Heat insulating material for combustion chamber, water heater and boiler
A plate-shaped molded body with varying bulk densities enhances insulation and reduces weight, addressing the limitations of existing insulating materials by creating an air layer and ensuring stable, cost-effective installation and maintenance.
Patent Information
- Application Number
- JP2023058375
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing combustion chamber insulating materials face issues with insufficient insulation, heavy weight, long drying time, poor workability, and high cost, necessitating improved insulation performance, stable installation, and durability.
A plate-shaped molded body composed of inorganic fibers with varying bulk densities, featuring a first main surface with lower density than the central portion, is used to create an air layer for enhanced insulation, and is manufactured using a papermaking method to ensure ease of installation and maintenance.
The solution provides superior heat insulation, reduced weight, improved workability, and cost-effectiveness, while maintaining durability and stability within the combustion chamber.
Smart Images

Figure 2024145841000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a combustion chamber insulation material, a water heater, and a boiler. [Background technology]
[0002] 2. Description of the Related Art Boilers and water heaters are used as devices that supply steam or hot water using fuels such as petroleum.
[0003] Boilers and water heaters generate steam or hot water from water by burning fuel in a combustion chamber and transferring the heat of combustion to water through water pipes placed inside the combustion chamber.
[0004] Because the combustion chamber becomes very hot, it is usually protected by refractories and heat insulating materials in order to protect surrounding equipment from heat damage and to reduce energy loss (see, for example, Patent Documents 1 and 2).
[0005] In particular, in combustion chambers where the temperature rises due to combustion gas, refractories and heat insulating materials are generally made by pouring a fluid containing heat-resistant material onto the surface of the object to be installed and solidifying it. Such materials are also called castable materials. Although castable materials can conform to any surface shape and provide a certain degree of heat insulation, they have problems such as insufficient heat insulation, heavy weight, long drying time, and poor workability during construction. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4946594 [Patent Document 2] Patent No. 4640705 Summary of the Invention [Problem to be solved by the invention]
[0007] The use of insulating materials containing inorganic fibers instead of castable materials is being considered, but insulating materials installed inside combustion chambers are required to have improved insulating performance, be stable and easy to install and maintain, be durable, and be able to be supplied at low cost.
[0008] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a combustion chamber insulation material which has a greater insulating effect, can be stably and easily installed and maintained, is durable, and can be supplied at low cost. [Means for solving the problem]
[0009] In other words, the combustion chamber insulating material of the present invention is a plate-shaped molded body containing inorganic fibers, and is characterized in that when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion located between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion, and the first main surface portion is positioned toward the inner wall surface of the combustion chamber. The combustion chamber insulating material of the present invention has a low bulk density of the first main surface portion and is positioned such that the first main surface portion faces the inner wall surface of the combustion chamber, thereby creating an air layer on the inner wall surface side of the combustion chamber, thereby enhancing the insulating effect.
[0010] It is preferable that the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) smaller than the bulk density of the central portion.
[0011] The combustion chamber insulating material of the present invention is preferably formed by a papermaking method. By forming the material using a papermaking method and drying it, the bulk density of the combustion chamber insulating material in the thickness direction can be easily adjusted.
[0012] The combustion chamber insulating material of the present invention preferably has a flat or curved shape. When the combustion chamber insulating material of the present invention has the above-mentioned shape, it can be disposed at various locations inside the combustion chamber.
[0013] The combustion chamber insulating material of the present invention has an overall bulk density of 0.20 to 0.35 g / cm 3 It is preferable that: When the overall bulk density is within the above range, the strength required for the heat insulating material is ensured, while the weight can be reduced in comparison with a fireproof material using an amorphous material.
[0014] It is preferable that the bulk density of the first main surface portion is smaller by 3% or more than the larger of the bulk density of the second main surface portion and the bulk density of the central portion. When the bulk density of the first main surface portion is within the above range, an air layer is formed on the inner wall surface side of the combustion chamber, thereby improving the heat insulating effect. In addition, by making the larger of the bulk density of the second main surface portion and the bulk density of the central portion 3% or more higher than the bulk density of the first main surface portion, the wind corrosion resistance against contact with combustion gas is improved, and the strength as a heat insulating material is ensured, allowing the combustion chamber insulating material of the present invention to be used stably for a long period of time.
[0015] The water heater of the present invention comprises a combustion chamber, a heat exchanger installed within the combustion chamber, and a combustion chamber insulation material of the present invention, and is characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing toward the inner wall surface of the combustion chamber.
[0016] The water heater of the present invention is equipped with the combustion chamber insulation material of the present invention, and because the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, enhancing the insulation effect, and providing an excellent effect in suppressing CO2 emissions.
[0017] The boiler of the present invention comprises a combustion chamber and the combustion chamber insulation material of the present invention, and is characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.
[0018] The boiler of the present invention is equipped with the combustion chamber insulation material of the present invention, and since the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, thereby enhancing the insulation effect, and achieving excellent CO2 emission suppression effect. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a perspective view that illustrates an example of a combustion chamber insulating material of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line AA of FIG. 1, showing a schematic example of the internal structure of the combustion chamber insulating material. [Diagram 3] FIG. 3 is a cross-sectional view taken along the line AA, which shows a schematic diagram of another example of the internal structure of the combustion chamber insulating material shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates an example of a process for producing the combustion chamber insulating material of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates another example of the steps for producing a combustion chamber insulating material of the present invention. [Figure 6] FIG. 6 is a cross-sectional view that illustrates an example of a water heater of the present invention. [Figure 7] FIG. 7 is a cross-sectional view that illustrates an example of a boiler of the present invention.
[0020] Detailed Description of the Invention [Insulation material for combustion chamber] First, the combustion chamber insulating material of the present invention will be described. The combustion chamber insulating material of the present invention is a plate-shaped molded body containing inorganic fibers, and is characterized in that when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion, and the first main surface portion is positioned toward the inner wall surface of the combustion chamber.
[0021] In this specification, the term "plate-like" refers to a shape having two opposing main surfaces with relatively large areas and a side surface connecting the two main surfaces. The direction in which the two main surfaces extend is also called the surface direction, and the direction connecting the two main surfaces is also called the thickness direction. At least one of the two opposing main surfaces may be curved.
[0022] FIG. 1 is a perspective view that illustrates an example of a combustion chamber insulating material of the present invention. A combustion chamber insulating material 1 shown in FIG. 1 is composed of a plate-like molded body 10 containing inorganic fibers. The plate-like molded body 10 has a plate-like shape having first and second main surfaces 10a and 10b that face each other and have relatively large areas, and a side surface 10c that connects the first and second main surfaces 10a and 10b.
[0023] The first and second main surfaces 10a, 10b have a substantially circular shape when viewed in the thickness direction. Therefore, the outer shape of the plate-like molded body 10 and the combustion chamber insulating material 1 can be said to be a disk shape having a predetermined thickness.
[0024] The combustion chamber insulating material of the present invention preferably has a flat or curved shape. With the above-mentioned shape, the combustion chamber insulating material of the present invention can be disposed at various locations inside the combustion chamber. The shape of the combustion chamber insulating material is the shape of the plate-shaped molded body.
[0025] Since the combustion chamber insulating material 1 is composed only of the plate-shaped molded body 10, the plate-shaped molded body 10 can be said to be the combustion chamber insulating material 1. That is, in the combustion chamber insulating material of the present invention, the plate-like molded body itself may be the combustion chamber insulating material.
[0026] The plate-like molded body contains inorganic fibers. The inorganic fibers preferably include at least one selected from the group consisting of biosoluble fibers, alumina fibers, rock wool, and glass fibers. As the biosoluble fiber, for example, alkaline earth silicate fiber (AES fiber) can be used. Also, shot components of non-fibrous particles may be contained. When the inorganic fibers contain the above-mentioned material, a plate-shaped molded product having excellent heat resistance can be obtained.
[0027] The combustion chamber insulation material 1 is made of a plate-shaped molded body 10 containing inorganic fibers, so it has a smaller weight per volume and is easier to work with than castable materials. The plate-shaped molded body 10 has the property of being less prone to deformation with less localized bias of the inorganic fibers, making it suitable as an insulation material to be placed inside a combustion chamber.
[0028] The plate-shaped molded body may be a paper molded body or a needle body. The paper molded body is a molded body obtained by pouring a slurry containing inorganic fibers into a mold, and performing paper molding by suction dehydration and drying (papermaking method). The plate-shaped molded body obtained by the papermaking method is also called a plate-shaped paper molded body. The needle body is a molded body obtained by performing a needling process on an inorganic fiber aggregate, and the plate-shaped molded body obtained by the needling process is also called a plate-shaped needle body.
[0029] The plate-like molded body is preferably one molded by a papermaking method. Papermaking bodies have the property of having little localized unevenness of inorganic fibers and being resistant to deformation, and are therefore suitable as a heat insulating material to be placed inside a combustion chamber.
[0030] The average fiber diameter of the inorganic fibers is not particularly limited, but is preferably 2.0 to 15.0 μm when the plate-shaped molded product is a paper product. When the average fiber diameter of the inorganic fibers is within the above range, a dense plate-shaped molded product with little local deviation in bulk density can be obtained.
[0031] The average fiber length of the inorganic fibers is not particularly limited, but is preferably 0.05 to 3.0 mm when the plate-shaped molded product is a paper molded product. When the average fiber length of the inorganic fibers is within the above range, a plate-shaped molded product can be obtained in which the inorganic fibers are laminated with little local bias, and the bulk density and heat insulation properties are stable.
[0032] The combustion chamber insulating material of the present invention has a different bulk density in the thickness direction of the plate-shaped molded body. Specifically, when comparing the bulk densities of the first main surface portion, the second main surface portion, and the central portion between the first main surface portion and the second main surface portion in the thickness direction of the plate-shaped molded body, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion.
[0033] The internal structure of a combustion chamber insulating material 1A, which is a first embodiment of the combustion chamber insulating material 1, will be described below with reference to FIG. Fig. 2 is a cross-sectional view taken along line AA, which is a schematic diagram showing an example of the internal structure of the combustion chamber insulating material in Fig. 1. The combustion chamber insulating material 1A is composed of a plate-shaped molded body 10A. When comparing the bulk densities of the first main surface portion 11, the second main surface portion 12, and the central portion 13 between the first main surface portion 11 and the second main surface portion 12 in the thickness direction of the plate-shaped molded body 10A, the first main surface portion 11 has the smallest bulk density, followed by the central portion 13 and the second main surface portion 12 in that order. The first principal surface portion 11 includes a first principal surface 10Aa, and the second principal surface portion 12 includes a second principal surface 10Ab.
[0034] Next, the internal structure of a combustion chamber insulating material 1B, which is a second embodiment of the combustion chamber insulating material 1, will be described below with reference to Fig. 3. Only the differences from the combustion chamber insulating material 1A, which is the first embodiment, will be described here, and explanations of common points will be omitted. FIG. 3 is a cross-sectional view taken along the line AA, which shows a schematic diagram of another example of the internal structure of the combustion chamber insulating material shown in FIG. In the plate-like molded body 10B constituting the combustion chamber insulating material 1B, the first main surface portion 11 and the second main surface portion 12 have low bulk density, and the central portion 13 has high bulk density. The second main surface portion 12 may have a bulk density intermediate between the bulk density of the first main surface portion 11 and the bulk density of the central portion 13.
[0035] In Figures 2 and 3, the first main surface portion 11, the second main surface portion 12, and the central portion 13 are divided equally into three parts in the thickness direction, but the thicknesses of the first main surface portion 11, the second main surface portion 12, and the central portion 13 do not have to be the same.
[0036] The bulk density of the second main surface portion is preferably (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion. The bulk density of the second main surface portion may be approximately the same as the bulk density of the central portion.
[0037] In the combustion chamber insulation material of the present invention, the bulk density of the first main surface portion of the plate-shaped molded body is preferably at least 3% smaller than the larger of the bulk density of the second main surface portion and the bulk density of the central portion, and more preferably at least 5% smaller.
[0038] In the combustion chamber insulating material of the present invention, the first main surface portion is disposed facing the inner wall surface of the combustion chamber. By disposing the first main surface portion, which has a low bulk density, facing the inner wall surface of the combustion chamber, a large insulating effect can be obtained.
[0039] The combustion chamber insulating material of the present invention is an integrally formed plate-like molded body, and is not an assembly of a plurality of plate-like molded bodies having different bulk densities laminated in the thickness direction.
[0040] The bulk density of the combustion chamber insulation material is 0.20 to 0.35 g / cm 3 It is preferable that: When the bulk density of the plate-shaped molded body is within the above range, the strength (bending strength) and insulating properties required for a combustion chamber insulation material can be maintained, while the weight increase of the combustion chamber can be suppressed compared to fireproof materials and insulation materials made of amorphous materials.
[0041] The bulk density can be adjusted, for example, by adjusting the fiber length of the inorganic fibers and the aggregate floc size, or by adjusting the compression conditions during slurry dewatering and drying.
[0042] The bulk density of fireproofing materials and heat insulating materials made of amorphous materials is usually 0.7 to 1.5 g / cm 3 This does not satisfy the preferable bulk density of the combustion chamber insulating material described above.
[0043] The thickness of the plate-like molded product is preferably 1 to 10 cm. When the thickness of the plate-like molded product is within the above range, the plate-like molded product can exhibit sufficient heat insulating properties as a heat insulating material.
[0044] The area of the plate-shaped molded body as viewed in the thickness direction (planar area) is 350 to 15,000 cm 2 It is preferable that:
[0045] The volume of the plate-shaped molded body is 700 to 150,000 cm 3 When the volume of the plate-like molded article is within the above range, breakage due to thermal shrinkage is particularly unlikely to occur.
[0046] The plate-shaped molded body may have holes penetrating in the thickness direction. By forming such holes, it becomes easier to cover the inner wall surface of the combustion chamber in which piping such as water pipes and smoke pipes are arranged.
[0047] The plate-like molded product may contain components other than the inorganic fibers, such as inorganic particles, inorganic binders, organic binders, and flocculants.
[0048] Examples of inorganic particles include silica particles, alumina particles, titania particles, zirconia particles, and natural mineral particles. Examples of the inorganic binder include silica sol, alumina sol, titania sol, zirconia sol, and fumed silica. Examples of the organic binder include polyvinyl alcohol, starch, acrylic resin, and polyacrylamide.
[0049] The weight ratio of the inorganic fibers in the plate-like molded product is preferably 30 to 97% by weight.
[0050] The method for producing the combustion chamber insulating material of the present invention is not particularly limited, but it can be produced, for example, by the following procedure. A method for producing the combustion chamber insulating material 1A will be described below with reference to FIG. FIG. 4 is a cross-sectional view that illustrates an example of a process for producing the combustion chamber insulating material of the present invention. Step (1) A slurry containing water, inorganic fibers, an inorganic binder, an organic binder and a flocculant is prepared, and a base sheet 50 of the heat insulating material is obtained by a papermaking method (A in FIG. 4). Step (2) After papermaking, a stainless steel plate HP heated to 150° C. is placed on the first main surface 50a of the original sheet containing moisture, and dried for 30 minutes (FIG. 4B). Step (3): Next, the original sheet 50 of (2) is sandwiched between two SUS plates HP heated to 150°C from the first main surface 50a side and the second main surface 50b side, and dried for one hour while compressing the original sheet 50 to a desired thickness (FIG. 4C). In this way, a combustion chamber insulating material 1A can be obtained (FIG. 4D).
[0051] In the above method, the organic binder solidifies on the first main surface 50a side of the original sheet 50 where drying has progressed, and even when compressed, the original sheet 50 does not collapse and the bulk density does not change. When the original sheet 50 is sandwiched between two SUS plates HP, the undried parts are compressed, and the bulk density of the inorganic fibers in the central portion 13 and the second main surface portion 12 of the obtained plate-like molded body 10A increases. In the plate-like molded body 10A, the second main surface portion 12 has a higher bulk density than the central portion 13, which is thought to be because the central portion of the original sheet 50 was slightly dried in the above step (2).
[0052] Next, a method for producing the combustion chamber insulating material 1B will be described with reference to FIG. FIG. 5 is a cross-sectional view that illustrates another example of the steps for producing a combustion chamber insulating material of the present invention. (1) A slurry containing water, inorganic fibers, an inorganic binder, an organic binder and a flocculant is prepared, and a base sheet 50 of the heat insulating material is obtained by a papermaking method (FIG. 5A). (2) After papermaking, a SUS plate HP heated to 150° C. is placed on the second main surface 50b of the moist original sheet, and dried for 30 minutes (FIG. 5B). (3) After that, the original sheet 50 is turned upside down, and a SUS plate HP heated to 150° C. is placed on the first main surface 50a, and dried for 30 minutes (FIG. 5C). (4) Next, the original sheet 50 of (3) is sandwiched between two SUS plates HP heated to 150°C from the first main surface 50a side and the second main surface 50b side, and dried for one hour while compressing the original sheet 50 to a desired thickness (D in FIG. 5). In this way, a combustion chamber insulating material 1B can be obtained (E in FIG. 5).
[0053] In the above method, the organic binder solidifies on the first main surface 50a and the second main surface 50b of the original sheet 50 where drying has progressed, and the original sheet 50 does not collapse even when compressed, and the bulk density does not change. When the original sheet 50 is sandwiched between two SUS plates HP, only the undried central portion is compressed, and the bulk density of the central portion 13 of the obtained plate-like molded body 10B becomes large.
[0054] The combustion chamber insulation material of the present invention has a surface with a low bulk density facing the inner wall surface of the combustion chamber, so that the insulation effect is greater. Since the combustion chamber insulation material of the present invention is a plate-shaped molded body containing inorganic fibers, it is lighter in weight than a castable molded body of the same volume, and can be stably and easily attached and maintained on the inner wall surface of the combustion chamber. Furthermore, since the combustion chamber insulation material of the present invention contains inorganic fibers, it has durability and can be supplied at low cost.
[0055] The heat insulating material for a combustion chamber of the present invention can be used, for example, in an apparatus equipped with a combustion chamber, such as a water heater or a boiler.
[0056] [Water heater] The water heater of the present invention comprises a combustion chamber, a heat exchanger installed within the combustion chamber, and a combustion chamber insulation material of the present invention, and is characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing toward the inner wall surface of the combustion chamber. The water heater of the present invention is equipped with the combustion chamber insulation material of the present invention, and because the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, enhancing the insulation effect, and providing an excellent effect in suppressing CO2 emissions.
[0057] An example of a water heater according to the present invention will be described below. FIG. 6 is a cross-sectional view that illustrates an example of a water heater of the present invention. The water heater 500 has a combustion chamber 540 and a heat exchanger 170 disposed within the combustion chamber 540 . The combustion chamber 540 has a metal container 150 and two combustion chamber insulation materials 1 arranged on a top surface 150a and a bottom surface 150b of the metal container 150. The combustion chamber insulation material 1 is arranged such that a first main surface 10a faces the inner wall surface of the combustion chamber. Water flows in heat exchanger 170, and the water in heat exchanger 170 is heated in combustion chamber 540 to become hot water (hot water), and the hot water (hot water) is supplied to the outside of water heater 500.
[0058] The temperature of the hot water supplied can be appropriately adjusted by adjusting the amount of fuel burned in the combustion chamber and the amount of water passing through the heat exchanger per unit time.
[0059] [boiler] The boiler of the present invention comprises a combustion chamber and the combustion chamber insulation material of the present invention, and is characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber. The boiler of the present invention is equipped with the combustion chamber insulation material of the present invention, and since the bulk density of the first main surface portion is low, an air layer can be created on the inner wall surface side of the combustion chamber, thereby enhancing the insulation effect, and achieving excellent CO2 emission suppression effect.
[0060] An example of a boiler according to the present invention will now be described. FIG. 7 is a cross-sectional view that illustrates an example of a boiler of the present invention. The boiler 600 includes a combustion chamber 550 and water tubes 180 disposed within the combustion chamber 550 . The combustion chamber 550 has a metal container 160 and two combustion chamber insulation materials 1 arranged on a top surface 160a and a bottom surface 160b of the metal container 160. The combustion chamber insulation material 1 is arranged such that a first main surface 10a faces the inner wall surface of the combustion chamber. Water is supplied into the water pipe 180 from the lower part of the combustion chamber 550 , and the water passing through the water pipe 180 is heated in the combustion chamber 550 to become steam, which is discharged from the upper part of the combustion chamber 550 . The discharged water vapor is used for power generation, heating, cleaning, cooking, drying, disinfection, sterilization, etc. after separating the liquid water or superheating as necessary.
[0061] The method for arranging the combustion chamber insulating material on the inner wall surface of the combustion chamber is not particularly limited, and for example, it can be fixed with bolts and nuts. The first main surface portion of the combustion chamber insulating material may be arranged on the inner wall surface of the combustion chamber via an inorganic adhesive.
[0062] The present specification discloses the following:
[0063] The present disclosure (1) is an insulating material for a combustion chamber, which is a plate-like molded body containing inorganic fibers, characterized in that, when comparing the bulk densities of a first main surface portion, a second main surface portion, and a central portion between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion, and the first main surface portion is arranged toward the inner wall surface of the combustion chamber.
[0064] The present disclosure (2) is a combustion chamber insulating material according to the present disclosure (1), wherein the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion.
[0065] The present disclosure (3) is a combustion chamber insulating material according to the present disclosure (1) or (2), which is formed by a papermaking method.
[0066] The present disclosure (4) is a combustion chamber insulating material according to any one of the present disclosures (1) to (3), which has a flat or curved shape.
[0067] The present disclosure (5) relates to a method for producing a granular sieve having a bulk density of 0.20 to 0.35 g / cm 3 The insulating material for a combustion chamber according to any one of the present disclosures (1) to (4),
[0068] The present disclosure (6) is a combustion chamber insulating material according to any one of the present disclosures (1) to (5), in which the bulk density of the first main surface portion is smaller by 3% or more than the larger of the bulk density of the second main surface portion and the bulk density of the central portion.
[0069] The present disclosure (7) is a water heater comprising a combustion chamber, a heat exchanger installed in the combustion chamber, and a combustion chamber insulation material described in any one of the present disclosures (1) to (6), characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing an inner wall surface of the combustion chamber.
[0070] The present disclosure (8) is a boiler comprising a combustion chamber and a combustion chamber insulation material described in any one of the present disclosures (1) to (6), wherein a first main surface portion of the combustion chamber insulation material is arranged facing an inner wall surface of the combustion chamber.
[0071] (Example) Examples that more specifically disclose the present invention are shown below. Note that the present invention is not limited to these examples. In the following examples, the upper layer of the plate-shaped molded body corresponds to the first main surface portion, the middle layer corresponds to the center portion, and the lower layer corresponds to the second main surface portion.
[0072] Example 1 Water, AES fiber, inorganic binder (silica sol), organic binder (acrylate-based latex) and coagulant (aluminum sulfate) were added to a commercially available pulper and dispersed to prepare a slurry liquid. The prepared slurry liquid was poured into a mold, dehydrated, and a master sheet was obtained by a papermaking method. The master sheet had a thickness of 38 mm. A Teflon (registered trademark)-coated SUS metal plate was placed on the first main surface of the obtained master sheet and dried at 150 ° C for 30 minutes. Thereafter, the master sheet was sandwiched between two of the same SUS metal plates from the first main surface side and the second main surface side, and the thickness of the master sheet was adjusted to 30 mm, and dried at 150 ° C for 1 hour to obtain a plate-shaped molded body. The bulk density of the upper layer of the obtained plate-shaped molded body was 0.294 g / cm 3 , the bulk density of the middle layer is 0.316g / cm 3 , the bulk density of the lower layer is 0.338 g / cm 3 It was.
[0073] Example 2 Water, AES fiber, inorganic binder (silica sol), organic binder (acrylate-based latex) and coagulant (aluminum sulfate) were added to a commercially available pulper and dispersed to prepare a slurry liquid according to Example 2. The prepared slurry liquid was poured into a mold, dehydrated, and a prototype sheet was obtained by a papermaking method. The thickness of the prototype sheet was 35 mm. A Teflon (registered trademark)-coated SUS metal plate was placed on the second main surface of the obtained prototype sheet and dried at 150 ° C for 30 minutes. Next, the prototype sheet was turned over, the same SUS metal plate was placed on the first main surface, and dried at 150 ° C for 30 minutes. Thereafter, the prototype sheet was sandwiched between two of the same SUS metal plates from the first main surface side and the second main surface side, the thickness of the prototype sheet was adjusted to 30 mm, and it was dried at 150 ° C for 1 hour to obtain a plate-shaped molded body. The bulk density of the upper layer of the obtained plate-shaped molded body was 0.221 g / cm 3 , the bulk density of the middle layer is 0.239 g / cm 3 , the bulk density of the lower layer is 0.226 g / cm 3 It was.
[0074] Example 3 Using the slurry prepared in Example 1, a base sheet was made and dried in the same manner as in Example 2 to obtain a plate-like molded product having a thickness of 30 mm. The bulk density of the upper layer of the obtained plate-like molded product was 0.291 g / cm. 3 , the bulk density of the middle layer is 0.320g / cm 3 , the bulk density of the lower layer is 0.293 g / cm 3 It was.
[0075] Comparative Example 1 A 30 mm thick original sheet was obtained in the same manner as in Example 1. The obtained original sheet was placed on a plate-shaped shelf in a dryer and dried at 150° C. for 3 hours to obtain a 30 mm thick plate-shaped product. The obtained plate-shaped product had a uniform bulk density of 0.300 g / cm. 3 It was.
[0076] Comparative Example 2 A 30 mm thick original sheet was obtained in the same manner as in Example 2. The obtained original sheet was placed on a plate-shaped shelf in a dryer and dried at 150° C. for 3 hours to obtain a 30 mm thick plate-shaped product. The obtained plate-shaped product had a uniform bulk density of 0.220 g / cm. 3 It was.
[0077] Comparative Example 3 Water, AES fiber, inorganic binder (silica sol), organic binder (acrylate-based latex) and coagulant (aluminum sulfate) were charged into a commercially available pulper and dispersed to prepare a slurry liquid according to Comparative Example 3. The prepared slurry liquid was poured into a mold, dehydrated, and a 15 mm thick original sheet was obtained by a papermaking method. The obtained original sheet was placed on a plate-shaped shelf in a dryer and dried at 150°C for 3 hours to obtain a plate-shaped molded product S. The obtained plate-shaped molded product had a uniform bulk density of 0.350 g / cm. 3 It was. The same procedure as in Comparative Example 2 was used to produce a 15 mm thick slab with a bulk density of 0.220 g / cm 3 A plate-shaped molded product T was obtained. The plate-like molded body T was placed on the plate-like molded body S to obtain a plate-like molded body having a thickness of 30 mm.
[0078] Comparative Example 4 The castable refractory material was soaked in an appropriate amount of water, molded, and dried to obtain a plate-shaped molded product with a diameter of 70 mm and a thickness of 30 mm. The bulk density was 0.760 g / cm. 3 It was.
[0079] (Measurement of bulk density) For the plate-shaped bodies of Examples 1 to 3, the plate-shaped bodies were punched out into squares with sides of 50 mm, and cut into three equal parts in the thickness direction. Next, the weight and thickness of each of the plate-shaped bodies cut into three parts were measured. The thickness was measured with a vernier caliper. Then, the bulk density of the first main surface portion, the bulk density of the second main surface portion, and the bulk density of the central portion were each calculated from the surface specific gravity (weight / area) calculated from the weight and the thickness, as shown in the formula below. (weight / area) / thickness = bulk density [g / cm 3 ]
[0080] The bulk density of the plate-like molded bodies of Comparative Examples 1 and 2 and the castable molded body of Comparative Example 4 was calculated from the above formula by measuring the weight and thickness without cutting.
[0081] For the plate-like molded products S and T of Comparative Example 3, the weight and thickness were measured, and the bulk density was calculated from the above formula.
[0082] (Insulation rating) The heat insulating properties of the plate-like molded articles of Examples 1 to 3 and Comparative Examples 1 to 3, and the castable molded article of Comparative Example 4 were evaluated by the following method. A heating plate (Inconel: registered trademark) with a heater embedded therein to reproduce the temperature state in the combustion chamber and a stainless steel plate were prepared, and the plate-shaped molded body or castable molded body was sandwiched and fixed between these two plates. The plate-shaped molded bodies of Examples 1 to 3 and Comparative Example 3 were arranged so that the main surface of the upper layer side or the side with low bulk density was in contact with the stainless steel plate. In Comparative Example 5, the plate-shaped molded body of Example 1 was arranged so that the main surface of the side with high bulk density was in contact with the stainless steel plate. The heating plate was heated to 1000°C and maintained for 10 minutes. Thereafter, the temperature of the stainless steel plate on the surface in contact with the plate-shaped molded body or castable molded body was measured. The results are shown in Table 1.
[0083] (Bending strength evaluation) The bending strength of the plate-like molded product in the present invention was measured by preparing a sample of the plate-like molded product having a width of 40 mm, a length of 200 mm, and a thickness of 30 mm, using a universal material testing machine (model number: 5567, manufactured by Instron). The measurement method was in accordance with JIS R2619 (test method for bending strength of insulating firebricks), and the maximum load was determined with the above-mentioned sample dimensions, a pressure speed of 10 mm / min, and a distance between supporting rolls of 150 mm, and the bending strength was calculated. A bending strength of 0.28 MPa or more was evaluated as ◯, and a bending strength of less than 0.28 MPa was evaluated as △. The results are shown in Table 1.
[0084] [Table 1]
[0085] As shown in Table 1, the heat insulating materials of Examples 1 to 3, in which the upper layer (metal surface side) of the plate-shaped molded body is smaller in bulk density than the middle layer, were superior in thermal insulation properties compared to the heat insulating materials of Comparative Examples 1 and 2 using plate-shaped molded bodies with uniform bulk density and Comparative Example 4 using a castable molded body. In Comparative Example 3, the bulk density of the plate-shaped molded body on the metal surface side was small, and the thermal insulation properties were equivalent to those of Examples 1 to 3, but since multiple plate-shaped molded bodies were stacked, the bending strength was lower than that of the heat insulating materials of Examples 1 to 3, which are integrated plate-shaped molded bodies, and the risk of breakage of the low density part during handling was high. In Comparative Example 2, the bulk density was too small, so the bending strength was insufficient, and the risk of breakage during handling was high. In Comparative Example 5, the same plate-shaped molded body as in Example 1 was used, but the bulk density on the metal surface side was high, so the thermal insulation properties were inferior to those of Example 1. [Explanation of symbols]
[0086] 1, 1A, 1B Combustion chamber insulation material 10, 10A, 10B Plate-shaped molded body 10a, 10Aa, 10Ba: First main surface of plate-shaped molded body 10b, 10Ab, 10Bb: second main surface of plate-shaped molded body 10c Side of plate-shaped molded body 11 First main surface portion 12 Second main surface portion 13 Central part 50 Original Sheet 50a: first main surface of original sheet 50b second main surface of original sheet HP SUS board 150, 160 metal container 150a, 160a Top surface of metal container 150b, 160b Bottom surface of metal container 170 Heat exchanger 180 Water pipe 540, 550 combustion chamber 500 Water Heater 600 Boiler
Claims
1. A plate-like molded body containing inorganic fibers, When comparing the bulk densities of the first main surface portion, the second main surface portion, and the central portion between the first main surface portion and the second main surface portion in the thickness direction, the bulk density of at least the first main surface portion is smaller than the bulk density of the central portion; 13. A combustion chamber insulating material, comprising: a first main surface portion disposed facing an inner wall surface of the combustion chamber.
2. 2. The combustion chamber insulating material according to claim 1, wherein the bulk density of the second main surface portion is (i) greater than the bulk density of the central portion, or (ii) less than the bulk density of the central portion.
3. 2. The combustion chamber insulating material according to claim 1, which is formed by a papermaking method.
4. 2. The combustion chamber insulating material according to claim 1, which has a flat or curved shape.
5. The overall bulk density is 0.20 to 0.35 g / cm 3 The heat insulating material for a combustion chamber according to claim 1,
6. 2. The combustion chamber insulating material according to claim 1, wherein the bulk density of the first main surface portion is 3% or more smaller than the larger of the bulk density of the second main surface portion and the bulk density of the central portion.
7. A combustion chamber; A heat exchanger installed in the combustion chamber; The combustion chamber insulating material according to any one of claims 1 to 6, A water heater characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing an inner wall surface of the combustion chamber.
8. A combustion chamber; The combustion chamber insulating material according to any one of claims 1 to 6, A boiler characterized in that a first main surface portion of the combustion chamber insulation material is arranged facing the inner wall surface of the combustion chamber.
Citation Information
Patent Citations
JP1974046594A
Combustion device
JP4640705B2