Laminated film
The laminated film with controlled heat shrinkage and peel force properties addresses wrinkle and peeling issues on curved surfaces, ensuring stable attachment and smooth removal.
Patent Information
- Application Number
- JP2023057967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Laminated films attached to curved surfaces with a radius of curvature of 5 cm or less tend to wrinkle or partially peel off, affecting the adherend and requiring improved attachment and peeling mechanisms.
A laminated film comprising a base film made of a resin material with a heat shrinkage rate of 0.20% or less at ±10°C of the glass transition temperature and a peel force of 1.0 N/25 mm to 3.0 N/25 mm, using a (meth)acrylic adhesive layer, to ensure stable attachment and smooth peeling.
The laminated film effectively prevents wrinkles and lifting from curved surfaces while allowing smooth peeling, maintaining stability and functionality on adherends.
Smart Images

Figure 2024145560000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated film. [Background technology]
[0002] It is known that a laminate film having a base film and a pressure-sensitive adhesive layer is attached to the surface of various industrial products for various purposes. The purpose of attaching a laminate film includes providing a desired design to an adherend using a laminate film further having a printing layer, protecting the surface of an adherend, etc. As such a laminate film, for example, a surface protection film for a polarizing plate having a support film and a pressure-sensitive adhesive layer formed on one or both sides of the support film has been proposed (see Patent Document 1).
[0003] In recent years, the applications of laminate films have become more diverse, and laminate films are sometimes attached to curved surfaces. However, when a laminate film is attached to a curved surface with a curvature radius of 5 cm or less, wrinkles may occur in the laminate film, adversely affecting the adherend, or the laminate film may float (partially peel off) from the curved surface. In addition, there are cases where the laminate film is required to be peeled off from the curved surface at a desired time depending on the application of the adherend. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-32768 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a laminated film that can suppress the occurrence of wrinkles and lifting from the curved surface even when the laminated film is attached to a curved surface with a radius of curvature of 5 cm or less, and can be smoothly peeled off from the curved surface. [Means for solving the problem]
[0006] [1] A laminated film according to one embodiment of the present invention includes a base film and a pressure-sensitive adhesive layer. The base film is made of a resin material. The pressure-sensitive adhesive layer is laminated on the base film. The base film has a heat shrinkage of 0.20% or less at a glass transition temperature of the resin material ±10°C. The peel force of the laminated film against an acrylic plate is 1.0 N / 25 mm or more and 3.0 N / 25 mm or less at a pulling speed of 30 m / min and a peel angle of 180°. [2] In the laminate film described in [1] above, the glass transition temperature of the resin material may be 125° C. or higher. [3] In the laminate film according to the above [1] or [2], the resin material may be amorphous. [4] In the laminate film according to any one of the above [1] to [3], the resin material may contain a polycarbonate-based resin and / or a cycloolefin-based resin. [5] In the laminate film according to any one of the above [1] to [4], the pressure-sensitive adhesive layer may be made of a (meth)acrylic pressure-sensitive adhesive. Effect of the Invention
[0007] According to an embodiment of the present invention, a laminate film can be realized that is suppressed from wrinkling and lifting from the curved surface even when attached to a curved surface with a curvature radius of 5 cm or less, and can be smoothly peeled off from the curved surface. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0010] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film).
[0011] A. Overall structure of laminated film FIG. 1 is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention. The laminated film 100 in the illustrated example includes a base film 1 and a pressure-sensitive adhesive layer 2. The base film 1 is made of a resin material. The pressure-sensitive adhesive layer 2 is laminated on the base film 1. At the glass transition temperature of the resin material constituting the base film 1 ±10° C., the heat shrinkage rate of the base film 1 is 0.20% or less, preferably 0.18% or less, and more preferably 0.15% or less. The lower limit of the heat shrinkage rate of the base film is typically 0.001%. The peel force of the laminated film 100 from the acrylic plate is, at a tensile speed of 30 m / min and a peel angle of 180°, 1.0 N / 25 mm or more, preferably 1.2 N / 25 mm or more, and 3.0 N / 25 mm or less, preferably 2.5 N / 25 mm or less, more preferably 2.0 N / 25 mm or less, and even more preferably 1.8 N / 25 mm or less. When the heat shrinkage rate of the base film is equal to or less than the upper limit and the peel strength of the laminated film is equal to or more than the lower limit, the laminated film can be prevented from wrinkling even when it is attached to a curved surface with a radius of curvature of 5 cm or less, and the laminated film can be prevented from floating (partially peeling) from the curved surface. Therefore, the laminated film can be stably maintained in a state where it conforms to the curved surface while suppressing the influence of the laminated film on the adherend. In addition, since the peel strength of the laminated film is equal to or less than the upper limit, the laminated film can be smoothly peeled from the curved surface.
[0012] The glass transition temperature (hereinafter sometimes referred to as Tg) of the resin material constituting the base film 1 is, for example, 80° C. or higher, preferably 125° C. or higher. If the Tg of the resin material is equal to or higher than the above lower limit, the occurrence of wrinkles in the laminated film can be stably suppressed when the laminated film is attached to a curved surface with a curvature radius of 5 cm or less. The upper limit of the Tg of the base film is typically 180° C. The glass transition temperature can be measured by any appropriate simultaneous thermogravimetry-differential thermal analyzer (TG-DTA).
[0013] The components of the laminated film will be described below.
[0014] B. Base film The base film 1 contains a resin material as a main component. Specific examples of the resin material include transparent resins such as cycloolefin (COP) resins such as polynorbornene resins, polyester resins such as polyethylene terephthalate (PET) resins, cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC) resins, (meth)acrylic resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polyolefin resins, and acetate resins. In addition, the base film 1 may include thermosetting resins or ultraviolet curing resins such as (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins. The term "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers may also be used. In addition, the polymer films described in JP 2001-343529 A (WO01 / 37007) may also be used. The material of this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition having an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion product of the above resin composition. The materials of the resin film may be used alone or in combination.
[0015] In one embodiment, the resin material of the base film 1 is amorphous. When the base film is made of an amorphous resin material, excellent transparency can be imparted to the laminate film.
[0016] Of these resin materials, preferably, PC-based resin and / or COP-based resin is used, and more preferably, PC-based resin is used.
[0017] The PC resin contains at least a structural unit derived from a dihydroxy compound having a bond structure represented by the following structural formula (1), and is produced by reacting a dihydroxy compound containing at least a dihydroxy compound having at least one bond structure -CH2-O- in the molecule with a carbonate diester in the presence of a polymerization catalyst. In other words, the PC resin contains a structural unit derived from a dihydroxy compound and a carbonate group derived from a carbonate diester. [ka]
[0018] Here, as the dihydroxy compound having a bond structure represented by structural formula (1), any compound can be used as long as it has two alcoholic hydroxyl groups, contains a structure having a linking group -CH2-O- in the molecule, and can react with a carbonate diester in the presence of a polymerization catalyst to produce a polycarbonate, and multiple types of compounds can be used in combination.
[0019] In addition, a dihydroxy compound not having the bond structure represented by the above structural formula (1) may be used in combination as a dihydroxy compound for use in a PC resin. Hereinafter, a dihydroxy compound having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (A), and a dihydroxy compound not having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (B).
[0020] (Dihydroxy compound (A)) The "linking group -CH2-O-" in the dihydroxy compound (A) means a structure that bonds with atoms other than hydrogen atoms to form a molecule. In this linking group, the atom to which at least an oxygen atom can be bonded or the atom to which a carbon atom and an oxygen atom can be bonded simultaneously is preferably a carbon atom. The number of "linking groups -CH2-O-" in the dihydroxy compound (A) is preferably 1 or more, more preferably 2 to 4.
[0021] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, and 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene. )-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene;Bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2-bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl] 1,1-bis[4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-phenylphenyl]propane, isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane bis(hydroxyalkoxyaryl)alkanes, such as 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; bis(hydroxyalkoxyaryl)cycloalkanes, such as 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxy diaryl ethers, such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxy aryl sulfides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxy aryl sulfoxides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfone and 4,4'-bis[4-(2- bishydroxyalkoxyarylsulfones, such as 1,4-bishydroxyethoxybenzene, bishydroxyalkoxybenzenes, such as 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane, anhydrous sugar alcohols, such as dihydroxy compounds represented by the following formula (2), and compounds having a cyclic ether structure, such as spiro glycols, such as those represented by the following general formula (3). The dihydroxy compounds (A) may be used alone or in combination.
[0022] [ka]
[0023] [ka]
[0024] Of these dihydroxy compounds (A), preferred is the dihydroxy compound represented by the above formula (2). Examples of the dihydroxy compound represented by the above formula (2) include isosorbide, isomannide, and isoidite, which are stereoisomeric, and these may be used alone or in combination of two or more. Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as resources, is most preferred in terms of availability, ease of production, optical properties, and moldability.
[0025] The ratio of the structural units derived from the dihydroxy compound (A) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 10 mol% or more, preferably 40 mol% or more, more preferably 60 mol% or more, and for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and further preferably 70 mol% or less. When the ratio of the dihydroxy compound (A) is within the above range, the heat shrinkability of the base film can be suitably adjusted.
[0026] (Dihydroxy Compound (B)) As the dihydroxy compound that is the structural unit of the PC resin, the dihydroxy compound (A) and the dihydroxy compound (B) can be used together. By using the dihydroxy compounds (A) and (B) in combination, the heat shrinkability of the base film can be more suitably adjusted.
[0027] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compounds (B) may be used alone or in combination. Of the dihydroxy compounds (B), preferably, alicyclic dihydroxy compounds are used.
[0028] The alicyclic dihydroxy compound is not particularly limited, but preferably includes a compound having a 5-membered ring structure or a 6-membered ring structure. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. When the alicyclic dihydroxy compound has a 5-membered ring or a 6-membered ring structure, the heat resistance of the resulting PC resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, more preferably 30 or less.
[0029] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II). HOCH2-R 1 -CH2OH (I) H.O.R. 2 -OH (II) (In formulas (I) and (II), R 1 and R 2 Each of represents a cycloalkylene group having 4 to 20 carbon atoms.
[0030] Cyclohexanedimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 is represented by the following general formula (Ia) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.
[0031] [ka]
[0032] The alicyclic dihydroxy compound represented by the above general formula (I), tricyclodecane dimethanol or pentacyclopentadecanedimethanol, is represented by the general formula (I), 1is represented by the following general formula (Ib) (wherein n is 0 or 1):
[0033] [ka]
[0034] Decalin dimethanol or tricyclotetradecane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is a compound represented by the general formula (I) 1 is represented by the following general formula (Ic) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol.
[0035] [ka]
[0036] Norbornane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 The isomers include various isomers represented by the following general formula (Id): Specific examples of such isomers include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.
[0037] [ka]
[0038] Adamantane dimethanol, which is an alicyclic dihydroxy compound represented by general formula (I), is 1 The isomers include various isomers represented by the following general formula (Ie): A specific example of such isomers is 1,3-adamantanedimethanol.
[0039] [ka]
[0040] Cyclohexanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.
[0041] [ka]
[0042] The alicyclic dihydroxy compound represented by the above general formula (II), tricyclodecanediol or pentacyclopentadecanediol, is a compound represented by the general formula (II), 2 is represented by the following general formula (IIb) (wherein n is 0 or 1):
[0043] [ka]
[0044] Decalindiol or tricyclotetradecanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is a compound represented by the general formula (II) in which R 2 is represented by the following general formula (IIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol.
[0045] [ka]
[0046] Norbornanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IId): Specific examples of such isomers include 2,3-norbornanediol and 2,5-norbornanediol.
[0047] [ka]
[0048] The adamantanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is represented by the following general formula (II): 2 is represented by the following general formula (IIe): A specific example of such an isomer is 1,3-adamantanediol.
[0049] [ka]
[0050] Among the specific examples of the alicyclic dihydroxy compound described above, preferred are cyclohexanedimethanols, tricyclodecane dimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoints of availability and ease of handling, more preferred are 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecane dimethanol, and even more preferred is tricyclodecane dimethanol.
[0051] The proportion of the structural units derived from the dihydroxy compound (B) relative to all the structural units derived from dihydroxy compounds contained in the PC resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more, and is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.
[0052] Details of these PC resins are described, for example, in JP 2012-31370 A (Patent No. 5448264), the disclosure of which is incorporated herein by reference.
[0053] In one embodiment, the PC resin contains a structural unit derived from the dihydroxy compound (A) represented by the above formula (2), a structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group linking them together. When a PC resin containing these structural units is used for a substrate film, the heat shrinkability of the substrate film can be more suitably adjusted. In such a PC resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2. In such a PC resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.
[0054] The base film 1 may contain any suitable additive in addition to the above-mentioned resin material. Examples of the additive include antioxidants, UV absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents. Any suitable surface treatment layer may be provided on the surface of the base film 1 (the surface opposite to the pressure-sensitive adhesive layer 2). Examples of the surface treatment layer include an easy-adhesion layer, an easy-slip layer, an antiblocking layer, an antistatic layer, an antireflection layer, and an oligomer prevention layer.
[0055] The thickness of the base film 1 is, for example, 5 μm or more, preferably 20 μm or more, and for example, 200 μm or less, preferably 100 μm or less.
[0056] The in-plane retardation Re(550) of the base film 1 is, for example, 100 nm or less, preferably 50 nm or less, more preferably 30 nm or less, further preferably 20 nm or less, particularly preferably 10 nm or less, and particularly preferably 5 nm or less. The lower limit of the in-plane retardation Re(550) of the base film 1 is typically 0 nm.
[0057] The thickness direction retardation Rth(550) of the base film 1 is, for example, 100 nm or less, preferably 50 nm or less, more preferably 30 nm or less, further preferably 20 nm or less, particularly preferably 10 nm or less, and particularly preferably 5 nm or less. The lower limit of Rth(550) of the base film 1 is typically 0 nm.
[0058] The haze value of the base film 1 is, for example, 2% or less, preferably 1.5% or less, more preferably 0.4% or less, and typically 0.05% or more.
[0059] C.Adhesive layer The adhesive layer 2 is provided on the surface of the base film 1 in order to attach the laminate film 100 to the surface of an adherend, particularly a curved surface with a radius of curvature of 5 cm or less. The adhesive layer 2 is made of an adhesive (pressure-sensitive adhesive).
[0060] Examples of adhesives constituting the adhesive layer 2 include (meth)acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, etc., an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more types.
[0061] In one embodiment, the pressure-sensitive adhesive layer 2 is composed of a (meth)acrylic pressure-sensitive adhesive (a (meth)acrylic pressure-sensitive adhesive composition). When the pressure-sensitive adhesive layer is composed of a (meth)acrylic pressure-sensitive adhesive, the peel force of the laminated film can be stably adjusted to within the above-mentioned range.
[0062] The (meth)acrylic pressure-sensitive adhesive composition typically contains a (meth)acrylic polymer as a main component. The content of the (meth)acrylic polymer in the solid content of the pressure-sensitive adhesive composition is, for example, 50 mass% or more, preferably 70 mass% or more, more preferably 90 mass% or more, and for example, 100 mass% or less.
[0063] The (meth)acrylic polymer contains a structural unit derived from an alkyl (meth)acrylate. In the (meth)acrylic polymer, the content of the structural unit derived from an alkyl (meth)acrylate is, for example, 70 mass% or more, preferably 80 mass% or more, and, for example, 90 mass% or less. Examples of the alkyl group of the alkyl (meth)acrylate include linear or branched alkyl groups having 1 to 18 carbon atoms. The average number of carbon atoms in the alkyl group is preferably 3 to 12, and more preferably 3 to 8. Among the alkyl (meth)acrylates, preferred are butyl acrylate and 2-ethylhexyl acrylate, and more preferably 2-ethylhexyl acrylate.
[0064] The (meth)acrylic polymer may contain a structural unit derived from a copolymerizable monomer polymerizable with the alkyl (meth)acrylate, in addition to the structural unit derived from the alkyl (meth)acrylate. Examples of the copolymerizable monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, an amide group-containing monomer, an aromatic ring-containing (meth)acrylate, and a heterocyclic ring-containing vinyl monomer. The copolymerizable monomer may be used alone or in combination. Of the copolymerizable monomers, preferred are carboxyl group-containing monomers and hydroxyl group-containing monomers. In one embodiment, the (meth)acrylic polymer contains structural units derived from an alkyl (meth)acrylate, structural units derived from a carboxyl group-containing monomer, and structural units derived from a hydroxyl group-containing monomer.
[0065] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, and crotonic acid, and preferably (meth)acrylic acid. When the (meth)acrylic polymer contains a structural unit derived from the carboxyl group-containing monomer, the adhesive properties of the adhesive layer can be improved.
[0066] When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the content of the structural unit derived from the carboxyl group-containing monomer is, for example, 0.01 mass% or more, preferably 0.10 mass% or more, and for example, 10 mass% or less, preferably 5.0 mass% or less, more preferably 1.0 mass% or less, and even more preferably 0.5 mass% or less.
[0067] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methylacrylate, preferably 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, more preferably 4-hydroxybutyl (meth)acrylate. When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the durability of the adhesive layer can be improved.
[0068] When the (meth)acrylic polymer contains structural units derived from hydroxyl group-containing monomers, the content of the structural units derived from hydroxyl group-containing monomers is, for example, 0.01 mass% or more, preferably 1.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 8.0 mass% or more, and for example, 10 mass% or less.
[0069] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, from 100,000 to 2,000,000, and preferably from 200,000 to 1,000,000. The weight average molecular weight Mw can be calculated, for example, from the results of GPC measurement in terms of styrene.
[0070] In addition, the (meth)acrylic adhesive may contain a crosslinking agent. As the crosslinking agent, representative examples include organic crosslinking agents and polyfunctional metal chelates, and preferably organic crosslinking agents. As the organic crosslinking agent, for example, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents are included, and more preferably, isocyanate crosslinking agents are included.
[0071] The content of the crosslinking agent is, for example, 0.01 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.2 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer. When the content of the crosslinking agent is within the above range, the peel force of the laminated film can be stably adjusted to the above range.
[0072] Furthermore, the (meth)acrylic pressure sensitive adhesive may contain various additives (for example, a silane coupling agent, a polymerization initiator, a solvent, a crosslinking catalyst) in an appropriate ratio. Details of these adhesives are described, for example, in JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712, the disclosures of which are incorporated herein by reference.
[0073] The thickness of the pressure-sensitive adhesive layer 2 is typically 1 μm or more, preferably 5 μm or more, and typically 30 μm or less, preferably 15 μm or less.
[0074] D. Release Liner The laminated film 100 may further include a release liner 3 in addition to the base film 1 and the pressure-sensitive adhesive layer 2. The release liner 3 is typically temporarily attached to the pressure-sensitive adhesive layer 2 until the laminated film is attached to an adherend, and is peeled off from the pressure-sensitive adhesive layer 2 when the laminated film is attached. The release liner 3 is formed of any appropriate resin film that can be used as a release liner. A release treatment layer may be provided on the surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive layer 2.
[0075] E. Applications of laminated films The laminated films described in the above items A to D are used by being attached to the surface of various adherends. More specifically, the laminated film 100 is attached to the surface of the adherend (particularly a curved surface with a radius of curvature of 5 cm or less) by the pressure-sensitive adhesive layer 2. Examples of the adherend include optical members and electronic members, and preferably optical members. Representative examples of the optical members include a polarizing plate, a retardation film, an optical laminate including a polarizing plate and / or a retardation film, a display, an imaging device, a lens, and a (half) mirror. The radius of curvature of the curved surface of the adherend is, for example, 5 cm or less, or, for example, 3 cm or less, and, for example, 0.5 cm or more.
[0076] In one embodiment, the laminate film 100 is a decorated film. When the laminate film 100 is a decorative film, the laminate film 100 has a printed layer (not shown) in addition to the base film 1 and the pressure-sensitive adhesive layer 2. The printed layer is provided on the surface of the pressure-sensitive adhesive layer 2 opposite to the base film 1. Such decorative films are attached to the surface of an adherend (typically a curved surface with a radius of curvature of 5 cm or less) so that the printed layer comes into contact with the adherend. They are then heated as necessary and peeled off from the surface of the adherend. The printed layer is then transferred to the surface of the adherend (particularly a curved surface with a radius of curvature of 5 cm or less), and the desired design can be imparted to the adherend.
[0077] In another embodiment, the laminate film 100 is a film with a pressure-sensitive adhesive layer, and can be suitably used as a surface protection film. Such a surface protection film is attached to the surface of an adherend (typically a curved surface with a radius of curvature of 5 cm or less). This makes it possible to protect the surface of the adherend during processing and / or transportation of the adherend. Thereafter, the surface protection film is peeled off and removed from the surface of the adherend at a desired timing. EXAMPLES
[0078] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.
[0079] (1) Glass transition temperature (Tg) of the base film The glass transition temperature of the resin material constituting the base film used in the examples and comparative examples was measured using a differential scanning calorimeter DSC6220 manufactured by SII NanoTechnology. More specifically, about 10 mg of the resin sample was placed in an aluminum pan manufactured by the same company and sealed, and the temperature was raised from 30°C to 200°C at a heating rate of 20°C / min under a nitrogen flow of 50 mL / min. After holding the temperature for 3 minutes, it was cooled to 30°C at a rate of 20°C / min. It was held at 30°C for 3 minutes and then heated again to 200°C at a rate of 20°C / min. From the DSC data obtained in the second heating, the extrapolated glass transition onset temperature, which is the temperature at the intersection of a straight line extending the low-temperature side baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change part of the glass transition is maximum, was obtained, and this was taken as the glass transition temperature (Tg). The results are shown in Table 1.
[0080] (2) Measurement of heat shrinkage rate of base film The substrate film used in the examples and comparative examples was attached to a glass plate with a thickness of 1 mm via an adhesive layer to prepare a measurement sample, and the four corners of the film were marked. The length L0 between the marks at the four corners of the film was measured using an image measuring device (Quick Vision) manufactured by Mitutoyo Corporation. The measured sample was placed in a heating oven at the glass transition temperature (Tg) of the resin material ±10°C for 120 hours, and then the length L500 between the marks at the four corners of the polarizing film was measured again. The dimensional change rate was calculated using the following formula. The results are shown in Table 1. Dimensional change rate (%) = {(L500-L0) / L0} x 100
[0081] (3) Peel strength measurement of laminated film The laminated films obtained in the examples and comparative examples were cut into strips of 25 mm x 100 mm to prepare samples. The samples were roll-pressed onto the surface of an acrylic plate ("Acrylite" manufactured by Mitsubishi Chemical Corporation, thickness: 2 mm, width: 70 mm, length: 100 mm) with the adhesive layer at a pressure of 0.25 MPa and a feed rate of 0.3 m / min. The samples were left to stand for 30 minutes in an environment with a temperature of 23°C and a relative humidity of 50%, and then a peel test was performed in the same environment at a peel angle of 180° and a tensile speed of 30 m / min to measure the peel force. The evaluation results are shown in Table 1.
[0082] (4) Evaluation of curved surface workability An adherend having a curved surface with a radius of curvature of 3 cm was prepared. Next, the laminated films obtained in the examples and comparative examples were attached to the curved surface of the adherend with the adhesive layer. Thereafter, the presence or absence of wrinkles in the laminated film and the presence or absence of lifting of the laminated film from the adherend were confirmed by visual and microscopic observation. The results are shown in Table 1. Next, the laminated film was visually inspected for peeling from the adherend. The results are shown in Table 1.
[0083] <<Preparation Example 1: Adhesive Composition A>> In a reaction vessel equipped with a thermometer, a stirrer, a cooler and a nitrogen gas inlet tube, 100 parts by mass of 2-ethylhexyl acrylate (2EHA), 10 parts by mass of 4-hydroxybutyl acrylate (4HBA), 0.02 parts by mass of acrylic acid (AA), and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were charged together with 157 parts by mass of ethyl acetate, and nitrogen gas was introduced while gently stirring at 23°C to perform nitrogen substitution. Thereafter, the liquid temperature was kept at around 65°C and a polymerization reaction was carried out for 6 hours to prepare a solution of (meth)acrylic polymer A (concentration 40% by mass). The weight average molecular weight of acrylic polymer A was 540,000.
[0084] Ethyl acetate was added to the solution of acrylic polymer A to dilute it to a concentration of 20% by mass. 1.5 parts by mass of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 parts by mass (solid content 0.03 parts by mass) of dibutyltin dilaurate (1% by mass ethyl acetate solution) as a crosslinking catalyst were added to 500 parts by mass of this solution (solid content 100 parts by mass) and stirred to prepare adhesive composition A.
[0085] <<Preparation Example 2: Adhesive Composition B>> Pressure-sensitive adhesive composition B was prepared in the same manner as in Preparation Example 1, except that the amount of the isocyanurate of hexamethylene diisocyanate added as the crosslinking agent was changed to 3.0 parts by mass.
[0086] <<Preparation Example 3: Adhesive Composition C>> A pressure-sensitive adhesive composition C was prepared in the same manner as in Preparation Example 1, except that the amount of the isocyanurate of hexamethylene diisocyanate added as the crosslinking agent was changed to 0.3 parts by mass.
[0087] <<Preparation Example 4: Preparation of PC resin film>> 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecane dimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, the temperature of the heating vessel was heated to 150°C as the first step of the reaction, and the raw materials were dissolved (about 15 minutes) while stirring as necessary. Next, the pressure was changed from normal pressure to 13.3 kPa, and the temperature of the heating vessel was raised to 190°C in one hour, while the generated phenol was extracted outside the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, the pressure in the reaction vessel was changed to 6.67 kPa, the temperature of the heating vessel was raised to 230°C in 15 minutes, and the generated phenol was extracted outside the reaction vessel as the second step. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure in the reaction vessel was allowed to reach 0.200 kPa or less in order to remove the phenol that was generated. After reaching a predetermined stirring torque, the reaction was terminated, and the reaction product was extruded into water to obtain pellets of PC-based resin. The obtained PC-based resin was vacuum-dried at 100°C for 12 hours, and then a PC-based resin film having a thickness of 20 μm was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 1700 mm, setting temperature: 250°C), a cast roll (setting temperature: 60°C), and a winder.
[0088] [Example 1] The pressure-sensitive adhesive composition A of Preparation Example 1 was applied to the surface of the PC resin film (substrate film) of Preparation Example 4, and then dried to form a pressure-sensitive adhesive layer having a thickness of 15 μm. In this manner, a laminate film was obtained.
[0089] [Example 2] A laminated film was obtained in the same manner as in Example 1, except that the PC resin film in Preparation Example 4 was changed to a COP resin film (manufactured by Zeon Corporation, product number ZF16).
[0090] [Comparative Example 1] A laminated film was obtained in the same manner as in Example 1, except that the PC resin film in Preparation Example 4 was changed to a PET film (manufactured by Toray Industries, Inc., product number "50U48").
[0091] [Comparative Example 2] A laminated film was obtained in the same manner as in Example 1, except that the PC resin film in Preparation Example 4 was changed to an acrylic resin film (manufactured by Kaneka Corporation, product name "HTX-Z").
[0092] [Comparative Example 3] A laminated film was obtained in the same manner as in Example 1, except that the pressure-sensitive adhesive composition A in Preparation Example 1 was changed to the pressure-sensitive adhesive composition B in Preparation Example 2.
[0093] [Comparative Example 4] A laminated film was obtained in the same manner as in Example 1, except that the pressure-sensitive adhesive composition A in Preparation Example 1 was changed to the pressure-sensitive adhesive composition C in Preparation Example 3.
[0094] [Table 1]
[0095] [evaluation] As is clear from Table 1, when the heat shrinkage rate of the base film is equal to or less than the upper limit and the peel strength of the laminate film is equal to or greater than the lower limit, the laminate film can be prevented from wrinkling and from lifting off from the adherend even when the laminate film is attached to a curved surface with a radius of curvature of 5 cm or less by the adhesive layer. Furthermore, when the peel strength of the laminate film is equal to or less than the upper limit, the laminate film can be smoothly peeled off from the adherend. [Industrial Applicability]
[0096] The laminated film of the present invention can be used in the production of various industrial products, and can be particularly suitably used in the production of industrial products having curved surfaces. [Explanation of symbols]
[0097] 1. Base film 2 Adhesive layer 100 Laminated Film
Claims
1. A base film made of a resin material; A pressure-sensitive adhesive layer laminated on the base film, The heat shrinkage rate of the base film at a glass transition temperature of the resin material ±10° C. is 0.20% or less, A laminated film having a peel strength from an acrylic plate of 1.0 N / 25 mm or more and 3.0 N / 25 mm or less at a tensile speed of 30 m / min and a peel angle of 180°.
2. The laminated film according to claim 1 , wherein the resin material has a glass transition temperature of 125° C. or higher.
3. The laminated film according to claim 1 , wherein the resin material is amorphous.
4. The laminated film according to claim 1 , wherein the resin material contains a polycarbonate-based resin and / or a cycloolefin-based resin.
5. The laminate film according to claim 1 or 2, wherein the pressure-sensitive adhesive layer is composed of a (meth)acrylic pressure-sensitive adhesive.
Citation Information
Patent Citations
Surface protective film
JP2008194886A
Solvent-based releasable pressure-sensitive adhesive composition and releasable pressure-sensitive adhesive product
JP2009227737A
Surface protective film and optical member having protective film
JP2019099751A
Base material for surface protective film, production method of the base material, surface protective film using the base material, and optical film with surface productive film
JP2020033418A
Adhesive sheet and image display device
JP2021120437A