Power storage module and manufacturing method thereof

By strategically placing power storage devices with varying peak intensity ratios in the power storage module based on temperature zones, the module achieves improved high-rate resistance, energy density, and fuel efficiency, addressing the limitations of uniform confining pressures in conventional designs.

JP2024146106AActive Publication Date: 2024-10-15PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023058823
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional power storage modules face challenges in equalizing high-rate resistance among power storage devices due to uniform confining pressures, leading to reduced volumetric energy density and potential fuel efficiency issues, especially when mounted on vehicles.

Method used

The power storage module is designed with a configuration that adjusts the placement of power storage devices based on their peak intensity ratios of negative electrode active material layers, positioning devices with lower peak intensity ratios in low-temperature regions and those with higher ratios in high-temperature regions, using X-ray crystal structure analysis to optimize high-rate resistance.

Benefits of technology

This approach enhances the high-rate resistance of the entire module, reduces the need for restraining members, improves volumetric energy density, and increases fuel efficiency by flexibly adjusting high-rate tolerance according to temperature distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146106000001_ABST
    Figure 2024146106000001_ABST
Patent Text Reader

Abstract

To provide a power storage module with a novel configuration that can equalize the high-rate resistance of multiple power storage devices.SOLUTION: A power storage module 500 disclosed herein includes a plurality of power storage devices 100. The power storage module 500 includes a low temperature region A1 where the temperature is relatively low and a high temperature region A2 where the temperature is relatively high during charging and discharging of the plurality of power storage devices 100, and among the plurality of power storage devices 100, a first power storage device 110 arranged in the low temperature region A1 has a lower peak intensity ratio (I004 / I110) of a negative electrode active material layer than a second power storage device 120 arranged in the high temperature region A2.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electricity storage module including a plurality of electricity storage devices and a manufacturing method thereof. [Background technology]

[0002] Conventionally, power storage modules formed by electrically connecting a plurality of power storage devices (single cells) have been widely used as power sources for driving vehicles, etc. Patent documents 1 to 4 are examples of related art documents.

[0003] For example, Patent Document 1 discloses an electricity storage module having a plurality of submodules and a housing that houses the plurality of submodules at predetermined positions. In Patent Document 1, each of the plurality of submodules includes a cell group in which a plurality of electricity storage devices (single cells) are arranged, and a binding member that applies a binding pressure in the arrangement direction to bind the cell group. The housing includes an area that is relatively prone to low temperatures, and the submodules arranged in the area that is prone to low temperatures are configured so that the binding pressure of the binding member is relatively lower than that of the other submodules. Patent Document 1 describes that the high-rate resistance (increase in resistance when high-rate charging and discharging are repeated) of the plurality of electricity storage devices can be leveled out by lowering the binding pressure on the electricity storage devices in such an area where the high-rate resistance is likely to decrease (area that is prone to low temperatures). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-44212 [Patent Document 2] Patent Publication No. 2022-81868 [Patent Document 3] JP 2012-221816 A [Patent Document 4] JP 2015-90794 A [Patent Document 5] JP 2015-138644 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the technology described in Patent Document 1, the multiple power storage devices included in one cell group cannot have different restraining pressures. Therefore, according to the study by the present inventors, when a temperature distribution occurs in the cell group, it is sometimes difficult to equalize the high-rate resistance of the multiple power storage devices. In addition, since a restraining member is required for each cell group, the restraining member becomes bulky and the volumetric energy density of the entire power storage module decreases, and for example, when the power storage module is mounted on a moving body such as a vehicle, there is a risk that the weight becomes heavy and fuel efficiency deteriorates.

[0006] The present invention has been made in consideration of the above circumstances, and its main object is to provide a novel energy storage module that can equalize the high-rate resistance of multiple energy storage devices, and a manufacturing method thereof. [Means for solving the problem]

[0007] According to the present invention, there is provided an electricity storage module including a plurality of electricity storage devices, each of the plurality of electricity storage devices having a positive electrode and a negative electrode, the negative electrode having a negative electrode active material layer including graphite, the electricity storage module includes a low-temperature region where the temperature is relatively low and a high-temperature region where the temperature is relatively high during charging and discharging of the plurality of electricity storage devices, and when the negative electrode active material layer is measured by X-ray crystal structure analysis, a peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110 ) is a peak intensity ratio, a first power storage device arranged in the low temperature region among the plurality of power storage devices has a lower peak intensity ratio than a second power storage device arranged in the high temperature region, thereby providing a power storage module.

[0008] The present invention also provides a method for producing an electricity storage module including a plurality of electricity storage devices, each of which has a positive electrode and a negative electrode, and the negative electrode including a negative electrode active material layer containing graphite. This method is characterized in that, when the negative electrode active material layer is measured by X-ray crystal structure analysis, a peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110 ) is a peak intensity ratio, the method includes a preparation step of preparing, as the plurality of electricity storage devices, a first electricity storage device having a relatively low peak intensity ratio of the negative electrode active material layer and a second electricity storage device having a relatively high peak intensity ratio; a temperature distribution prediction step of predicting a temperature distribution in the electricity storage module when the plurality of electricity storage devices are charged and discharged; and a construction step of constructing the electricity storage module by arranging the first electricity storage device in a low temperature region where the temperature is relatively low and arranging the second electricity storage device in a high temperature region where the temperature is relatively high based on the temperature distribution.

[0009] As a result of various studies, the inventors of the present invention have found that an electricity storage device having a low peak intensity ratio of the negative electrode active material layer has relatively better high-rate resistance than an electricity storage device having a high peak intensity ratio of the negative electrode active material layer. Therefore, in the present invention, an electricity storage device having a relatively low peak intensity ratio (having excellent high-rate resistance) is arranged in a low temperature region where the high-rate resistance is likely to decrease. This makes it possible to equalize the high-rate resistance of a plurality of electricity storage devices. In addition, the high-rate resistance of the entire electricity storage module can be improved. In addition, unlike the technology of Patent Document 1, there is no need to be bound by the framework of a "cell group," so the high-rate resistance of each electricity storage device can be flexibly adjusted. Furthermore, since the number of binding members can be reduced compared to the technology of Patent Document 1, the volumetric energy density and fuel efficiency can also be improved.

[0010] Although not particularly related to the technology disclosed herein, Patent Document 5 describes a range of the degree of orientation of a negative electrode active material layer suitable for an electricity storage device. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a perspective view illustrating a power storage module according to one embodiment. [Diagram 2] FIG. 2 is a perspective view illustrating the secondary battery of FIG. [Diagram 3] FIG. 3 is a schematic vertical cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a schematic diagram showing the configuration of the electrode body of FIG. [Diagram 5] FIG. 5 is a plan view that typically illustrates the electricity storage module and the cooling device of FIG. [Figure 6] FIG. 6 is a plan view that illustrates a power storage module according to a first modified example. [Figure 7] FIG. 7 is a plan view illustrating a schematic configuration of an electricity storage module according to a second modified example. [Figure 8] FIG. 8 is a plan view illustrating a power storage module according to a third modified example. [Figure 9] FIG. 9 is a plan view illustrating a power storage module according to a fourth modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, preferred embodiments of the technology disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification that are necessary for implementing the present invention (for example, the general configuration and manufacturing process of the energy storage module or energy storage device that does not characterize the present invention) can be understood as design matters of a person skilled in the art based on the prior art in the field. The energy storage module disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field.

[0013] In the following drawings, the same reference numerals are used for components and parts having the same function, and duplicated explanations may be omitted or simplified. In addition, in this specification, the expression "A to B" indicating a range includes the meaning of "A or more and B or less," as well as "preferably larger than A" and "preferably smaller than B."

[0014] [Energy storage module] 1 is a perspective view that typically illustrates an energy storage module 500. Here, the energy storage module 500 includes a plurality of energy storage devices 100, a plurality of spacers 200, and a restraining mechanism 300. However, the plurality of spacers 200 and the restraining mechanism 300 are not essential and may be omitted in other embodiments.

[0015] In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction, the long side direction perpendicular to the short side direction, and the up-down direction, respectively, of the power storage device 100. The short side direction X is also the arrangement direction of the power storage devices 100. However, these directions are merely for the convenience of description, and do not limit the installation form of the power storage module 500 in any way.

[0016] The restraining mechanism 300 is a member that restrains the multiple power storage devices 100. Here, there is one restraining mechanism 300. Here, the restraining mechanism 300 is configured to apply an equal restraining pressure to all the power storage devices 100 and the spacers 200 from the arrangement direction X. The restraining mechanism 300 includes a pair of end plates 310, a pair of side plates 320, and multiple screws 330. The pair of end plates 310 and the pair of side plates 320 can also be understood as a housing that houses the multiple power storage devices 100. The pair of end plates 310 and the pair of side plates 320 are preferably made of metal.

[0017] The pair of end plates 310 are disposed at both ends of the power storage module 500 in the arrangement direction X. The pair of end plates 310 sandwich the plurality of power storage devices 100 and the plurality of spacers 200 in the arrangement direction X. The pair of side plates 320 bridge the pair of end plates 310. The pair of side plates 320 are fixed to the end plates 310 by a plurality of screws 330 so that the restraining load is, for example, about 10 to 15 kN. As a result, a uniform restraining load is applied to the plurality of power storage devices 100 from the arrangement direction X, and the plurality of power storage devices 100 are held integrally. However, the configuration of the restraining mechanism is not limited to this. The restraining mechanism 300 may include, for example, a plurality of restraining bands, bind bars, or the like, instead of the side plates 320.

[0018] Here, the spacers 200 are disposed between the multiple power storage devices 100 in the arrangement direction X. That is, the power storage devices 100 and the spacers 200 are arranged alternately in the arrangement direction X. However, when the power storage module 500 does not include the spacers 200, the power storage devices 100 adjacent to each other in the arrangement direction X may abut (directly contact) with each other. The spacers 200 preferably include a portion having a porous structure through which a fluid (typically a gas such as air) can pass.

[0019] The power storage device 100 is a device capable of repeated charging and discharging. In this specification, the term "power storage device" is a concept that encompasses secondary batteries such as lithium ion secondary batteries and nickel metal hydride batteries, and capacitors such as lithium ion capacitors and electric double layer capacitors. Here, the multiple power storage devices 100 are arranged between a pair of end plates 310 along an arrangement direction X (in other words, a thickness direction X of the power storage device 100). The multiple power storage devices 100 are preferably restrained by a restraining mechanism 300. The shape, size, number, and the like of the multiple power storage devices 100 are not limited to the embodiment disclosed in FIG. 1, and can be changed as appropriate.

[0020] Although not shown here, when the energy storage module 500 is used, the multiple energy storage devices 100 are electrically connected to each other by conductive members such as bus bars. The connection method is not particularly limited, and may be, for example, series, parallel, or multi-series and multi-parallel. In a preferred embodiment, the multiple energy storage devices 100 are connected in series. This makes it possible to suitably improve the output characteristics to a level suitable for use in a moving body such as a vehicle. In addition, in the case of series connection, the performance deterioration of some of the energy storage devices 100 is likely to lead to the performance deterioration of the entire energy storage module 500. For this reason, it is particularly effective to apply the technology disclosed herein.

[0021] Fig. 2 is a perspective view of the electricity storage device 100. As can be seen from Figs. 1 and 2, the electricity storage devices 100 are all flat and rectangular, and have the same shape here. The electricity storage devices 100 are arranged so that their long side walls 12b, which will be described later, are parallel to each other. The electricity storage devices 100 are lined up in the arrangement direction X here so that the long side walls 12b face each other via the spacers 200.

[0022] 3 is a schematic longitudinal sectional view taken along line III-III in FIG. 2. As shown in FIG. 3, the electricity storage device 100 includes a battery case 10, an electrode assembly 20, a positive electrode terminal 30, and a negative electrode terminal 40. Although not shown, the electricity storage device 100 further includes a non-aqueous electrolyte. The electricity storage device 100 is configured by accommodating the electrode assembly 20 and the non-aqueous electrolyte in a battery case 10 to which the positive electrode terminal 30 and the negative electrode terminal 40 are attached. The electricity storage device 100 is typically a non-aqueous electrolyte secondary battery, and is a lithium ion secondary battery here. When the electricity storage device 100 is a non-aqueous electrolyte secondary battery (particularly a lithium ion secondary battery), it is particularly effective to apply the technology disclosed herein.

[0023] The battery case 10 is a container that contains the electrode assembly 20 and the nonaqueous electrolyte. As shown in FIG. 2, the battery case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the battery case 10 may be the same as that used conventionally, and is not particularly limited. The battery case 10 is made of, for example, aluminum, aluminum alloy, iron, iron alloy, or the like. As shown in FIG. 3, the battery case 10 includes an exterior body 12 having an opening 12h, and a sealing plate (lid body) 14 that seals the opening 12h. As shown in FIG. 2, the exterior body 12 includes a substantially rectangular bottom wall 12a having long and short sides, a pair of long side walls 12b that extend from the long side of the bottom wall 12a and face each other, and a pair of short side walls 12c that extend from the short side of the bottom wall 12a and face each other. The long side walls 12b are flat.

[0024] The sealing plate 14 is a plate-like member. The sealing plate 14 has a substantially rectangular shape. As shown in FIG. 3, the sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The battery case 10 is integrated by joining (preferably welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The battery case 10 is hermetically sealed (closed). The sealing plate 14 is provided with a liquid injection hole 15 and two terminal extraction holes 18 and 19. The liquid injection hole 15 is for injecting a nonaqueous electrolyte after the sealing plate 14 is assembled to the exterior body 12. The liquid injection hole 15 is sealed with a sealing member 16. The terminal extraction holes 18 and 19 penetrate the sealing plate 14 in the up-down direction Z.

[0025] The positive electrode terminal 30 is disposed at one end of the sealing plate 14 in the long side direction Y (the left end in FIG. 2 and FIG. 3), and the negative electrode terminal 40 is disposed at the other end of the sealing plate 14 in the long side direction Y (the right end in FIG. 2 and FIG. 3). As shown in FIG. 3, the positive electrode terminal 30 and the negative electrode terminal 40 extend from the inside to the outside of the sealing plate 14 through the terminal pull-out holes 18 and 19, respectively. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal pull-out holes 18 and 19 of the sealing plate 14 by crimping. The crimped portions 30c and 40c are formed at the ends of the positive electrode terminal 30 and the negative electrode terminal 40 on the side of the exterior body 12 (the lower end in FIG. 3). As a result, the positive electrode terminal 30 and the negative electrode terminal 40 are fixed to the sealing plate 14.

[0026] As shown in Fig. 3, the positive electrode terminal 30 is electrically connected to the positive electrode tab group 23 of the electrode body 20 via the positive electrode current collector 50 inside the exterior body 12. The positive electrode terminal 30 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90. The negative electrode terminal 40 is electrically connected to the negative electrode tab group 25 of the electrode body 20 via the negative electrode current collector 60 inside the exterior body 12. The negative electrode terminal 40 is insulated from the sealing plate 14 by the internal insulating member 80 and the gasket 90.

[0027] As shown in FIG. 2 and FIG. 3, a plate-shaped positive electrode external conductive member 32 and a plate-shaped negative electrode external conductive member 42 are attached to the outer surface of the sealing plate 14. The positive electrode external conductive member 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive member 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are members to which conductive members such as bus bars that electrically connect a plurality of power storage devices 100 to each other are attached. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are insulated from the sealing plate 14 by an external insulating member 92. For example, the power storage module 500 is connected in series by electrically connecting the positive electrode external conductive member 32 of one power storage device 100 and the negative electrode external conductive member 42 of the other power storage device 100 by a bus bar or the like among the power storage devices 100 adjacent to each other in the arrangement direction X.

[0028] FIG. 4 is a schematic diagram showing the configuration of the electrode body 20. As shown in FIG. 4, the electrode body 20 has a positive electrode 22, a negative electrode 24, and a separator 26. The electrode body 20 is a wound electrode body in which a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 are stacked with a strip-shaped separator 26 interposed therebetween and wound around a winding axis WL. The electrode body 20 has a flat outer shape. The electrode body 20 is arranged inside the exterior body 12 with the winding axis WL oriented substantially parallel to the long side direction Y. However, in other embodiments, the electrode body 20 may be arranged inside the exterior body 12 with the winding axis WL oriented substantially parallel to the up-down direction Z. The electrode body 20 may also be a laminated electrode body in which a plurality of square-shaped (typically rectangular) positive electrodes and a plurality of square-shaped (typically rectangular) negative electrodes are stacked in an insulated state.

[0029] The configuration of the positive electrode 22 may be the same as that of the conventional one. Here, the positive electrode 22 has a positive electrode collector 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode collector 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode collector 22c is strip-shaped. The positive electrode collector 22c is preferably made of metal, and more preferably made of metal foil. Here, the positive electrode collector 22c is aluminum foil.

[0030] A plurality of positive electrode tabs 22t are provided at one end (left end in FIG. 4) in the long side direction Y of the positive electrode current collector 22c. The plurality of positive electrode tabs 22t protrude toward one side (left end in FIG. 4) in the long side direction Y. The plurality of positive electrode tabs 22t protrude in the long side direction Y beyond the separator 26. Here, the positive electrode tab 22t is a part of the positive electrode current collector 22c, and is made of metal foil (aluminum foil). The plurality of positive electrode tabs 22t are stacked at one end (left end in FIG. 4) in the long side direction Y to form a positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode current collector 50.

[0031] The positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the positive electrode current collector 22c. The positive electrode active material layer 22a contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. An example of the positive electrode active material is a lithium transition metal composite oxide. The positive electrode active material layer 22a may contain any component other than the positive electrode active material, such as various additive components such as a binder and a conductive material.

[0032] The positive electrode protective layer 22p is provided at the boundary between the positive electrode current collector 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, etc.

[0033] The negative electrode 24 has a negative electrode current collector 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode current collector 24c. The negative electrode current collector 24c is strip-shaped. The negative electrode current collector 24c is preferably made of metal, more preferably made of metal foil. In this embodiment, the negative electrode current collector 24c is copper foil.

[0034] A plurality of negative electrode tabs 24t are provided at one end (right end in FIG. 4) in the long side direction Y of the negative electrode current collector 24c. The plurality of negative electrode tabs 24t protrude toward one side (right end in FIG. 4) in the long side direction Y. The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. The negative electrode tab 24t is a part of the negative electrode current collector 24c here, and is made of metal foil (copper foil). The plurality of negative electrode tabs 24t are stacked at one end (right end in FIG. 4) in the long side direction Y to form a negative electrode tab group 25. The negative electrode tab group 25 is provided at a position symmetrical to the positive electrode tab group 23 in the long side direction Y. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via the negative electrode current collector 60.

[0035] The negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the negative electrode current collector 24c. The length Ln of the negative electrode active material layer 24a in the long side direction Y is preferably equal to or longer than the length Lp of the positive electrode active material layer 22a in the long side direction Y. The negative electrode active material layer 24a contains a negative electrode active material capable of reversibly absorbing and releasing charge carriers. The negative electrode active material essentially contains graphite. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material. The negative electrode active material may further contain a material other than graphite, for example, a carbon material such as hard carbon or soft carbon, or a compound containing silicon (Si-containing material).

[0036] Although not particularly limited, the ratio of the negative electrode active material in the negative electrode active material layer 24a is preferably 90% by mass or more, and more preferably, for example, 95 to 99% by mass. The negative electrode active material layer 24a may contain any component other than the negative electrode active material, for example, various additive components such as a binder, a thickener, a dispersant, etc. Examples of the binder include styrene butadiene rubber (SBR) and polyvinylidene fluoride (PVdF). Examples of the thickener include carboxymethyl cellulose (CMC).

[0037] The separator 26 is disposed between the positive electrode 22 and the negative electrode 24. The separator 26 is a member that insulates the positive electrode 22 and the negative electrode 24. The configuration of the separator 26 may be the same as that of a conventional separator. The length Ls of the separator 26 in the long side direction Y is preferably equal to or longer than the length Ln of the negative electrode active material layer 24a in the long side direction Y. The separator 26 is preferably a resin porous sheet (microporous film) made of a polyolefin resin such as polyethylene (PE) or polypropylene (PP). The separator 26 may have a functional layer (e.g., an adhesive layer or a heat resistance layer (HRL)) on the surface of the resin porous sheet.

[0038] The configuration of the non-aqueous electrolyte may be the same as that of the conventional one. The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). The non-aqueous solvent is, for example, a carbonate such as ethylene carbonate, dimethyl carbonate, or ethyl methyl carbonate. The supporting salt is, for example, a fluorine-containing lithium salt such as lithium hexafluorophosphate (LiPF6) or lithium bis(fluorosulfonyl)imide (LiFSI). The non-aqueous electrolyte may further contain an additive as necessary. The non-aqueous electrolyte is typically liquid, but may be gelled. In another embodiment, the electricity storage device 100 may include a solid electrolyte instead of the non-aqueous electrolyte. In that case, the separator 26 can be omitted.

[0039] Fig. 5 is a plan view showing a schematic diagram of the power storage module 500 and the cooling device 400. Note that detailed illustration of the spacer 200 and the upper surface of the power storage device 100 is omitted in Fig. 5. As shown in Fig. 5, the cooling device 400 includes an air inlet IP, an exhaust outlet OP, an air-cooled fan 410, a temperature sensor 420, and a control device 430. The cooling device 400 is an air-cooled type cooling device that uses air as a refrigerant. However, in other embodiments, the cooling device 400 may be a liquid-cooled type cooling device that uses a liquid refrigerant.

[0040] In this embodiment, the air intake port IP is provided on one side (front F side) of the arrangement direction X of the power storage module 500. The exhaust port OP is provided on the other side (rear Rr side) of the arrangement direction X. The air-cooled fan 410 is attached to the air intake port IP. The air-cooled fan 410 is configured to send wind (air) to the air intake port IP. The configuration of the air-cooled fan 410 is not limited, but includes, for example, an electric motor (not shown). The temperature sensor 420 is disposed in the center of the power storage module 500 in the XY plane here. The temperature sensor 420 is, for example, a thermocouple or a thermistor.

[0041] The control device 430 is electrically connected to the temperature sensor 420 and the electric motor of the air-cooling fan 410. For example, when the temperature sensor 420 detects that the temperature inside the power storage module 500 has reached a predetermined first temperature or higher, the control device 430 operates the air-cooling fan 410. As a result, low-temperature air outside the power storage module 500 is supplied into the power storage module 500 from the air intake port IP, and an air flow AF is generated inside the power storage module 500. The supplied air passes through the power storage module 500 while cooling the power storage device 100, and is discharged from the exhaust port OP. For example, when the temperature sensor 420 detects that the temperature inside the power storage module 500 has reached a predetermined second temperature or lower, the control device 430 stops the air-cooling fan 410. According to such an air-cooling type cooling device 400, the power storage device 100 can be cooled at low cost.

[0042] According to the study by the present inventors, a temperature distribution occurs in the power storage module 500 equipped with a cooling mechanism such as the cooling device 400 during charging and discharging of the multiple power storage devices 100, and a low-temperature region A1 where the temperature is relatively low and a high-temperature region A2 where the temperature is relatively high may occur. Specifically, when the power storage devices 100 generate heat as they are charged and discharged, the adjacent power storage devices 100 heat each other up. As a result, in the center of the arrangement direction X, a chain reaction of heat generation occurs between the power storage devices 100, and the temperature tends to become relatively high. On the other hand, the two ends of the arrangement direction X (the front part F and the rear part Rr in FIG. 5) have higher heat dissipation properties than the center, so that a chain reaction of heat generation is less likely to occur. Therefore, the temperature tends to become relatively low at both ends of the arrangement direction X.

[0043] Particularly in this embodiment, the intake port IP and the air-cooled fan 410 to which the refrigerant (air) is supplied are arranged on the front F side of the arrangement direction X, and the exhaust port OP is arranged on the rear Rr side of the arrangement direction X. For this reason, both ends in the arrangement direction X tend to become low temperature. Therefore, the center part in the arrangement direction X tends to become a high temperature area A2 with a relatively high temperature, and both ends in the arrangement direction X (the front F part and the rear Rr part in FIG. 5) tend to become a low temperature area A1 with a relatively low temperature. In particular, the front F part in the arrangement direction X where the intake port IP and the air-cooled fan 410 are arranged tends to become the coldest. That is, in this embodiment, at least the front F side in the arrangement direction X tends to become a low temperature area A1 with a relatively low temperature.

[0044] For example, as described in Patent Document 1 and the like, when a temperature distribution occurs in the power storage module 500, the high-rate resistance of the power storage device 100 may vary. More specifically, the high-rate resistance of the power storage device 100 may be low in the low-temperature region A1. In this case, if the charge and discharge of the entire power storage module 500 is controlled based on the high-rate resistance of the power storage device 100 in the low-temperature region A1, the high high-rate resistance of the power storage device 100 in the high-temperature region A2 cannot be fully utilized. On the other hand, when the high-rate resistance of the power storage device 100 in the high-temperature region A2 is used as a standard, a high voltage is applied to the power storage device 100 in the low-temperature region A1, and high-rate deterioration is likely to be accelerated. In this way, when a temperature distribution occurs in the power storage module 500, the high-rate resistance of the entire power storage module 500 may be reduced due to the high-rate resistance of the power storage device 100 in the low-temperature region A1. Furthermore, when the power storage module is mounted on a moving body such as a vehicle, there is a risk of fuel efficiency being deteriorated.

[0045] In the technology disclosed herein, the peak intensity ratio (I 004 / I 110) are used. The first electricity storage device 110 has a lower peak intensity ratio of the negative electrode active material layer 24a than the second electricity storage device 120. As will be described in detail later, the inventors have confirmed that the higher the high-rate resistance, the lower the peak intensity ratio of the negative electrode active material layer 24a. For this reason, in this embodiment, the first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a (high high-rate resistance) is arranged in the low-temperature region A1 where the temperature is relatively low, here at both ends in the arrangement direction X (the front part F and the rear part Rr in FIG. 5). In addition, the second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a (low high-rate resistance) is arranged in the high-temperature region A2 where the temperature is relatively high, here at the center in the arrangement direction X.

[0046] According to such a configuration, the high-rate resistance of the plurality of power storage devices 100 can be equalized at a high level. In addition, the acceleration of deterioration can be suppressed, and the high-rate resistance of the entire power storage module 500 can be improved. In addition, unlike the technology of Patent Document 1, since there is no need to be bound by the framework of a "cell group", the high-rate resistance of the plurality of power storage devices 100 can be flexibly adjusted according to the temperature distribution in the power storage module 500. Therefore, there are cases where the high-rate resistance of the plurality of power storage devices 100 can be equalized with higher accuracy than the technology of Patent Document 1. Furthermore, since the number of restraining mechanisms 300 can be reduced compared to the technology of Patent Document 1, the volumetric energy density and fuel efficiency can also be improved. In addition, the number of parts can be reduced, and manufacturing costs can be reduced.

[0047] The peak intensity ratio (I 004 / I 110) is an index showing the degree of orientation of the hexagonal mesh plane of graphite in the thickness direction of the negative electrode 24 (the normal direction of the negative electrode current collector 24c), and the smaller the value, the more the hexagonal mesh plane is aligned perpendicularly to the negative electrode current collector 24c. The peak intensity ratio can be calculated based on the measurement results of X-ray crystal structure analysis. Specifically, for example, when the negative electrode active material layer 24a is measured by X-ray diffraction (XRD), the peak derived from the (110) plane of graphite appears in the XRD chart in the range of 2θ=76.5° to 78.5°, and the peak derived from the (004) plane of graphite appears in the range of 2θ=53.5° to 56.0°. Therefore, the peak intensity (maximum intensity) I of the peak derived from the (004) plane is calculated from the XRD chart using commercially available analysis software. 004 and the peak intensity (maximum intensity) of the peak originating from the (110) plane, I 110 and are respectively obtained, and the peak intensity ratio can be obtained by calculating the ratio between them.

[0048] The peak intensity ratio of the negative electrode active material layer 24a can be adjusted relatively easily, for example, by changing the type of graphite used as the negative electrode active material (the crystal orientation of the graphite itself) in the negative electrode preparation step (A-1) of the manufacturing method described below, or by applying a magnetic field to the negative electrode composite on the negative electrode current collector 24c.

[0049] In the case where there are a plurality of first electricity storage devices 110 and a plurality of second electricity storage devices 120 as in this embodiment, it is preferable that each of the plurality of first electricity storage devices 110 has a lower peak intensity ratio of the negative electrode active material layer 24a than the plurality of second electricity storage devices 120. In addition, although not particularly limited, from the viewpoint of balancing the energy density and the high-rate resistance at a high level, it is preferable that the peak intensity ratio of the negative electrode active material layer 24a of each of the first electricity storage devices 110 and the second electricity storage device 120 is in the range of approximately 1 to 50, more preferably in the range of 2 to 40, and more preferably in the range of, for example, 2.9 to 32.5. In particular, by setting the peak intensity ratio to a predetermined value or less, the expansion of the negative electrode 24 during high-rate charging can be better suppressed.

[0050] Although it depends on the temperature distribution in the electricity storage module 500, in one embodiment, the peak intensity ratio of the negative electrode active material layer 24a of the first electricity storage device 110 is preferably approximately 40 or less, for example, in the range of 1 to 35, 2 to 30, or even more preferably 2 to 20 or 2 to 15. The peak intensity ratio of the negative electrode active material layer 24a of the second electricity storage device 120 is preferably approximately 50 or less, for example, in the range of 2 to 50, 5 to 40, or even more preferably 10 to 35.

[0051] The difference in packing density between the negative electrode active material layer 24a of the first power storage device 110 and the negative electrode active material layer 24a of the second power storage device 120 is a design item that is appropriately adjusted, for example, depending on the temperature distribution in the power storage module 500. For this reason, although not particularly limited, when the temperature distributions of the first power storage device 110 and the second power storage device 120 are significantly different, the difference in peak intensity ratio of the negative electrode active material layer 24a between the first power storage device 110 and the second power storage device 120 is preferably 0.5 or more, more preferably 1 or more, and further preferably 2 or more, 3 or more, or 4 or more. By setting the difference in peak intensity ratio to a predetermined value or more, the effect of the technology disclosed herein can be more significantly exhibited. The difference in the peak intensity ratio may be, for example, 8 or less, 7 or less, or 5 or less. This allows the high-rate charging characteristics of the first power storage device 110 and the second power storage device 120 to be accurately equalized. When there are a plurality of first power storage devices 110 and a plurality of second power storage devices 120, the difference in peak intensity ratio may be the difference between the average of the peak intensity ratios of the plurality of first power storage devices 110 and the average of the peak intensity ratios of the plurality of second power storage devices 120.

[0052] In a preferred embodiment, the first electricity storage device 110 contains artificial graphite as the graphite, and the second electricity storage device 120 contains natural graphite as the graphite. Preferably, in the first electricity storage device 110, artificial graphite constitutes the main negative electrode active material (meaning that it accounts for 50 mass% or more; the same applies below), and in the second electricity storage device 120, natural graphite constitutes the main negative electrode active material. This allows the peak intensity ratios of the first electricity storage device 110 and the second electricity storage device 120 to differ greatly.

[0053] In another preferred embodiment, the first electricity storage device 110 and the second electricity storage device 120 contain the same type of graphite. For example, both the first electricity storage device 110 and the second electricity storage device 120 contain artificial graphite. Alternatively, both the first electricity storage device 110 and the second electricity storage device 120 contain natural graphite. When the first electricity storage device 110 and the second electricity storage device 120 contain the same type of graphite, in the (A-1) negative electrode preparation step of the manufacturing method described later, when preparing the negative electrode 24 of the first electricity storage device 110, a magnetic field is applied to the negative electrode mixture on the negative electrode current collector 24c, thereby decreasing the peak intensity ratio, and the peak intensity ratio can be made significantly different from that of the second electricity storage device 120.

[0054] In one embodiment, the first electricity storage device 110 and the second electricity storage device 120 are preferably configured to have the same thickness and basis weight (the mass of the negative electrode active material layer 24a per unit area of ​​the negative electrode current collector 24c) of the negative electrode active material layer 24a and to have the same negative electrode capacity (manufacturing errors and the like are acceptable). This allows the energy densities of the first electricity storage device 110 and the second electricity storage device 120 to be equalized, thereby achieving a high energy density in the electricity storage module 500 as a whole.

[0055] In one embodiment, the first electricity storage device 110 and the second electricity storage device 120 preferably have the same configuration other than the negative electrode active material layer 24a, for example, the configuration of the positive electrode 22, the separator 26, and the nonaqueous electrolyte. This makes it easier to equalize the battery performance other than the high rate resistance between the first electricity storage device 110 and the second electricity storage device 120.

[0056] [Method of manufacturing energy storage module] Next, a method for manufacturing a power storage module 500 including a plurality of power storage devices 100 will be described. The power storage module 500 can be manufactured by a manufacturing method including, for example, a preparation step (step A) of preparing a first power storage device 110 and a second power storage device 120, a temperature distribution prediction step (step B) of predicting a temperature distribution in the power storage module 500, and a construction step (step C) of constructing the power storage module 500 by combining the first power storage device 110 and the second power storage device 120. The order of the preparation step (step A) and the temperature distribution prediction step (step B) is not particularly limited. For example, the temperature distribution prediction step (step B) may be performed after the preparation step (step A), the preparation step (step A) may be performed after the temperature distribution prediction step (step B), or both steps may be performed simultaneously. The manufacturing method disclosed herein may further include other steps at any stage.

[0057] In the (step A) preparation step, a first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a and a second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a are prepared as a plurality of electricity storage devices 100. In this embodiment, the (step A) preparation step includes, in this order, (A-1) a negative electrode fabrication step of fabricating the negative electrode 24, (A-2) an electrode assembly fabrication step of fabricating the electrode assembly 20 using the negative electrode 24, (A-3) an accommodation step of accommodating the electrode assembly 20 and a nonaqueous electrolyte in the battery case 10, and (A-4) a conditioning step.

[0058] In the (A-1) negative electrode preparation step, at least two types of negative electrodes 24 having different peak intensity ratios of the negative electrode active material layer 24a are prepared. In detail, a first negative electrode having a relatively low peak intensity ratio for the first electricity storage device 110 and a second negative electrode having a relatively high peak intensity ratio for the second electricity storage device 120 are prepared. That is, this step includes a first negative electrode preparation step of preparing a first negative electrode for the first electricity storage device 110 and a second negative electrode preparation step of preparing a second negative electrode for the second electricity storage device 120.

[0059] Here, this process includes a preparation process, an application process, and a magnetic field application process. In the preparation process, for example, first, a negative electrode composite paste containing at least graphite is prepared by dispersing the above-mentioned solid materials (for example, graphite as a negative electrode active material, a binder, a thickener, etc.) in a predetermined solvent (for example, water, N-methyl-2-pyrrolidone, etc.). The type of graphite may be the same in the first negative electrode and the second negative electrode, or may be different. In this embodiment, the type of graphite is the same. For example, both the first negative electrode and the second negative electrode contain artificial graphite. Alternatively, both the first negative electrode and the second negative electrode contain natural graphite. This can omit the effort of separately preparing the negative electrode composite paste.

[0060] Next, in the application step, the prepared negative electrode composite paste is applied onto the negative electrode current collector 24c using a conventionally known coating device. Then, in the magnetic field application step, a magnetic field is applied to the first negative electrode in the thickness direction before the applied negative electrode composite paste solidifies (completely dries). As a result, the graphite contained in the negative electrode composite paste is oriented in the thickness direction so as to be parallel to the magnetic field lines, and the peak intensity ratio is reduced. Note that the application of the magnetic field can be performed by a conventionally known method following, for example, Patent Document 4, etc., so that the graphite is appropriately oriented. Then, after the graphite is oriented, the negative electrode composite paste is dried, whereby the negative electrode composite is fixed to the surface of the negative electrode current collector 24c, and a first negative electrode with an increased peak intensity ratio can be produced.

[0061] On the other hand, for the second negative electrode, the negative electrode composite paste is applied to the surface of the negative electrode current collector 24c, and then the negative electrode is dried without applying a magnetic field. As a result, the negative electrode composite is fixed to the surface of the negative electrode current collector 24c, and a second negative electrode having a relatively low peak intensity ratio can be produced. However, a magnetic field may also be applied to the second negative electrode by the same method as that for the first negative electrode. In that case, it is preferable to make the conditions for applying the magnetic field (for example, the strength of the magnetic field, the application time, etc.) smaller than those for the first negative electrode. For example, the magnetic flux density of the magnetic field in the second negative electrode may be lower than that of the first negative electrode. This allows the peak intensity ratios of the negative electrode active material layers 24a to be greatly different from each other. In this manner, at least two types of negative electrodes 24 in which the negative electrode active material layers 24a having different peak intensity ratios are formed can be produced.

[0062] In the (A-2) electrode assembly preparation step, the first and second negative electrodes prepared in the negative electrode preparation step are each opposed to a separately prepared positive electrode 22 via the separator 26 as described above, and then wound up. In this way, an electrode assembly 20 for the first electricity storage device 110 and an electrode assembly 20 for the second electricity storage device 120 are prepared.

[0063] In the (A-3) accommodation step, the electrode body 20 prepared in the electrode body preparation step and the nonaqueous electrolyte as described above are accommodated in the battery case 10. In a preferred embodiment, first, the positive electrode tab group 23 of the electrode body 20 is joined to the positive electrode current collector 50, and the negative electrode tab group 25 of the electrode body 20 is joined to the negative electrode current collector 60. This integrates the sealing plate 14 and the electrode body 20. Next, the opening 12h of the exterior body 12 is covered with the sealing plate 14, and the electrode body 20 is placed inside the exterior body 12. Next, the sealing plate 14 is welded to the periphery of the opening 12h of the exterior body 12, and the exterior body 12 and the sealing plate 14 are integrated. Next, the nonaqueous electrolyte as described above is prepared and injected into the inside of the battery case 10 through the injection hole 15 of the sealing plate 14. In this way, a battery assembly for the first power storage device 110 and a battery assembly for the second power storage device 120 are fabricated.

[0064] In the (A-4) conditioning step, the prepared battery assembly is charged at least once. Preferably, the battery assembly is charged and discharged at least once. The battery assembly can be charged and discharged in the same manner as in the past. Typically, an external power source is connected between the positive electrode terminal 30 and the negative electrode terminal 40, and charging or discharging is performed until a predetermined state of charge (SOC) is reached between the terminals. Then, the battery case 10 is hermetically sealed (closed). In this manner, a first electricity storage device 110 and a second electricity storage device 120 having different peak intensity ratios of the negative electrode active material layer 24a can be prepared.

[0065] (Step B) In the temperature distribution prediction step, the temperature distribution in the power storage module 500 is predicted when a plurality of power storage devices 100 are charged and discharged. That is, for example, in the embodiment shown in FIG. 5, both ends in the arrangement direction X (particularly, the front F part in the arrangement direction X) tend to become the low temperature area A1. However, the temperature distribution in the power storage module 500 may change depending on the configuration of the cooling device 400 (for example, the installation positions and number of the intake port IP, the exhaust port OP, and the air-cooling fan 410) and the heat dissipation path. In addition, for example, the range of the low temperature area A1 (the length in the arrangement direction X) may also change depending on, for example, the number of the power storage devices 100 and the charge and discharge conditions. Therefore, it is preferable to predict the temperature distribution in the power storage module 500 during charging and discharging by a preliminary experiment or a simulation using commercially available analysis software. In particular, it is preferable to construct a power storage module for a preliminary test simulating the power storage module 500, measure the temperature distribution, and predict the temperature distribution in the power storage module 500 based on the actual measurement.

[0066] In a preferred embodiment, first, a plurality of power storage devices for a preliminary test, which are different from the first power storage device 110 and the second power storage device 120 produced in the preparation step, are prepared, and a temperature sensor is attached to each of them. Next, a power storage module for a preliminary test simulating the power storage module 500 is assembled using the plurality of power storage devices for the preliminary test. Next, the plurality of power storage devices for the preliminary test are actually charged and discharged (preferably at a high rate), and the temperature distribution at this time is predicted. The charge and discharge conditions are preferably conditions assuming the manner in which the device will actually be used. Then, based on the acquired temperature distribution, the temperature distribution in the power storage module 500 is predicted, and the device is divided (e.g., divided into two), for example, into a low temperature region A1 and a high temperature region A2.

[0067] In the (Step C) construction step, the first electricity storage device 110 and the second electricity storage device 120 are arranged based on the temperature distribution predicted in the temperature distribution prediction step to construct the electricity storage module 500. Specifically, the first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a is arranged in an area separated from the low temperature area A1, and the second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a is arranged in an area separated from the high temperature area A2. Then, the first electricity storage device 110 and the second electricity storage device 120 are restrained by the restraining mechanism 300 together with, for example, a plurality of spacers 200, and held together as one body. In this manner, the electricity storage module 500 can be constructed.

[0068] [Uses of energy storage modules] The power storage module 500 can be used for various purposes, but because it has excellent high-rate resistance, it can be suitably used in purposes requiring high output, for example, as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car or truck. The type of vehicle is not particularly limited, but examples include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and a battery electric vehicle (BEV). By mounting the power storage module 500 on a moving object such as a vehicle, the fuel efficiency (electricity cost) of the moving object can be improved.

[0069] Some test examples relating to the present invention will be described below, but it is not intended that the present invention be limited to these test examples.

[0070] In this test example, power storage devices with different types of graphite as the negative electrode active material and / or different peak intensity ratios of the negative electrode active material layer were constructed, and the high rate resistance was confirmed. Specifically, first, a negative electrode composite paste was prepared using the types of graphite shown in Table 1, and a negative electrode (Examples 1 to 5) was fabricated. In addition, in Examples 3 and 5, a magnetic field with magnetic lines oriented in the normal direction of the negative electrode current collector was applied before the negative electrode composite paste was dried. The application conditions were a magnetic flux density of 500 mT and an application time of 3 seconds. In this way, a negative electrode equipped with a negative electrode active material layer was fabricated.

[0071] The obtained negative electrode active material layer was measured using a commercially available X-ray diffraction device, and the peak intensity ratio (I 004 / I 110 Specifically, X-rays were applied from the normal direction of the negative electrode current collector, and measurements were performed under the following conditions. The peak intensity ratio between the (110) plane and the (004) plane was then calculated. Measurement device: Ultima IV (Rigaku Corporation) X-ray source: CuKα ray Measurement range: 5~90° Step width: 0.02° Slits: Divergence slit = 1 degree, receiving slit = 0.1 mm, scattering slit = 1 degree

[0072] Next, a wound electrode body was produced using the produced negative electrodes (Examples 1 to 5), and an electricity storage device (lithium ion secondary battery, Examples 1 to 5) was constructed. The configurations other than the above (type of graphite and / or peak intensity ratio of the negative electrode active material layer) were common to all electricity storage devices. Next, in a temperature environment of 25°C, the electricity storage device was adjusted to a state of SOC 50%, and constant current discharge was performed at 150A for 10 seconds, and the discharge resistance was measured. Next, the battery voltage ΔV that had dropped in 10 seconds was read, and the IV resistance (initial resistance) was calculated based on the battery voltage ΔV and the discharge current value (150A).

[0073] Next, in a temperature environment of 25°C, the power storage device was adjusted to a state of SOC 50%, and constant current charging was performed at a charge rate of 150A for 10 seconds, followed by a pause for 5 seconds, followed by a constant current discharge at a discharge rate of 10A for 150 seconds, followed by a pause for 5 seconds. This cycle was repeated 1000 times to perform a high-rate durability test. After the high-rate durability test, the IV resistance was measured in the same manner as the initial resistance, and the resistance increase rate was calculated from the ratio of the IV resistance after the durability test to the initial resistance (IV resistance after the durability test / initial resistance). The results are shown in Table 1. In addition, Table 1 shows relative values ​​when the resistance increase rate of Example 2 is set to 1.00 (reference).

[0074] [Table 1]

[0075] As shown in Table 1, when comparing Examples 3 and 5, in which a magnetic field was applied before the negative electrode composite paste dried, with Examples 1 and 2, in which a magnetic field was not applied, the peak intensity ratio was significantly reduced by applying a magnetic field. This shows that the peak intensity ratio can be adjusted by applying a magnetic field. In more detail, by applying a magnetic field, the direction of the hexagonal mesh plane of the graphite becomes perpendicular to the negative electrode current collector, and the I 004 becomes smaller (I 100It was found that, as a result of using artificial graphite, the peak intensity ratio was lower. Furthermore, when Example 4, which used artificial graphite, was compared with Examples 1 and 2, which used natural graphite, the peak intensity ratio was relatively lower when artificial graphite was used. Therefore, it was found that the peak intensity ratio can be adjusted by changing the type of graphite (the crystal orientation of the graphite itself).

[0076] In addition, the lower the peak intensity ratio of the negative electrode active material layer, the smaller the increase in resistance after the high-rate durability test, i.e., the higher the high-rate resistance. Although it is not intended to be interpreted in a particularly limited manner, the reason for this is thought to be that the lower the peak intensity ratio of the negative electrode, the less likely the negative electrode is to expand and contract in the thickness direction, especially during high-rate charging and discharging, and the discharge of the electrolyte from both ends in the winding direction of the wound electrode body is suppressed. From the above, the experimental results also support the fact that a power storage device with a low peak intensity ratio of the negative electrode active material layer is relatively superior in high-rate resistance compared to a power storage device with a high peak intensity ratio of the negative electrode active material layer.

[0077] Although the preferred embodiment of the present invention has been described above, the above embodiment is merely an example. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes of the above-exemplified embodiment. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. Furthermore, if a technical feature is not described as essential, it can be appropriately deleted.

[0078] (1) For example, in the above embodiment, in the preparation step (step A), a magnetic field is applied to the first negative electrode for the first power storage device 110 to adjust (specifically, to reduce) the peak intensity ratio of the negative electrode active material layer 24a. However, this is not limited to this. As described in the above test example, when the types of negative electrode active materials (particularly the crystal orientation of the graphite itself) are different between the first negative electrode and the second negative electrode, specifically when the negative electrode composite paste for the first negative electrode and the negative electrode composite paste for the second negative electrode are adjusted separately, the application of a magnetic field to the first negative electrode may be omitted.

[0079] (2) For example, in the above embodiment, in the preparation step (step A), the electricity storage device 100 is manufactured in which the peak intensity ratio of the negative electrode active material layer 24a is intentionally made different. However, this is not limited to this. For example, the first electricity storage device 110 and the second electricity storage device 120 may be prepared by selecting from a large number of electricity storage devices having different peak intensity ratios of the negative electrode active material layer 24a within a predetermined range of non-defective products.

[0080] A specific example is a case where a used electricity storage device (which may be in the form of an electricity storage module) is collected from the market and reused, that is, the electricity storage device 100 is a reused product. In recent years, electricity storage devices such as lithium ion secondary batteries are sometimes provided with identification information from the viewpoint of traceability. In one example, an optical symbol that can be read by a reading device is provided on the surface of the electricity storage module (e.g., sealing plate 14). Alternatively, a small substrate including identification information is mounted inside the electricity storage device. The identification information may include, in addition to ID information such as model number, manufacturer name, country of manufacture, name of manufacturing plant, and date of manufacture, material information such as the type of negative electrode active material.

[0081] In this case, the (step A) preparation step may include (Aa) an acquisition step of reading out the identification information attached to each of the many collected electricity storage devices and acquiring information on the type of the negative electrode active material, and (Ab) a selection step of selecting a first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a (e.g., containing artificial graphite) and a second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a (e.g., containing natural graphite) based on the acquired information on the type of the negative electrode active material. Such a manufacturing method of an electricity storage module may also be understood as a method for reusing electricity storage devices. In this specification, the term "optical symbol" is a general term for an information medium that stores information by combining a portion with high optical reflectance and a portion with low optical reflectance, and is a concept that includes two-dimensional symbols (also called two-dimensional codes, two-dimensional bar codes, etc.) such as QR Code (registered trademark), data matrix, and data tag.

[0082] (3) For example, in the embodiment of FIG. 5 described above, both ends in the arrangement direction X (the front F part and the rear Rr part in FIG. 5) are the low temperature area A1 with a relatively low temperature, and the center part in the arrangement direction X is the high temperature area A2 with a relatively high temperature. However, this is not limited to this. As described above, the temperature distribution in the power storage module 500 can change depending on the configuration of the cooling device 400 (for example, the installation positions and number of the intake port IP, the exhaust port OP, and the air-cooling fan 410), the number of the power storage devices 100, the charge and discharge conditions, etc. Also, in the embodiment of FIG. 5 described above, the power storage module 500 is divided into two temperature areas, the low temperature area A1 and the high temperature area A2, and further, the temperature distribution is symmetrical in the arrangement direction X. However, this is not limited to this. For example, the power storage module 500 can be divided into three or more temperature areas. In this case, in the embodiment of Fig. 5, the low temperature area A1 on the rear Rr side in the arrangement direction X may be a medium temperature area A3 having a higher temperature than the low temperature area A1 and a lower temperature than the high temperature area A2. In addition, when the cooling path and the heat dissipation path are complicated, the temperature distribution may be random, for example, with the low temperature area A1 and the high temperature area A2 appearing alternately. Some specific modified examples will be described below with reference to Figs. 6 to 9. Note that the cooling device is not shown in Figs. 6 to 9.

[0083] (First Modification) Fig. 6 is a plan view of a power storage module 500a according to a first modification. As described above, it is known that chained heat generation between the power storage devices 100 is likely to occur in the center of the arrangement direction X. For this reason, although not shown in Fig. 6, an air intake port IP and / or an air-cooling fan 410 through which a coolant (air) is supplied may be additionally installed in the center of the arrangement direction X to strongly cool the center. Then, as shown in Fig. 6, the temperature distribution of the power storage module 500a is opposite to that in Fig. 5, with the center of the arrangement direction X being a low-temperature region A1 with a relatively low temperature, and both ends of the arrangement direction X (the front part F and the rear part Rr in Fig. 6) being high-temperature regions A2 with a relatively high temperature.

[0084] In such a case, as shown in FIG. 6, it is advisable to arrange a first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a (high high-rate resistance) in the center of the arrangement direction X, which is the low-temperature region A1, and to arrange a second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a (low high-rate resistance) at both ends of the arrangement direction X, which are the high-temperature regions A2.

[0085] (Second and third modified examples) Fig. 7 is a plan view of a power storage module 500b according to a second modified example. Fig. 8 is a plan view of a power storage module 500c according to a third modified example. For example, if the air-cooling fan 410 installed on the front F side in the arrangement direction X in Fig. 5 is powerful and has high cooling capacity, the temperature distribution in the power storage modules 500b and 500c may be such that the front F part in the arrangement direction X becomes a low-temperature region A1 with a relatively low temperature, and the rear Rr part in the arrangement direction X becomes a high-temperature region A2 with a relatively high temperature, as shown in Figs. 7 and 8, respectively.

[0086] In such a case, as shown in Figures 7 and 8, it is advisable to arrange a first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a (high high-rate resistance) in the front F part of the arrangement direction X, which is the low-temperature region A1, and to arrange a second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a (low high-rate resistance) in the rear Rr part of the arrangement direction X, which is the high-temperature region A2.

[0087] Furthermore, the distribution of the low temperature region A1 and the high temperature region A2 may differ depending on, for example, the number of the power storage devices 100, the charge / discharge conditions, etc. For this reason, the low temperature region A1 and the high temperature region A2 may be provided uniformly in the arrangement direction X as shown in Fig. 7, or may be provided non-uniformly in the arrangement direction X as shown in Fig. 8. In other words, the number of first power storage devices 110 and the number of second power storage devices 120 included in the power storage module 500 may be the same or different.

[0088] (Fourth Modification) Fig. 9 is a plan view of a power storage module 500d according to a fourth modification. As shown in Fig. 9, the temperature distribution of the power storage module 500d is divided in more detail than in Fig. 5. That is, both ends in the arrangement direction X (the front F part and the rear Rr part in Fig. 6) are low temperature areas A1 with a relatively low temperature, the center part in the arrangement direction X is a high temperature area A2 with a relatively high temperature, and between the low temperature area A1 and the high temperature area A2 is a medium temperature area A3 with a higher temperature than the low temperature area A1 and a lower temperature than the high temperature area A2.

[0089] In such a case, as shown in Fig. 9, a first electricity storage device 110 having a relatively low peak intensity ratio of the negative electrode active material layer 24a (high high-rate resistance) may be arranged at both ends of the arrangement direction X, which is the low temperature region A1, a second electricity storage device 120 having a relatively high peak intensity ratio of the negative electrode active material layer 24a (low high-rate resistance) may be arranged at the center of the arrangement direction X, which is the high temperature region A2, and a third electricity storage device 130 having a lower peak intensity ratio of the negative electrode active material layer 24a than the second electricity storage device 120 and a higher peak intensity ratio of the negative electrode active material layer 24a than the first electricity storage device 110 may be arranged in a medium temperature region A3 between the low temperature region A1 and the high temperature region A2. In other words, a plurality of electricity storage devices 100 may be arranged in the order of the high temperature region A2, the medium temperature region A3, and the low temperature region A1, in this case, such that the peak intensity ratio of the negative electrode active material layer 24a decreases stepwise from the center to both ends of the arrangement direction X.

[0090] 9, the inside of the power storage module 500 is divided into three temperature zones, but it is of course possible to divide it into four or more temperature zones. By dividing the inside of the power storage module 500 into smaller zones according to the temperature distribution in this manner, the effect of the technology disclosed herein can be exerted to a high level, and the high-rate resistance of the entire power storage module 500 can be improved.

[0091] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A power storage module including a plurality of power storage devices, each of the plurality of power storage devices having a positive electrode and a negative electrode, the negative electrode having a negative electrode active material layer including graphite, the power storage module having a low-temperature region where the temperature is relatively low and a high-temperature region where the temperature is relatively high during charging and discharging of the plurality of power storage devices, wherein when the negative electrode active material layer is measured by X-ray crystal structure analysis, a peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110) is a peak intensity ratio, a first power storage device arranged in the low temperature region among the plurality of power storage devices has a lower peak intensity ratio than a second power storage device arranged in the high temperature region. Item 2: The energy storage module according to item 1, wherein, between the low temperature region and the high temperature region, there is a medium temperature region within the energy storage module, the medium temperature region having a temperature higher than that of the low temperature region and lower than that of the high temperature region, and the plurality of energy storage devices are arranged such that the peak intensity ratio of the negative electrode active material layer decreases stepwise in the order of the high temperature region, the medium temperature region, and the low temperature region. Item 3: The electricity storage module according to item 1 or 2, wherein the difference in the peak intensity ratio of the negative electrode active material layer between the first electricity storage device and the second electricity storage device is 0.5 or more. Item 4: The electricity storage module according to any one of Items 1 to 3, wherein the peak intensity ratio of the negative electrode active material layer of each of the first electricity storage device and the second electricity storage device is in the range of 1 or more and 50 or less. Item 5: The electricity storage module according to any one of items 1 to 4, wherein the first electricity storage device contains artificial graphite as the graphite, and the second electricity storage device contains natural graphite as the graphite. Item 6: The power storage module according to any one of Items 1 to 5, wherein the first power storage device and the second power storage device are connected in series. Item 7: A method for producing an electricity storage module comprising a plurality of electricity storage devices, each of the plurality of electricity storage devices having a positive electrode and a negative electrode, the negative electrode comprising a negative electrode active material layer containing graphite, wherein when the negative electrode active material layer is measured by X-ray crystal structure analysis, a peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110) is a peak intensity ratio, the peak intensity ratio being a relatively low peak intensity ratio of the negative electrode active material layer, and the peak intensity ratio being a relatively high peak intensity ratio of the negative electrode active material layer, as the plurality of electricity storage devices; a temperature distribution prediction step of predicting a temperature distribution in the electricity storage module when the plurality of electricity storage devices are charged and discharged; and a construction step of constructing the electricity storage module by arranging the first electricity storage device in a low temperature region where the temperature is relatively low and arranging the second electricity storage device in a high temperature region where the temperature is relatively high, based on the temperature distribution. Item 8: The manufacturing method according to item 7, wherein the preparation step includes a first negative electrode preparation step of preparing a negative electrode for the first electricity storage device, and the first negative electrode preparation step includes an application step of applying a paste-like negative electrode composite material containing the graphite onto a negative electrode current collector, and a magnetic field application step of applying a magnetic field to the negative electrode composite material before the negative electrode composite material on the negative electrode current collector solidifies to orient the graphite. [Explanation of symbols]

[0092] 10 Battery case 20 Electrode body 24 Negative electrode 100 Energy storage device 110 First power storage device 120 Second power storage device 130 Third Energy Storage Device 300 Restraint mechanism 400 Cooling device 410 Air Cooling Fan 500 Energy Storage Module A1 Low temperature area A2 High temperature area A3 Medium temperature range

Claims

1. A power storage module including a plurality of power storage devices, Each of the plurality of power storage devices has a positive electrode and a negative electrode, the negative electrode comprises a negative electrode active material layer containing graphite, Within the power storage module, there are a low-temperature region where the temperature is relatively low and a high-temperature region where the temperature is relatively high during charging and discharging of the plurality of power storage devices, Here, when the negative electrode active material layer is measured by X-ray crystal structure analysis, the peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110 ) is the peak intensity ratio, Among the plurality of power storage devices, a first power storage device arranged in the low temperature region has a lower peak intensity ratio than a second power storage device arranged in the high temperature region. Energy storage module.

2. a middle temperature region between the low temperature region and the high temperature region in the energy storage module, the middle temperature region having a temperature higher than that of the low temperature region and lower than that of the high temperature region; the plurality of power storage devices are arranged such that the peak intensity ratio of the negative electrode active material layer decreases stepwise in the order of the high temperature region, the intermediate temperature region, and the low temperature region. The energy storage module according to claim 1 .

3. a difference between the peak intensity ratios of the negative electrode active material layers of the first electricity storage device and the second electricity storage device is 0.5 or more; The energy storage module according to claim 1 .

4. In both of the first electricity storage device and the second electricity storage device, the peak intensity ratio of the negative electrode active material layer is in the range of 1 or more and 50 or less. The energy storage module according to claim 1 .

5. The first power storage device contains artificial graphite as the graphite, The second power storage device contains natural graphite as the graphite. The energy storage module according to claim 1 .

6. The first power storage device and the second power storage device are connected in series. The energy storage module according to claim 1 .

7. A method for manufacturing an electricity storage module comprising: a plurality of electricity storage devices, each of the plurality of electricity storage devices having a positive electrode and a negative electrode, the negative electrode having a negative electrode active material layer including graphite, the method comprising the steps of: Here, when the negative electrode active material layer is measured by X-ray crystal structure analysis, the peak intensity I 110 The peak intensity I originating from the (004) plane of the graphite 004 The ratio (I 004 / I 110 ) is the peak intensity ratio, a preparation step of preparing, as the plurality of electricity storage devices, a first electricity storage device in which the peak intensity ratio of the negative electrode active material layer is relatively low, and a second electricity storage device in which the peak intensity ratio of the negative electrode active material layer is relatively high; a temperature distribution prediction step of predicting a temperature distribution in the power storage module when the plurality of power storage devices are charged and discharged; a construction step of constructing the power storage module by arranging the first power storage device in a low temperature region having a relatively low temperature and arranging the second power storage device in a high temperature region having a relatively high temperature based on the temperature distribution; Including, A method for manufacturing an energy storage module.

8. the preparing step includes a first negative electrode fabricating step of fabricating a negative electrode for the first electricity storage device, The first negative electrode preparation step includes: an application step of applying a paste-like negative electrode mixture containing the graphite onto a negative electrode current collector; and a magnetic field application step of applying a magnetic field to the negative electrode mixture before the negative electrode mixture on the negative electrode current collector solidifies to orient the graphite. A method for manufacturing the electricity storage module according to claim 7.

Citation Information

Patent Citations

  • Negative electrode for nonaqueous electrolyte secondary battery

    JP2004220926A

  • Battery pack, method for manufacturing the same, battery pack, battery pack module, vehicle mounting the same, and battery mounting equipment

    JP2010170942A

  • Composite graphite particles and lithium secondary batteries using the same

    JP2012519124A

  • Negative electrode for a rechargeable lithium battery

    US20220029153A1

  • Non-aqueous electrolyte secondary battery and method for manufacturing negative electrode for secondary battery

    WO2013088540A1