that it contains at least one structural unit derived from a compound selected from an alkylene oxide and an epihalohydrin, and the molar ratio of alkylene oxide:epihalohydrin is in the range of 0:100 to 90:10. [Appendix 3] The epihalohydrin rubber according to appendix 1 or 2, which is a decomposition product of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000. [Appendix 4] A rubber composition comprising 100 parts by mass of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 and 10 to 150 parts by mass of the epihalohydrin rubber according to any one of Appendices 1 to 3. [Appendix 5] A method for producing an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000, comprising reacting an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 in the presence of an oxidizing agent. [Appendix 6] A method for producing an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000 according to Appendix 5, wherein the oxidizing agent is at least one selected from the group consisting of organic peroxides and inorganic peroxides.
Claims
1. An epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000.
2. The epihalohydrin rubber according to claim 1, characterized in that it contains at least one structural unit derived from a compound selected from an alkylene oxide and an epihalohydrin, and the molar ratio of alkylene oxide:epihalohydrin is in the range of 0:100 to 90:
10.
3. 3. The epihalohydrin rubber according to claim 1 or 2, which is a decomposition product of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000.
4. A rubber composition comprising 100 parts by mass of an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 and 10 to 150 parts by mass of the epihalohydrin rubber according to claim 1 or 2.
5. A method for producing an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000, comprising reacting an epihalohydrin rubber having a weight average molecular weight (Mw) of 600,000 to 3,000,000 in the presence of an oxidizing agent.
6. 6. The method for producing an epihalohydrin rubber having a weight average molecular weight (Mw) of 30,000 to 200,000 according to claim 5, wherein the oxidizing agent is at least one selected from the group consisting of organic peroxides and inorganic peroxides.
Citation Information
Patent Citations
Conductive rubber composition for electrophotographic apparatus and conductive roll
JP1998087892A
Epihalohydrin rubber and method for producing the same
JP2006232997A
Manufacturing method of hollow fiber membrane
JP2008161755A
Method for producing polyether-based polymer, and polyether-based polymer
JP2010053217A
High polymer of oxirane compound, and method for producing the same
JP2010265425A