Laminated film and adhesive tape

The laminated film with a controlled layer structure and material composition addresses curling and tearability issues, ensuring easy tearing and curl suppression for adhesive tapes.

JP2024145702AInactive Publication Date: 2024-10-15NICHIBAN KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058170
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Adhesive tapes with a laminated structure experience curling issues and reduced tearability when attempting to suppress curling.

Method used

A laminated film with a specific layered structure, comprising an inner layer and outer layers with controlled thickness ratios and materials, such as high and low-density polyethylene, to enhance tearability and prevent curling.

Benefits of technology

The laminated film is easy to tear and effectively suppresses curling, maintaining flexibility and symmetry, suitable for applications requiring hand-tearable adhesive tapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145702000003
    Figure 2024145702000003
  • Figure 2024145702000001
    Figure 2024145702000001
  • Figure 2024145702000002
    Figure 2024145702000002
Patent Text Reader

Abstract

To provide a film material which suppresses the occurrence of curling while having easy tearability.SOLUTION: A laminated film has an internal layer, a first external layer provided on one main surface side of the internal layer, and a second external layer provided on the other main surface side of the internal layer. The ratio (T12 / T11) of the thickness T12 of the second external layer to the thickness T11 of the first external layer is 0.85 to 1.20. The internal layer is configured to facilitate tearing in at least one direction, or the first external layer and the second external layer are configured to facilitate tearing in at least one direction.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film and an adhesive tape. [Background technology]

[0002] 2. Description of the Related Art Hand-tearable adhesive tapes that can be cut by hand alone without the need for tools such as scissors have been developed.

[0003] For example, Patent Document 1 discloses an adhesive tape using, as a substrate, a laminate in which a non-stretched synthetic resin film and a biaxially stretched synthetic resin film are laminated together. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 05-287243 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the adhesive tape according to Patent Document 1 may curl because it is produced by laminating two layers, and when attempting to suppress such curling, the ease of tearing may be deteriorated.

[0006] Therefore, an object of the present invention is to provide a film material that is easy to tear and yet suppresses curling. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by using a laminated film having a layered structure, and have completed the present invention.

[0008] The embodiment (1) of the present invention is The insulating sheet has an internal layer, a first external layer provided on one main surface side of the internal layer, and a second external layer provided on the other main surface side of the internal layer, The thickness T of the first outer layer 11 The thickness T of the second outer layer 12 The ratio (T 12 / T 11 ) is 0.85 to 1.20, The inner layer is configured to facilitate tearing in at least one direction, or the first outer layer and the second outer layer are configured to facilitate tearing in at least one direction. The laminated film is characterized by the above.

[0009] The laminated film preferably has a total thickness of 140 μm or less. The laminated film preferably has a flexibility of 120 mm or less as measured by the following measurement method. (Measurement method) The flexibility of the laminated film was measured in accordance with JIS L 1096 bending flexibility method A (45° cantilever method), where the value was the average of the values ​​on the front (n=5) and back (n=5) of the laminated film. It is preferred that the first and second outer layers are both high density polyethylene, or that the first and second outer layers are both low density polyethylene. It is preferred that the first and second outer layers are both high density polyethylene and the inner layer is low density polyethylene, or that the first and second outer layers are both low density polyethylene and the inner layer is high density polyethylene. The laminated film preferably has a laminated structure consisting of only three layers: the inner layer, the first outer layer, and the second outer layer.

[0010] The second aspect of the present invention is The insulating sheet has an internal layer, a first external layer provided on one main surface side of the internal layer, and a second external layer provided on the other main surface side of the internal layer, The thickness T of the first outer layer 11 The thickness T of the second outer layer 12 The ratio (T 12 / T 11 ) is 0.85 to 1.20, the inner layer is made of low density polyethylene, and the first outer layer and the second outer layer are both made of high density polyethylene; or The inner layer is made of high density polyethylene, and the first outer layer and the second outer layer are both made of low density polyethylene. The laminated film is characterized by the above.

[0011] A third aspect of the present invention is an adhesive tape comprising the laminate film of the first or second aspect and an adhesive layer laminated on at least one of the main surfaces of the laminate film. Effect of the Invention

[0012] According to the present invention, there is provided a film material which is easy to tear and yet inhibits curling. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of a laminated film of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In this specification, when the upper limit and the lower limit of a numerical range are separately described, all combinations of the lower limit and the upper limit are substantially described, provided that there is no contradiction.

[0015] In this specification, unless otherwise specified, various measurements are performed at room temperature (25° C.).

[0016] The laminate film of the present disclosure and a pressure-sensitive adhesive tape including the laminate film of the present disclosure will be described below, but the present invention is not limited to the following in any way.

[0017] <<<Laminated film 100>>> As shown in FIG. 1, the laminated film 100 has an internal layer 10, a first external layer 11 provided on one main surface side of the internal layer 10, and a second external layer 12 provided on the other main surface side of the internal layer.

[0018] It is preferred that the laminated film 100 has the inner layer 10 configured to be easily torn in at least one direction, or that the first outer layer 11 and the second outer layer 12 are both configured to be easily torn in at least one direction.

[0019] For example, when the tear strength of a single layer (or a single film constituting a layer) is 100N or less, 80N or less, 50N or less, 40N or less, 35N or less, or 30N or less, it can be determined that the layer is easy to tear. (Measurement method) The film is measured for tear strength in accordance with JIS Z 0237 bending flexibility method A (45° cantilever method). However, the weight of about 2500g attached to the pendulum is not used in the measurement, and the value is the result of measuring one sheet of laminated film.

[0020] Such a film can be adjusted so that it is easy to tear in at least one direction by changing the material and by imparting anisotropy in the planar direction (for example, by axial stretching).

[0021] Hereinafter, a film that is configured to be easily torn in at least one direction may be simply referred to as an easy-tear film.

[0022] When the first outer layer 11 and the second outer layer 12 are both anisotropic, easy-to-tear films, it is preferable to laminate the first outer layer 11 and the second outer layer 12 so that the directions in which they are easy to tear are the same.

[0023] On the other hand, a film having a relatively high tear strength compared to such an easy-to-tear film may be called a hard-to-tear film. In addition, when the tear strength of the easy-to-tear film is TA and the tear strength of the hard-to-tear film is TB, it is preferable that TB / TA is more than 1, 2 or more, 5 or more, or 15 or more. The upper limit of TB / TA is not particularly limited, but is, for example, 100, 80, 70, or 60.

[0024] Thickness T of the first outer layer 11 11 The thickness T of the second outer layer 12 12 The ratio (T 12 / T 11 ) is preferably 0.85 to 1.20, 0.90 to 1.11, 0.95 to 1.05, or 0.97 to 1.03. In this way, by disposing an easy-to-tear film having a similar thickness as an outer layer and sandwiching the inner layer, or disposing a film having a similar thickness as an outer layer and sandwiching the easy-to-tear film, symmetry is generated in the thickness direction of the laminated film 100 while maintaining the ease of tearing derived from the easy-to-tear film, and the occurrence of curling is suppressed.

[0025] The resin material constituting each layer (the inner layer 10, the first outer layer 11, and the second outer layer 12) is not particularly limited, and is preferably a thermoplastic material such as a polyolefin resin, a polystyrene resin, or a polyester resin. The resin material constituting each layer is preferably a polyolefin, and more preferably a polyethylene. The polyethylene may be a low-density polyethylene (density range, for example, 930 kg / m 3 or less), medium density polyethylene, and high density polyethylene (density range is, for example, 940 kg / m 3 High density polyethylene tends to form an easily tearable film, whereas low density polyethylene tends to form a difficult to tear film.

[0026] Specifically, it is preferable that the first outer layer 11 and the second outer layer 12 are both high density polyethylene and the inner layer 10 is low density polyethylene, or that the first outer layer 11 and the second outer layer 12 are both low density polyethylene and the inner layer 10 is high density polyethylene. By using such a combination, it is easy to suppress the occurrence of curling while improving the ease of tearing. In addition, the transparency of the entire laminated film 100 can be improved.

[0027] From the viewpoint of increasing the symmetry in the thickness direction of the laminated film 100 and further enhancing the curl suppression effect, it is preferable that the first outer layer 11 and the second outer layer 12 are made of the same resin material. The first outer layer 11 and the second outer layer 12 are made of the same resin material if (condition 1) the constituent monomers of the resin materials constituting the first outer layer 11 and the second outer layer 12 are the same (for example, both resin materials are polyethylene), and (condition 2) the ratio of the glass transition temperature of the resin material constituting the second outer layer 12 to the glass transition temperature of the resin material constituting the first outer layer 11 (second outer layer / first outer layer) is within the range of 0.8 to 1.2 or 0.9 to 1.1. The glass transition temperatures shown here are measured by DSC. In this case, it is preferable that the resin material constituting the internal layer 10 is made of a resin material different from the resin materials constituting the first outer layer 11 and the second outer layer 12 (at least one of the above conditions 1 and 2 is not satisfied). In addition, the first outer layer 11, the second outer layer 12 and the inner layer 10 may each be a multilayer film formed by laminating multiple films made of the same resin material to form a single layer in order to achieve a thickness within the desired range.

[0028] Methods for imparting anisotropy to a film include a method using a stretched film and a method in which holes or slits are provided in the film at predetermined intervals.

[0029] The laminated film 100 preferably consists of only three layers, that is, the inner layer 10, the first outer layer 11, and the second outer layer 12, in order to improve symmetry in the thickness direction.

[0030] The total thickness of the laminated film is preferably 140 μm or less, or 120 μm or less. The lower limit of the total thickness of the laminated film is not particularly limited, but is, for example, 50 μm or 75 μm. By setting the thickness of the laminated film in this range, it is easy to suppress the occurrence of curling while improving the ease of tearing.

[0031] The specific thickness of each layer (the inner layer 10, the first outer layer 11, and the second outer layer 12) is not particularly limited and may be appropriately set depending on the material, etc. For example, the thickness of each layer is preferably 5 to 100 μm or 10 to 90 μm.

[0032] The laminated film preferably has a flexibility of 120 mm or less as measured by the following measurement method, which makes it easier to prevent curling while improving ease of tearing. (Measurement method) The flexibility of the laminated film was measured in accordance with JIS L 1096 bending flexibility method A (45° cantilever method), where the value was the average of the values ​​on the front (n=5) and back (n=5) of the laminated film.

[0033] The laminated film 100 can be manufactured by pressurizing and heating the layers in a laminated state. When forming a laminated film by laminating and heating the layers in this manner, curling may occur due to distortion caused by heat or a restoring force during cooling or storage. Similarly, curling may occur due to the storage environment (light, heat, humidity, etc.) of the laminated film 100. The laminated film 100 of the present disclosure has a specific laminated structure, which suppresses the occurrence of such curling.

[0034] The width and length of the laminated film can be appropriately changed depending on the application.

[0035] The laminated film may include an adhesive layer, a printed layer, etc., which do not affect the above-mentioned properties. For example, when the material of the films constituting the laminated film is polyethylene, the films may be laminated together with a polyethylene having a low softening temperature interposed between them to increase the adhesive strength.

[0036] <Preferred embodiments 1 and 2 of the laminated film 100> Here, preferred embodiments of the laminated film 100 of the present disclosure include the following embodiment 1 or embodiment 2.

[0037] The laminated film 100 of form 1 has an internal layer 10, a first external layer 11 provided on one main surface side of the internal layer 10, and a second external layer 12 provided on the other main surface side of the internal layer, with the internal layer 10 being a layer made of low-density polyethylene, and the first external layer 11 and the second external layer 12 both being layers made of high-density polyethylene.

[0038] The laminated film 100 of form 2 has an internal layer 10, a first external layer 11 provided on one main surface side of the internal layer 10, and a second external layer 12 provided on the other main surface side of the internal layer, where the internal layer 10 is a layer made of high-density polyethylene, and the first external layer 11 and the second external layer 12 are both layers made of low-density polyethylene.

[0039] In the first and second embodiments, the thickness of the layer made of high-density polyethylene is preferably 5 μm or more, 10 μm or more, or 15 μm or more, and is preferably 30 μm or less, 25 μm or less, or 20 μm or less.

[0040] In the first and second embodiments, the thickness of the layer made of low-density polyethylene is preferably more than 30 μm, 35 μm or more, or 40 μm or more, and is preferably 150 μm or less, 100 μm or less, or 75 μm or less.

[0041] In Form 1 and Form 2, the ratio of the thickness of the layer (one layer) composed of high density polyethylene to the thickness of the layer (one layer) composed of low density polyethylene (high density polyethylene / low density polyethylene) for all layers is preferably 1.20 or less, 1.00 or less, 0.90 or less, or 0.80 or less, and is also preferably 0.10 or more, 0.20 or more, 0.30 or more, or 0.35 or more.

[0042] In form 1, the ratio of the total thickness of the layers made of high density polyethylene (total thickness of the layers made of high density polyethylene / total thickness) to the total thickness (total thickness) of the three layers, i.e., the layers made of high density polyethylene (first outer layer 11 and second outer layer 12) and the layer made of low density polyethylene (internal layer 10), is preferably 10% or more, 15% or more, 20% or more, 25% or more, or 30% or more, and is preferably 70% or less, 65% or less, or 60% or less.

[0043] In form 2, the ratio of the total thickness of the layers made of high density polyethylene to the total thickness (total thickness) of the three layers, namely the layer made of high density polyethylene (inner layer 10) and the layers made of low density polyethylene (first outer layer 11 and second outer layer 12), is preferably 8% or more, 10% or more, or 12% or more, and is preferably 70% or less, 65% or less, 50% or less, 40% or less, 30% or less, or 20% or less.

[0044] As mentioned above, the thickness T of the first outer layer 11 11 The thickness T of the second outer layer 12 12 The ratio (T 12 / T 11 ) is preferably 0.85 to 1.20, 0.90 to 1.11, 0.95 to 1.05, or 0.97 to 1.03. As described above, the first outer layer 11 and the second outer layer 12 are preferably made of the same resin material.

[0045] In this way, by combining a layer made of low density polyethylene and a layer made of high density polyethylene and laminating them symmetrically in the thickness direction, the occurrence of curling can be easily suppressed.

[0046] <Preferred embodiments 3 and 4 of the laminated film 100> From another viewpoint, preferred embodiments of the laminate film 100 of the present disclosure include the following embodiment 3 or 4.

[0047] The laminated film 100 of form 3 has an internal layer 10, a first external layer 11 provided on one main surface side of the internal layer 10, and a second external layer 12 provided on the other main surface side of the internal layer, wherein the internal layer 10 is composed of a tear-resistant film, and the first external layer 11 and the second external layer 12 are both composed of easy-tear films.

[0048] The laminated film 100 of form 4 has an internal layer 10, a first external layer 11 provided on one main surface side of the internal layer 10, and a second external layer 12 provided on the other main surface side of the internal layer, wherein the internal layer 10 is composed of an easy-tear film, and the first external layer 11 and the second external layer 12 are both composed of difficult-tear films.

[0049] In the third and fourth embodiments, the thickness of the easily tearable film is preferably 5 μm or more, 10 μm or more, or 15 μm or more, and is preferably 30 μm or less, 25 μm or less, or 20 μm or less.

[0050] In the third and fourth embodiments, the thickness of the tear-resistant film is preferably more than 30 μm, 35 μm or more, or 40 μm or more, and is preferably 150 μm or less, 100 μm or less, or 75 μm or less.

[0051] In forms 3 and 4, the thickness of the easy-tear film relative to the thickness of the hard-tear film (easy-tear film / hard-tear film) is preferably 1.20 or less, 1.00 or less, 0.90 or less, or 0.80 or less for all films, and is preferably 0.10 or more, 0.20 or more, 0.30 or more, or 0.35 or more.

[0052] In form 3, the ratio of the total thickness of the easy-tear film to the total thickness (total thickness) of the three layers, the easy-tear film (first outer layer 11 and second outer layer 12) and the hard-tear film (internal layer 10) (total thickness of easy-tear film / total thickness) is preferably 10% or more, 15% or more, 20% or more, 25% or more, or 30% or more, and is preferably 70% or less, 65% or less, or 60% or less.

[0053] In form 4, the ratio of the total thickness of the easy-tear film to the total thickness (total thickness) of the three layers consisting of the easy-tear film (inner layer 10) and the layers consisting of the hard-tear film (first outer layer 11 and second outer layer 12) is preferably 8% or more, 10% or more, or 12% or more, and is preferably 70% or less, 65% or less, 50% or less, 40% or less, 30% or less, or 20% or less.

[0054] As mentioned above, the thickness T of the first outer layer 11 11 The thickness T of the second outer layer 12 12 The ratio (T 12 / T 11 ) is preferably 0.85 to 1.20, 0.90 to 1.11, 0.95 to 1.05, or 0.97 to 1.03. As described above, the first outer layer 11 and the second outer layer 12 are preferably made of the same resin material.

[0055] In this way, by combining an easy-to-tear film and a difficult-to-tear film and laminating them symmetrically in the thickness direction, the occurrence of curling can be easily suppressed.

[0056] <<<Adhesive tape>>> Next, a pressure-sensitive adhesive tape obtained using the laminate film 100 of the present disclosure will be described.

[0057] The adhesive tape has an adhesive layer laminated on at least one main surface of the laminate film 100. The adhesive tape may be a single-sided adhesive tape in which an adhesive layer is laminated on only one side of the laminate film 100, or a double-sided adhesive tape in which adhesive layers are laminated on both main surfaces of the laminate film 100.

[0058] The adhesive that forms the adhesive layer is not particularly limited, and known adhesives can be used. Examples of the adhesive that forms the adhesive layer include acrylic adhesives, rubber adhesives, silicone adhesives, vinyl alkyl ether adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, fluorine adhesives, epoxy adhesives, and adhesives containing other synthetic resins.

[0059] The pressure-sensitive adhesive layer may contain known additives such as a tackifier, a plasticizer, an antioxidant, an ultraviolet absorber, a filler, a flame retardant, a conductive agent, and a foaming agent for each of the pressure-sensitive adhesive layer and the release separator layer.

[0060] The thickness of the adhesive layer is not particularly limited and can be appropriately adjusted depending on the application of the adhesive tape.

[0061] The method for producing the adhesive tape is not particularly limited, and the adhesive tape can be formed by utilizing a known method for forming an adhesive layer. The adhesive tape can be produced, for example, by a method of applying and drying an adhesive composition on the outer layer (on the first outer layer 11 and / or on the second outer layer 12) of the laminated film 100 to form an adhesive layer, or by a method of providing an adhesive layer on a release film and laminating the adhesive layer on the outer layer (on the first outer layer 11 and / or on the second outer layer 12) of the laminated film 100.

[0062] The adhesive tape may have a protective film or the like laminated on the adhesive layer.

[0063] An adhesive tape obtained using the laminate film 100 of the present disclosure can be used for a variety of purposes, such as surface protection, packaging, decoration, electrical insulation, bundling, medical use, and sticky notes.

[0064] Furthermore, the laminated film 100 of the present disclosure is easy to tear and inhibits curling, and can be suitably used as a hand-tearable adhesive tape. EXAMPLES

[0065] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following.

[0066] <<Raw materials>> <Low density polyethylene film (LLDPE)> AJ-1 (Tamapoly Co., Ltd.) was used. <High density polyethylene film (HDPE)> The Karalyan YA-2 (Denka Co., Ltd.) was used. In addition, a low-density polyethylene film (LLDPE) is a film that is relatively difficult to tear, while a high-density polyethylene film (HDPE) is a film that is relatively easy to tear.

[0067] <<Laminated film manufacturing method>> <Example 1> RU-80 / H-1 ​​was diluted with ethyl acetate to a solid content of 20%, and applied at a dry rate of 4 g / m using the Meyer bar coating method. 2 A dry laminate layer was formed by a drying process at 100°C for 3 minutes, and a film was laminated on the above surface to produce a laminated film.

[0068] <Examples 2-6, Comparative Examples 1-2> Except for changing the materials and thicknesses of the outer layer 1, outer layer 2, and inner layer to those shown in Tables 1 and 2, laminated films according to Examples 2-6 and Comparative Examples 1-2 were produced in the same manner as in Example 1. Note that in Comparative Example 1, the outer layer 2 was not provided.

[0069] <<Evaluation>> The flexibility of each laminate film was evaluated based on the above-mentioned measurement method. In addition, the hand-tearability and curl suppression of each laminate film were evaluated based on the following measurement methods. The evaluation results are shown in Tables 1 and 2.

[0070] <Easy to cut by hand> For each of the laminated films of the Examples and Comparative Examples, a test piece having a width of 18 mm and a length of 80 mm was cut out, which was torn by hand in the width direction and the hand tearability was evaluated according to the following evaluation criteria. ◎: Easy to tear without getting caught ○: Only some parts are caught, but it can be torn. △: There is some snagging but it can be torn ×: The film stretches without tearing

[0071] <Curl suppression> For each of the laminate films in the Examples and Comparative Examples, a test piece of 50 mm in width and 50 mm in length was punched out. The test piece was placed in a stainless steel square tray and fixed with adhesive tape at four points in the center of each side of the test piece. The test piece was then placed in a drying oven set at 100°C and heated for 3 minutes, and the curl suppression was evaluated according to the following evaluation criteria. ○: No change even after heating ×: The corners of the test piece rise vertically.

[0072] [Table 1]

[0073] [Table 2]

Claims

1. an internal layer, a first external layer provided on one main surface side of the internal layer, and a second external layer provided on the other main surface side of the internal layer; The thickness T of the first outer layer 11 The thickness T of the second outer layer 12 The ratio (T 12 / T 11 ) is 0.85 to 1.20, The inner layer is configured to facilitate tearing in at least one direction, or the first outer layer and the second outer layer are configured to facilitate tearing in at least one direction. A laminated film characterized by:

2. 2. The laminated film according to claim 1, having a total thickness of 140 μm or less.

3. 3. The laminated film according to claim 2, wherein the flexibility measured according to the following measurement method is 120 mm or less. (Measurement method) The flexibility of the laminated film is measured in accordance with JIS L 1096, bending resistance, method A (45° cantilever method), where the value is the average of the values ​​for the front (n=5) and back (n=5) of the laminated film.

4. 4. The laminated film according to claim 3, wherein the first outer layer and the second outer layer are both high density polyethylene, or the first outer layer and the second outer layer are both low density polyethylene.

5. the first outer layer and the second outer layer are both high density polyethylene and the inner layer is low density polyethylene; or The first outer layer and the second outer layer are both low-density polyethylene, and the inner layer is high-density polyethylene. The laminated film according to claim 3.

6. The laminated film according to claim 5, having a laminated structure consisting of only three layers: the inner layer, the first outer layer, and the second outer layer.

7. an internal layer, a first external layer provided on one main surface side of the internal layer, and a second external layer provided on the other main surface side of the internal layer; The thickness T of the first outer layer 11 The thickness T of the second outer layer 12 The ratio (T 12 / T 11 ) is 0.85 to 1.20, the inner layer is made of low density polyethylene, and the first outer layer and the second outer layer are both made of high density polyethylene; or The inner layer is made of high-density polyethylene, and the first outer layer and the second outer layer are both made of low-density polyethylene. A laminated film characterized by:

8. An adhesive tape comprising the laminated film according to any one of claims 1 to 7 and an adhesive layer laminated on at least one main surface of the laminated film.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive tape of good manual tearability

    JP1993287243A