Rapid-curing agent for blast-furnace cement, spraying material, and sprayed concrete

A rapid setting agent for blast furnace cement, formulated with calcium aluminate, sodium sulfate, and aluminum sulfate, addresses the issues of short-term strength and hydrogen sulfide gas generation, achieving enhanced setting properties and long-term strength.

JP2024146114APending Publication Date: 2024-10-15DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023058835
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Blast furnace cement faces challenges in achieving short-term strength development and can generate hydrogen sulfide gas when combined with certain quick-setting agents.

Method used

A rapid setting agent for blast furnace cement comprising specific proportions of calcium aluminate, sodium sulfate, and aluminum sulfate, along with optional additives, is developed to enhance short-term strength and suppress hydrogen sulfide gas generation.

Benefits of technology

The solution provides excellent short-term strength development and effectively suppresses hydrogen sulfide gas generation, ensuring rapid setting properties and long-term strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146114000001
    Figure 2024146114000001
  • Figure 2024146114000002
    Figure 2024146114000002
  • Figure 2024146114000003
    Figure 2024146114000003
Patent Text Reader

Abstract

To provide a rapid-curing agent for blast-furnace cement, which has excellent short-term strength and can suppress the generation of hydrogen sulfide gas.SOLUTION: A rapid-curing agent for blast-furnace cement contains 40 to 70 mass% of calcium aluminate, 3 to 25 mass% of sodium sulfate, and 0.1 to 10 mass% or less of aluminum sulfate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an accelerator for blast-furnace cement, a spraying material, and a sprayed concrete. [Background technology]

[0002] Conventionally, in order to prevent the collapse of exposed natural ground such as in tunnel excavation, a method of spraying quick-setting concrete in which an accelerator is mixed into the concrete has been used. In this method, materials are measured and mixed in a measuring plant installed at the excavation site to prepare the shotcrete, which is then pumped and mixed with the accelerator pumped from the other side of the junction pipe, and sprayed onto the natural ground until a specified thickness is reached.

[0003] As quick-setting admixtures, there have been proposed a liquid quick-setting admixture comprising a combination of a fluoride-containing water-soluble aluminum complex obtained by the reaction of aluminum sulfate with hydrofluoric acid, aluminum hydroxide, and phosphorous acid and / or an organic acid salt thereof (see Patent Document 1); a concrete quick-setting admixture containing at least one selected from the group consisting of aluminum fluoride, an acidic or basic solution of aluminum, lithium silicate, and lithium aluminate (see Patent Document 2); and a liquid quick-setting admixture comprising a fluoride-containing water-soluble aluminum salt obtained by the reaction of aluminum sulfate with hydrofluoric acid, aluminum hydroxide, and lithium hydroxide, lithium carbonate, lithium sulfate, or the like (see Patent Document 3).

[0004] On the other hand, in recent years, there has been a demand to reduce the amount of cement used in order to reduce carbon dioxide emissions, and the use of by-products such as blast furnace cement has been considered. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2006-193388 A [Patent Document 2] JP 2001-130935 A [Patent Document 3] JP 2005-89276 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, blast-furnace slag cement has the problem that it is difficult to obtain short-term strength, and there is also concern that hydrogen sulfide gas derived from the blast-furnace slag in the blast-furnace slag cement may be generated depending on the combination with the quick-setting admixture used.

[0007] In view of the above, an object of the present invention is to provide an accelerated setting admixture for blast-furnace slag cement which is excellent in short-term strength development and capable of suppressing the generation of hydrogen sulfide gas. [Means for solving the problem]

[0008] As a result of intensive research conducted by the inventors in light of the above problems, they found that a blast furnace cement quick-setting admixture containing calcium aluminate, sodium sulfate, and aluminum sulfate in predetermined amounts can solve the above problems, and thus completed the present invention.

[0009] [1] A quick-setting admixture for blast-furnace slag cement, containing 40 to 70 mass% calcium aluminate, 3 to 25 mass% sodium sulfate, and 0.1 to 10 mass% or less aluminum sulfate. [2] A spraying material containing the quick-setting admixture for blast-furnace slag cement described in [1] above and blast-furnace slag cement. [3] The spraying material according to the above [2], wherein the blast furnace slag content in the blast furnace cement is 30 to 90 mass%. [4] Shotcrete containing the spraying material described in [2] or [3] above. Effect of the Invention

[0010] According to the present invention, it is possible to provide an accelerator for blast-furnace cement which is excellent in short-term strength development and capable of suppressing generation of hydrogen sulfide gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to the embodiment. In addition, "%" in this specification is based on mass unless otherwise specified.

[0012] [Accelerating agent for blast furnace cement] The quick-setting admixture for blast-furnace cement according to the present embodiment contains 40 to 70 mass% calcium aluminate, 3 to 25 mass% sodium sulfate, and 0.1 to 10 mass% or less aluminum sulfate. Note that the blast-furnace cement in the present invention refers to blast-furnace cement as specified in JIS R 5211:2009 "Blast-furnace cement" or blast-furnace cement obtained by mixing blast-furnace slag with ordinary Portland cement or the like and containing blast-furnace slag in an amount equal to or greater than the amount specified in the above JIS.

[0013] The calcium aluminate contained in the quick-setting admixture for blast furnace cement according to this embodiment is a general term for a compound having CaO and Al2O3 as main components and having hydration activity, and is a compound in which a portion of CaO and / or Al2O3 is replaced with an alkali metal oxide, an alkaline earth metal oxide, silicon oxide, titanium oxide, iron oxide, an alkali metal halide, an alkaline earth metal halide, an alkali metal sulfate, an alkaline earth metal sulfate, or the like, or a substance in which a small amount of these are dissolved in a substance mainly composed of CaO and Al2O3, and calcium aluminate may be either crystalline or amorphous.

[0014] Specific examples of crystalline materials include CaO, Al2O3, and R2O (Na2O, K2O, Li2O), and include C3A and C, which is a solid solution of alkali metals. 14 RA5, CA, C 12 A7 and C 11 Examples include A7·CaF2, C4A·Fe2O3, and C3A3·CaSO4, but amorphous calcium aluminate is preferred because of its good quick-setting properties. In addition, in the case of amorphous calcium aluminate, it is preferable that the vitrification rate is 80% or more.

[0015] The quick-setting admixture for blast-furnace cement according to the present embodiment contains 40 to 70 mass% calcium aluminate. If the calcium aluminate content is less than 40 mass%, the short-term strength development may not be sufficiently exhibited, and hexavalent chromium may be eluted. If it exceeds 70 mass%, the short-term strength development and quick-setting property may not be sufficiently exhibited. The calcium aluminate content is preferably 45 to 65 mass%, and more preferably 50 to 60 mass%. If the calcium aluminate content is within the above range, it is easy to improve the short-term strength development.

[0016] The CaO / Al2O3 molar ratio of calcium aluminate is not particularly limited, but from the viewpoint of short-term strength development and suppression of elution of hexavalent chromium, the molar ratio is preferably 1.3 to 3.0, more preferably 1.6 to 2.7.

[0017] Methods for obtaining calcium aluminate include heat treating CaO raw materials such as calcium carbonate and calcium hydroxide with Al2O3 raw materials such as bauxite in a rotary kiln, electric furnace, etc. Specifically, the raw materials are mixed in a predetermined ratio, heated and melted in an electric furnace, etc., and quenched by contacting with compressed air or water, etc. The CaO / Al2O3 molar ratio can be adjusted by adjusting the ratio of the raw materials, and the vitrification rate can be adjusted by the temperature during heating and melting and the cooling method.

[0018] When calcium aluminate is obtained industrially, it may contain impurities. Specific examples of impurities include SiO2, Fe2O3, MgO, TiO2, MnO, Na2O, KO, Li2O, S, PO5, and F, but the presence of these impurities is not a problem as long as they do not substantially impede the object of the present invention. Specifically, it is not a problem as long as the total amount of these impurities is 10% or less.

[0019] The Blaine specific surface area value (Blaine value) of calcium aluminate is not particularly limited, but is usually 3,000 to 9,000 cm 2 / g is preferable, and 4,000 to 8,000 cm 2 / g is more preferable. By the Blaine value being within the above range, the handleability can be improved. The Blaine specific surface area is measured based on the specific surface area test described in JIS R 5201:2015 "Physical test method for cement".

[0020] The quick-setting admixture for blast furnace cement according to the present embodiment contains 3 to 25% by mass of sodium sulfate. If the content of sodium sulfate is less than 3% by mass, the short-term strength development and quick-setting property may not be sufficiently exhibited, and if it exceeds 25% by mass, the short-term strength development and long-term strength development may be reduced. The content of sodium sulfate is preferably 5 to 20% by mass, and more preferably 10 to 15% by mass. If the content of sodium sulfate is within the above range, the short-term strength development is easily improved. Note that sodium sulfate may contain one or both of a hydrate and an anhydrate, and it is preferable that sodium sulfate decahydrate is 0 to 40% by mass.

[0021] The quick-setting admixture for blast furnace cement according to the present embodiment contains 0.1 to 10% by mass of aluminum sulfate. If the content of aluminum sulfate is less than 0.1% by mass, the short-term strength development and quick-setting property may not be exhibited, and if it exceeds 10% by mass, the generation of hydrogen sulfide gas may not be suppressed. The aluminum sulfate is preferably in the form of a powder, more preferably a 14 to 18 hydrate, and further preferably less than 50% of the particles have a particle size of 150 μm or less. The content of aluminum sulfate is preferably 1 to 8% by mass, and more preferably 2 to 5% by mass. If the content of aluminum sulfate is within the above range, it is easy to improve the short-term strength development and quick-setting property, and easy to suppress the generation of hydrogen sulfide gas.

[0022] The blast furnace cement quick-setting admixture may contain slaked lime. The content of slaked lime is not particularly limited, but is preferably 1 to 30 mass%, and more preferably 3 to 15 mass%. When the content of slaked lime is within the above range, adhesion is improved, making it easier to suppress rebound.

[0023] The quick-setting admixture for blast furnace cement may further contain an alkali metal salt other than the sodium sulfate. The alkali metal salt may include silicates such as sodium silicate and potassium silicate, and carbonates such as sodium carbonate and potassium carbonate. The content of the alkali metal salt is not particularly limited, but is preferably 0.1 to 15 mass%, more preferably 0.3 to 10 mass%, from the viewpoint of long-term strength development and adhesion properties.

[0024] The quick-setting admixture for blast furnace cement may further contain an alkaline earth metal salt. The alkaline earth metal salt may include carbonates such as calcium carbonate, and sulfates such as calcium sulfate. The content of the alkaline earth metal salt is not particularly limited, but is preferably 3 to 50 mass%, more preferably 5 to 30 mass%, from the viewpoint of long-term strength development and adhesion properties.

[0025] [Spraying material] The spraying material according to the present embodiment contains the quick-setting admixture for blast-furnace cement of the present invention and blast-furnace cement. By containing the quick-setting admixture for blast-furnace cement and blast-furnace cement, the spraying material has excellent short-term strength development and quick-setting properties and can suppress the generation of hydrogen sulfide gas.

[0026] The content of the quick-setting admixture for blast-furnace cement in the spraying material is preferably 3 to 20 parts by mass, and more preferably 5 to 15 parts by mass, per 100 parts by mass of blast-furnace cement. When the content of the quick-setting admixture for blast-furnace cement is within the above range, it is easy to achieve excellent short-term strength development and quick setting properties, and it is easy to suppress the generation of hydrogen sulfide gas.

[0027] The amount of blast furnace slag in the blast furnace cement is preferably 30 to 90 mass%, more preferably 40 to 70 mass%. When the amount of blast furnace slag is within the above range, it is easy to suppress the generation of hydrogen sulfide gas and the elution of hexavalent chromium.

[0028] [Shocked concrete] The sprayed concrete according to the present embodiment contains the sprayed material of the present invention. The sprayed concrete can be obtained by mixing the sprayed material with water and spraying the mixture, and has excellent short-term strength development and quick-setting properties and can suppress the generation of hydrogen sulfide gas.

[0029] The content of the sprayed material in the shotcrete is preferably 10 to 30 mass%, more preferably 15 to 25 mass%. When the content of the sprayed material is within the above range, it is easy to achieve excellent short-term strength development and quick setting properties, and it is easy to suppress the generation of hydrogen sulfide gas.

[0030] The water-cement ratio of the sprayed concrete is preferably 30 to 70%, more preferably 40 to 60%, based on the blast furnace cement in the sprayed material. By having the water-cement ratio within the above range, it is easy to achieve excellent short-term strength development and quick setting, and it is easy to suppress the generation of hydrogen sulfide gas.

[0031] In practice, sprayed concrete uses aggregate, but the aggregate is not particularly limited, and preferably has low water absorption and high aggregate strength. The maximum size of the aggregate is not particularly limited as long as it can be sprayed. River sand, mountain sand, sea sand, lime sand, and silica sand can be used as fine aggregate, and river gravel, mountain gravel, and lime gravel can be used as coarse aggregate, and crushed sand and crushed stone can also be used.

[0032] The content of aggregate in the shotcrete is preferably 60 to 80 mass %, and more preferably 65 to 75 mass %. EXAMPLES

[0033] The present invention will be described in more detail below using examples and comparative examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.

[0034] [Experimental Example 1] <Preparation of Accelerator for Blast-furnace Slag Cement> The materials shown below were mixed in the ratios shown in Table 1 to prepare an accelerator for blast-furnace slag cement.

[0035] <Materials used> Calcium aluminate: Amorphous calcium aluminate melted and quenched in an electric furnace to have a CaO / Al2O3 molar ratio of 2.3. Vitrification rate 97% (measured by powder X-ray diffraction), Blaine value 5,800 cm 2 / g, amorphous. Sodium sulfate: anhydrous, 98% purity, industrial raw material. Aluminum sulfate: 14-18 hydrate, powder, industrial raw material. Slaked lime: purity 95%, Blaine value 5,000 cm 2 / g. Alkali metal salts: Sodium carbonate, powder, Blaine value 1,100 cm 2 / g. Alkaline earth metal salts: Anhydrous gypsum by-product, powder, Blaine value 4,500 cm 2 / g.

[0036] <Preparation of spraying materials> 400 g of ordinary Portland cement (manufactured by Denka Co., Ltd.) and 400 g of ground blast furnace slag (manufactured by Esment Kanto Co., Ltd.: product name Esment 4000) were mixed to prepare blast furnace cement (blast furnace slag content 50% by mass), and 2,000 g of fine aggregate (river sand from the Hime River system in Niigata Prefecture) and water to a water-cement ratio of 50% were added and kneaded. 10 parts by mass of the prepared blast furnace cement quick-setting admixture was added per 100 parts by mass of the blast furnace cement to prepare the spraying material.

[0037] <Coagulation test> The prepared spray material was quickly sprayed onto a formwork measuring 30 cm in length, 30 cm in width, and 10 cm in depth, and the Proctor penetration resistance was measured over time from the addition of the accelerator, reaching 3.5 N / mm 2 The time when this occurs is the starting time, 28.0N / mm 2 The time when the reaction time reached the end was determined as the termination time. The results are shown in Table 1 below.

[0038] <Compressive strength test> The prepared spray material was quickly sprayed onto a triple-section formwork measuring 4 cm length x 4 cm width x 16 cm depth, and the compressive strength was measured at 10 minutes, 30 minutes, 24 hours, and 28 days after the addition of the quick-setting admixture. The results are shown in Table 1. In the present invention, the compressive strengths at 10 minutes, 30 minutes, and 24 hours are indicators of short-term strength, and the compressive strength at 28 days is an indicator of long-term strength.

[0039] <Amount of eluted hexavalent chromium> The prepared spraying material was quickly sprayed onto the formwork after preparation, and the amount of hexavalent chromium eluted from the sprayed concrete, which had an age of 3 hours depending on the time elapsed since the addition of the accelerator, was measured based on the method specified in the "Elution Test to be carried out at the Mix Design Stage, Notification No. 46 of the Environment Agency, dated August 23, 1991. The results are shown in Table 1.

[0040] <Amount of hydrogen sulfide gas generated> In a 20℃ environment, 100g of blast furnace cement and 50g of water were added to a vinyl bag measuring 340mm long x 230mm wide to prepare a cement paste, and after 1 minute, 10g of the prepared blast furnace cement accelerator was added and the bag was closed. After 10 minutes, 1mL of gas was collected from the bag and the amount of hydrogen sulfide gas was quantified using gas chromatography. The results are shown in Table 1.

[0041] [Table 1]

[0042] [Experimental Example 2] Using the blast-furnace slag cement quick-setting admixture prepared in the same manner as in Experimental Example 1, each test was carried out in the same manner as in Experimental Example 1, except that the amount added per 100 parts by mass of blast-furnace slag cement was changed. The results are shown in Table 2.

[0043] [Table 2]

[0044] [Experimental Example 3] Each test was carried out in the same manner as in Experimental Example 1, except that the blast-furnace slag content in the blast-furnace slag cement was changed by using the blast-furnace slag cement accelerator prepared in the same manner as in Experimental Example 1. The results are shown in Table 3.

[0045] [Table 3] [Industrial Applicability]

[0046] The quick-setting admixture for blast-furnace cement of the present invention can be suitably used for cement concrete to be sprayed onto exposed natural ground surfaces such as tunnels for roads, railways, and waterways, and slopes.

Claims

1. The quick-setting admixture for blast furnace cement contains 40 to 70 mass % of calcium aluminate, 3 to 25 mass % of sodium sulfate, and 0.1 to 10 mass % or less of aluminum sulfate.

2. A spraying material comprising the quick-setting admixture for blast-furnace slag cement according to claim 1 and blast-furnace slag cement.

3. The spraying material according to claim 2, wherein the blast furnace slag content in the blast furnace cement is 30 to 90 mass%.

4. A sprayed concrete comprising the spraying material according to claim 2 or 3.

Citation Information

Patent Citations

  • Wet spraying concrete

    JP2002037656A

  • Cement admixture and cement composition

    JP2010024110A

  • Quick setting admixture

    JP2019210167A

  • Rapid-hardening additive agent, and spray material

    JP2021178751A

  • Set accelerating agent for spraying, spraying material, and spraying method using the same

    WO2005123620A1