Rubber composition for tire and rubber material for tire
The use of fumed silica with controlled surface area and additives in tire rubber compositions addresses the balance of fuel efficiency, wear resistance, and heat aging resistance, enhancing tire performance.
Patent Information
- Application Number
- JP2023058362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing rubber materials for tires face challenges in achieving a balance between low fuel consumption, wear resistance, and heat aging resistance, as previous compositions using carbon black and wet silica either compromise on abrasion resistance or fuel efficiency.
A tire rubber composition is developed using fumed silica as a filler, controlled by its specific surface area, combined with a silane coupling agent and diol, to enhance dispersibility and crosslinking, thereby improving hardness, abrasion resistance, and heat aging resistance.
The composition results in a tire rubber material with improved fuel efficiency, wear resistance, and heat aging resistance, suitable for various tire components.
Smart Images

Figure 2024145837000001 
Figure 2024145837000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tires and a rubber material for tires. Specifically, the present invention relates to a rubber material for tires that is particularly excellent in fuel economy, abrasion resistance, and heat aging resistance, and a composition suitable for producing the rubber material for tires. [Background technology]
[0002] In addition to being fuel-efficient, automobile tires are required to have a long life. To achieve a long life, it is necessary to improve the wear resistance and heat aging resistance of tires. To improve the wear resistance, carbon black has been blended as a reinforcing filler into rubber compositions for tires.
[0003] On the other hand, it is known that wet silica is effective in improving fuel economy, but the abrasion resistance when wet silica is blended is inferior to that when carbon black is blended. Therefore, when wet silica is used as a reinforcing filler, a part of the carbon black blended amount is replaced by wet silica, and the amount of carbon black blended is relatively reduced, so that it is known that a decrease in the abrasion resistance of the rubber material for tires is unavoidable.
[0004] Patent Document 1 proposes a rubber material for tires that contains a rubber component, carbon black and wet silica as fillers, and an inorganic compound powder, for the purpose of obtaining a rubber material for tires that has excellent fuel efficiency and wet grip performance without reducing abrasion resistance.
[0005] In addition, Patent Document 2 proposes replacing a part of wet silica with dry silica. Patent Document 2 describes that dry silica can improve fuel economy more than wet silica and suppress deterioration of rubber hardness.
[0006] Furthermore, Patent Document 3 discloses a rubber composition for tires containing a predetermined amount of an organic acid cobalt or cobalt complex, a phenol derivative, a cyclic polysulfide, and polymethylolmelamine in order to improve heat aging resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-213353 A [Patent Document 2] JP 2016-104840 A [Patent Document 3] Patent Publication No. 2021-172733 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the tire rubber materials described in Patent Documents 1 to 3 have a problem in that they are not materials that can simultaneously achieve low fuel consumption, abrasion resistance, and heat aging resistance.
[0009] The present invention has been made in view of the above circumstances, and has an object to provide a rubber material for tires excellent in fuel economy, abrasion resistance and heat aging resistance, and a rubber composition for tires suitable for producing the same. [Means for solving the problem]
[0010] The present inventors have discovered that by blending fumed silica as a filler in a rubber composition for tires, and further controlling the contents of predetermined additives in accordance with the specific surface area of the fumed silica, a rubber material for tires excellent in fuel economy, abrasion resistance and heat aging resistance can be obtained, and have thus completed the present invention.
[0011] Based on the above, the aspects of the present invention are as follows.
[0012] [1] Diene rubber and surface silanol group density of 3 / nm2 The composition includes a fumed silica, a silane coupling agent, and a diol, The content of the silane coupling agent is 0.50 μmol / m relative to the BET specific surface area per 1 g of fumed silica. 2 More than 3.9 μmol / m 2 is as follows: The diol content is 3 μmol / m2 relative to the BET specific surface area per gram of fumed silica. 2 More than 14 μmol / m 2 The rubber composition for tires is as follows:
[0013] [2] The rubber composition for tires according to [1], wherein the silane coupling agent is a sulfide-based silane coupling agent.
[0014] [3] The rubber composition for tires according to [1] or [2], further comprising 10 parts by mass or more and 70 parts by mass or less of fumed silica per 100 parts by mass of diene rubber.
[0015] [4] The BET specific surface area of fumed silica is 180m 2 / g or more 500m 2 / g or less.
[0016] [5] The rubber composition for a tire according to any one of [1] to [4], wherein the fumed silica is untreated fumed silica.
[0017] [6] A rubber material for tires obtained by vulcanizing the rubber composition for tires according to any one of [1] to [5]. Effect of the Invention
[0018] According to the present invention, it is possible to provide a rubber material for tires excellent in fuel economy, abrasion resistance and heat aging resistance, and a rubber composition for tires suitable for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in detail based on specific embodiments in the following order. 1. Rubber composition for tires 1.1. Diene rubber 1.2. Fumed Silica 1.3.Silane coupling agents 1.4. Diols 1.5.Other Ingredients 2. Method for producing rubber composition for tires 3. Rubber materials for tires
[0020] (1. Rubber composition for tires) The rubber composition for tires according to the present embodiment is a rubber composition comprising a diene rubber and a silanol group having a surface density of 3 / nm 2 The composition includes the following: fumed silica, a silane coupling agent, and a diol:
[0021] (1.1. Diene rubber) The diene rubber contained in the rubber composition for tires according to the present embodiment is preferably at least one selected from natural rubber, isoprene rubber, butadiene rubber, styrene butadiene rubber, acrylonitrile butadiene rubber, butyl rubber, ethylene-propylene-diene rubber, and chloroprene rubber. The content of each of the above rubbers constituting the diene rubber may be appropriately determined depending on the application, etc. Among these, at least one selected from natural rubber and styrene butadiene rubber is preferable.
[0022] Examples of natural rubber include natural rubber (NR) and modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR). These natural rubbers may be used alone or in combination of two or more. In this embodiment, unmodified NR is preferred as the natural rubber.
[0023] Examples of styrene-butadiene rubber (SBR) include unmodified solution-polymerized SBR (S-SBR), unmodified emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR).
[0024] (1.2. Fumed Silica) Fumed silica is fine particle silicon dioxide produced by high temperature hydrolysis of silicon tetrachloride in an oxyhydrogen flame. Therefore, fumed silica is also called dry silica because its production method is different from that of wet silica, which is produced by wet methods such as precipitation and gelation. Fumed silica has a smaller primary particle size of the primary aggregate (smallest constituent) and a larger nitrogen adsorption BET specific surface area than wet silica. Fumed silica particles are aggregated and fused in a beaded shape, forming bulky aggregates.
[0025] Fumed silica has siloxane bonds, but on the surface of the fumed silica, in addition to the siloxane groups, there are silanol groups in which a hydroxyl group is bonded to a silicon atom. The density of silanol groups on the surface of fumed silica (surface silanol group density) is lower than that of wet silica due to differences in the manufacturing method. In this embodiment, the surface silanol group density of the fumed silica is 3 / nm 2 By having the surface silanol group density within the above range, there is an advantage that the amount of silanol groups, which are reaction sites with a silane coupling agent described later, is maintained, while a decrease in wettability with rubber due to adsorption of moisture to the silica surface can be prevented, and thus further fine dispersion can be expected.
[0026] The surface silanol group density may be measured by, for example, the Karl Fischer method, the Igros method, or active hydrogen titration using a Grignard reagent.
[0027] In addition, silanol groups are prone to adsorb water. Therefore, surface treatments are sometimes performed to reduce water adsorption by reacting the silanol groups with other substances. Surface-treated fumed silica is called surface-treated fumed silica, and untreated fumed silica is called untreated fumed silica.
[0028] In this embodiment, the surface-treated fumed silica and the untreated fumed silica are distinguished by the modification hydrophobicity (M value) shown below. The modification hydrophobicity (M value) is a value obtained by a measurement method utilizing the fact that the surface-treated fumed silica floats in water but is completely suspended in methanol. The method described in the examples of International Publication No. 2004 / 099075 can be used to measure the M value. When the surface-treated fumed silica and the untreated fumed silica are expressed using the M value, the M value of the surface-treated fumed silica is 1 or more, and the M value of the untreated fumed silica is less than 1.
[0029] In this embodiment, from the viewpoint that the molecular structure of the silane coupling agent is bulky and a sufficient amount can react with the silica surface, it is preferable that the fumed silica is untreated fumed silica in which the moisture content that induces self-condensation of the coupling agent is small but the silanol groups, which are reaction sites, are sufficiently secured.
[0030] From the viewpoint of industrial productivity, it is preferable that the tap density of the fumed silica is relatively high. Specifically, the tap density of the fumed silica is preferably 200 g / L or more. As described above, since the fumed silica is bulky, it is preferable to compress the fumed silica when the tap density is to be 200 g / L or more.
[0031] Examples of methods for compressing fumed silica include a method of compressing it with a ball mill and a method of compressing it with a vibration mill.
[0032] In this embodiment, the tap density of the fumed silica may be less than 200 g / L.
[0033] In this embodiment, the BET specific surface area of the fumed silica is 200 m 2 / g or more, 250m 2 / g or more, 300m 2 When the BET specific surface area of the fumed silica is within the above range, the number of silanol groups that serve as reaction points with the diene rubber or the silane coupling agent can be sufficiently secured in the fumed silica.
[0034] The upper limit of the BET specific surface area of the fumed silica is not particularly limited, but it is preferably, for example, 500 m 2 / g. If the BET specific surface area of the fumed silica is too small, the flame temperature during the production of the fumed silica must be increased, and the structure specific to the fumed silica is lost, making it difficult to produce the fumed silica stably. If the BET specific surface area of the fumed silica is too large, it tends to make it difficult to produce the fumed silica stably.
[0035] The true density of fumed silica is 2.0 g / cm 3 More than 2.4g / cm 3 It is preferable that the density is 2.1 g / cm or less. 3 More than 2.3g / cm 3 More preferably, it is 2.15 g / cm or less. 3 More than 2.25g / cm 3 When the true density of the fumed silica is within the above range, the elastic modulus of the silica becomes higher than when the true density is lower than 2.0, and the reinforcing effect in the rubber composition is more easily exhibited.
[0036] One of the reasons why the true density is lower than the commonly known 2.2 of amorphous silica is that there are pores inside the silica. According to MacKenzie, E=E0(1-P) 2 It is known that the elastic modulus drops sharply as the pores increase according to the formula. E0 = Elastic modulus of a solid material P = Pore volume E = Elastic modulus of a material with pore volume P
[0037] Filling with a filler with a low modulus of elasticity reduces the reinforcing effect. On the other hand, if the true density is too high, the surface free energy of the silica particle surface increases, which increases the difference in surface free energy with the rubber, and this may cause the dispersibility to deteriorate. In addition, since the reinforcing effect generally increases with the volume fraction of the filler, filling with a substance with too high a density makes it difficult to achieve the effect of improving the modulus of elasticity.
[0038] Known methods for producing amorphous silica with high true density include synthesis under high pressure, rapid cooling during melting, etc. The true density of fumed silica can be measured, for example, by the pycnometer method.
[0039] The amount of fumed silica is preferably 10 parts by mass or more and 70 parts by mass or less per 100 parts by mass of diene rubber. By setting the amount of fumed silica within the above range, a rubber material for tires having excellent fuel efficiency and abrasion resistance can be obtained. If the amount of fumed silica is too large, the viscosity increases, so that the fumed silica is not sufficiently dispersed in the rubber component, and a good kneaded product tends not to be obtained.
[0040] The amount of the fumed silica is more preferably 20 parts by mass or more, and even more preferably 32 parts by mass or more, per 100 parts by mass of the diene rubber, while the amount of the fumed silica is more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the diene rubber.
[0041] (1.3. Silane coupling agents) Hydrophobic diene rubber and fumed silica having hydrophilic silanol groups have low affinity, and are difficult to mix during kneading. Therefore, by blending a silane coupling agent, a crosslinked structure between the diene rubber and the fumed silica is easily formed via the silane coupling agent, and the fumed silica is easily dispersed uniformly in the diene rubber. As a result, the presence of coarse fumed silica that is not dispersed in the rubber can be suppressed in the rubber material for tires, and the wear resistance of the rubber material for tires can be improved.
[0042] As the silane coupling agent, a sulfur-containing silane coupling agent is preferable. Examples of the sulfur-containing silane coupling agent include bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, γ-mercaptopropyl triethoxysilane, 3-octanoylthiopropyl triethoxysilane, and mercapto-thiocarboxylate oligomer. In this embodiment, from the viewpoint of the heat resistance (thermal aging property) of the rubber composition for tires, a sulfide-based silane coupling agent is preferable.
[0043] In order for fumed silica to be uniformly dispersed in diene rubber, the silanol groups of the fumed silica must be bonded with a silane coupling agent to increase the affinity with the hydrophobic diene rubber. Therefore, the silane coupling agent must be blended in an amount that reacts with the silanol groups just right. The surface silanol group density corresponds to the BET specific surface area per gram of fumed silica, so the amount of silane coupling agent to be blended can be determined according to the BET specific surface area per gram of fumed silica.
[0044] Therefore, from the viewpoint of enhancing the dispersibility of the fumed silica, the blending amount of the silane coupling agent (the content of the silane coupling agent in the rubber composition for tires) is set to 0.50 μmol / m with respect to the BET specific surface area per 1 g of the fumed silica. 2 More than 3.9 μmol / m 2 The following is the result.
[0045] The amount of the compound is 0.7 μmol / m 2 On the other hand, the blending amount is preferably 2.0 μmol / m 2 It is preferable that the concentration is 1.5 μmol / m or less. 2 It is more preferable that:
[0046] (1.4. Diol) The diol is a dihydric alcohol and a hydrocarbon having two hydroxyl groups. Although the Mooney viscosity of the tire rubber composition is reduced by blending the diol, the A hardness of the tire rubber material is increased, so that the amount of fumed silica blended can be reduced. As a result, the fuel economy and abrasion resistance of the tire rubber material are improved. Furthermore, blending the diol together with the above-mentioned silane coupling agent provides a tire rubber material with good heat aging resistance. Note that the above-mentioned effects tend not to be obtained with monohydric alcohols and alcohols having trihydric or higher hydricities.
[0047] In this embodiment, preferred examples of diols include propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of about 200 to 1000, and propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of 300 to 500 are more preferred.
[0048] Similarly to the silane coupling agent, the effect obtained by blending the diol may be determined according to the density of the surface silanol groups. Therefore, the blending amount of the diol (the content of the diol in the rubber composition for tires) is set to 3 μmol / m2 relative to the BET specific surface area per gram of the fumed silica. 2 More than 14 μmol / m 2 The following is the result.
[0049] The amount of the compound is 3.4 μmol / m 2It is preferable that the concentration is 6.8 μmol / m or more. 2 More preferably, the amount is 11 μmol / m 2 It is preferable that:
[0050] (1.5. Other Ingredients) In this embodiment, the rubber composition for tires may contain components to be blended in rubber compositions other than the above-mentioned components (diene rubber, fumed silica, silane coupling agent, and diol). An example of such a component is a lubricant. Blending the lubricant improves the kneadability of each component, and makes it easier to obtain a rubber composition for tires in which each component is well dispersed.
[0051] Examples of lubricants include process oils such as stearic acid, mineral oil, and chemically synthesized oil. The lubricants may be used alone or in combination of two or more. Examples of process oils include aromatic oils, paraffin oils, and naphthenic oils. These may be used alone or in combination of two or more.
[0052] The amount of lubricant (content of lubricant in rubber composition for tires) is not limited within the range in which the effects of the present invention can be obtained. For example, the amount of lubricant is preferably 2 parts by mass or more and 60 parts by mass or less, and more preferably 4 parts by mass or more and 50 parts by mass or less, per 100 parts by mass of diene rubber. Specifically, the amount of lubricant may be determined according to the type of diene rubber. For example, when the diene rubber is NR, the amount of lubricant is relatively small, and when the diene rubber is SBR, the amount of lubricant is relatively large, including the lubricant contained in the SBR itself.
[0053] If the amount of lubricant is too small, the viscosity becomes high and kneading becomes poor, and the abrasion resistance of the resulting rubber material for tires may not be sufficiently improved, whereas if the amount of lubricant is too large, shearing is not applied during kneading, and the fumed silica may not be sufficiently dispersed in the diene rubber.
[0054] Furthermore, the rubber composition for tires may contain a reinforcing filler other than hydrophilic fumed silica. Examples of the reinforcing filler include carbon black, wet silica, clay, mica, talc, calcium carbonate, aluminum hydroxide, aluminum oxide, and titanium oxide. When the reinforcing filler is blended, an appropriate amount of a filler coupling agent can also be blended. The blending amount of the reinforcing filler is not limited within the range in which the effects of the present invention can be obtained, and may be a general blending amount.
[0055] Furthermore, the rubber composition for tires may contain various additives such as zinc oxide, antioxidants, plasticizers, processing aids, liquid polymers, thermosetting resins, etc. The amounts of these additives to be blended are not limited as long as the effects of the present invention can be obtained, and may be general amounts.
[0056] (2. Method for producing rubber composition for tires) The rubber composition for tires according to this embodiment is obtained by kneading the above-mentioned diene rubber, the above-mentioned fumed silica, the above-mentioned silane coupling agent, the above-mentioned diol, and, as necessary, other components.
[0057] In this embodiment, the rubber composition for tires may be produced by kneading predetermined components to prepare a master batch, and then blending and kneading the remaining components into the master batch, or by kneading all of the components together.
[0058] When preparing the master batch, it is preferable to knead the above-mentioned diene rubber, the above-mentioned fumed silica, the above-mentioned silane coupling agent, the above-mentioned diol, and, if necessary, other components.
[0059] As a kneading device for preparing the master batch, for example, a Banbury mixer, a kneader, or other known kneading device can be used.
[0060] After the master batch is prepared, other components are blended and kneaded into the master batch to obtain a rubber composition for tires. The master batch and other components can be kneaded using a known kneading device such as a Banbury mixer or a kneader.
[0061] When all the components are kneaded to produce a rubber composition for tires, a known kneading device such as a Banbury mixer or a kneader can be used.
[0062] The kneading conditions may be set so that each component is thoroughly kneaded.
[0063] (3. Rubber materials for tires) The rubber material for a tire according to this embodiment is a material obtained by vulcanizing the above-mentioned rubber composition for a tire.
[0064] In order to improve the dispersibility of fumed silica in the rubber composition for tires, the content of the silane coupling agent is set according to the BET specific surface area of the fumed silica, so that the silane coupling agent can crosslink the diene rubber and the fumed silica without excess or deficiency. As a result, the fumed silica is uniformly kneaded in the rubber composition for tires, and the generation of coarse particles in the rubber material for tires is suppressed. Such an effect is particularly noticeable when the fumed silica is compressed to produce compressed fumed silica.
[0065] Furthermore, rubber materials for tires contain diols. The inclusion of diols increases the A hardness of the rubber after vulcanization, making it possible to reduce the amount of filler used. As a result, fuel economy, abrasion resistance, and heat aging resistance can be improved.
[0066] Therefore, the rubber material for tires according to the present embodiment is excellent in fuel economy, wear resistance, and heat aging resistance. Such rubber material for tires can be suitably used for tires for passenger cars, trucks, buses, etc. It can be suitably used for each component of tires. In particular, it can be suitably used for treads, base treads, sidewalls, clinches, etc.
[0067] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0068] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0069] (Experiment 1) (Preparation of Rubber Composition for Tires) In experiment 1, the diene rubber was SBR rubber. The following components (A) to (D) and (E-1) to (E-4) were charged into a 0.6 L Plastomill, BB600 model, manufactured by Toyo Seiki Co., Ltd., so that the compounding amounts per 100 parts by mass of SBR rubber were as shown in Table 1. After charging, the rotor rotation speed was adjusted within the range of 20 to 100 rpm so that the temperature of the kneaded material was within the range of 140 to 150°C, and the kneading was continued for 5 minutes after the temperature was reached. The air cylinder pressure was 0.5 MPa. After kneading was completed, the mixture was cooled to room temperature and taken out to obtain a master batch. (A) Diene rubber (A-1) SBR (Asahi Kasei S-SBR E-581) (A-2) BR (ENEOS BR01) (B) Filler (B-1) Carbon black (Tokai Carbon, Seast 6, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400g / L) (B-2) Wet silica (Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300g / L, silanol group density: 6 / nm 2 , Pycnometer true density 2.1g / cm 3 ) (B-3) Hydrophilic fumed silica (Tokuyama, Reolosil QS-40, nitrogen adsorption BET specific surface area: 380 m 2 / g, tap density: 50g / L, silanol group density: 2.3 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (B-4) Hydrophilic fumed silica (Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 70g / L, silanol group density: 2.1 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (B-5) (B-4) was compressed in a ball mill to obtain a highly compressed fumed silica with a tap density of 200 g / L (silanol group density: 2.5 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (B-6) (B-4) was compressed in a ball mill to obtain a highly compressed fumed silica with a tap density of 250 g / L (silanol group density: 3 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (B-7) Hydrophilic fumed silica (Tokuyama, Reolosil CP-102, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 100g / L, silanol group density: 1.8 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (B-8) (B-7) was compressed in a ball mill to obtain a highly compressed fumed silica with a tap density of 250 g / L (silanol group density: 3 / nm 2 , Pycnometer true density 2.2g / cm 3 ) (C) Silane coupling agent (C-1) Polysulfide coupling agent (EVONIK Si69) (D) Diol (D-1) 1,3-Propanediol (E) Other ingredients (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, Seido Chemical, zinc oxide type 2) (E-3) Anti-aging agent (Seiko Chemical, Ozonone 6C) (E-4) Process oil (Fuji Kosan, Aromax 3 (TDAE Oil))
[0070] The surface silanol group density of the fumed silica was measured using a Kyoto Electronics Manufacturing Co., Ltd. MKC-610 coulometric titration device equipped with an ADP-512 moisture vaporizer. That is, the temperature was raised to 130°C in the low-temperature side furnace of the moisture vaporizer, and the moisture amount corresponding to the silica drying loss was measured by coulometric titration using the MKC-610 model. Then, the moisture amount corresponding to the ignition loss was measured in the high-temperature side furnace heated to 1000°C in the same manner by coulometric titration. The moisture amount corresponding to the ignition loss generated between 130°C and 1000°C was converted to silanol group density using the following formula. Silanol group density (pcs / nm 2 ) = 668.9 × H 2 O(%) / specific surface area(m 2 / g)
[0071] The above-obtained master batch was mixed with the following (E-5), (E-6) and (E-7) using a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur was determined taking into consideration the amount of sulfur contained in other additive components. (E-5) Sulfur (Tsurumi Chemical Industry, 5% oil-containing fine sulfur) (E-6) Vulcanization accelerator (Sansera CM-G N-cyclohexyl-2-benzothiazole sulfamide (CBS), manufactured by Sanshin Chemical Industry Co., Ltd.) (E-7) Sancerer D-G 1,3-diphenylguanidine (DPG)
[0072] The compressed fumed silica (B-5) was obtained by putting 200 g of the fumed silica (B-4) into a ball mill with a volume of 7 L (ball diameter: φ32 mm, ball filling rate: 30%) and grinding at room temperature at a rotation speed of 300 rpm for about 5 hours. The tap density of the compressed fumed silica (B-6) and the compressed fumed silica (B-8) was adjusted by changing the grinding time.
[0073] The nitrogen adsorption BET specific surface area of the fillers (B-1) to (B-8) was measured for each filler by the nitrogen adsorption BET method using a Microtrac BELSOP MINI X. The tap density of the fillers (B-1) to (B-8) was measured as follows. First, a 1 L resin graduated cylinder was placed on an electronic balance, tared, and filled with about 1 L of filler, and the weight M (g) was recorded. After that, the cylinder was manually tapped 30 times from a height of about 10 cm, and the volume V (ml) was measured, and the tap density ρ was calculated from the following formula. Tap density ρ=1000×M / V(g / L)
[0074] [Table 1]
[0075] Test specimens were prepared for the resulting rubber composition for tires to carry out the following evaluations. The resulting test specimens were used to evaluate the following physical properties.
[0076] (Processability: Mooney viscosity) The Mooney viscosity (ML1+4 100°C) at 100°C of the obtained rubber composition for tires was measured using a Mooney viscometer (VR-1132 manufactured by Ueshima Seisakusho) in accordance with JIS K6300-1. When the Mooney viscosity is low, the processability of the rubber composition for tires tends to be good. The results are shown in Table 1.
[0077] (Preparation of tire rubber material test pieces) The resulting rubber composition for tires was press-vulcanized at T90+1 min, determined under conditions of 160°C for 30 min according to JIS K6300-2, to obtain a rubber material for tires. Test pieces for the following evaluations were prepared from the resulting rubber material for tires. The following physical properties were evaluated using the resulting test pieces.
[0078] (A hardness) The hardness (Shore A hardness) of the obtained test piece of the rubber material for tires was measured using a durometer in accordance with JIS K6253 Type A. Since the target A hardness of the rubber material for tires is 65, it is preferable that the A hardness of the test piece is also around 65. The results are shown in Table 1.
[0079] (Fuel efficiency: tan δ at 60℃) The obtained test pieces of the rubber material for tires were measured under the following conditions using a dynamic viscoelasticity tester (VR-7130 manufactured by Ueshima Seisakusho) in accordance with JIS K6394. Tan δ (60°C) was calculated from the measured value at 60°C. Measurement temperature: 60℃ Static strain: 10% Dynamic Distortion: ±2% Frequency: 10Hz
[0080] The rolling resistance index was calculated by the following formula, taking the calculated tan δ (60° C.) of Reference Example 1 (Comparative Example 1) as 1.0. The larger the index, the better the rolling resistance. The results are shown in Table 1. (Rolling resistance index) = (tan δ of standard example 1 (60°C)) / (tan δ of example (60°C))
[0081] (Wear resistance: FPS wear amount) For the test pieces of the obtained rubber material for tires, the FPS abrasion amount was measured using an FPS abrasion tester (AB-2012 manufactured by Ueshima Seisakusho) under the conditions of a temperature of 35°C, a load of 40N, a slip rate of 10%, and a test time of 2 minutes. The volume loss was calculated from the FPS abrasion amount, and the abrasion index was calculated using the following formula, with the loss amount of Standard Example 1 (Comparative Example 1) being set at 1.0. The higher the index, the better the abrasion resistance. The results are shown in Table 1. (Wear index) = (loss amount of control example 1) / (loss amount of example)
[0082] (Heat aging resistance) The obtained rubber composition for tires was vulcanized at 160°C for T90+1 minutes using a 2mm thick mold, and the obtained vulcanized rubber sheet was punched out with a JIS No. 3 dumbbell to obtain a sample. The sample was heat aged for 5 days (120 hours) in a gear oven set at a temperature of 80°C, and then the strength at break (break strength) was measured together with an unaged sample using a tensile tester according to JIS K6251. The ratio of the unaged break strength to the break strength after aging was taken as an index of heat aging resistance. The heat resistance index was calculated using the following formula. When the heat resistance index is 1 or more, the heat aging resistance is excellent, and when the heat resistance index is less than 1, the break strength decreases due to thermal degradation, so the heat aging resistance is poor. The results are shown in Table 1. (Heat resistance index)={(breaking strength after heat aging) / (breaking strength of unaged sample)}
[0083] Furthermore, for the samples before the heat aging test, the strength index was calculated by the following formula, taking the breaking strength of Control Example 1 (Comparative Example 1) as 1.00. The higher the strength index, the better the strength. The results are shown in Table 1. (Strength index)=(Breaking strength of Example) / (Breaking strength of Reference Example 1)
[0084] From Table 1, it was confirmed that when the diene rubber is an SBR rubber, the tire rubber material in which the amount of the silane coupling agent and the diol added is within the above-mentioned range has higher abrasion resistance than the tire rubber material produced by kneading carbon black or wet silica. At the same time, it was also confirmed that it has high heat aging resistance.
[0085] (Experiment 2) In experiment 2, the diene rubber was NR rubber. The following components (A) to (D) and (E-1) to (E-4) were added to a Moriyama pressure kneader with a volume of 0.5 L so that the compounding amounts per 100 parts by mass of NR rubber were as shown in Table 2. After the materials were added one by one, the rotor rotation speed was 30 rpm, and after the temperature of the kneaded material reached a range of 140 to 150°C, the kneading was continued for 5 minutes. The ram pressure during kneading was in the range of 0.4 to 0.5 MPa. After kneading was completed, the kneaded material was cooled to room temperature to obtain a kneaded material. (A) Diene rubber (A-3) Vietnamese natural rubber: SVR (B) Filler (B-1) Carbon black (Tokai Carbon, Seast 6, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400g / L) (B-2) Wet silica (Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300g / L, silanol group density: 6 / nm 2 ) (B-4) Hydrophilic fumed silica (Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 70g / L) (B-5) (B-4) is compressed in a ball mill to produce highly compressed fumed silica with a tap density of 200 g / L. (B-6) (B-4) is compressed in a ball mill to produce highly compressed fumed silica with a tap density of 250 g / L. (C) Silane coupling agent (C-1) Polysulfide coupling agent (EVONIK Si69) (D) Diol (D-1) 1,3-Propanediol (E) Other ingredients (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, Seido Chemical, zinc oxide type 2) (E-3) Anti-aging agent (Seiko Chemical, Ozonone 6C) (E-4) Process oil (Fuji Kosan, Aromax 3 (TDAE Oil))
[0086] The following (E-5) and (E-8) were added to the obtained kneaded product and mixed using a 6-inch roll tester to obtain a rubber composition for tires. (E) Other ingredients (E-5) Sulfur (Tsurumi Chemical Industry, 5% oil-containing fine sulfur) (E-8) Vulcanization accelerator (N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS), Sanshin Chemical Industry, Sancerer NS-G)
[0087] [Table 2]
[0088] For the obtained rubber composition for tires, test specimens were prepared for the same evaluation as in Experiment 1. The obtained test specimens were used to evaluate the physical properties (Mooney viscosity) evaluated in Experiment 1. The results are shown in Table 2.
[0089] (Preparation of rubber material for tires) The obtained rubber composition for tires was then press-vulcanized for T90+1 min, determined according to JIS K6300-2 at 150°C for 60 min, to obtain a rubber material for tires. Test pieces were prepared for the obtained rubber material for tires to perform the same evaluations as in Experiment 1. Using the obtained test pieces, some of the physical properties evaluated in Experiment 1 were evaluated. The strength index was based on that of Standard Example 2 (Comparative Example 5). The results are shown in Table 2.
[0090] From Table 2, it was confirmed that even if the diene rubber is NR, the tire rubber material in which the amount of the silane coupling agent and the diol added is within the above-mentioned range has higher heat aging resistance than the tire rubber material produced by kneading carbon black or wet silica.
Claims
1. Diene rubber and surface silanol group density of 3 / nm 2 The composition includes a fumed silica, a silane coupling agent, and a diol, The content of the silane coupling agent is 0.50 μmol / m with respect to the BET specific surface area per 1 g of the fumed silica. 2 3.9 μmol / m or more 2 is as follows: The content of the diol is 3 μmol / m with respect to the BET specific surface area per 1 g of the fumed silica. 2 14 μmol / m or more 2 A rubber composition for tires, comprising:
2. 2. The rubber composition for tires according to claim 1, wherein the silane coupling agent is a sulfide-based silane coupling agent.
3. The rubber composition for tires according to claim 1 or 2, comprising 10 parts by mass or more and 70 parts by mass or less of the fumed silica per 100 parts by mass of the diene rubber.
4. The BET specific surface area of the fumed silica is 180 m 2 / g or more 500m 2 The rubber composition for tires according to claim 1 or 2, wherein the viscosity is 0.1 to 100 MPa.
5. 3. The rubber composition for tires according to claim 1, wherein the fumed silica is untreated fumed silica.
6. A rubber material for tires obtained by vulcanizing the rubber composition for tires according to claim 1 or 2.
Citation Information
Patent Citations
Manufacturing method of rubber composition, rubber composition and pneumatic tire
JP2005213353A
Tire rubber composition
JP2016104840A
Rubber composition for tires
JP2021172733A