Molding, and method for manufacturing the same

A laminated antistatic layer of glycerin-based fatty acid esters on poly(3-hydroxybutyrate) resin addresses immediate antistatic inadequacies, enhancing production efficiency and quality by preventing contamination and maintaining mechanical properties.

JP2024145935APending Publication Date: 2024-10-15KANEKA CORP

Patent Information

Application Number
JP2023058551
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Molded articles made from poly(3-hydroxybutyrate)-based resins exhibit insufficient antistatic properties immediately after molding, leading to issues like dust and dirt attraction, which can contaminate food contact products such as straws and cutlery, and the antistatic agents used can soften the molded products over time.

Method used

A laminated structure is created by applying a specific antistatic layer composed of glycerin-based fatty acid esters with saturated fatty acid residues onto a poly(3-hydroxybutyrate) resin component, ensuring a weight per unit area of 5.0 μg/cm² to 100 μg/cm², and a manufacturing process involving melt extrusion, water contact, and controlled drying.

Benefits of technology

The laminated structure provides excellent antistatic properties immediately after molding, improving production efficiency and quality by preventing foreign matter adhesion and maintaining mechanical integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145935000001
    Figure 2024145935000001
Patent Text Reader

Abstract

To provide a molding where an anti-static layer is laminated on the surface of a base material layer containing a poly(3-hydroxybutyrate)-based resin component which has excellent anti-static properties immediately after molding, and a method for manufacturing the same.SOLUTION: There is provided a molding where a base material layer containing a poly(3-hydroxybutyrate)-based resin component (A), and an anti-static layer containing an anti-static agent component (B) selected from the group consisting of a monoglycerol fatty acid ester, a diglycerol fatty acid ester and a polyglycerol fatty acid ester are laminated.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article in which an antistatic agent layer is laminated on the surface of a base layer containing a poly(3-hydroxybutyrate) resin component, and a method for producing the same. [Background technology]

[0002] In recent years, environmental issues caused by waste plastics have been attracting attention. In particular, marine pollution caused by waste plastics is serious, and there are hopes for the widespread use of biodegradable resins that decompose in the natural environment.

[0003] Various types of such biodegradable resins are known, but among them, poly(3-hydroxybutyrate) resins, in particular a copolymer of 3-hydroxybutyrate (hereinafter sometimes referred to as "3HB") and 3-hydroxyhexanoate (hereinafter sometimes referred to as "3HH") (hereinafter sometimes referred to as "PHBH"), are thermoplastic polyesters that are produced and accumulated as energy storage substances within the cells of many microbial species, and are a material that can biodegrade not only in soil but also in seawater, and therefore have attracted attention as a material that can solve the above problems.

[0004] Since PHBH is a material in which the copolymerization ratio of 3-hydroxybutyrate and 3-hydroxyhexanoate and the weight-average molecular weight can be controlled relatively easily, its tensile properties, bending properties, etc. can be easily adjusted to suit the intended application and shape. Taking advantage of this feature, it has been deployed in many food contact applications in recent years, such as films and straws.

[0005] On the other hand, PHBH is easily charged with static electricity, and charging during the transport process of the molded body and the secondary processing process of the molded body often becomes a problem. Excessive charging can attract dust, dirt, metal shavings, etc. during the process, increasing the risk of foreign matter being mixed into films, straws, etc. Patent Document 1 discloses a resin composition that is difficult to charge, in which a specific aliphatic polyester resin antistatic agent is kneaded into poly(3-hydroxybutyrate) resin or polybutylene succinate resin to reduce the surface resistivity, and a technology for using the composition. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2021-50286 A Summary of the Invention [Problem to be solved by the invention]

[0007] The molded body containing the resin composition of Patent Document 1 is considered to exhibit antistatic properties due to bleeding out of the antistatic agent onto the surface of the molded body, and the antistatic properties may not be fully exhibited for several days immediately after molding, leaving room for improvement. From the viewpoint of suppressing adhesion of foreign matter to the molded body in the manufacturing process of food contact products such as straws and cutlery and the like, as well as in the product packaging process, it has been required that the molded body has sufficient antistatic properties immediately after molding. In addition, since the kneaded antistatic agent has a plasticizing effect on the resin constituting the molded body, there have been frequent problems in that the molded body is unexpectedly softened or mechanical properties change due to bleeding out over time.

[0008] In view of the above-mentioned current situation, the present invention aims to provide a molded article having an antistatic layer laminated on the surface of a base layer containing a poly(3-hydroxybutyrate)-based resin component, which has excellent antistatic properties even immediately after molding, and a method for producing the same. [Means for solving the problem]

[0009] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a molded article in which an antistatic layer containing a specific amount of an antistatic agent component made of a glycerin-based fatty acid ester having a specific saturated fatty acid residue is laminated to a poly(3-hydroxybutyrate)-based resin component (A), and have thus completed the present invention.

[0010] That is, the present invention provides a molded article comprising a substrate layer containing a poly(3-hydroxybutyrate)-based resin component (A) and an antistatic layer containing an antistatic agent component (B) laminated on the substrate layer, The present invention relates to a molded body, wherein the antistatic agent component (B) is a fatty acid ester selected from the group consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one selected from fatty acid esters having saturated fatty acid residues with 6, 8, 10, or 12 carbon atoms, and the antistatic agent component (B) is contained in the antistatic layer so that the weight per unit area on the surface of the base layer is 5.0 μg / cm2 or more and less than 100 μg / cm2.

[0011] The present invention also relates to a molded article which is a resin tube.

[0012] The present invention also provides a method for producing a poly(3-hydroxybutyrate)-based resin component (A), comprising: a first step of feeding a mixture containing a poly(3-hydroxybutyrate)-based resin component (A) into an extruder equipped with a die at the tip thereof, and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; A second step of contacting the mixture discharged from the die outlet with water at 30° C. or higher and lower than 90° C. to form a base layer; a third step of applying an aqueous dispersion (C) containing the antistatic agent component (B) to a surface of the base layer to form an antistatic agent layer; and a fourth step of drying the antistatic layer in an atmosphere at 40° C. or higher and lower than 100° C. Effect of the Invention

[0013] According to the present invention, it is possible to provide a molded article that includes a base layer containing a poly(3-hydroxybutyrate)-based resin component and an antistatic layer on the surface of the base layer, and has excellent antistatic properties even immediately after molding, and a method for producing the same. The laminate of the present invention makes it possible to improve the production efficiency and quality of the molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.

[0015] [Poly(3-hydroxybutyrate) resin component] The substrate layer in the molded article according to this embodiment contains a poly(3-hydroxybutyrate)-based resin component (A) described below, but may contain other additives within the scope of not impairing the effects of the present invention.

[0016] [Poly(3-hydroxybutyrate) resin component (A)] The poly(3-hydroxybutyrate) resin (hereinafter sometimes referred to as P3HB) according to this embodiment is a polymer having a 3-hydroxybutyrate unit.

[0017] The poly(3-hydroxybutyrate)-based resin is preferably a poly(3-hydroxybutyrate)-based resin produced from a microorganism, in which all 3-hydroxybutyrate units are contained as (R)-3-hydroxybutyrate units.

[0018] The poly(3-hydroxybutyrate) resin preferably contains 3-hydroxybutyrate units (particularly units represented by general formula (1)) in an amount of 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more of the total structural units. The poly(3-hydroxybutyrate) resin may contain only 3-hydroxybutyrate units as structural units of the polymer, or may contain 3-hydroxybutyrate units and one or more types of 3-hydroxyalkanoate units other than the 3-hydroxybutyrate units or other units (e.g., 4-hydroxyalkanoate units, etc.).

[0019] In the poly(3-hydroxybutyrate) resin component (A) according to this embodiment, all of the 3-hydroxybutyrate units are preferably (R)-3-hydroxybutyrate units. The poly(3-hydroxybutyrate)-based resin is preferably a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units.

[0020] Specific examples of poly(3-hydroxybutyrate)-based resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH), Examples of such poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), and the like.In particular, from the viewpoint of achieving both processability into molded articles and physical properties of the obtained molded articles, poly(3-hydroxybutyrate) (PHB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHB3HV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (PHB3HV3HH), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (PHB4HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) (PHB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (PHB3H Poly(3-hydroxybutyrate-co-3-hydroxydecanoate) (PHB3HD) can be preferably used, and in particular, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate) are preferred, with PHB3HH being the most preferred due to its ease of industrial production.

[0021] The poly(3-hydroxybutyrate)-based resin component (A) may contain one or more biodegradable resins other than P3HB, such as aliphatic polyester-based resins such as polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate, as long as the effects of the present invention are not impaired.

[0022] The poly(3-hydroxybutyrate)-based resin component (A) may contain one or more of other additives that are usually added to resin materials, such as inorganic fillers, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, sliding property improvers, and other secondary additives, within the scope of not impairing the effects of the present invention. However, these are optional components, and the poly(3-hydroxybutyrate)-based resin component (A) may not contain these components, as well as the poly(3-hydroxybutyrate)-based resin component (A). As optional components, lubricants and inorganic fillers are preferably used from the viewpoint of further improving the molding stability of the poly(3-hydroxybutyrate)-based resin component (A).

[0023] Examples of the lubricant include saturated or unsaturated fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, oleic acid amide, and erucic acid amide; alkylene fatty acid amides such as methylene bisstearic acid amide and methylene bisstearic acid amide; and aliphatic amide compounds, such as pentaerythritol.

[0024] The amount of the lubricant in the poly(3-hydroxybutyrate)-based resin component (A) is preferably 0.1 to 2 parts by weight, more preferably 0.2 to 1 part by weight, based on 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A). By making the amount 0.1 part by weight or more, it is possible to obtain an effect of improving the releasability by adding the lubricant. On the other hand, if the amount exceeds 2 parts by weight, the lubricant bleeds out during compression and adheres to the compression surface of the cooling roll, etc., which makes it difficult to perform continuous processing for a long time.

[0025] Examples of the inorganic filler include talc, calcium carbonate, mica, silica, clay, kaolin, titanium oxide, alumina, and zeolite, each having an average particle size of 0.5 μm or more.

[0026] The amount of inorganic filler in the poly(3-hydroxybutyrate)-based resin component (A) is preferably 0.5 to 5 parts by weight, more preferably 1 to 3 parts by weight, based on 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A). By making the amount 0.5 parts by weight or more, it is possible to obtain an effect of improving the peelability due to the incorporation of the inorganic filler. On the other hand, if the amount exceeds 5 parts by weight, cracks may easily occur in the poly(3-hydroxybutyrate)-based resin component (A) layer.

[0027] Among poly(3-hydroxybutyrate) resins, PHBH in particular is an especially useful plastic industrially because its melting point and crystallinity can be altered by changing the composition ratio of the repeating units, and as a result, its physical properties such as Young's modulus and heat resistance can be easily adjusted, and it is also possible to impart physical properties between those of polypropylene and polyethylene.

[0028] A specific method for producing PHBH is described in, for example, International Publication No. 2010 / 013483. Commercially available PHBH products include Kaneka Biodegradable Polymer Green Planet (registered trademark) manufactured by Kaneka Corporation.

[0029] The ratio of 3-hydroxyhexanoate (3HH) in the PHBH is not particularly limited, but the ratio of 3HH is preferably 2 mol% or more and less than 25 mol%, and more preferably 3 mol% or more and 15 mol% or less. When the ratio of 3HH in the PHBH contained in the poly(3-hydroxybutyrate)-based resin component (A) is 2 mol% or more, the melting point does not become too high and the difference between the decomposition temperature and the processing temperature can be set large, so that stable extrusion processing is possible. In addition, PHBH having a ratio of 3HH of less than 25 mol% does not have a too slow crystallization rate, and it is relatively easy to manufacture a pellet-shaped compound containing PHBH. The ratio of 3HH is the monomer ratio of 3HH to all monomers constituting PHBH, and can be determined by a method known to those skilled in the art, for example, the method described in paragraph

[0047] of International Publication WO 2013 / 147139 or by NMR measurement. In addition, when multiple PHBHs are contained, it is the ratio to the total amount of constituent monomers contained in all components of PHBH.

[0030] The weight average molecular weight (hereinafter sometimes referred to as Mw) of the entire poly(3-hydroxybutyrate)-based resin component (A) according to this embodiment is preferably 100,000 or more and less than 750,000, more preferably 200,000 or more and less than 650,000, and even more preferably 250,000 or more and less than 550,000, from the viewpoint of achieving both an appropriate crystallization rate and mechanical strength. If the weight average molecular weight is less than 100,000, there is a possibility that the amount of elution during heating will increase, and not only may the container be unusable as a food container, but the contribution of decomposition products during extrusion processing may become large, and extrusion processability may become unstable. If the weight average molecular weight exceeds 750,000, the melt viscosity will increase, and there is a possibility that problems will occur in appearance, such as the surface of the extruded molded product becoming rough. In this application, the weight average molecular weight of PHBH can be determined as the molecular weight converted into polystyrene by gel permeation chromatography (GPC) (Shodex GPC-101 manufactured by Showa Denko K.K.) using polystyrene gel (Shodex K-804 manufactured by Showa Denko K.K.) as a column and chloroform as a mobile phase.

[0031] In this embodiment, a mixture of multiple types of PHBH having different weight average molecular weights can be used for the poly(3-hydroxybutyrate) resin component (A).

[0032] In addition, when a mixture of multiple types of PHBH is used, or when other resin components are mixed, the weight average molecular weight of the poly(3-hydroxybutyrate)-based resin component (A) refers to the weight average molecular weight of the entire poly(3-hydroxybutyrate)-based resin component (A).

[0033] [Antistatic layer] The antistatic layer in the molded product according to this embodiment contains the antistatic agent component (B) described below, but may also contain other additives within the range that does not impair the effects of the present invention.

[0034] [Antistatic agent component (B)] The antistatic agent component (B) according to the present embodiment is preferably excellent in solubility or dispersibility in water or an aqueous solvent consisting of water / ethanol, and contains at least one type of material having good wettability with PHBH, and contains at least one type of fatty acid ester having a saturated fatty acid residue with a carbon number of 6, 8, 10, or 12 selected from the group of fatty acid esters consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters. This tends to form a coating film evenly on the surface of PHBH and to exhibit high antistatic properties. The glycerin-based fatty acid esters can be used alone, or two or more types of resins can be mixed in any ratio as necessary.

[0035] In the molded article according to the present embodiment, the weight per unit area of ​​the antistatic agent component (B) on the surface of the base layer made of the poly(3-hydroxybutyrate)-based resin component is 5.0 μg / cm 2 More than 100μg / cm 2 Less than 5.0μg / cm 2 If the concentration is less than 100 μg / cm, the antistatic effect will not be fully demonstrated. 2If the weight is more than this, it may be difficult to dry the aqueous dispersion liquid after it has been applied, and the molded bodies may stick to each other, or the excess antistatic agent component may contaminate the transport process, causing the molded bodies to stick to the device during the transport process. The lower limit of the weight per unit area of ​​the antistatic agent component (B) on the surface of the base layer is 10.0 μg / cm. 2 More than 15.0 μg / cm is preferable. 2 The upper limit is preferably 80 μg / cm 2 Less than 60 μg / cm is preferred 2 The following is more preferred:

[0036] [Aqueous dispersion of antistatic agent component (B)] When the antistatic agent component according to the present invention is used as an aqueous dispersion, the solid content concentration of the antistatic agent component contained in the aqueous dispersion is preferably 0.1 wt% or more and less than 10 wt%. If it is less than 0.1 wt%, the antistatic agent component does not have good wettability on the surface of a molded body mainly composed of a poly(3-hydroxybutyrate) resin, so that a sufficient amount of the antistatic agent component cannot be laminated, and the desired effect may not be sufficiently obtained. If it is 10 wt% or more, the antistatic agent component does not have good dispersibility and forms aggregates, so that, for example, when a spraying method using a spray nozzle is used, not only may the nozzle be clogged, but the antistatic agent component applied in excess may contaminate the process due to contact with the process.

[0037] The liquid constituting the aqueous dispersion may be composed of water alone. The water may be ordinary city water that has not been ion-exchanged, or may be pure water that has been ion-exchanged if the effect on the dispersibility of the antistatic agent component is minor. In addition, alcohol may be mixed for the purpose of improving the dispersibility of the antistatic agent component or the wettability with a molded body mainly composed of a poly(3-hydroxybutyrate)-based resin. In this case, when the molded body to be obtained is used for food contact or when a drying process is required thereafter, it is preferable that the alcohol is ethanol. Here, when ethanol is used as the alcohol component, the volume ratio with water (volume of water / volume of ethanol) is preferably in the range of 100 / 0 to 50 / 50. If the volume of ethanol exceeds 50%, the wettability with a molded body mainly composed of a poly(3-hydroxybutyrate)-based resin becomes too good, which may adversely affect the drying characteristics thereafter.

[0038] The volume ratio of the water / ethanol mixture is more preferably in the range of 95 / 5 to 55 / 45, and particularly preferably in the range of 90 / 10 to 60 / 40. [Method for producing molded body] The molded article according to this embodiment can be produced by a production method including a step of melt-extruding a mixture containing a poly(3-hydroxybutyrate)-based resin component (A) (first step), a step of forming a base layer by cooling the molten mixture (second step), a step of coating the surface of the base layer with an aqueous dispersion containing an antistatic agent component (B) to form an antistatic layer (third step), and a step of drying the antistatic layer (fourth step). (First and second steps) In the manufacturing method of the molded body according to this embodiment, the base layer can be manufactured by melt-kneading the respective components using a general method, for example, by feeding the respective components into an extruder equipped with a die at the tip and melt-kneading a mixture of resins containing the respective components. It is also possible to pelletize the mixture after melt kneading, and then remelt and mold the pellets.

[0039] First, the poly(3-hydroxybutyrate)-based resin component (A) and any additives as necessary are added, and the components are melt-kneaded using an extruder, kneader, Banbury mixer, roll, or the like to prepare a mixture of the components. The molten mixture is then cooled and solidified to form the base layer.

[0040] The mixture may be extruded into a strand shape and then cut to obtain pellets having a particle shape such as a cylinder, an elliptical cylinder, a sphere, a cube, a rectangular parallelepiped, etc. The produced pellets are desirably sufficiently dried at 40 to 80° C. to remove moisture, and then subjected to the next molding step.

[0041] The temperature at which the melt kneading is carried out cannot be generally defined because it depends on the melting point, melt viscosity, etc. of the resin used, but the temperature of the resin mixture at the die outlet of the melt kneaded product is preferably 150° C. or more and less than 175° C., more preferably 155° C. or more and less than 170° C., even more preferably 158° C. or more and less than 167° C., and particularly preferably 160° C. or more and less than 165° C. If the resin temperature of the melt kneaded product is less than 150° C., the poly(3-hydroxybutyrate)-based resin component (A) may not be melted, and if it exceeds 175° C., the poly(3-hydroxybutyrate)-based resin component (A) may be thermally decomposed.

[0042] In order to promote solidification, the molten mixture discharged from the die outlet is preferably cooled in a water tank at 30° C. or higher and lower than 90° C. for 5 seconds or longer and shorter than 20 seconds.

[0043] That is, in the method for producing a molded article according to the embodiment, a mixture containing a poly(3-hydroxybutyrate)-based resin component (A) is fed into an extruder equipped with a die at the tip thereof, and the mixture is melt-extruded so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C. (first step); and a step (second step) of contacting the mixture discharged from the die outlet with water at a temperature of 30° C. or higher and lower than 90° C. to form a base layer.

[0044] (Steps 3 and 4) In the manufacturing method of the molded body according to the present embodiment, the method of laminating the antistatic layer on the base layer is not particularly limited, but from the viewpoint of obtaining sufficient antistatic effect by laminating uniformly and evenly, it is preferable to carry out by applying an aqueous dispersion. The method of applying the aqueous dispersion may be any method that coats the entire surface of the obtained molded body, for example, a method of passing the molded body through a water tank containing the aqueous dispersion, or a method of applying droplets using a liquid delivery pump, but from the viewpoint of easy adjustment of the amount of application and easy integration into a production line, a spraying method using a spray nozzle can be preferably used. The coated aqueous dispersion of the antistatic agent component does not require any particular post-treatment unless there are problems such as sticking between the coated molded bodies or between the molded body and the transport process, but if necessary, a method such as passing through a drying oven can be used. In this case, a good drying state can be obtained if the temperature of the drying oven is 40° C. or higher and lower than 100° C.

[0045] That is, in the method for producing a molded body according to the embodiment, it is preferable to sequentially include, following the first step and the second step, a step (third step) of applying an aqueous dispersion (C) containing the antistatic agent component (B) to the surface of the base layer to form an antistatic agent layer, and a step (fourth step) of drying the antistatic layer in an atmosphere of 40°C or higher and lower than 100°C.

[0046] The amount of the antistatic layer applied is not particularly limited. However, from the viewpoint of adjusting the amount of the antistatic agent present on the surface of the base layer within an appropriate range and enabling efficient production, it is preferable that the weight per unit area on the surface of the base layer is, for example, 10 μg / cm 2 More than 200μg / cm 2 It is preferred that the thickness is less than 1 mm.

[0047] [Resin tube] The thickness of the resin tube according to the present embodiment is preferably 0.01 mm to 0.6 mm, more preferably 0.05 mm to 0.5 mm, and even more preferably 0.1 mm to 0.4 mm, because it is not crushed by suction when drinking a beverage as a straw, has moderate flexibility, is unlikely to break, is unlikely to cause injury when poking a fingertip, and is rapidly biodegradable even in seawater. The outer diameter of the resin tube is not particularly limited, but is preferably 2 to 10 mm, more preferably 4 to 8 mm, and even more preferably 5 to 7 mm, from the viewpoint of ease of use when drinking a beverage as a straw. The cross-sectional shape of the biodegradable resin tube is approximately circular, but from the viewpoint of usability as a straw or pipe, the closer to a perfect circle the more preferable. Therefore, the flatness of the cross-sectional shape of the resin tube [100 x (maximum outer diameter - minimum outer diameter) / maximum outer diameter] is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, and even more preferably 3% or less. A flatness of 0% means that the cross-sectional shape is a perfect circle. The length of the resin tube is not particularly limited, but when the resin tube is used as a straw, the length of the resin tube is preferably 50 to 350 mm, more preferably 70 to 300 mm, and even more preferably 90 to 270 mm, from the viewpoint of ease of use when using the tube as a straw to drink a beverage. When the resin tube is used as a straw, it may be a tube that has not been subjected to secondary processing, or a tube that has been subjected to secondary processing such as the formation of a stopper portion or a bellows portion.

[0048] The resin tube according to this embodiment can be manufactured by a known method. For example, it can be manufactured by melting a blend of the resin composition according to this embodiment and any additives in an extruder, extruding it from an annular die connected to the outlet of the extruder, and pouring it into water to solidify it into a tubular shape.

[0049] In the resin tube according to the present embodiment, the antistatic layer on the base material layer may be formed on either the inner or outer surface of the tube, or on both surfaces, but from the viewpoint of achieving a higher dustproofing effect and thereby reducing the rate of contamination by foreign matter, it is preferable to form it on both surfaces. In this case, the thicknesses of the antistatic layers formed on the outer and inner surfaces may be the same or may be different as necessary.

[0050] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A substrate layer containing a poly(3-hydroxybutyrate)-based resin component (A); A molded article having an antistatic layer containing an antistatic agent component (B) laminated on its surface, The antistatic agent component (B) is a fatty acid ester selected from the group consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with 6, 8, 10, or 12 carbon atoms; The antistatic agent component (B) has a weight per unit area on the surface of the substrate layer of 5.0 μg / cm 2 More than 100μg / cm 2 The antistatic layer is formed so that the surface area of ​​the molded article is less than 100 nm. [Item 2] 2. The molded article according to item 1, wherein the poly(3-hydroxybutyrate)-based resin component (A) comprises a poly(3-hydroxybutyrate)-based copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units. [Item 3] The molded article according to any one of items 1 to 3, wherein the poly(3-hydroxybutyrate)-based copolymer is at least one selected from the group consisting of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate). [Item 4] 5. The molded article according to any one of items 1 to 4, which is a resin tube. [Item 5] 5. The resin tube according to item 4, wherein the antistatic layer is laminated on one of the inner and outer surfaces of the base material layer. [Item 6] 5. The resin tube according to item 4, wherein the antistatic agent layer is laminated on both the inner and outer surfaces of the base material layer. [Item 7] A step (first step) of feeding a mixture containing a poly(3-hydroxybutyrate)-based resin component (A) into an extruder equipped with a die at the tip thereof and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; A step (second step) of contacting the mixture discharged from the die outlet with water at 30° C. or higher and lower than 90° C. to form a base layer; a step (third step) of applying an aqueous dispersion (C) containing the antistatic agent component (B) onto the surface of the base layer to form an antistatic agent layer; and (fourth step) drying the antistatic layer in an atmosphere at 40° C. or higher and lower than 100° C. [Item 8] 8. The method for producing a molded body according to Item 7, wherein the solid content concentration of the antistatic agent component (B) in the aqueous dispersion (C) is 0.1 wt % or more and less than 10 wt %. [Item 9] Item 9. The method for producing a molded body according to item 7 or 8, wherein the aqueous dispersion contains water and ethanol, and a volume ratio of water to ethanol (volume of water / volume of ethanol) is 100 / 0 to 50 / 50. EXAMPLES

[0051] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited to these examples.

[0052] [Raw materials used] The following raw materials were used in each of the Examples and Comparative Examples. (Poly(3-hydroxybutyrate)-based resin component (A)) The PHBH powder used in the poly(3-hydroxybutyrate) resin component (A) used in the examples and comparative examples was produced in accordance with the method described in International Publication WO2019-142845. The specific formulation is shown below.

[0053] PHBH powder: PHBH powder with a weight-average molecular weight of 500,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 9 mol%. (Antistatic agent) Poem DL-100 (diglycerin monolaurate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 12 carbon atoms as the main component Poem M-100 (glycerin monocaprylate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 8 carbon atoms as the main component Poem M-300 (glycerin monolaurate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 12 carbon atoms as the main component Rikemal S-100 (glycerin monostearate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 18 carbon atoms as the main component Rikemal L-250A (sorbitan laurate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 12 carbon atoms as the main component Example 1 [Preparation of aqueous dispersion of antistatic component (B)] Poem DL-100 was used as the antistatic agent component (B), and ion-exchanged water was added so that the solid concentration of Poem DL-100 became 1.0%, and the mixture was stirred for 30 minutes with a tabletop ultrasonic cleaner (manufactured by Velvoclear Co., Ltd., product number: VS100III) to obtain an aqueous dispersion.

[0054] [Preparation of strands of resin composition] PHBH powder (100 parts by weight) was dry-blended with behenic acid amide (0.5 parts by weight) as a crystal nucleating agent and lubricant, and the mixture was melt-kneaded and extruded into strands using a twin-screw extruder so that the die outlet resin temperature immediately after leaving the extruder was 168°C, and the mixture was passed through water at 40°C (solidification temperature 1) to solidify and cut to obtain pellets. Note that the time spent in the warm water was adjusted to 15 seconds.

[0055] [Making resin tubes] The cylinder temperature and die temperature of a φ50 mm single-screw extruder connected to a circular die (outer diameter 15 mm, inner diameter 13.5 mm) were set to 160°C, and the pellets of the resin composition obtained by the above method were added and extruded into a tube. The extruded tube was passed through water at 50°C (solidification temperature 2) located 100 mm away from the circular die, and taken up at a speed of 60 m / min with a take-up machine. Subsequently, a spray nozzle was installed at a position 10 cm away from the resin tube being transported, and the aqueous dispersion prepared by the above method was sprayed and applied, and the tube was passed through a small box-type drying oven heated to 60°C (drying temperature), and then cut out with a tube cutter to obtain a resin tube with an outer diameter of 6 mm, a wall thickness of 0.2 mm, and a length of 200 mm. For the resin tubes produced by the above method, the weight per unit area of ​​the antistatic agent component (B) on the surface of the base layer, the adhesion between the tubes immediately after molding, and the antistatic properties were evaluated using the evaluation methods described below, and the results are shown in Table 1.

[0056] (Weight of antistatic agent component (B) per unit area on substrate layer surface) The weight (coating weight) of the antistatic agent component per unit area on the surface of the base layer was measured by gas chromatography. Specifically, the obtained resin tube was cut into a length of 2 cm and immersed in 10 ml of ethanol to dissolve the antistatic agent component coated on the surface to prepare an extract, and 0.1 μl of the extract was used for separation using a gas column chromatography device (Agilent 7890B-GC system manufactured by Agilent Technology Co., Ltd.), and the weight of the antistatic agent component per unit area was calculated from the obtained spectrum intensity. (Adhesion between resin tubes) Immediately after molding, ten resin tubes were randomly selected and visually observed to see if any of the resin tubes were stuck together. This procedure was repeated ten times, and the degree of sticking between the resin tubes was evaluated according to the following criteria, based on the number of times that sticking was observed.

[0057] <Evaluation criteria> ◎: No stuck tube was found even once out of 10 times 〇: The tube was found stuck on the skin once out of 10 times. △: The tube was found stuck to the skin 2 times out of 10 times. ×: Tubes were found stuck to the skin 3 or more times out of 10 times. If the above evaluation result is ⊚, ○, or △, it can be determined that the sticking of the tubes to each other does not pose a significant problem. (Antistatic) After preparation of the resin tube, it was cured for 1 hour in a constant temperature and humidity environment of 23°C and 50% humidity. Immediately after curing, The tubes were cut to a length of 200 mm and laid out without gaps in a SUS304 container with a length of 300 mm and a width of 200 mm. A smaller container made of the same material as the container was placed on top of the tubes, and the tubes were rubbed together in the longitudinal direction for 30 seconds to generate static electricity on the surface, charging the tubes. The amount of charge on the surface of the tubes was measured using a digital static electricity detector (model number: EG-1) manufactured by Sanhayato Co., Ltd.

[0058] <Evaluation criteria> ◎: Less than 0.1 kV ○: 0.1 kV or more and less than 0.5 kV △: 0.6kV or more and less than 2.0kV ×: 2.0kV or more If the above evaluation result is ⊚, ◯, or Δ, it indicates that the antistatic property is rapid and sufficient.

[0059] [Table 1]

[0060] (Examples 2 to 8, Comparative Examples 1 to 4) Strands and resin tubes were prepared in the same manner as in Example 1, except that the antistatic agent component (B), the solids concentration of the aqueous dispersion of the antistatic agent component (B), the drying temperature of the tube, or the weight per unit area of ​​the antistatic agent component on the surface of the base layer was changed as shown in Table 1, and evaluations were performed in the same manner as in Example 1. The results are summarized in Table 1.

[0061] <Result> From Table 1, it can be seen that in the examples, the sticking of tubes to each other was not a problem, and the antistatic effect was sufficiently exhibited even 30 minutes after molding.

[0062] On the other hand, in the comparative examples, sticking of the tubes to each other frequently occurs, and sufficient antistatic effect is not obtained immediately after molding. Therefore, the present invention can provide a biodegradable laminate having sufficient antistatic properties even immediately after molding, and a method for producing the same, in a molded product obtained by laminating a specific amount of an antistatic agent component made of a glycerin-based fatty acid ester having a specific saturated fatty acid residue on a poly(3-hydroxybutyrate)-based resin component (A).

Claims

1. A substrate layer containing a poly(3-hydroxybutyrate)-based resin component (A); A molded article having an antistatic layer containing an antistatic agent component (B) laminated on its surface, The antistatic agent component (B) is a fatty acid ester selected from the group consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue having 6, 8, 10, or 12 carbon atoms; The antistatic agent component (B) has a weight per unit area on the surface of the substrate layer of 5.0 μg / cm 2 100 μg / cm or more 2 The antistatic layer is formed so that the surface area of ​​the molded article is less than 100 nm.

2. The molded article according to claim 1, wherein the poly(3-hydroxybutyrate)-based resin component (A) contains a poly(3-hydroxybutyrate)-based copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units.

3. The molded article according to claim 1 or 2, wherein the poly(3-hydroxybutyrate)-based copolymer is at least one selected from the group consisting of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate).

4. The molded article according to claim 1 or 2, which is a resin tube.

5. The resin tube according to claim 4 , wherein the antistatic layer is laminated on one of an inner surface and an outer surface of the base material layer.

6. The resin tube according to claim 4 , wherein the antistatic agent layer is laminated on both the inner and outer surfaces of the base material layer.

7. A first step of feeding a mixture containing a poly(3-hydroxybutyrate)-based resin component (A) into an extruder equipped with a die at its tip and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; A second step of contacting the mixture discharged from the die outlet with water at 30° C. or higher and lower than 90° C. to form a base layer; a third step of applying an aqueous dispersion (C) containing the antistatic agent component (B) onto a surface of the base layer to form an antistatic agent layer; A fourth step of drying the antistatic layer in an atmosphere at a temperature of 40° C. or higher and lower than 100° C.

8. The method for producing a molded body according to claim 7 , wherein a solid content concentration of the antistatic agent component (B) in the aqueous dispersion (C) is 0.1 wt % or more and less than 10 wt %.

9. The method for producing a molded body according to claim 7, wherein the aqueous dispersion contains water and ethanol, and a volume ratio of water to ethanol (volume of water / volume of ethanol) is 100 / 0 to 50 / 50.

Citation Information

Patent Citations

  • Resin composition and use thereof

    JP2021050286A

Cited By

  • Method for producing resin pellet, resin pellet, and method for producing molded body

    WO2025206006A1