Decorative sheet and building member

The decorative sheet with a urethane resin surface, polyester resin base, and metal layer addresses followability issues, ensuring a luxurious finish and adherence to complex metal surfaces by controlling elastic modulus and thickness.

JP2024145721APending Publication Date: 2024-10-15NIPPON CARBIDE KOGYO KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023058200
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing decorative sheets for metal surfaces, particularly at right-angled or acute-angled portions, face issues with followability, leading to lifting or insufficient adherence, as they are either too rigid or lack sufficient conformability.

Method used

A decorative sheet with a specific layer structure comprising a urethane resin surface layer, a polyester resin base layer, and a metal layer, with controlled elastic modulus and thicknesses, ensuring flexibility and adherence to complex surfaces.

Benefits of technology

The decorative sheet provides excellent followability, preventing lifting at right-angled or acute-angled portions, maintaining a luxurious mirror-like finish while adhering effectively to metal shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145721000001_ABST
    Figure 2024145721000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet with superior adaptability.SOLUTION: A decorative sheet includes a surface layer, a substrate layer, and a metal layer in that order, the surface layer containing an urethane resin, the substrate layer containing a polyester resin, and an elastic modulus being less than 155 N / 25 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to decorative sheets and building components. [Background technology]

[0002] Metal shaped materials made of aluminum and the like are often used as building materials. In order to give the surface of the metal shaped material a mirror finish in order to give it a design and a luxurious feel, it is possible to polish the surface of the metal shaped material or to paint the surface of the metal shaped material with a paint containing metal powder or a lustrous pigment. However, when these methods are used, although a metallic appearance can be obtained, the surface of the metal shaped material tends to have a dull color, and it is difficult to obtain a luxurious mirror finish.

[0003] As a simple method for making the surface of a metal shaped material have a mirror finish, it is considered to attach a metallic decorative sheet to the metal shaped material. For example, Patent Document 1 discloses a metallic decorative sheet as a composite material having a metallic mirror-like luster, in which a metal layer, a pattern layer, and a fluorine-based resin film are laminated in this order on one side of a base film. Patent Document 2 discloses a metal-deposited laminate usable as a decorative sheet, which is made by laminating a metal-deposited layer on the surface of a substrate made of a polymer resin and a resin layer made of a resin on the opposite surface. In Patent Document 2, one or more of an acrylic resin, a urethane resin, and a polyester resin are used as the resin. By attaching these decorative sheets to metal shapes, a luxurious, mirror-like appearance can be obtained. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-58660 [Patent Document 2] JP 2007-216608 A Summary of the Invention [Problem to be solved by the invention]

[0005] When the decorative sheet described in Patent Document 1 was applied to a metal shaped material having a right angle or acute angle, a luxurious mirror finish was obtained, but it was found that the decorative sheet did not conform sufficiently to the surface of the lumber at the right angle or acute angle, causing the decorative sheet to float. The decorative sheet in Patent Document 1 uses a weather-resistant fluororesin film as the surface layer, and a highly smooth PET film as the base film. It is believed that the decorative sheet did not conform to the surface of the lumber because the fluororesin film and the PET film are both highly rigid. On the other hand, the resin layer containing a urethane-based resin or the like used in the metal vapor deposition laminate described in Patent Document 2 is softer than a fluororesin film. However, even with the metal vapor deposition laminate described in Patent Document 2, the conformability to the surface of a square timber is not necessarily sufficient. It has been difficult to control the conformability of a decorative sheet or metal vapor deposition laminate at right angles or acute angles by simply adjusting the composition of the resin constituting the substrate or resin layer. In other words, it was found that there is still room for improvement in the prior art with respect to conformability to right angles or acute angles of building materials. The present disclosure has been made in consideration of the above-mentioned conventional circumstances, and has an object to provide a decorative sheet with excellent conformability and a building component using the same. [Means for solving the problem]

[0006] Specific means for achieving the above object are as follows. <1> The laminate includes a surface layer, a base layer, and a metal layer in this order, The surface layer contains a urethane resin, The base layer contains a polyester resin, A decorative sheet having an elastic modulus of less than 155N / 25mm. <2> The average thickness of the base layer is 40 μm or less. <1> The decorative sheet according to claim 1. <3> The metal layer comprises a metal, a metal oxide, or an alloy. <1> or <2> The decorative sheet according to claim 1. <4> The average thickness of the surface layer is 50 μm or less. <1> ~ <3> 13. The decorative sheet according to claim 12. <5> The average thickness of the metal layer is 1 μm or less. <1> ~ <4> 13. The decorative sheet according to claim 12. <6> Used as a building material <1> ~ <5> 13. The decorative sheet according to claim 12. <7> An adherend and a coating material for covering at least a portion of the surface of the adherend. <1> ~ <6> A building member comprising the decorative sheet according to any one of claims 1 to 5. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a decorative sheet with excellent conformability and a building component using the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view of a decorative sheet 1 according to a first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a decorative sheet 2 according to a second embodiment. [Diagram 3] FIG. 2 is a cross-sectional view of a decorative sheet 3 according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless specifically stated. The same applies to the numerical values ​​and their ranges, and do not limit the present disclosure.

[0010] In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple types of substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area. In this disclosure, the term "lamination" refers to stacking layers, where two or more layers may be bonded together or two or more layers may be removable. In the present disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic. In this disclosure, the thickness of a layer or film refers to a value measured using a micrometer. In the present disclosure, the average thickness of a layer or film is a value obtained by measuring the thicknesses of any five points of the layer or film in question and calculating the arithmetic mean value of the measured thicknesses. In the present disclosure, the solid content concentration (mass %) refers to the mass ratio of components other than the solvent contained in the solution.

[0011] <Decorative sheet> The decorative sheet of the present disclosure comprises a surface layer, a base layer, and a metal layer, in that order, the surface layer containing a urethane-based resin, the base layer containing a polyester-based resin, and has an elastic modulus of less than 155 N / 25 mm. After extensive research, the inventors discovered that not only the type of resin components constituting the surface layer and base material layer, but also the elastic modulus of the decorative sheet as a whole, contributes to its ability to conform to right angles or acute angles of metal profiles, and thus completed the present invention.

[0012] The decorative sheet of the present disclosure is preferably used as a building material for improving the design of the surface of an adherend, which will be described later. In addition to building materials, the decorative sheet of the present disclosure can also be applied to emblems, badges, badges, stickers, seals, labels, nameplates, ribbons, and the like that are attached to the exterior parts of vehicles such as automobiles and the surfaces of objects installed outdoors.

[0013] The elastic modulus of the decorative sheet of the present disclosure is less than 155N / 25mm, preferably 154N / 25mm or less, more preferably 153N / 25mm or less, and even more preferably 152N / 25mm or less. From the viewpoint of the handleability of the decorative sheet, the elastic modulus of the decorative sheet of the present disclosure is preferably 130N / 25mm or more, more preferably 135N / 25mm or more, and even more preferably 140N / 25mm or more. The elastic modulus of the decorative sheet of the present disclosure is preferably 130N / 25mm or more and less than 155N / 25mm. The elastic modulus of a decorative sheet is the value obtained by carrying out a tensile test on a test piece of 25 mm width and 100 mm length. The test conditions are a pulling speed of 200 mm / min. The elastic modulus of the decorative sheet can be adjusted to fall within the desired range by adjusting the thicknesses of the surface layer, the base layer and any other layers that are provided as necessary, as well as the components of each layer.

[0014] The average thickness of the decorative sheet of the present disclosure is preferably 100 μm to 200 μm, more preferably 120 μm to 190 μm, and even more preferably 140 μm to 180 μm, from the viewpoint of setting the elastic modulus of the decorative sheet within the above desired range.

[0015] The decorative sheet of the present disclosure includes a surface layer, a base layer, and a metal layer in this order, and may include other layers as necessary. The decorative sheet of the present disclosure will be described below with reference to the drawings. Note that the sizes of the members in each drawing are conceptual, and the relative relationship between the sizes of the members is not limited thereto. In addition, members or parts having similar functions are given the same reference numerals throughout the drawings, and their description may be omitted.

[0016] [First embodiment] 1 is a cross-sectional view of a decorative sheet 1 according to a first embodiment. The decorative sheet 1 includes a surface layer 10, a base layer 20, and a metal layer 30, in this order. Each layer will be described below.

[0017] (Base material layer 20) The base layer 20 contains a polyester resin. The base layer 20 can function as a support layer for supporting the metal layer 30. The base layer 20 is preferably substantially transparent. "Substantially transparent" means that the decorative sheet 1 has sufficient transparency to allow the metal layer 30 to exhibit a metallic appearance.

[0018] Examples of polyester-based resins constituting the base layer include polyesters such as polyethylene terephthalate (PET) and modified polyesters such as glycol-modified polyethylene terephthalate (PETG). Glycol-modified polyethylene terephthalate has a molecular structure in which a part of the structural units derived from ethylene glycol in the PET monomer is replaced with structural units derived from cyclohexanedimethanol. As the polyester-based resin, polyethylene terephthalate (PET) is preferred. The substrate layer may contain other resins besides polyester-based resins, such as (meth)acrylic resins, polyurethane resins, polycarbonate resins, polyolefin resins, vinyl chloride resins, and acrylonitrile-butadiene-styrene (ABS) resins. When the base layer contains a resin other than the polyester-based resin, the proportion of the polyester-based resin in the resin components constituting the base layer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 99% by mass or more. The substrate layer may be made of a polyester resin, and in this case, it is more preferable that the substrate layer is made of polyethylene terephthalate (PET).

[0019] The average thickness of the base layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the decorative sheet in a desirable range, the average thickness of the base layer is preferably 40 μm or less, more preferably 39 μm or less, and even more preferably 38 μm or less. From the viewpoint of the handleability of the decorative sheet, the average thickness of the base layer is preferably 20 μm or more. The average thickness of the base layer is preferably 20 μm to 40 μm.

[0020] (metal layer 30) The metal layer 30 is a layer that imparts the appearance of metallic luster to the decorative sheet. The metal layer 30 may usually be a thin layer of metal, and the metal can be appropriately selected within a range that exhibits metallic luster and that exhibits sufficient malleability when the thin film is attached to the substrate. The metal layer may comprise a metal, a metal oxide or an alloy. Specific examples of the metal contained in the metal layer include aluminum, indium, chromium, zinc, gallium, nickel, tin, silver, gold, silicon, titanium, platinum, palladium, stainless steel, and Hastelloy. Among these, the metal is preferably aluminum from the viewpoint of processability.

[0021] The metal layer 30 may be composed of a metal foil, or may be a vapor-deposited film formed on the surface of the base layer 20. The metal layer 30 is preferably a layer formed directly on the surface of the base layer 20, such as a vapor-deposited film, from the viewpoints of being able to omit the step of producing an adhesive layer that bonds the metal layer 30 and the base layer 20, reducing costs, and of suppressing the adhesive layer from increasing the rigidity of the decorative sheet. The metal layer can be formed on the surface of the substrate layer using known techniques such as vacuum deposition, sputtering, and chemical vapor deposition (CVD).

[0022] The average thickness of the metal layer is determined based on various conditions such as the optical effect and the desired conformability of the decorative sheet. The average thickness of the metal layer is preferably 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. The average thickness of the metal layer may be 0.01 μm or more. The average thickness of the metal layer is preferably 0.01 μm to 1 μm.

[0023] (Surface layer 10) The surface layer 10 contains a urethane resin. The surface layer 10 constitutes the surface of the decorative sheet and protects the surface of the decorative sheet. It is more preferable that the surface layer 10 has optical transparency from the viewpoint of fully expressing the design provided by the metal layer 30. It is also preferable that the surface layer 10 has weather resistance, particularly in applications for decorating adherends. Furthermore, it is preferable that the surface layer 10 has sufficiently high mechanical strength from the viewpoint of increasing the tensile strength and surface hardness of the decorative sheet.

[0024] The surface layer may contain other resins besides the urethane resin, such as (meth)acrylic resin, polyester resin, polycarbonate resin, polyolefin resin, vinyl chloride resin, and acrylonitrile-butadiene-styrene (ABS) resin. When the surface layer contains a resin other than the urethane-based resin, the proportion of the urethane-based resin in the resin components constituting the surface layer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 99% by mass or more. The surface layer may contain only the urethane-based resin as a resin component.

[0025] The surface layer may contain a stabilizer from the viewpoint of improving the weather resistance of the decorative sheet. Examples of the stabilizer include a heat stabilizer, a light stabilizer, and a stabilization assistant. Examples of the heat stabilizer include phosphite compounds, hindered amine compounds, and metal perchlorates. Examples of the light stabilizer include benzophenone compounds, benzotriazole compounds, cyanoacrylate compounds, and hydroxyphenyltriazine compounds. As the stabilizing aid, epoxy compounds such as epoxidized soybean oil, epoxidized linseed oil, bisphenol A diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether, and β-diketone compounds such as benzoylacetone, dibenzoylmethane, and stearoylbenzoylmethane may be used. The content of the stabilizer in the surface layer is not particularly limited, and is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, and even more preferably 1 to 3 parts by mass, relative to a total of 100 parts by mass of the resin contained in the surface layer.

[0026] The average thickness of the surface layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the decorative sheet in a desirable range, the average thickness of the surface layer is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. From the viewpoint of the handleability of the decorative sheet, the average thickness of the surface layer is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. The average thickness of the surface layer is preferably 10 μm to 50 μm.

[0027] The surface layer may contain a matting agent so as to make the surface of the decorative sheet matte, or the surface of the surface layer may be coated with a matting agent.

[0028] Other additives that can be added to the surface layer include a leveling agent, an antifoaming agent, an additive for preventing soiling such as a silicone resin, a slip agent, a filler, and the like.

[0029] [Second embodiment] 2 is a cross-sectional view of a decorative sheet 2 according to a second embodiment. The decorative sheet 2 includes a surface layer 10, an adhesive layer 40, a resin layer 50, a substrate layer 20, and a metal layer 30, in this order. In the decorative sheet 2, the details of the surface layer 10, the base layer 20, and the metal layer 30 are similar to those of the decorative sheet 1, and therefore a description thereof will be omitted.

[0030] (Resin layer 50) In the decorative sheet 2, a resin layer 50 is provided between the surface layer 10 and the base layer 20 from the standpoint of design. The resin layer may contain polyester resin, (meth)acrylic resin, polyurethane resin, polycarbonate resin, polyolefin resin, vinyl chloride resin, acrylonitrile-butadiene-styrene (ABS) resin, etc. Among these, (meth)acrylic resin is preferred from the viewpoint of transparency. The (meth)acrylic resin may be a homopolymer consisting of structural units derived from a single (meth)acrylic monomer, or a copolymer consisting of structural units derived from two or more types of (meth)acrylic monomers. Here, the (meth)acrylic monomer means at least one of acrylic acid, derivatives of acrylic acid such as acrylic acid alkyl esters, and derivatives of methacrylic acid such as methacrylic acid alkyl esters. The derivatives of acrylic acid and the derivatives of methacrylic acid may have a substituent such as a hydroxyl group, an amino group, a carboxyl group, or a glycidyl group. In addition, the (meth)acrylic resin may contain other monomers than the (meth)acrylic monomer. The total proportion of structural units derived from monomers containing a carboxy group in the molecule, such as acrylic acid, methacrylic acid, and other monomers containing a carboxy group, in the total structural units of the (meth)acrylic resin is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. The total proportion of structural units derived from monomers containing a carboxy group in the molecule in the total structural units of the (meth)acrylic resin may be 0.5% by mass or more. The total proportion of structural units derived from monomers containing a carboxy group in the molecule in the total structural units of the (meth)acrylic resin is preferably 0.5% by mass to 20% by mass.

[0031] The weight average molecular weight (Mw) of the (meth)acrylic resin is preferably within the range of 5,000 to 1,000,000, more preferably within the range of 10,000 to 800,000, and even more preferably within the range of 100,000 to 750,000. If the weight average molecular weight (Mw) of the (meth)acrylic resin is 5,000 or more, the resin layer tends not to become brittle. Also, if the weight average molecular weight (Mw) of the (meth)acrylic resin is 1,000,000 or less, the film-forming property tends to be excellent. When two or more types of (meth)acrylic resins are used in combination as the (meth)acrylic resin, the weight average molecular weight (Mw) of the mixture of two or more types of (meth)acrylic resins is preferably within the above range.

[0032] The weight average molecular weight (Mw) of the (meth)acrylic resin is a value measured by the following method, specifically, according to the following (1) to (3). (1) A solution of a (meth)acrylic resin is applied to a release paper and dried at 100° C. for 1 minute to obtain a film of the (meth)acrylic resin. (2) Using the (meth)acrylic resin film obtained in (1) above and tetrahydrofuran, a sample solution with a solid concentration of 0.2% by mass is obtained. (3) The weight average molecular weight of the (meth)acrylic resin is measured in terms of standard polystyrene using gel permeation chromatography (GPC) under the following conditions.

[0033] ~Conditions~ Measurement equipment: High-speed GPC [Model: HLC-8220 GPC, manufactured by Tosoh Corporation] Detector: Differential refractometer (RI) [installed in HLC-8220, manufactured by Tosoh Corporation] Column: 4 TSKgel GMHXL (Tosoh Corporation) columns Column temperature: 40°C Eluent: tetrahydrofuran Sample solution injection volume: 100μL Flow rate: 0.8mL / min

[0034] From the viewpoint of mechanical strength, the glass transition temperature Tg of the (meth)acrylic resin is preferably -20°C or higher, more preferably 0°C or higher, and even more preferably 10°C or higher. From the viewpoint of good workability of the resin film and resistance to brittleness, the glass transition temperature Tg of the (meth)acrylic resin may be 100°C or lower. The glass transition temperature Tg of the (meth)acrylic resin is preferably -20°C to 100°C. The glass transition temperature Tg of the (meth)acrylic resin refers to the value determined as the inflection point of the DSC curve obtained by measuring 10 mg of a measurement sample in a nitrogen gas flow at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) (e.g., EXSTAR6000 manufactured by Seiko Instruments Inc.). When two or more inflection points are observed in the DSC curve using the differential scanning calorimeter (DSC), the temperature at the highest inflection point is regarded as the glass transition temperature Tg of the (meth)acrylic resin.

[0035] In addition, when the structural units constituting the (meth)acrylic resin are known, the Tg of the (meth)acrylic resin may be a value obtained by converting the absolute temperature (K) calculated by the following formula into Celsius temperature (°C).

[0036]

number

[0037] In the formula, Tg1, Tg2, . . . and Tg nare the glass transition temperatures of the homopolymers of monomer 1, monomer 2, ..., and monomer n, expressed in absolute temperature (K). m1, m2, ..., and m n are the mole fractions of each monomer.

[0038] The "glass transition temperature of a homopolymer expressed in absolute temperature (K)" refers to the glass transition temperature of a homopolymer produced by polymerizing the monomer alone, expressed in absolute temperature (K). The glass transition temperature of a homopolymer can be measured by the above-mentioned method using a differential scanning calorimeter (DSC).

[0039] The "glass transition temperatures expressed as Celsius temperatures (°C) of homopolymers" of representative monomers are as follows: 10°C for methyl acrylate, -22°C for ethyl acrylate, -54°C for n-butyl acrylate, -70°C for 2-ethylhexyl acrylate, -15°C for 4-hydroxybutyl acrylate, -80°C for t-butyl acrylate, 43°C for vinyl acetate, 32°C for acrylic acid, 106°C for methyl methacrylate, and 85°C for 2-hydroxyethyl methacrylate. For example, by using these representative monomers, it is possible to appropriately adjust the above-mentioned glass transition temperatures. Regarding the "glass transition temperature when made into a homopolymer" of a monomer other than the above-mentioned monomers, the value described in Polymer Handbook (4th edition, Wiley-Interscience; the same applies hereinafter) is adopted. When there is no description in the Polymer Handbook, the glass transition temperature of the homopolymer obtained by the above-mentioned measurement method is adopted. In addition, absolute temperature (K) can be converted to Celsius temperature (℃) by subtracting 273 from absolute temperature (K), and Celsius temperature (℃) can be converted to absolute temperature (K) by adding 273 to Celsius temperature (℃).

[0040] When two or more (meth)acrylic resins are used in combination, the glass transition temperature Tg of the (meth)acrylic resin exhibiting the highest glass transition temperature Tg is preferably within the above range.

[0041] The method for producing the (meth)acrylic resin is not particularly limited, and the resin can be produced by polymerizing monomers by a method such as solution polymerization, emulsion polymerization, suspension polymerization, etc. In addition, when preparing a resin composition after the production of the (meth)acrylic resin, solution polymerization is preferred because the treatment process is relatively simple and can be carried out in a short time.

[0042] The (meth)acrylic resin may be a commercially available product. Examples of commercially available (meth)acrylic resins include KP-1876E (product name: Nissetsu (registered trademark), manufactured by Nippon Carbide Industries Co., Ltd.) and H-4002 (manufactured by Negami Chemical Industries Co., Ltd.).

[0043] The resin layer may contain, as required, a colorant for coloring the resin layer, a leveling agent, an anti-foaming additive such as a silicone resin, a slip agent, a filler, and the like.

[0044] The average thickness of the resin layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the decorative sheet in a desirable range, the average thickness of the resin layer is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less. From the viewpoint of the handleability of the decorative sheet, the average thickness of the resin layer is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. The average thickness of the resin layer is preferably 15 μm to 50 μm.

[0045] (adhesive layer 40) The adhesive layer 40 bonds the surface layer 10 and the base layer 20, which are separately prepared, via the resin layer 50 provided on the surface of the base layer 20. In this case, the adhesive layer 40 may be provided on the surface of the surface layer 10, or on the surface of the resin layer 50 in the base layer 20. In the second embodiment, when the surface layer 10 is provided directly on the surface of the resin layer 50, the adhesive layer 40 does not necessarily have to be provided.

[0046] The adhesive layer is made of a resin composition. Examples of the resin composition used in the adhesive layer include a (meth)acrylic adhesive, a silicone adhesive, and a synthetic rubber adhesive. From the viewpoint of increasing the adhesion between the resin layer and the adhesive layer, a (meth)acrylic adhesive is more preferable.

[0047] The average thickness of the adhesive layer is not particularly limited, but is preferably in the range of 5 μm to 100 μm. When the average thickness of the adhesive layer is in the above range, the workability (e.g., handleability) when bonding the surface layer and the base layer, which are separately prepared, is improved.

[0048] [Third embodiment] 3 is a cross-sectional view of a decorative sheet 3 according to a third embodiment. The decorative sheet 3 includes a surface layer 10, a first adhesive layer 42, a resin layer 50, a substrate layer 20, a metal layer 30, a primer layer 60, and a second adhesive layer 44, in this order. In the decorative sheet 3, the details of the surface layer 10, base layer 20, metal layer 30 and resin layer 50 are the same as those in the decorative sheet 1 or decorative sheet 2, and therefore a description thereof will be omitted. Furthermore, in the decorative sheet 3, the details of the first adhesive layer 42 are similar to those of the adhesive layer 40, and therefore a description thereof will be omitted.

[0049] (Primer layer 60) The primer layer 60 is provided to improve adhesion between the metal layer 30 and the second adhesive layer 44 . The primer layer may be formed from a primer layer composition containing, for example, a urethane resin and a (meth)acrylic resin. In particular, it is more preferable that the urethane resin contained in the primer layer is a water-based urethane resin from the viewpoint of not corroding the second adhesive layer 44. Examples of water-based urethane resins include self-emulsifying urethane resins, forced emulsifying urethane resins, and water-soluble urethane resins. The self-emulsifying urethane resin is a water-based urethane resin in which the molecular structure of the urethane resin has hydrophilic groups such as anionic and nonionic groups, and the urethane resin is emulsified and dispersed in a water-based system by these hydrophilic groups. The forced emulsifying urethane resin is a water-based urethane resin in which the urethane resin or urethane prepolymer is emulsified and dispersed in a water-based system by surfactants such as anionic surfactants and nonionic surfactants. Examples of such urethane resins include Takelac (registered trademark) WS series (manufactured by Mitsui Chemicals).

[0050] The primer layer may further contain a crosslinking agent, silica powder, a coloring agent, and the like.

[0051] The average thickness of the primer layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, from the viewpoint of increasing the adhesion between the metal layer 30 and the second adhesive layer 44. Moreover, the average thickness of the primer layer is preferably 6 μm or less, more preferably 4 μm or less, from the viewpoint of transparency. The average thickness of the primer layer is preferably 0.1 μm to 6 μm.

[0052] (Second adhesive layer 44) The second adhesive layer 44 is provided for attaching the decorative sheet 3 to an adherend. The components constituting the second adhesive layer 44 are the same as those of the adhesive layer 40 . Although there are no particular restrictions on the average thickness of the second adhesive layer 44, it is preferably in the range of 5 μm to 100 μm. If the average thickness of the second adhesive layer 44 is in the above range, the workability (e.g., handleability) when attaching the decorative sheet 3 to an adherend is improved.

[0053] [Manufacturing method of decorative sheet] The decorative sheet of the present disclosure can be manufactured by a method that can realize the layer structure described above, and such a method can be realized by utilizing known methods for manufacturing laminates. For example, the decorative sheet 1 can be produced by forming a metal layer 30 on one surface of a base layer 20, for example by vacuum deposition, and applying a resin composition constituting the surface layer 10 to the other surface of the base layer 20, drying it, and optionally subjecting it to a treatment such as heating. The decorative sheet 2 having the resin layer 50 can be produced by laminating two laminates. That is, the metal layer 30 is formed on one surface of the base layer 20 by, for example, vacuum deposition, and the resin composition constituting the resin layer 50 is applied to the other surface of the base layer 20, dried, and if necessary, subjected to a treatment such as heating, to prepare a first laminate. Next, an adhesive layer 40 is formed on one surface of the surface layer 10 to prepare a second laminate. The surface of the first laminate facing the resin layer 50 and the surface of the second laminate facing the adhesive layer 40 may be brought into contact with each other and pressure-bonded to integrate the two, thereby obtaining the decorative sheet 2. When forming the adhesive layer 40, a resin composition for forming the adhesive layer may be applied onto a temporary support, dried, and heated, if necessary, to form the adhesive layer 40 on the temporary support, and then the obtained adhesive layer 40 may be brought into contact with one surface of the surface layer 10 and pressed to integrate the two, and then the temporary support may be removed to form the adhesive layer 40 on one surface of the surface layer 10. The decorative sheet 3 can be produced by applying a primer layer composition to the surface of the metal layer 30 in the decorative sheet 2, drying it, and, if necessary, heating it to form a primer layer 60 on the metal layer 30, and then forming the second adhesive layer 44 on the primer layer 60. When forming the second adhesive layer 44, the method using the temporary support already described can also be applied. It should be noted that the method for producing the decorative sheet of the present disclosure is not limited to the above method.

[0054] <Building materials> A building component of the present disclosure comprises an adherend and the decorative sheet of the present disclosure covering at least a portion of the surface of the adherend. Examples of the substrate include surface materials of sliding doors, doors, kitchen doors, bathroom cabinet doors, etc., bottom panels of the inside of kitchen cabinets, the inside of bathroom cabinets, etc., and sashes. The method of attaching the decorative sheet to the surface of the adherend is not particularly limited. When an adhesive layer is provided on the surface of the decorative sheet opposite to the surface layer, the adhesive layer side can be brought into contact with the surface of the adherend. When an adhesive layer is not provided on the surface of the decorative sheet opposite to the surface layer, an adhesive is applied to the portion of the surface of the adherend where the decorative sheet is to be attached, and then the surface of the decorative sheet opposite to the surface layer can be brought into contact with the surface of the adherend.

[0055] Because the decorative sheet of the present disclosure has excellent conformability, even when the decorative sheet is attached to the surface of a component having right angles or acute angles, such as a metal profile, the decorative sheet is prevented from lifting at the right angles or acute angles. EXAMPLES

[0056] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to these examples.

[0057] (Synthesis of acrylic copolymer A) In a reaction vessel of a reaction apparatus equipped with a stirrer, a reflux condenser, a successive dropping device, and a thermometer, 70 parts by mass of ethyl acetate was charged. In addition, 100.0 parts by mass of a monomer mixture consisting of 62.5 parts by mass of methyl methacrylate, 29.5 parts by mass of ethyl acrylate, 7.0 parts by mass of 2-hydroxyethyl methacrylate, and 1.0 part by mass of acrylic acid was prepared in a separate vessel. 20.0 parts by mass of this prepared monomer mixture was charged into the reaction vessel, and then heated and refluxed at the reflux temperature for 10 minutes. Next, under reflux temperature conditions, the remaining 80.0 parts by mass of the monomer mixture, 50.0 parts by mass of ethyl acetate, and 0.026 parts by mass of 2,2'-azobisisobutyronitrile [AIBN; polymerization initiator] were successively dropped into the reaction vessel over 120 minutes, and after the dropwise addition was completed, the reaction was continued for another 150 minutes to complete the reaction. The solution after the reaction was completed was diluted with ethyl acetate to a solid content concentration of 26.5% by mass, and an acrylic copolymer A solution having a weight average molecular weight of 200,000 to 250,000 and a glass transition temperature of 49°C was obtained.

[0058] (Synthesis of Acrylic Copolymer B) An acrylic copolymer B solution having a solid content of 40.0% by mass, a weight average molecular weight of 200,000 to 250,000, and a glass transition temperature of 1°C was obtained in the same manner as in the synthesis of acrylic copolymer A, except that a monomer mixture consisting of 65.0 parts by mass of ethyl acrylate, 20.0 parts by mass of methyl methacrylate, 14.0 parts by mass of 2-hydroxyethyl methacrylate, and 1.0 part by mass of acrylic acid was used.

[0059] (Synthesis of acrylic copolymer C) An acrylic copolymer C solution having a solid content of 33.5% by mass, a weight average molecular weight of 600,000 to 700,000, and a glass transition temperature of -37°C was obtained in the same manner as in the synthesis of acrylic copolymer A, except that a monomer mixture consisting of 90 parts by mass of butyl acrylate and 10 parts by mass of acrylic acid was used.

[0060] <Example 1> An aluminum metal layer (average thickness 0.05 μm) was provided by vacuum deposition on one surface of a substrate layer made of a polyethylene terephthalate film (manufactured by Toyobo STC Co., Ltd., product name "A4360", average thickness 38 μm). Next, a resin composition for forming a resin layer was prepared by adding 0.6 parts by mass of a hexamethylene diisocyanate (HMDI)-based crosslinking agent (manufactured by Asahi Kasei Corporation, product name "Duranate E405-70B", solid content concentration 70% by mass) to a mixture of 71.5 parts by mass of acrylic copolymer A solution and 28.5 parts by mass of acrylic copolymer B solution, and the resin composition was applied to the other surface of the base layer so that the thickness after solvent drying was 30 μm. The resin composition was then heated and dried for 3 minutes in an atmosphere of 120°C to obtain a resin layer. To 100 parts by mass of the acrylic copolymer C solution, 2.5 parts by mass of a toluene diisocyanate crosslinking agent (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L45E", solid content concentration 45% by mass) was added to prepare a resin composition for forming an adhesive layer. This resin composition for forming an adhesive layer was applied to one surface of another polyethylene terephthalate film that had been subjected to a peeling treatment so that the average thickness after solvent drying was 38 μm, and the film was heated and dried for 1 minute in a 100 ° C. atmosphere to obtain an adhesive layer (second adhesive layer). Next, the metal layer and the adhesive layer were bonded together to obtain a laminate A having a laminate structure of resin layer / base layer / metal layer / adhesive layer / polyethylene terephthalate film.

[0061] Next, 100 parts by mass of polyurethane resin A solution (Urethane A, Dainichi Seika Chemicals Co., Ltd., trade name "NE-8836", solid content concentration 25.0 mass%), 0.5 parts by mass of hydroxyphenyltriazine (HPT)-based ultraviolet absorber (BASF Japan Ltd., trade name "Tinuvin 477", solid content 100 mass%), and 10 parts by mass of a 50:50 (mass%) mixed solution of isopropanol and toluene as a dilution solvent were added to prepare a surface layer forming resin composition. This surface layer forming resin composition was applied to one surface of a polyethylene terephthalate film that had been subjected to a release treatment so that the average thickness after solvent drying was 30 μm, and the surface layer was obtained by heating and drying in a 140 ° C. atmosphere for 3 minutes. 0.13 parts by mass of an aluminum chelate crosslinking agent (manufactured by Kawaken Fine Chemical Co., Ltd., product name "Aluminum Chelate A", solid content 100% by mass) was added to 100 parts by mass of the acrylic copolymer C solution to prepare a resin composition for forming an adhesive layer. This resin composition for forming an adhesive layer was applied to one surface of another polyethylene terephthalate film that had been subjected to a peeling treatment so that the average thickness after solvent drying was 25 μm, and the film was heated and dried for 1 minute in a 100°C atmosphere to obtain an adhesive layer. Next, the surface layer and the adhesive layer were bonded together to obtain a laminate B having a laminate structure of polyethylene terephthalate film / adhesive layer / surface layer / polyethylene terephthalate film.

[0062] The polyethylene terephthalate film on the side in contact with the adhesive layer in laminate B was peeled off, and the adhesive layer was brought into contact with the surface on the resin layer side of laminate A to laminate the adhesive layer and surface layer on the resin layer, and then the polyethylene terephthalate film on the side in contact with the surface layer was peeled off to obtain decorative sheet 1 having a laminated structure of polyethylene terephthalate film / adhesive layer / metal layer / substrate layer / resin layer / adhesive layer / surface layer.

[0063] <Example 2> Decorative sheet 2 was obtained under the same conditions as in Example 1, except that polyurethane resin B solution (Urethane B, manufactured by Dainichi Seikagaku Chemical Co., Ltd., product name "NE-8811", solid content concentration 25.0 mass%) was used instead of polyurethane resin A solution, and a surface layer was obtained so that the average thickness after solvent drying was 30 μm.

[0064] <Example 3> A decorative sheet 3 was obtained in the same manner as in Example 1, except that the base layer was changed to a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "E5100", average thickness 25 μm).

[0065] <Example 4> A decorative sheet 4 was obtained in the same manner as in Example 1, except that the average thickness of the surface layer after drying of the solvent was set to 40 μm.

[0066] <Example 5> A decorative sheet 5 was obtained in the same manner as in Example 1, except that the average thickness of the surface layer after drying of the solvent was set to 20 μm.

[0067] <Comparative Example 1> A decorative sheet 6 was obtained in the same manner as in Example 1, except that the base layer was changed to a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine (registered trademark) A4160", average thickness 50 μm).

[0068] <Comparative Example 2> Decorative sheet 7 was obtained in the same manner as in Example 1, except that the base layer was changed to a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine (registered trademark) A4160", average thickness 100 μm).

[0069] <Comparative Example 3> A decorative sheet 8 was obtained in the same manner as in Example 1, except that the surface layer (average thickness: 30 μm) of the laminate B was formed in the same process as in Example 1 to form the resin layer.

[0070] <Comparative Example 4> A decorative sheet 9 was obtained in the same manner as in Example 1, except that a polyvinyl chloride film (vinyl chloride resin, manufactured by Nippon Carbide Industries Co., Ltd., product name "08C040M", average thickness 50 μm) was used for the surface layer.

[0071] <Comparative Example 5> A decorative sheet 10 was obtained in the same manner as in Example 1, except that a fluorine film (fluorine resin, manufactured by Denka Company, trade name "Denka DX Film", average thickness 30 μm) was used for the surface layer.

[0072] <Comparative Example 6> A decorative sheet 11 was obtained in the same manner as in Example 1, except that a fluororesin film (fluororesin, manufactured by Denka Company, trade name "Denka DX Film", average thickness 40 μm) was used as the substrate layer.

[0073] <Comparative Example 7> A decorative sheet 12 was obtained in the same manner as in Example 1, except that a polyvinyl chloride film (vinyl chloride resin, manufactured by Nippon Carbide Industries Co., Ltd., product name "08C040M", average thickness 40 μm) was used as the base layer.

[0074] <Elasticity measurement> The elastic modulus was measured using a Tensilon (manufactured by A&D) at a tensile speed of 200 mm / min. Each decorative sheet was cut into test pieces measuring 25 mm in width and 100 mm in length, and evaluation was performed. The results are shown in Table 1.

[0075] <Follow-up evaluation> Each decorative sheet obtained as described above was attached to an aluminum profile of 50 mm x 30 mm x 100 mm, and the presence or absence of lifting of each decorative sheet was visually observed at the right corners of the aluminum profile and evaluated according to the following criteria. The results are shown in Table 1. -Judgment criteria- A: There was no lifting of the decorative sheet at any of the right-angled parts of the aluminum profile. B: There was no lifting of the decorative sheet at any of the right-angled parts of the aluminum profile, but wrinkles occurred in the decorative sheet when it was applied. C: The decorative sheet had lifted off at some or all of the right-angled parts of the aluminum profile.

[0076] [Table 1]

[0077] The thickness (average thickness) of each layer was measured by the method described above.

[0078] The evaluation results shown in Table 1 reveal the following: Because polyester film is a highly rigid material, in order to attach a decorative sheet using a polyester film as a base layer so that it conforms to the right angle or acute angle of a metal profile, it was necessary to adjust the rigidity of the decorative sheet. When a fluorofilm was used for the surface layer as in Comparative Example 5, the decorative sheet had high rigidity and insufficient conformability to right-angled portions. On the other hand, when films other than fluorofilm were examined as films to be applied to the surface layer, it was not possible to improve conformability with acrylic films or PVC films as in Comparative Example 3 and Comparative Example 4. On the other hand, it was found that when a urethane film was used for the surface layer as in Examples 1 to 5, the rigidity of the decorative sheet was reduced and conformability to right-angled portions was improved. It was found that, when a polyester film having an average thickness of 50 μm or more was used as the base layer as in Comparative Example 1 or Comparative Example 2, the adhesive force was defeated by the restoring force of the polyester film trying to return to its original state, and the decorative sheet was lifted from the aluminum molded material. However, when a polyester film having an average thickness of 40 μm or less was used as the base layer as in Examples 1 to 5, the decorative sheet could be attached to the right angle without lifting. In addition, it was found that even when the base layer was changed to a fluorine film having an average thickness of 40 μm or less as in Comparative Example 6, the restoring force was high and the decorative sheet was lifted from the aluminum molded material. On the other hand, it was found that when the base layer was changed to a PVC film having an average thickness of 40 μm or less as in Comparative Example 7, the rigidity of the decorative sheet was too low, and wrinkles were generated when the decorative sheet was attached to the aluminum molded material. [Explanation of symbols]

[0079] 1, 2, 3 Decorative sheet 10 Surface layer 20 Base material layer 30 metal layer 40, 42, 44 Adhesive layer 50 Resin layer 60 primer layer

Claims

1. The laminate includes a surface layer, a base layer, and a metal layer in this order, The surface layer contains a urethane resin, The base layer contains a polyester resin, A decorative sheet having an elastic modulus of less than 155 N / 25 mm.

2. 2. The decorative sheet according to claim 1, wherein the average thickness of the substrate layer is 40 μm or less.

3. The decorative sheet of claim 1 , wherein said metal layer comprises a metal, a metal oxide, or an alloy.

4. 2. The decorative sheet according to claim 1, wherein the average thickness of the surface layer is 50 μm or less.

5. 2. The decorative sheet according to claim 1, wherein the average thickness of the metal layer is 1 μm or less.

6. 2. The decorative sheet according to claim 1, which is used as a building material.

7. A construction member comprising an adherend and the decorative sheet according to any one of claims 1 to 6, which covers at least a portion of the surface of the adherend.

Citation Information

Patent Citations

  • Decorative sheet having metallic appearance

    JP1999058660A

  • Metal vapor deposition laminate

    JP2007216608A