Resin concrete composition, resin concrete hardened product, and fiber-reinforced plastic composite pipe

A resin concrete composition with specific aggregate particle size distribution simplifies the molding process and enhances the strength of fiber-reinforced plastic composite pipes by optimizing resin mortar layer integrity and reducing porosity.

JP2024145492APending Publication Date: 2024-10-15SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023057867
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The complexity of molding fiber-reinforced plastic composite pipes is increased by coating the resin mortar layer with a coupling agent, necessitating a simpler method to enhance the strength of these pipes.

Method used

A resin concrete composition is developed using aggregate with a specific particle size distribution to reduce porosity and increase the strength of the resin mortar layer, comprising aggregate and thermosetting resin, with conditions on particle size ratios and volume fractions to optimize filling structure and porosity.

Benefits of technology

The composition improves the strength of fiber-reinforced plastic composite pipes by enhancing the resin mortar layer's integrity, reducing porosity, and alleviating thermal stress, while potentially lowering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145492000004
    Figure 2024145492000004
  • Figure 2024145492000005
    Figure 2024145492000005
  • Figure 2024145492000001
    Figure 2024145492000001
Patent Text Reader

Abstract

To provide: a resin concrete composition capable of improving strength of fiber-reinforced plastic composite pipes by a composition of resin concrete composition only; a resin concrete hardened material; and a fiber-reinforced plastic composite pipe.SOLUTION: A resin concrete composition includes an aggregate and a thermosetting resin, and the aggregate satisfies the following conditions. <Conditions> When the most frequent particle diameter is a particle diameter (1) among the particle diameters with a cumulative frequency of 80% or less from the small diameter side of the aggregate volume basis, and when the most frequent particle diameter is a particle diameter (2) among the particle diameters with a cumulative frequency of more than 80% from the small diameter side of the aggregate volume basis, the proportion of the particle diameter (1) in the frequency distribution is 15% or more, the proportion of the particle diameter (2) in the frequency distribution is 15% or more, a ratio of the volume fraction of the particle diameter (2) to the particle diameter (1) is 0.60 or more and 1.5 or less, and a ratio of the particle diameter (1) to the particle diameter (2) is 0.3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin concrete composition, a hardened resin concrete product, and a fiber-reinforced plastic composite pipe. [Background technology]

[0002] Fiber-reinforced plastic composite pipes generally have a structure in which a fiber-reinforced resin layer containing fiber-reinforced resin is laminated on at least one of the inner and outer surfaces of a resin mortar layer formed by molding a resin concrete composition and hardening the resin mortar layer. The resin concrete composition is a composition containing a synthetic resin as a binder and aggregate. The synthetic resin is a thermosetting resin such as unsaturated polyester, acrylic resin, epoxy resin, or phenolic resin.

[0003] The resin mortar layer made of the resin concrete composition affects the strength of the fiber reinforced plastic composite pipe.

[0004] It is known that the bending strength of a fiber-reinforced plastic composite pipe can be improved by coating the resin mortar layer with a coupling agent (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-164400 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, coating the resin mortar layer with a coupling agent makes the molding of the fiber-reinforced plastic composite pipe complicated, so there has been a demand for a fiber-reinforced plastic composite pipe that has improved strength only through the composition of the resin concrete composition.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a resin concrete composition that can improve the strength of a fiber-reinforced plastic composite pipe solely through the composition of the resin concrete composition, a hardened resin concrete product obtained by hardening the resin concrete composition, and a fiber-reinforced plastic composite pipe. [Means for solving the problem]

[0008] The inventors discovered that by using aggregate with a specific particle size distribution in a resin concrete composition, the porosity of the resin mortar layer can be reduced and the strength of the resin mortar layer can be increased, and thus completed the present invention. The present invention has the following aspects. [1] A resin concrete composition comprising aggregate and a thermosetting resin, A resin concrete composition, wherein the aggregate satisfies the following conditions: <Condition> Among the particle sizes of the aggregate whose cumulative frequency from the small diameter side on a volume basis is 80% or less, the most frequent particle size is defined as particle size (1), and among the particle sizes of the aggregate whose cumulative frequency from the small diameter side on a volume basis is more than 80%, the most frequent particle size is defined as particle size (2). The proportion of particle size (1) in the frequency distribution is 15 volume % or more, The proportion of particle size (2) in the frequency distribution is 15 volume % or more, a ratio of the volume fraction of the particle size (2) to the particle size (1) is 0.60 or more and 1.5 or less; The ratio of the particle size (1) to the particle size (2) is 0.3 or less. [2] A resin concrete composition as described in [1], wherein the average particle size in the volume-based particle size distribution of the aggregate is 10 μm or more and 5,000 μm or less. [3] The resin concrete composition according to [1] or [2], further comprising a filler. [4] The resin concrete composition according to any one of [1] to [3], wherein the filler is at least one of calcium carbonate and crushed resin concrete. [5] A hardened resin concrete product comprising a hardened resin concrete composition according to any one of [1] to [4]. [6] A fiber-reinforced plastic composite pipe having a resin mortar layer and a fiber-reinforced resin layer laminated on at least one of the inner and outer surfaces of the resin mortar layer, The resin mortar layer is made of a hardened product of the resin concrete composition according to any one of [1] to [4], The fiber reinforced plastic composite pipe, wherein the fiber reinforced resin layer is made of fiber reinforced resin. Effect of the Invention

[0009] According to the present invention, it is possible to provide a resin concrete composition and a fiber reinforced plastic composite pipe that can improve the strength of a fiber reinforced plastic composite pipe simply by using the composition of the resin concrete composition. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view showing a fiber-reinforced plastic composite pipe according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing particle size distributions of aggregates in an example and comparative examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The resin concrete composition, the resin concrete hardened product, and the fiber-reinforced plastic composite pipe of the present invention will be described below with reference to the embodiments, however, the present invention is not limited to the following embodiments. In this specification, numerical ranges expressed using "to" include both ends of the numerical range.

[0012] [Resin concrete composition] A resin concrete composition according to one embodiment of the present invention contains aggregate and a thermosetting resin. The resin concrete composition of this embodiment is a composition containing aggregate and resin, and is not limited to the type of aggregate, the size of the aggregate, the type of resin, the presence or absence of other fillers, etc. The resin concrete composition of the present embodiment includes compositions called resin concrete, resin mortar, and resin mortar, which are described in JIS A 1181 "Testing methods for resin concrete."

[0013] "aggregate" The resin concrete composition of the present embodiment contains aggregate, thereby reducing the content of thermosetting resin in the resin concrete composition. This reduces the amount of heat generated when the thermosetting resin hardens, and reduces the temperature difference between the surface and the inside of the resin concrete composition when the resin concrete composition hardens, thereby suppressing the occurrence of cracks. In addition, the amount of shrinkage when the thermosetting resin hardens is reduced, and the shrinkage when the resin concrete composition hardens is reduced. Furthermore, the amount of thermosetting resin used can be reduced, thereby reducing the cost of the resin concrete composition.

[0014] The type of aggregate is not particularly limited, but aggregates that have been conventionally mixed in resin concrete compositions, such as silica sand, gravel, crushed stone, boulders, blast furnace slag aggregate, or artificial lightweight aggregate, can be used. As an aggregate, an aggregate with a high silicon dioxide content is preferred, and silica sand is particularly preferred, because this has low reactivity with carbon dioxide and water in the atmosphere and slows down deterioration of the hardened product of the resin concrete composition of this embodiment. The aggregate may be used alone or in combination of two or more kinds.

[0015] The average particle size (median diameter) in the volumetric particle size distribution of the aggregate is not particularly limited, but is preferably 10 μm or more and 5000 μm or less, more preferably 75 μm or more and 3000 μm or less, and even more preferably 180 μm or more and 2500 μm or less.

[0016] When silica sand is used as the aggregate, commercially available products include, for example, silica sand No. 6 (average particle size 0.3 mm: manufactured by Mikyu Kaiun Co., Ltd.), silica sand No. 3 (average particle size 1 mm: manufactured by Mikyu Kaiun Co., Ltd.), and silica sand No. 7 (average particle size 0.1 mm: manufactured by Mikyu Kaiun Co., Ltd.), but are not limited to these. As commercially available silica sand, it is preferable to use one or more types selected from the group consisting of silica sand No. 6, silica sand No. 3, and silica sand No. 7, and silica sand may be used alone or two or more types of silica sand may be mixed together.

[0017] The content of the aggregate in the resin concrete composition of the present embodiment is not particularly limited, but is preferably 60 parts by mass to 90 parts by mass per 100 parts by mass of the resin concrete composition.

[0018] In the resin concrete composition of this embodiment, the total volume of the aggregate is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more in the resin concrete composition. If the total volume of the aggregate is less than the lower limit, there is a high possibility that the particles will not come into contact with each other and the intended packed structure will not be obtained.

[0019] In the resin concrete composition of this embodiment, the total volume of aggregate is preferably 90% or less, more preferably 85% or less, and even more preferably 80% or less, of the resin concrete composition.

[0020] In the resin concrete composition of this embodiment, the aggregate satisfies the following conditions. <Condition> Among the particle sizes of the aggregate whose cumulative frequency from the small diameter side on a volume basis is 80% or less, the most frequent particle size is defined as particle size (1), and among the particle sizes of the aggregate whose cumulative frequency from the small diameter side on a volume basis is more than 80%, the most frequent particle size is defined as particle size (2). The proportion of particle size (1) in the frequency distribution is 15 volume % or more, The proportion of particle size (2) in the frequency distribution is 15 volume % or more, a ratio of the volume fraction of the particle size (2) to the particle size (1) is 0.60 or more and 1.5 or less; The ratio of the particle size (1) to the particle size (2) is 0.3 or less.

[0021] In the resin concrete composition of this embodiment, the particle size distribution of the aggregate is measured by a sieve shaker using a sieve conforming to JIS Z 8801 "Test sieves - Part 1: Metal mesh sieves".

[0022] The proportion of particle size (1) in the frequency distribution is 15 volume % or more, preferably 17 volume % or more, and more preferably 19 volume % or more. If the particle size (1) is less than the lower limit, the packed structure collapses and the porosity deteriorates (increases).

[0023] The proportion of particle size (1) in the frequency distribution is preferably 70 vol % or less, more preferably 50 vol % or less, and even more preferably 30 vol % or less.

[0024] The proportion of the particle size (2) in the frequency distribution is 15 volume % or more, preferably 17 volume % or more, and more preferably 19 volume % or more. If the particle size (2) is less than the lower limit, the packed structure collapses and the porosity deteriorates (increases).

[0025] The proportion of particle size (2) in the frequency distribution is preferably 70 vol. % or less, more preferably 50 vol. % or less, and even more preferably 30 vol. % or less.

[0026] The sum of the proportion of particle size (1) in the frequency distribution and the proportion of particle size (2) in the frequency distribution is 30% by volume or more, preferably 50% by volume or more, and more preferably 70% by volume or more. If the sum is less than the lower limit, the packing structure collapses and the porosity deteriorates (increases).

[0027] The sum of the proportion of particle size (1) in the frequency distribution and the proportion of particle size (2) in the frequency distribution is preferably 30 vol. % or less, more preferably 34 vol. % or less, and even more preferably 38 vol. % or less.

[0028] The ratio of the volume fraction of the particle diameter (2) to the particle diameter (1) (volume fraction of particle diameter (1) / volume fraction of particle diameter (2)) is 0.60 or more and 1.5 or less, preferably 0.8 or more and 1.3 or less, and more preferably 0.9 or more and 1.2 or less. If the ratio is less than the lower limit, the packing structure collapses and the porosity deteriorates (increases). If the ratio exceeds the upper limit, the packing structure collapses and the porosity deteriorates (increases).

[0029] The difference between the proportion of particle size (1) in the frequency distribution and the proportion of particle size (2) in the frequency distribution is preferably 15% by volume or less, more preferably 10% by volume or less, and even more preferably 5% by volume or less. If the difference is greater than the lower limit, the packed structure collapses and the porosity deteriorates (increases).

[0030] The ratio of the particle size (1) to the particle size (2) (particle size (1) / particle size (2)) is 0.3 or less, preferably 0.26 or less, and more preferably 0.22 or less. If the ratio exceeds the upper limit, the packed structure collapses and the porosity deteriorates (increases).

[0031] The particle ratio is preferably 0.002 or more, more preferably 0.004 or more, and even more preferably 0.012 or more.

[0032] The difference between the particle size (1) and the particle size (2) is preferably 4890 μm or less, more preferably 2490 μm or less, and even more preferably 2470 μm or less. If the difference is equal to or greater than the lower limit, the packed structure collapses and the porosity deteriorates (increases).

[0033] The difference in mode diameter between the particle diameter (1) and the particle diameter (2) is preferably 900 μm or more and 1000 μm or less.

[0034] "Thermosetting resin" Examples of the thermosetting resin include unsaturated polyester resin, vinyl ester resin, epoxy resin, acrylic resin, phenol resin, polyimide resin, melamine resin, urethane resin, etc. Among these, unsaturated polyester resin is preferred from the viewpoints of cost and moldability.

[0035] <Unsaturated polyester resin> The unsaturated polyester resin contains an unsaturated polyester (a) and a polymerizable unsaturated monomer (b).

[0036] The unsaturated polyester (a) is preferably prepared by using a saturated dibasic acid (a1), an unsaturated dibasic acid (a2), and a glycol (a3) ​​as raw materials.

[0037] The saturated dibasic acid (a1) is a dibasic acid that does not contain a non-conjugated double bond between carbon atoms in one molecule, such as orthophthalic acid, isophthalic acid, terephthalic acid, adipic acid, etc. The saturated dibasic acid (a1) may be used alone or in combination of two or more kinds, as necessary. The unsaturated dibasic acid (a2) is a dibasic acid containing one or more carbon-carbon non-conjugated double bonds in one molecule, such as maleic anhydride or fumaric acid. The unsaturated dibasic acid (a2) may be used alone or in combination of two or more kinds, as necessary.

[0038] The glycol (a3) ​​is a diol containing two hydroxy groups in one molecule, such as an alkylene glycol, such as ethylene glycol or propylene glycol, a polyoxyalkylene glycol, such as dialkylene glycol or trialkylene glycol, or a bisphenol, such as bisphenol A or bisphenol F. The glycol (a3) ​​may be used alone or in combination of two or more kinds, as necessary.

[0039] The unsaturated polyester (a) can further use, as a raw material, a monomer (a4) having one or two carbon atom-carbon non-conjugated double bonds in one molecule, which is not included in either the unsaturated dibasic acid (a2) or the glycol (a3). Examples of such monomer (a4) include, but are not limited to, styrene, propylene, dicyclopentadiene, and (meth)acrylic acid alkyl esters. The monomer (a4) may be used alone or in combination of two or more types, as necessary.

[0040] The method for synthesizing the unsaturated polyester (a) is not particularly limited, and may be a method in which a saturated dibasic acid (a1), an unsaturated dibasic acid (a2), a glycol (a3), and, if desired, a monomer (a4) are simultaneously charged and condensed.

[0041] Depending on the type of saturated dibasic acid (a1) or the type of glycol (a3), unsaturated polyester resins may be classified into ortho-unsaturated polyester resins, iso-unsaturated polyester resins, tere-unsaturated ester resins, and bis-unsaturated polyester resins.

[0042] The polymerizable unsaturated monomer (b) is not particularly limited, and any of those conventionally used in unsaturated polyester resins can be used. Examples of the polymerizable unsaturated monomer (b) include styrene, α-methylstyrene, chlorostyrene, dichlorostyrene, divinylbenzene, t-butylstyrene, vinyltoluene, vinyl acetate, diaryl phthalate, triaryl cyanurate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate. , (meth) acrylate stearyl, (meth) acrylate tridecyl, dicyclopentenyloxyethyl (meth) acrylate, ethylene glycol monomethyl ether (meth) acrylate, ethylene glycol monoethyl ether (meth) acrylate, ethylene glycol monobutyl ether (meth) acrylate, ethylene glycol monohexyl ether (meth) acrylate, ethylene glycol mono 2-ethylhexyl ether (meth) acrylate, diethylene glycol monomethyl ether (meth) acrylate, diethylene glycol monoethyl ether (meth) acrylate, diethylene glycol monobutyl ether (meth) acrylate, diethylene glycol monohexyl ether (meth) acrylate, diethylene glycol mono 2-ethylhexyl ether (meth) acrylate, dipropylene glycol monomethyl ether (meth) acrylate, dipropylene glycol monoethyl ether (meth) acrylate, dipropylene glycol monobutyl ether (meth) acrylate, dipropylene glycol monohexyl ether (meth) a Acrylate, dipropylene glycol mono 2-ethylhexyl ether (meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polytetramethylene glycol dimethacrylate, 1,3-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-hydroxy-1,3-dimethacryloxypropane, 2,2-bis[4-(methacryloxyethoxy)phenyl]propane, 2,Examples of the diacrylate include, but are not limited to, 2-bis[4-(methacryloxydiethoxy)phenyl]propane, 2,2-bis[4-(methacryloxypolyethoxy)phenyl]propane, tetraethylene glycol diacrylate, bisphenol A ethylene oxide adduct (n=2) diacrylate, isocyanuric acid ethylene oxide adduct (n=3) diacrylate, and pentaerythritol diacrylate monostearate. The polymerizable unsaturated monomer (b) may be used alone or in combination of two or more kinds, as necessary.

[0043] The number average molecular weight of the unsaturated polyester (a) is not particularly limited, but is preferably 400 to 1500, more preferably 400 to 1200, and even more preferably 400 to 1000. When the number average molecular weight of the unsaturated polyester (a) is within this range, the flowability and the like of the unsaturated polyester resin are good, and the moldability is improved.

[0044] The content of the unsaturated polyester (a) and the polymerizable unsaturated monomer (b) in the unsaturated polyester resin is not particularly limited, but it is preferable that the unsaturated polyester (a) is 80 to 60 parts by mass, and the polymerizable unsaturated monomer (b) is the remainder, based on the total amount of the unsaturated polyester (a) and the polymerizable unsaturated monomer (b) being 100 parts by mass. If it is within this range, the shrinkage, physical properties and moldability of the polyester resin will be better.

[0045] The unsaturated polyester resin may contain compounds other than the compound used in the synthesis of the unsaturated polyester (a) and the polymerizable unsaturated monomer (b) within the range that does not impair the effects of the present invention.

[0046] Commercially available unsaturated polyester resins include iso-type unsaturated polyester resins (manufactured by Nippon U-Pica Corporation).

[0047] The content of unsaturated polyester resin in the resin concrete composition of this embodiment is not particularly limited, but is preferably 10 to 30 parts by mass, more preferably 10 to 20 parts by mass, and even more preferably 10 to 15 parts by mass, per 100 parts by mass of the resin concrete composition. In addition, in the resin concrete composition of this embodiment, a thermosetting resin other than unsaturated polyester may be used in combination as a binder, but the content of the unsaturated polyester resin is more than 50 parts by mass and not more than 100 parts by mass per 100 parts by mass of the binder, preferably 65 to 100 parts by mass, more preferably 80 to 100 parts by mass, and even more preferably 95 to 100 parts by mass.

[0048] "Filling material" The resin concrete composition of the present embodiment may further contain a filler. When the resin concrete composition of the present embodiment contains a filler, the filler can penetrate into the gaps between the silica sand, enabling fine filling. It is expected that the workability of the composition will be improved by improving its moldability, and that the physical properties of the hardened product, such as toughness, will be improved.

[0049] The filler is not particularly limited, but is preferably at least one selected from the group consisting of calcium carbonate, silica, clay, mica, talc, wollastonite, alumina, aluminum hydroxide, kaolin, and crushed resin concrete, and more preferably at least one of calcium carbonate and crushed resin concrete. The filler may be used alone or in combination of two or more kinds, as required.

[0050] The particle size of the filler is not particularly limited, but is preferably 100 μm or less, more preferably 0.05 to 50 μm, and even more preferably 0.1 to 10 μm. Here, the particle size of the filler is a value measured by an optical microscope or an electron microscope.

[0051] When calcium carbonate is used as the filler, examples of commercially available products include, but are not limited to, Whiten (particle size 3 μm; manufactured by Shiraishi Kogyo Co., Ltd.).

[0052] When the resin concrete composition of this embodiment contains a filler, the content of the filler is not particularly limited, but the total amount of aggregate and filler is preferably 75 to 95 parts by mass per 100 parts by mass of the resin concrete composition of this embodiment.

[0053] "Polymerization inhibitor" The resin concrete composition of the present embodiment may further contain a polymerization inhibitor. By containing a polymerization inhibitor, the reaction between the unsaturated polyester and the polymerizable unsaturated monomer is suppressed, thereby improving safety. The polymerization inhibitor is not particularly limited, but examples of the polymerization inhibitor that can be used include hydroquinone, toluhydroquinone, trimethylhydroquinone, tertiary butylhydroquinone, ditertiary butylhydroquinone, tertiary butylcatechol, methoxyhydroquinone, benzoquinone, tertiary butylquinone, and phenothiazine. The polymerization inhibitor may be used alone or in combination of two or more kinds. When the resin concrete composition of this embodiment contains a polymerization inhibitor, the content of the polymerization inhibitor is not particularly limited, but is preferably 0.0001 to 0.1 part by mass per 100 parts by mass of the resin concrete composition of this embodiment.

[0054] "Hardening agents and curing accelerators" In order to harden the resin concrete composition of the present embodiment, it is preferable to add a hardener and heat the composition. The hardener may be used in combination with a hardening accelerator.

[0055] (hardening agent) The curing agent is not particularly limited, but an organic peroxide catalyst is preferable. Organic peroxides such as methyl ethyl ketone peroxide, benzoyl peroxide, dicumyl peroxide, diisopropyl peroxide, di-t-butyl peroxide, t-butyl peroxybenzoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3,3-isopropyl hydroperoxide, t-butyl hydroperoxide, dicumyl peroxide, dicumyl hydroperoxide, acetyl peroxide, bis(4-t-butylcyclohexyl)peroxydicarbonate, diisopropyl peroxydicarbonate, isobutyl peroxide, 3,3,5-trimethylhexanoyl peroxide and lauryl peroxide, as well as azo-based polymerization initiators such as azobisisobutyronitrile and azobiscarbonamide can be used. The curing agent may be used alone or in combination of two or more kinds.

[0056] When a hardener is added to the resin concrete composition of this embodiment, the amount added is not particularly limited, but is preferably 0.1 to 4 parts by mass, and more preferably 0.3 to 3 parts by mass, per 100 parts by mass of the resin concrete composition of this embodiment. The hardener is preferably added before molding the resin concrete composition of the present embodiment. After molding the resin concrete composition of the present embodiment, the resin concrete composition is heated and hardened to obtain a shaped hardened resin concrete product.

[0057] (Cure accelerator) The curing accelerator is not particularly limited, but may be metal soaps such as vanadyl octenate, copper naphthenate, barium naphthenate, cobalt naphthenate, and cobalt octenate, Li3[Co(NO2)6], Li3[Co(NO2)5Cl], Li3[Co(NO2)5Br], Li3[Co(NO2)4Cl2], Li3[Co(NO2)4Br2], Na3[Co(NO2)6], Na3 Cobalt compounds such as [Co(NO2)5Cl], Na3[Co(NO2)5Br], Na3[Co(NO2)4Cl2], Na3[Co(NO2)4Br2], K3[Co(NO2)6], K3[Co(NO2)5Cl], K3[Co(NO2)5Br], K3[Co(NO2)4Cl2] and K3[Co(NO2)4Br2], vanadyl acetylacetate, cobalt acetylacetate Metal chelate compounds such as iron acetate and iron acetylacetonate, and amines such as N,N-dimethylamino-p-benzaldehyde, N,N-dimethylaniline, N,N-diethylaniline, methylhydroxyethylaniline, N,N-dimethyl-p-toluidine, N,N-bis(2-hydroxyethyl)-p-toluidine, 4-N,N-dimethylaminobenzaldehyde, 4-N,N-bis(2-hydroxyethyl)aminobenzaldehyde, 4-methylhydroxyethylaminobenzaldehyde, N,N-bis(2-hydroxypropyl)-p-toluidine, N-ethyl-m-toluidine, triethanolamine, m-toluidine, diethylenetriamine, pyridine, phenylmorpholine, piperidine, and diethanolaniline can be used. The curing accelerator may be used alone or in combination of two or more kinds.

[0058] When the resin concrete composition of the present embodiment contains a hardening accelerator, the content of the hardening accelerator is not particularly limited, but is preferably 0.001 to 5 parts by mass per 100 parts by mass of the resin concrete composition of the present embodiment. The hardening accelerator may be added to the resin concrete composition of this embodiment before the hardener is added, or may be added to the resin concrete composition simultaneously with the hardener.

[0059] "Other ingredients" In addition to the above-mentioned components, additives such as ultraviolet absorbers, pigments, viscosity reducers, antioxidants, plasticizers, flame retardants, stabilizers, or reinforcing materials may be contained within the scope of not impairing the effects of this embodiment.

[0060] "Method for producing resin concrete composition" The method for producing the resin concrete composition of the present embodiment is not particularly limited, but examples thereof include the following method. The aggregate, the thermosetting resin, and the hardener are mixed and kneaded using a mixer. When mixing the aggregate and the thermosetting resin, one or more selected from a filler, an additive, and a hardening accelerator may be mixed together, if desired. Various modifications are possible, such as adding the curing accelerator and curing agent just before producing the cured product.

[0061] [Hardened resin concrete] The hardened resin concrete according to one embodiment of the present invention is made of the hardened resin concrete composition according to the present embodiment.

[0062] Specific examples of hardened resin concrete products include the resin mortar portion of fiber-reinforced plastic composite pipes, manholes, drainage manholes, building material blocks, pavement blocks, covers, pipe materials, repair materials and other civil engineering and construction molded products, artificial marble molded products, landscaping molded products, chairs, benches, CC boxes (for underground burial of information and communication power) boxes, information-related molded products, and power-related molded products.

[0063] "Method for manufacturing hardened resin concrete" The method for producing the resin concrete composition of this embodiment is not particularly limited, but examples thereof include a cast molding method, a centrifugal molding method, a compression molding method, and a continuous molding method. In the cast molding method, the resin concrete composition of the present embodiment is poured into a mold and heated to harden. In the centrifugal molding method, the resin concrete composition of this embodiment is poured into a cylindrical mold, the mold is then rotated, and the centrifugal force causes the resin concrete composition to be shaped to a uniform thickness, and the composition is then heated and hardened. In the compression molding method, the resin concrete composition of the present embodiment is poured into a mold, compressed by a press, and then heated and hardened. In the continuous molding method, the mandrel is rotated and fed forward at a constant speed, while the resin concrete composition of this embodiment is wound around it, and the mandrel is passed through a curing furnace to be heated and cured.

[0064] The hardening temperature of the resin concrete composition of the present embodiment is not particularly limited, but is preferably 50°C or higher, more preferably 50 to 60°C, and even more preferably 55 to 65°C. The hardening time of the resin concrete composition of the present embodiment is not particularly limited, but is preferably 6 hours or more, more preferably 12 hours or more, and even more preferably 24 to 48 hours.

[0065] [Fiber reinforced plastic composite pipe] Hereinafter, a fiber reinforced plastic composite pipe (hereinafter sometimes abbreviated as "FRPM pipe") according to one embodiment of the present invention will be described with reference to FIG. The FRPM pipe 1 of this embodiment has a ring-shaped or cylindrical resin mortar layer 4, an inner surface fiber-reinforced resin layer 3 located on the inner surface of the resin mortar layer 4, an outer surface fiber-reinforced resin layer 5 located on the outer surface of the resin mortar layer 4, an inner surface protective layer 2 located on the inner surface of the inner surface fiber-reinforced resin layer 3, and an outer surface protective layer 6 located on the outer surface of the outer surface of the outer surface fiber-reinforced resin layer 5. That is, the FRPM pipe 1 is composed of, in order from the inner periphery, an inner protective layer 2, an inner fiber-reinforced resin layer 3, a resin mortar layer 4, an outer fiber-reinforced resin layer 5, and an outer protective layer 6. Either the inner fiber-reinforced resin layer 3 or the outer fiber-reinforced resin layer 5 is sufficient, but it is preferable to have both. The inner protective layer 2 and the outer protective layer 6 are not necessary, but it is preferable to have one or both.

[0066] In the FRPM pipe 1 of this embodiment, the resin mortar layer is made of a hardened product of the resin concrete composition of this embodiment. The inner surface fiber-reinforced resin layer 3 and the outer surface fiber-reinforced resin layer 5 are made of fiber-reinforced resin.

[0067] "FRPM pipe manufacturing method" The manufacturing method of the FRPM pipe 1 is not particularly limited, and examples thereof include conventionally known manufacturing methods such as a filament winding method, a centrifugal molding method, a pultrusion method, or a hand lay-up method. The filament winding method is a manufacturing method in which a core tube is rotated and fed at a constant speed, and the materials for the inner protective layer 2, inner fiber reinforced resin layer 3, resin mortar layer 4, outer fiber reinforced resin layer 5, and outer protective layer 6 are sequentially wound around the core tube and heated and hardened in sequence to continuously manufacture FRPM pipes. By changing the size of the core tube, FRPM pipes of various sizes can be manufactured. Further, examples of the manufacturing method of the FRPM pipe 1 include the manufacturing method of the FRPM pipe described in Japanese Patent Application Laid-Open No. 2001-205711, paragraphs

[0016] to

[0019] , the manufacturing method of the FRPM pipe described in Japanese Patent Application Laid-Open No. 2001-205712, paragraphs

[0020] to

[0028] , and the manufacturing method of the FRPM pipe described in Japanese Patent Application Laid-Open No. 10-193467, paragraphs

[0009] to

[0019] . EXAMPLES

[0068] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0069] [Example] The aggregates used were No. 3 silica sand (average diameter 1.3 mm: manufactured by Sunnet Co., Ltd.) and No. 7 silica sand (average diameter: 0.2 mm: manufactured by Mikyu Kaiun Co., Ltd.). The particle size distribution of this aggregate was measured with a sieve shaker using a sieve conforming to JIS Z 8801 "Test sieves - Part 1: Metal mesh sieves". The results are shown in Tables 1, 2 and Figure 2. In Figure 2, the vertical axis represents "volume fraction (%)" and the horizontal axis represents "particle diameter (μm)". Table 1 shows the proportion (volume %) of particle diameter in the frequency distribution of the aggregate. Table 2 shows the cumulative frequency (%) of particle diameter in the frequency distribution of the aggregate. In addition, from the measurement results of the aggregate particle size distribution, the above-mentioned "ratio of the proportion of particle size (1) in the frequency distribution to the proportion of particle size (2) in the frequency distribution (proportion of particle size (1) in the frequency distribution / proportion of particle size (2) in the frequency distribution)" and "ratio of particle size (1) to particle size (2) (particle size (1) / particle size (2))" were calculated. The results are shown in Table 3. This aggregate, heavy calcium carbonate (product name: Whiten P-30, manufactured by Shiraishi Kogyo Co., Ltd.), unsaturated polyester resin (4007, manufactured by Nippon U-Pica Co., Ltd.), and methyl ethyl ketone peroxide (Permec S, manufactured by NOF Corp.) were mixed using a mixer (product name: 2P-1 type, manufactured by Primix Corp.) to obtain a resin concrete composition. The mixing ratio of the aggregate, heavy calcium carbonate, unsaturated polyester resin, and methyl ethyl ketone peroxide was 7.5:0.45:0.99:0.01 by mass. The obtained resin concrete composition was placed in a form (a pipe-shaped form having an inner diameter of 46 mm) and the resin concrete composition was hardened to obtain a hardened resin concrete product. The porosity of the obtained hardened resin concrete was measured according to the following formula. Porosity (%) = (volume measurement result - theoretical volume) / volume measurement result Here, theoretical volume = {added volume of filler} / {added volume of resin} The results are shown in Table 3. The maximum compressive stress of the obtained resin concrete hardened product was measured by using the above hardened sample with a compression tester: Shimadzu hydraulic universal testing machine 500 kN, test speed: 1 mm / min. The results are shown in Table 3.

[0070] [Comparative Example 1] The particle size distribution of the aggregate was measured in the same manner as in the Example, except that the mixture ratio of the two types of silica sand was changed as the aggregate. The results are shown in Tables 1 and 2 and in Figure 2. In addition, in the same manner as in the examples, hardened resin concrete was prepared and the porosity and maximum compressive stress of the hardened resin concrete were measured. The results are shown in Table 3.

[0071] [Comparative Example 2] The particle size distribution of the aggregate was measured in the same manner as in the Example, except that the mixture ratio of the two types of silica sand was changed as the aggregate. The results are shown in Tables 1 and 2 and in Figure 2. In addition, in the same manner as in the examples, hardened resin concrete was prepared and the porosity and maximum compressive stress of the hardened resin concrete were measured. The results are shown in Table 3.

[0072] [Table 1]

[0073] [Table 2]

[0074] [Table 3]

[0075] As shown in Tables 1 and 2, the particle size (1) in the Example and Comparative Examples 1 and 2 was 250 μm, and the particle size (2) in the Example was 1180 μm. As shown in FIG. 2, it was found that the aggregates used in the example and comparative examples 1 and 2 had two peaks in the particle size distribution. From the results shown in Table 3, it was found that the maximum compressive stress of the hardened resin concrete of the Example was 1.6 times or more the maximum compressive stress of the hardened resin concrete of Comparative Examples 1 and 2. [Industrial Applicability]

[0076] The resin concrete composition of the present invention can provide a hardened product having excellent bending strength. Therefore, when the resin concrete composition of the present invention is used in a resin mortar layer, a fiber-reinforced plastic composite pipe having excellent bending strength can be produced. [Explanation of symbols]

[0077] 1. Fiber-reinforced plastic composite pipe 2 Inner protective layer 3. Inner fiber-reinforced resin layer 3a Inner fiber-reinforced resin layer (circumferential direction) 3b Inner fiber-reinforced resin layer (axial direction) 4 Resin mortar layer 5 Outer fiber-reinforced resin layer 5a Outer fiber-reinforced resin layer (axial direction) 5b Outer fiber-reinforced resin layer (circumferential direction) 6 Outer protective layer

Claims

1. A resin concrete composition comprising aggregate and a thermosetting resin, A resin concrete composition, wherein the aggregate satisfies the following conditions: <Conditions> Among the particle sizes of the aggregate having a cumulative frequency of 80% or less from the small diameter side based on volume, the most frequent particle size is defined as particle size (1), and among the particle sizes of the aggregate having a cumulative frequency of more than 80% from the small diameter side based on volume, the most frequent particle size is defined as particle size (2). The proportion of particle size (1) in the frequency distribution is 15% by volume or more; The proportion of particle size (2) in the frequency distribution is 15% by volume or more; a ratio of the volume fraction of the particle size (2) to the particle size (1) is 0.60 or more and 1.5 or less; The ratio of the particle size (1) to the particle size (2) is 0.3 or less.

2. The resin concrete composition according to claim 1, wherein the average particle size in the volumetric particle size distribution of the aggregate is 10 μm or more and 5000 μm or less.

3. The resin concrete composition of claim 1 further comprising a filler.

4. The resin concrete composition according to claim 3, wherein the filler is at least one of calcium carbonate and crushed resin concrete.

5. A hardened resin concrete product comprising the hardened resin concrete composition according to any one of claims 1 to 4.

6. A fiber-reinforced plastic composite pipe having a resin mortar layer and a fiber-reinforced resin layer laminated on at least one of an inner surface and an outer surface of the resin mortar layer, The resin mortar layer is made of a hardened product of the resin concrete composition according to any one of claims 1 to 4, The fiber reinforced plastic composite pipe, wherein the fiber reinforced resin layer is made of fiber reinforced resin.

Citation Information

Patent Citations

  • Coating method for inside surface of tubular body

    JP1989070174A

  • Fluidity imparting method to polymer mortar or polymer concrete

    JP1995101762A

  • Resin concrete molding

    JP2003301017A

  • Resin concrete composition, aggregate with coat, filler with coat and fiber-reinforced plastic composite tube

    JP2020164400A