Jelly-like food
Incorporating cellulose nanofibers into jelly-like foods addresses the issue of moisture leakage by enhancing texture retention and maintaining shape after freezing and thawing.
Patent Information
- Application Number
- JP2023058863
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Jelly-like foods experience moisture leakage (syneresis) after freezing and thawing, leading to reduced elasticity and texture.
Incorporation of cellulose nanofibers, specifically anion-modified cellulose nanofibers such as carboxymethylated cellulose nanofibers, into the jelly-like food composition to enhance texture retention.
The use of cellulose nanofibers significantly reduces syneresis and maintains the shape and texture of the jelly-like food after freezing and thawing.
Smart Images

Figure 2024146135000001 
Figure 2024146135000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a jelly-like food containing cellulose nanofibers and polysaccharides. [Background technology]
[0002] Jelly foods are produced by cooling and solidifying a jelly liquid made by mixing a gelling agent such as agar or gelatin with a sol-like liquid made by mixing fruit juice, fruit pulp, and sugar solution.
[0003] Locust bean gum has a thickening effect and can improve gel strength when used in combination with other polysaccharides, and is therefore used in foods such as jellies. For example, an additive for a thickening composition used in foods such as jellies, which contains two or more types of polysaccharides such as locust bean gum and fermented cellulose, has been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-178518 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the method of Patent Document 1 had a problem that after the jelly-like food was frozen and then thawed, water seeped out of the jelly-like food (syneresis), reducing the elasticity of the jelly-like food and deteriorating the texture.
[0006] Therefore, an object of the present invention is to provide a jelly-like food that prevents loss of texture by suppressing seepage of water (syneresis) from the jelly-like food after freezing and thawing. [Means for solving the problem]
[0007] As a result of extensive research into achieving this objective, the inventors discovered that it would be effective to create a jelly-like food containing cellulose nanofibers, and thus completed the present invention.
[0008] The present invention provides the following: (1) A jelly-like food containing cellulose nanofiber and thickening polysaccharides. (2) A jelly-like food according to (1), wherein the cellulose nanofiber is anionically modified cellulose nanofiber. (3) A jelly-like food according to (1) or (2), wherein the anion-modified cellulose nanofiber is a cellulose nanofiber having a carboxyl group or a cellulose nanofiber having a carboxyalkyl group. (4) The jelly food according to (3), wherein the anion-modified cellulose nanofiber is a carboxymethylated cellulose nanofiber having a degree of carboxymethyl substitution in the range of 0.01 to 0.50. (5) A jelly-like food according to (1) or (2), further comprising carboxymethyl cellulose. (6) A jelly-like food according to (1) or (2), in which the thickening polysaccharide is one or more selected from the group consisting of carrageenan, xanthan gum, locust bean gum, guar gum, and tamarind seed gum. Effect of the Invention
[0009] According to the present invention, a jelly-like food product can be provided which exhibits reduced syneresis after freezing and thawing and has excellent shape retention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The jelly food of the present invention will be described below. In the present invention, "to" includes the extreme values. In other words, "X to Y" includes the values X and Y at both ends.
[0011] The jelly food of the present invention contains cellulose nanofibers and thickening polysaccharides. The blending ratio of the cellulose nanofibers to the thickening polysaccharides is preferably 90:10 to 10:90.
[0012] The jelly food of the present invention may contain cellulose nanofibers at any content, but it is preferable to contain them in consideration of the effective amount of cellulose nanofibers. The content of cellulose nanofibers in the jelly food is preferably 0.001 to 3 mass%. If the amount of cellulose nanofiber added is less than the lower limit of the above-mentioned amount, the effect of preventing reduction in syneresis after freezing and thawing the jelly food is insufficient.
[0013] In addition to cellulose nanofibers and thickening polysaccharides, the jelly food of the present invention may contain gelatin, fruit juice, fruit pulp, sugars (monosaccharides such as glucose and fructose, disaccharides such as maltose, sucrose and lactose, isomerized sugar, starch syrup, reduced starch syrup, sugar alcohol, honey), dairy products, flavorings, acidulants, coloring agents, etc.
[0014] (Thickening polysaccharides) Examples of the thickening polysaccharides used in the jelly food of the present invention include pectin, guar gum, locust bean gum, tamarind seed gum, psyllium seed gum, soybean polysaccharides, tara gum, gum arabic, glucomannan, xanthan gum, gellan gum, curdlan, agar, carrageenan, alginic acid, gelatin, cellulose derivatives, karaya gum, cassia gum, and pullulan, and carrageenan, xanthan gum, locust bean gum, guar gum, and tamarind seed gum are preferred, as they can impart an appropriate hardness to the jelly food. These thickening polysaccharides may be used alone or in combination of two or more. The content of the thickening polysaccharide in the jelly food is preferably 0.05 to 3% by mass. If the amount of polysaccharide added is small, the jelly food may not be able to impart an appropriate hardness. Furthermore, if the amount of the additive exceeds the upper limit, when it is added to foods such as jelly, the hardness may become too high, resulting in a deterioration in the texture.
[0015] (Cellulose nanofiber) In the present invention, cellulose nanofibers (hereinafter sometimes referred to as CNF) are fine fibers with a fiber width of about 1 to 500 nm, which are made by pulp, a cellulose-based raw material, being refined to the nanometer level. The average fiber diameter and average fiber length of cellulose nanofibers can be obtained by averaging the fiber diameters and fiber lengths obtained from the observation of each fiber using an atomic force microscope (AFM) or a transmission electron microscope (TEM). The average aspect ratio of cellulose nanofibers is usually 50 or more. There is no particular upper limit, but it is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter
[0016] Cellulose nanofibers are obtained by applying mechanical force to pulp to make it finer, and can be obtained by defibrating unmodified cellulose, or modified cellulose such as carboxylated cellulose (also called oxidized cellulose), carboxymethylated cellulose, anion-modified cellulose such as cellulose with a phosphate ester group introduced therein, or cationized cellulose. The average fiber length and average fiber diameter of the fine fibers can be adjusted by oxidation treatment and defibration treatment. In the present invention, it is preferable to use carboxymethylated (CM) cellulose nanofibers obtained by defibrating carboxymethylated cellulose obtained by carboxymethylation treatment.
[0017] (Cellulose raw material) Examples of cellulose raw materials for producing the cellulose nanofibers used in the present invention include those originating from plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp), animal materials (e.g., ascidians), algae, and microbial (e.g., acetic acid bacteria (Acetobacter)) producing organisms. Examples of pulp include softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), hardwood unbleached sulfite pulp (LUSP), hardwood bleached sulfite pulp (LBSP), softwood dissolving kraft pulp (NDKP), hardwood dissolving kraft pulp (LDKP), thermomechanical pulp (TMP), recycled pulp, waste paper pulp, etc. Although all of these can be used, cellulose fibers derived from plants or microorganisms are preferred, and cellulose fibers derived from plants are more preferred.
[0018] (Carboxymethylated cellulose nanofiber) In the present invention, carboxymethylated cellulose nanofibers (hereinafter sometimes referred to as carboxymethylated CNF) are fine fibers having a fiber width of 3 to 500 nm, which are made by pulp, a cellulose-based raw material, being refined to the nanometer level. The average fiber diameter and average fiber length of the carboxymethylated cellulose nanofibers can be obtained by averaging the fiber diameters and fiber lengths obtained from the results of observing each fiber using an atomic force microscope (AFM) or a transmission electron microscope (TEM). The average aspect ratio of the carboxymethylated cellulose nanofibers is usually 50 or more. There is no particular upper limit, but it is usually 1000 or less. The average aspect ratio can be calculated by the following formula. Aspect ratio = average fiber length / average fiber diameter
[0019] (Carboxymethylation) In the present invention, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material by a known method, or a commercially available product may be used. In either case, the degree of carboxymethyl substitution per anhydrous glucose unit of cellulose is 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose can be mentioned as follows. Cellulose is used as a starting material, and 3 to 20 times by mass of water or a lower alcohol is used as a solvent. Specifically, water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc. can be used alone or in combination of two or more. When a mixed solvent of water and a lower alcohol is used, the mixing ratio of the lower alcohol is 60 to 95% by mass. As a mercerizing agent, 0.5 to 20 times the moles of an alkali metal hydroxide per anhydrous glucose residue of the starting material, specifically sodium hydroxide or potassium hydroxide, is used. The starting material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Then, a carboxymethylating agent is added at 0.05 to 10.0 times the moles per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.
[0020] <Carboxymethylated cellulose nanofiber> The carboxymethylated cellulose nanofibers of the present invention maintain at least a part of their fibrous shape even when dispersed in water. That is, when an aqueous dispersion of the carboxymethylated cellulose nanofibers is observed under an electron microscope, a fibrous substance can be observed. Furthermore, when the carboxymethylated cellulose nanofibers are measured by X-ray diffraction, a peak of cellulose type I crystals can be observed.
[0021] <Crystallization degree of cellulose type I> The degree of crystallinity of cellulose in the carboxymethylated cellulose nanofiber used in the present invention is 50% or more for crystalline type I. When the degree of crystallinity of cellulose type I is as high as 50% or more, the proportion of cellulose that does not dissolve in a solvent such as water and maintains its crystalline structure is high, so that the thixotropy is high and it becomes suitable for viscosity adjustment applications such as thickeners. In addition, for example, but not limited to, when added to a gel-like substance (e.g., food, cosmetics, etc.), it has the advantage of being able to impart excellent shape retention. The crystallinity of cellulose can be controlled by the concentration of the mercerizing agent, the temperature during treatment, and the degree of carboxymethylation. Since a high concentration of alkali is used in mercerization and carboxymethylation, cellulose type I crystals are easily converted to type II, but the desired crystallinity can be maintained by adjusting the degree of denaturation by adjusting the amount of alkali (mercerizing agent) used. There is no particular upper limit to the degree of crystallinity of cellulose type I. In reality, it is considered that the upper limit is about 90%.
[0022] The method for measuring the crystallinity of cellulose type I of carboxymethylated cellulose nanofiber is as follows.
[0023] The sample is placed in a glass cell and measured using an X-ray diffraction measuring device (LabX XRD-6000, manufactured by Shimadzu Corporation). The degree of crystallinity is calculated using the method of Segal et al., and is calculated from the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous part at 2θ = 18.5° using the diffraction intensity of the X-ray diffraction pattern at 2θ = 10° to 30° as the baseline, according to the following formula. Xc = (I002c - Ia) / I002c x 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of the amorphous part.
[0024] The proportion of type I crystals in carboxymethylated cellulose nanofibers is usually the same as that in the carboxymethylated cellulose before it is made into nanofibers.
[0025] <Degree of carboxymethyl substitution> The carboxymethylated cellulose nanofibers used in the present invention have a degree of carboxymethyl substitution per anhydrous glucose unit of cellulose of 0.01 to 0.50. If the degree of carboxymethyl substitution exceeds 0.50, it is considered that the cellulose dissolves in water and cannot maintain its fiber shape. In consideration of the operability, the degree of substitution is preferably 0.02 to 0.50, more preferably 0.05 to 0.40, and particularly preferably 0.10 to 0.40. By introducing a carboxymethyl group into cellulose, the cellulose particles electrically repel each other, so that the cellulose can be defibrated into nanofibers. However, if the degree of carboxymethyl substitution per anhydrous glucose unit is less than 0.01, defibration becomes insufficient, and cellulose nanofibers with high transparency may not be obtained. In the conventional aqueous medium method, it was difficult to obtain carboxymethylated cellulose nanofibers having a crystallinity of cellulose I type of 60% or more when the degree of carboxymethyl substitution was in the range of 0.20 to 0.40, but the present inventors have found that it is possible to produce carboxymethylated cellulose nanofibers having a degree of carboxymethyl substitution in the range of 0.20 to 0.40 and a crystallinity of cellulose I type of 60% or more, for example, by the method described below. The degree of carboxymethyl substitution can be adjusted by controlling the amount of the carboxymethylating agent to be reacted, the amount of the mercerizing agent, the composition ratio of water to the organic solvent, etc.
[0026] In the present invention, the anhydroglucose unit means each anhydroglucose (glucose residue) constituting cellulose. The degree of carboxymethyl substitution (also called the degree of etherification) indicates the ratio of hydroxyl groups in the glucose residues constituting cellulose that are substituted with carboxymethyl ether groups (the number of carboxymethyl ether groups per glucose residue). The degree of carboxymethyl substitution may be abbreviated as DS.
[0027] The method for measuring the degree of carboxymethyl substitution is as follows: Weigh out approximately 2.0 g of the sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of a solution of 1000 mL of nitric acid methanol and 100 mL of special-grade concentrated nitric acid, and shake for 3 hours to convert the salt of carboxymethylated cellulose nanofiber (CMC) to H-CMC (hydrogen-type carboxymethylated cellulose nanofiber). Weigh out 1.5 to 2.0 g of the bone-dry H-CMC and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten the H-CMC with 15 mL of 80% methanol, add 100 mL of 0.1 N-NaOH, and shake at room temperature for 3 hours. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N-H2SO4, and calculate the degree of carboxymethyl substitution (DS value) using the following formula. A=[(100×F'-0.1N-H2SO4(mL)×F)×0.1] / (H-CMC (bone dry mass (g)) Carboxymethyl substitution degree = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N NaOH. The degree of carboxymethyl substitution in the carboxymethyl cellulose nanofibers is usually the same as the degree of carboxymethyl substitution in the carboxymethyl cellulose before being made into nanofibers.
[0028] <Fiber diameter, aspect ratio> The carboxymethyl cellulose nanofibers used in the present invention have a nanoscale fiber diameter. The average fiber diameter is preferably 3 nm to 500 nm, more preferably 3 nm to 150 nm, more preferably 3 nm to 20 nm, more preferably 5 nm to 19 nm, and even more preferably 5 nm to 15 nm.
[0029] The aspect ratio of the carboxymethylated cellulose nanofiber is not particularly limited, but is preferably 350 or less, more preferably 300 or less, more preferably 200 or less, more preferably 120 or less, more preferably 100 or less, and even more preferably 80 or less. When the aspect ratio is 350 or less, the fibers are not excessively long, and the fibers are less entangled, which reduces the generation of lumps (lumps) of cellulose nanofibers, making it suitable for use as an additive. In addition, since the fluidity is high, it is easy to use even at high concentrations, and there is an advantage that it is easy to use in applications requiring a high solid content. The lower limit of the aspect ratio is not particularly limited, but is preferably 25 or more, more preferably 30 or more. When the aspect ratio is 25 or more, the fibrous shape has an effect of improving thixotropy. The aspect ratio of the carboxymethylated cellulose nanofiber can be controlled by the mixing ratio of the solvent and water during carboxymethylation, the amount of chemicals added, and the degree of carboxymethylation, and can be produced, for example, by the production method described below.
[0030] The average fiber diameter and average fiber length of carboxymethyl cellulose nanofibers can be measured by analyzing 200 randomly selected fibers using an atomic force microscope (AFM) if the diameter is 20 nm or less, or a field emission scanning electron microscope (FE-SEM) if the diameter is 20 nm or more, and calculating the average. The aspect ratio can be calculated using the following formula. Aspect ratio = average fiber length / average fiber diameter.
[0031] (Method of producing carboxymethylated cellulose nanofiber) The carboxymethylated cellulose nanofibers used in the present invention are not particularly limited, but can be produced by defibrating carboxymethylated cellulose produced by the following method.
[0032] Carboxymethylated cellulose can generally be produced by treating cellulose with an alkali (mercerization) and then reacting the resulting mercerized cellulose (also called alkali cellulose) with a carboxymethylating agent (also called etherifying agent). Carboxymethylated cellulose capable of forming nanofibers having the above-mentioned characteristics of the present invention can be produced by carrying out mercerization (alkali treatment of cellulose) in a solvent mainly composed of water, and then carrying out carboxymethylation (also called etherification) in a mixed solvent of water and an organic solvent.
[0033] (cellulose) In the present invention, cellulose refers to a polysaccharide having a structure in which D-glucopyranose (also simply referred to as "glucose residue" or "anhydroglucose") is linked by β-1,4 bonds. Cellulose is generally classified into natural cellulose, regenerated cellulose, fine cellulose, microcrystalline cellulose excluding non-crystalline regions, etc., based on the origin, manufacturing method, etc. In the present invention, any of these celluloses can be used as a raw material for mercerized cellulose, but in order to maintain a crystallinity of cellulose type I of preferably 40% or more in carboxymethylated cellulose nanofibers, it is preferable to use cellulose with a high crystallinity of cellulose type I as the raw material. The crystallinity of cellulose type I of the raw material cellulose is preferably 70% or more, more preferably 80% or more. The method for measuring the crystallinity of cellulose type I is as described above.
[0034] Examples of natural cellulose include bleached pulp or unbleached pulp (bleached wood pulp or unbleached wood pulp), linters, refined linters, and cellulose produced by microorganisms such as acetic acid bacteria. The raw material for bleached pulp or unbleached pulp is not particularly limited, and examples thereof include wood, cotton, straw, bamboo, hemp, jute, kenaf, etc. The method for producing bleached pulp or unbleached pulp is also not particularly limited, and may be a mechanical method, a chemical method, or a method that is an intermediate combination of the two. Examples of bleached or unbleached pulp classified according to the production method include mechanical pulp (thermomechanical pulp (TMP), groundwood pulp), chemical pulp (sulfite pulp such as softwood unbleached sulfite pulp (NUSP) and softwood bleached sulfite pulp (NBSP), and kraft pulp such as softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), and hardwood bleached kraft pulp (LBKP)). Furthermore, in addition to papermaking pulp, dissolving pulp may be used. Dissolving pulp is chemically refined pulp that is mainly used by dissolving it in chemicals, and is the main raw material for artificial fibers, cellophane, etc.
[0035] Examples of regenerated cellulose include cellulose dissolved in some solvent such as cuprammonium solution, cellulose xanthate solution, or morpholine derivative, and then spun again.
[0036] Examples of fine cellulose include those obtained by subjecting cellulosic materials, including the above-mentioned natural cellulose and regenerated cellulose, to depolymerization treatment (e.g., acid hydrolysis, alkaline hydrolysis, enzymatic decomposition, explosive crushing treatment, vibrating ball mill treatment, etc.), and those obtained by mechanically treating the above-mentioned cellulosic materials.
[0037] (Mercerization) Mercerized cellulose (also called alkali cellulose) is obtained by using the above-mentioned cellulose as a raw material and adding a mercerizing agent (alkali).
[0038] A solvent that mainly uses water (a solvent mainly made of water) refers to a solvent that contains water at a ratio of more than 50% by mass. The water content in the solvent mainly made of water is preferably 55% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. A particularly preferred solvent mainly made of water is 100% by mass (i.e., water).
[0039] Examples of the solvent other than water (used in a mixture with water) in the solvent mainly made of water include organic solvents used as a solvent in the subsequent carboxymethylation step. Examples include alcohols such as methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, and tertiary butanol, ketones such as acetone, diethyl ketone, and methyl ethyl ketone, as well as dioxane, diethyl ether, benzene, and dichloromethane. These can be used alone or in a mixture of two or more kinds in an amount of less than 50% by mass in water as a solvent in the mercerization step. The organic solvent in the solvent mainly made of water is preferably 45% by mass or less, more preferably 40% by mass or less, more preferably 30% by mass or less, more preferably 20% by mass or less, more preferably 10% by mass or less, more preferably 5% by mass or less, and more preferably 0% by mass.
[0040] Examples of the mercerizing agent include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, and any one or more of these can be used in combination. The mercerizing agent is not limited to these, but these alkali metal hydroxides can be added to the reactor as an aqueous solution of, for example, 1 to 60 mass %, preferably 2 to 45 mass %, and more preferably 3 to 25 mass %.
[0041] The amount of the mercerizing agent used is not particularly limited, but in one embodiment, it is preferably 0.1 mol or more and 2.5 mol or less, more preferably 0.3 mol or more and 2.0 mol or less, and even more preferably 0.4 mol or more and 1.5 mol or less, per 100 g of cellulose (bone dry).
[0042] The amount of the solvent mainly composed of water during mercerization is preferably 1.5 to 20 times by mass, and more preferably 2 to 10 times by mass, relative to the cellulose raw material. By using such an amount, stirring and mixing of the raw material becomes easy, and the reaction can be caused to occur uniformly in the raw material.
[0043] The mercerization treatment is carried out by mixing the bottom raw material (cellulose) with a solvent mainly composed of water, adjusting the temperature of the reactor to 0 to 70°C, preferably 10 to 60°C, more preferably 10 to 40°C, adding an aqueous solution of a mercerizing agent, and stirring for 15 minutes to 8 hours, preferably 30 minutes to 7 hours, more preferably 30 minutes to 3 hours, thereby obtaining mercerized cellulose (alkali cellulose).
[0044] The pH during mercerization is preferably 9 or more, which allows the mercerization reaction to proceed. The pH is more preferably 11 or more, further preferably 12 or more, and may be 13 or more. There is no particular upper limit to the pH.
[0045] The mercerization can be carried out using a reactor capable of mixing and stirring the above-mentioned components while controlling the temperature, and various reactors conventionally used for mercerization reactions can be used. For example, a batch-type stirring device having two shafts for stirring and mixing the above-mentioned components is preferred from the viewpoints of both uniform mixing ability and productivity.
[0046] (Carboxymethylation) Carboxymethylated cellulose is obtained by adding a carboxymethylating agent (also called an etherifying agent) to mercerized cellulose.
[0047] Examples of the carboxymethylating agent include monochloroacetic acid, sodium monochloroacetate, methyl monochloroacetate, ethyl monochloroacetate, isopropyl monochloroacetate, etc. Among these, monochloroacetic acid or sodium monochloroacetate is preferred in terms of availability of the raw material.
[0048] The amount of the carboxymethylating agent used is not particularly limited, but in one embodiment, it is preferably added in the range of 0.5 to 1.5 mol per anhydrous glucose unit of cellulose. The lower limit of the above range is more preferably 0.6 mol or more, even more preferably 0.7 mol or more, and the upper limit is more preferably 1.3 mol or less, even more preferably 1.1 mol or less. The carboxymethylating agent can be added to the reactor as, for example, a 5 to 80 mass % aqueous solution, more preferably 30 to 60 mass %, but is not limited thereto, or can be added in a powder state without dissolving.
[0049] The molar ratio of the mercerizing agent to the carboxymethylating agent (mercerizing agent / carboxymethylating agent) is generally 0.9 to 2.45 when monochloroacetic acid or sodium monochloroacetate is used as the carboxymethylating agent. The reason is that if it is less than 0.9, the carboxymethylation reaction may be insufficient, and unreacted monochloroacetic acid or sodium monochloroacetate may remain and be wasted, and if it exceeds 2.45, a side reaction between the excess mercerizing agent and monochloroacetic acid or sodium monochloroacetate may proceed, resulting in the production of an alkali metal glycolate, which may be uneconomical.
[0050] The concentration of the cellulose raw material in the carboxymethylation reaction is not particularly limited, but is preferably 1 to 40% (w / v).
[0051] Simultaneously with the addition of the carboxymethylating agent, or before or immediately after the addition of the carboxymethylating agent, an organic solvent or an aqueous solution of an organic solvent is appropriately added to the reactor, or the organic solvent other than water used in the mercerization treatment is appropriately reduced by reducing pressure or the like to form a mixed solvent of water and an organic solvent, and the carboxymethylation reaction is allowed to proceed in this mixed solvent of water and an organic solvent. The timing of the addition or reduction of the organic solvent may be any time between the end of the mercerization reaction and immediately after the addition of the carboxymethylating agent, and is not particularly limited, but is preferably within 30 minutes before or after the addition of the carboxymethylating agent, for example.
[0052] Examples of the organic solvent include alcohols such as methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, and tertiary butanol, ketones such as acetone, diethyl ketone, and methyl ethyl ketone, as well as dioxane, diethyl ether, benzene, and dichloromethane, and these can be used alone or in a mixture of two or more kinds as a solvent for carboxymethylation by adding them to water. Among these, monohydric alcohols having 1 to 4 carbon atoms are preferred because of their excellent compatibility with water, and monohydric alcohols having 1 to 3 carbon atoms are more preferred.
[0053] The ratio of the organic solvent in the mixed solvent during carboxymethylation is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more, based on the total of water and organic solvent. The upper limit of the ratio of the organic solvent is not limited, and may be, for example, 99% by mass or less. Considering the cost of the organic solvent to be added, it is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0054] The reaction medium for carboxymethylation (a mixed solvent of water and an organic solvent, etc., not containing cellulose) preferably has a lower proportion of water (in other words, a higher proportion of organic solvent) than the reaction medium for mercerization. By satisfying this range, it becomes easier to increase the degree of carboxymethyl substitution while maintaining the crystallinity of the resulting carboxymethylated cellulose. In addition, when the reaction medium for carboxymethylation has a lower proportion of water (a higher proportion of organic solvent) than the reaction medium for mercerization, there is also an advantage that when transferring from the mercerization reaction to the carboxymethylation reaction, a mixed solvent for the carboxymethylation reaction can be formed by the simple means of adding a desired amount of organic solvent to the reaction system after the mercerization reaction is completed.
[0055] A mixed solvent of water and an organic solvent is prepared, and a carboxymethylating agent is added to the mercerized cellulose, followed by stirring for 15 minutes to 4 hours, preferably 15 minutes to 1 hour, while maintaining a constant temperature, preferably in the range of 10 to 40°C. The liquid containing the mercerized cellulose and the carboxymethylating agent are preferably mixed in several batches or by dropwise addition, in order to prevent the reaction mixture from becoming too hot. After adding the carboxymethylating agent and stirring for a certain period of time, the temperature is raised if necessary to a reaction temperature of 30 to 90°C, preferably 40 to 90°C, more preferably 60 to 80°C, and an etherification (carboxymethylation) reaction is carried out for 30 minutes to 10 hours, preferably 1 hour to 4 hours, to obtain carboxymethylated cellulose.
[0056] In the carboxymethylation, the reactor used in the mercerization may be used as it is, or a separate reactor capable of mixing and stirring the above-mentioned components while controlling the temperature may be used.
[0057] After the reaction is completed, the remaining alkali metal salt may be neutralized with a mineral acid or an organic acid. If necessary, by-products such as inorganic salts and organic acid salts may be removed by washing with aqueous methanol, and then dried, pulverized, and classified to obtain carboxymethylated cellulose or a salt thereof. When washing to remove by-products, the cellulose may be converted to an acid form before washing, and then converted back to a salt form after washing. Examples of devices used in dry grinding include impact mills such as hammer mills and pin mills, media mills such as ball mills and tower mills, and jet mills. Examples of devices used in wet grinding include homogenizers, mass colloiders, pearl mills, and other devices.
[0058] (Defibrillation into nanofibers) The carboxymethylated cellulose obtained by the above method can be defibrated to convert it into cellulose nanofibers having nanoscale fiber diameters.
[0059] For defibration, a dispersion of the carboxymethylated cellulose obtained by the above method is prepared. The dispersion medium is preferably water for ease of handling. The concentration of carboxymethylated cellulose in the dispersion at the time of defibration is preferably 0.01 to 10% (w / v) in consideration of the efficiency of defibration and dispersion.
[0060] The device used for defibrating carboxymethylated cellulose is not particularly limited, but devices such as high-speed rotation, colloid mill, high-pressure, roll mill, and ultrasonic devices can be used. When defibrating, it is preferable to apply a strong shear force to the dispersion of carboxymethylated cellulose. In particular, for efficient defibration, it is preferable to apply a pressure of 50 MPa or more to the dispersion and to use a wet high-pressure or ultra-high-pressure homogenizer that can apply a strong shear force. The pressure is more preferably 100 MPa or more, and even more preferably 140 MPa or more. Furthermore, prior to defibration and dispersion treatment with the high-pressure homogenizer, the dispersion may be subjected to a pretreatment, if necessary, using a known mixing, stirring, emulsifying, and dispersing device such as a high-speed shear mixer.
[0061] A high-pressure homogenizer is a device that emulsifies, disperses, breaks down, pulverizes, and ultra-finely disperses a fluid by pressurizing it (high pressure) with a pump and ejecting it from extremely fine gaps in the flow path, using a total energy of collisions between particles and shear forces caused by pressure differences.
[0062] In the present invention, the carboxymethylated cellulose nanofibers may be used in the form of a dispersion, or may be used as a powder after drying (removal of the dispersion medium), pulverization, and classification.
[0063] When the carboxymethylated cellulose nanofibers used in the present invention are used as a powder, they may contain other components as necessary. For example, when producing the powder, it is necessary to make a water-soluble polymer coexist with the dispersion of carboxymethylated cellulose nanofibers before drying, which improves redispersibility. The reason why the water-soluble polymer improves redispersibility is not clear, but it is speculated that the water-soluble polymer covers the low charge density parts of the surface of the carboxymethylated cellulose nanofibers, suppresses the formation of hydrogen bonds, and prevents the nanofibers from agglomerating together during drying.
[0064] (Water-soluble polymer) Examples of the water-soluble polymers used in the present invention include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xyloglucan, dextrin, dextran, gum arabic, gellan gum, alginic acid, alginates, pullulan, modified starches (cationized starch, phosphorylated starch, phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, hydroxypropyl starch, hydroxypropylated phosphate cross-linked starch, acetylated adipic acid cross-linked starch, acetylated phosphate cross-linked starch, acetylated oxidized starch, sodium octenylsuccinate starch, starch acetate, oxidized starch), corn starch, polydextrose, etc. Examples of the water-soluble polymers include cellulose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acid, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agents, petroleum resin-based sizing agents, urea resins, melamine resins, epoxy resins, polyamide resins, polyamide-polyamine resins, polyethyleneimine, polyamines, vegetable gums, polyethylene oxide, hydrophilic crosslinked polymers, polyacrylates, polyacrylic acid copolymers, and colloidal silica, as well as mixtures of one or more thereof. In particular, when carboxymethylated cellulose nanofibers are used as powders, it is desirable to have these water-soluble polymers coexist during the production of the powders. Among these, cellulose derivatives are preferred in terms of affinity with carboxymethylated cellulose nanofibers, and carboxymethylcellulose and its salts are particularly preferred. It is believed that water-soluble polymers such as carboxymethyl cellulose and its salts penetrate between the carboxymethylated cellulose nanofibers and increase the distance between the nanofibers, thereby improving redispersibility.
[0065] When carboxymethylcellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use carboxymethylcellulose with a degree of carboxymethyl group substitution per anhydrous glucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. In addition, a molecule with a long length (high viscosity) is preferable because it has a high effect of widening the distance between nanofibers. In addition, the B-type viscosity of a 1% by mass aqueous solution of carboxymethylcellulose at 25°C and 60 rpm is preferably 3 mPa·s to 14000 mPa·s, more preferably 7 mPa·s to 14000 mPa·s, and even more preferably 1000 mPa·s to 8000 mPa·s. Note that the "carboxymethylcellulose or a salt thereof" as the water-soluble polymer referred to here is completely dissolved in water, and is therefore distinguished from the carboxymethylated cellulose nanofibers whose fiber shape can be confirmed in water.
[0066] The blending amount of the water-soluble polymer is preferably 5% by mass to 300% by mass, more preferably 20% by mass to 300% by mass, more preferably 25% by mass to 200% by mass, and even more preferably 25% by mass to 60% by mass, based on the carboxymethylated cellulose nanofiber (bone dry solid content). Blending 5% by mass or more of the water-soluble polymer can improve the redispersibility. On the other hand, if the blending amount of the water-soluble polymer exceeds 300% by mass, problems such as viscosity characteristics such as thixotropy, which is a characteristic of the carboxymethylated cellulose nanofiber, and a decrease in dispersion stability may occur. It is preferable that the blending amount of the water-soluble polymer is 25% by mass or more, since particularly excellent redispersibility can be obtained. In addition, in consideration of thixotropy, it is preferable that the blending amount is 200% by mass or less, and particularly preferably 60% by mass or less.
[0067] (Dry) A dispersion of carboxymethylated cellulose nanofibers, or a dispersion of carboxymethylated cellulose nanofibers mixed with a water-soluble polymer in some cases, is dried (to remove the dispersion medium) to obtain a dry solid material containing carboxymethylated cellulose nanofibers. In this case, it is preferable to adjust the pH of the dispersion to 9 to 11 before drying, since this improves redispersibility.
[0068] The drying method may be any known method, and is not particularly limited. For example, spray drying, squeezing, air drying, hot air drying, and vacuum drying may be used. The drying apparatus is not particularly limited, and may be a continuous tunnel drying apparatus, a band drying apparatus, a vertical drying apparatus, a vertical turbo drying apparatus, a multi-stage disk drying apparatus, an air drying apparatus, a rotary drying apparatus, an air flow drying apparatus, a spray dryer drying apparatus, a spray drying apparatus, a cylindrical drying apparatus, a drum drying apparatus, a belt drying apparatus, a screw conveyor drying apparatus, a rotary drying apparatus with a heating tube, a vibration transport drying apparatus, a batch type box drying apparatus, an air drying apparatus, a vacuum box drying apparatus, and an agitation drying apparatus, etc., which may be used alone or in combination of two or more.
[0069] Among these, the use of an apparatus for forming a thin film and drying is preferred from the viewpoint of energy efficiency, since it can uniformly supply heat energy directly to the material to be dried and can perform the drying process more efficiently and in a short time. In addition, an apparatus for forming a thin film and drying is also preferred because it can immediately recover the dried material by a simple means such as scraping off the thin film. Furthermore, it has been found that the redispersibility is further improved when the thin film is formed and then dried. Examples of an apparatus for forming a thin film and drying include a drum drying apparatus and a belt drying apparatus that form a thin film on a drum or belt using a blade or die, etc., and then dry the thin film. The thickness of the thin film when forming and drying the thin film is preferably 50 μm to 1000 μm, and more preferably 100 μm to 300 μm. If it is 50 μm or more, it is easy to scrape off after drying, and if it is 1000 μm or less, the effect of further improving the redispersibility is observed.
[0070] The residual moisture content after drying is preferably 2% by mass to 15% by mass based on the total dried product.
[0071] (Crushing) The pulverization method is not particularly limited, and a known method can be used, including a dry pulverization method in which the material is treated in a powder state and a wet pulverization method in which the material is treated in a dispersed or dissolved state in a liquid. When wet pulverization is performed, it may be performed before the above-mentioned drying.
[0072] Examples of the equipment used in the dry grinding method include, but are not limited to, a cutting mill, an impact mill, an airflow mill, and a media mill. These can be used alone or in combination, and can be used in several stages with the same model. Among these, an airflow mill is preferred. Examples of cutting mills include a mesh mill (manufactured by HORAI Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Seisakusho Co., Ltd.), a knife mill (manufactured by Parman Co., Ltd.), a granulator (manufactured by Herbolt Co., Ltd.), and a rotary cutter mill (manufactured by Nara Machinery Co., Ltd.). Examples of impact mills include Pulperizer (manufactured by Hosokawa Micron Corporation), Fine Impact Mill (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Sample Mill (manufactured by Seishin Corporation), Bantam Mill (manufactured by Seishin Corporation), Atomizer (manufactured by Seishin Corporation), Tornado Mill (Nikkiso Co., Ltd.), Turbo Mill (Turbo Kogyo Co., Ltd.), Bevel Impactor (Aikawa Iron Works Co., Ltd.), etc. Examples of airflow mills include CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), jet mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), Supersonic Jet Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), etc. Examples of media mills include vibration ball mills, etc. Examples of the apparatus used in the wet grinding method include a mass colloider (manufactured by Masuko Sangyo Co., Ltd.), a high pressure homogenizer (manufactured by Sanmaru Kikai Kogyo Co., Ltd.), and a media mill. An example of the media mill is a bead mill (manufactured by Imex Co., Ltd.).
[0073] (classification) After pulverization of the carboxymethylated cellulose nanofibers, classification is performed to adjust the particle size to a specific size. The classification method is not particularly limited, but can be performed, for example, by passing the nanofibers through a mesh (sieve) having a predetermined mesh size. As the mesh, preferably 20 to 400 mesh, more preferably 40 to 300 mesh, and even more preferably 60 to 200 mesh can be used, and these may be used in a multi-stage manner. The median diameter of the powder finally obtained is 10.0 μm to 150.0 μm, preferably 30.0 μm to 130.0 μm, and even more preferably 50.0 μm to 120.0 μm.
[0074] The cellulose nanofibers used in the present invention may be in the form of a dispersion or powder, but from the viewpoint of excellent workability during the production of the resulting jelly-like food, it is preferable to use it in the form of a dispersion. EXAMPLES
[0075] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these.
[0076] (Method for measuring degree of carboxymethyl substitution) 1) Accurately weigh out approximately 2.0 g of carboxymethylated cellulose fiber (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. 2) Add 100 mL of a solution of 100 mL of special-grade concentrated nitric acid to 1000 mL of nitric acid methanol, shake for 3 hours, and convert the carboxymethyl cellulose salt (carboxymethyl cellulose) into hydrogen-type carboxymethyl cellulose. 3) Accurately weigh out 1.5 to 2.0 g of hydrogenated carboxylated cellulose (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. 4) Wet the hydrogenated carboxylated cellulose with 15 mL of 80% methanol, add 100 mL of 0.1 N NaOH, and shake at room temperature for 3 hours. 5) Back-titrate excess NaOH with 0.1N H2SO4 using phenolphthalein as an indicator. 6) The degree of carboxymethyl substitution (DS) is calculated by the following formula: A = [(100 × F'-(0.1N H2SO4) (mL) × F) × 0.1] / (bone-dry mass of hydrogenated carboxylated cellulose (g)) DS = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1 g of hydrogenated carboxymethyl cellulose (mL) F': Factor of 0.1N H2SO4 F: Factor of 0.1N NaOH
[0077] (Method of measuring average fiber diameter and aspect ratio) The average fiber diameter and average fiber length of CNF were analyzed for 200 randomly selected fibers using an atomic force microscope (AFM). The aspect ratio was calculated using the following formula: Aspect ratio = average fiber length / average fiber diameter
[0078] [Example 1] (Production of carboxymethylated cellulose nanofibers) In a 5L twin-shaft kneader with the rotation speed adjusted to 100 rpm, 1089 parts of isopropanol (IPA) and 31 parts of sodium hydroxide dissolved in 121 parts of water were added, and 200 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) were added in terms of dry mass when dried at 100 ° C for 60 minutes. The mixture was stirred and mixed at 30 ° C for 60 minutes to prepare mercerized cellulose. 117 parts of sodium monochloroacetate were further added while stirring, and after stirring at 30 ° C for 30 minutes, the mixture was heated to 70 ° C over 30 minutes and carboxymethylation reaction was carried out at 70 ° C for 60 minutes. The proportion of water in the reaction medium during the mercerization reaction and the carboxymethylation reaction was 10 mass%. After the reaction was completed, the mixture was neutralized, washed with 65% water-containing methanol, deliquored, dried, and pulverized to obtain a sodium salt of carboxymethylated cellulose with a carboxymethyl substitution degree of 0.27 and a crystallinity of cellulose I type of 64%. The methods for measuring the degree of carboxymethyl substitution and the crystallinity of cellulose type I are as described above. The obtained sodium salt of carboxymethyl cellulose was dispersed in water to obtain a 1% (w / v) aqueous dispersion. This was treated three times with a high-pressure homogenizer at 150 MPa to obtain a dispersion of carboxymethyl cellulose nanofibers. The obtained carboxymethyl cellulose nanofibers had an average fiber diameter of 3.2 nm and an aspect ratio of 40.
[0079] (Manufacturing of CNF powder) The obtained carboxymethylated cellulose nanofibers were dispersed in water to a solid content of 0.7% by mass, and carboxymethyl cellulose (manufactured by Nippon Paper Industries Co., Ltd., product name: F350HC-4, viscosity (1% by mass, 25°C, 60 rpm) approximately 3000 mPa·s, degree of carboxymethyl substitution approximately 0.90) was added at 40% by mass relative to the carboxymethyl cellulose nanofibers (i.e., so that the solid content of carboxymethyl cellulose was 40 parts by mass when the solid content of the carboxymethylated cellulose nanofibers was 100 parts by mass), and the mixture was stirred for 60 minutes with a TK homomixer (12,000 rpm). To this dispersion, 0.5% by mass of sodium hydroxide solution was added to adjust the pH to 9, and then the mixture was applied to the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) and dried at 140°C for 1 minute. The resulting dried product was scraped off and then pulverized using an impact mill at a rate of 10 kg per hour to obtain a dried pulverized product with a moisture content of 5% by mass. The pulverized product was classified using a 30 mesh to obtain a powder containing carboxymethylated cellulose nanofibers and carboxymethyl cellulose (CNF powder).
[0080] (Production of jelly-like foods) 0.15 parts of the CNF powder obtained above, 22.5 parts of fructose glucose liquid sugar (manufactured by Nihon Shokuhin Kako Co., Ltd.), 4.9 parts of granulated sugar, gelling agent preparation (a mixture of 11% locust bean gum, 9% carrageenan, 3% monopotassium phosphate, and 77% glucose, manufactured by Nitta Gelatin Co., Ltd.), and 10.6 parts of water were placed in a stainless steel beaker and stirred at 85-90 ° C and 600 rpm for 3 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.). Next, 20 parts of syrup liquid separated from canned mandarin oranges (whole fruit, large fruit, manufactured by Mitsubishi Shokuhin Co., Ltd.), 40 parts of Unshu mandarin orange juice (100% straight juice, manufactured by UCC Ueshima Coffee Co., Ltd.), and 0.1 parts of citric acid were added and stirred at 600 rpm until the temperature reached 85 ° C to prepare a jelly liquid. Next, the mandarin oranges in syrup that were previously separated were placed in a jelly container (40 g), and the above jelly liquid (110 g) was poured on top of it. The container was kept in a freezer for 24 hours to freeze, and then kept in a refrigerator for another 24 hours, after which it was thawed to obtain a jelly-like food.
[0081] [Example 2] A jelly-like food was produced in the same manner as in Example 1, except that the amount of CNF powder added was 0.2 parts and the amount of granulated sugar added was 4.8 parts. [Comparative Example 1] A jelly-like food was produced in the same manner as in Example 1, except that the amount of granulated sugar added was 5 parts and no CNF powder was added.
[0082] For the thawed jelly-like foods obtained in Examples 1 and 2 and Comparative Example 1, the amount of water syneresis was measured by the following method, and the results are shown in Table 1. In addition, the thawed jelly-like foods were subjected to a taste evaluation, and the results are shown in Table 2. Measurement of water release rate 1) Thaw the chilled jelly food completely in the refrigerator. 2) Place a tea strainer over the beaker and pour the thawed jelly-like food from the container into the tea strainer. 3) Leave it as it is at room temperature for 30 minutes, and then allow the water to drip into the beaker. 4) Weigh the weight of the water that falls into the beaker (average value of three samples).
[0083] [Table 1]
[0084] As shown in Table 1, the jelly foods of Examples 1 and 2, in which CNF and thickening polysaccharides were added, showed suppressed syneresis after thawing.
[0085] [Table 2]
[0086] As shown in Table 2, the jelly-like foods of Examples 1 and 2, which contained CNF and thickening polysaccharides, received high taste ratings even after thawing.
Claims
1. A jelly-like food containing cellulose nanofiber and thickening polysaccharides.
2. The jelly food according to claim 1 , wherein the cellulose nanofiber is anionically modified cellulose nanofiber.
3. 3. The jelly-like food according to claim 1 or 2, wherein the anion-modified cellulose nanofiber is a cellulose nanofiber having a carboxyl group or a cellulose nanofiber having a carboxyalkyl group.
4. The jelly food according to claim 3, wherein the anion-modified cellulose nanofiber is a carboxymethylated cellulose nanofiber having a degree of carboxymethyl substitution in the range of 0.01 to 0.
50.
5. 3. The jelly food according to claim 1 or 2, further comprising carboxymethyl cellulose.
6. 3. The jelly food according to claim 1 or 2, wherein the thickening polysaccharide is one or more selected from the group consisting of carrageenan, xanthan gum, locust bean gum, guar gum and tamarind seed gum.
Citation Information