Photosensitive resin composition, dry film, cured product, and printed wiring board

A photosensitive resin composition with silica particles from sodium silicate sol maintains high resolution and coatability by preventing aggregation, addressing the storage stability issues of small-diameter silica in existing technologies.

JP2024146161APending Publication Date: 2024-10-15TAIYO HOLDINGS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023058897
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Small-diameter silica particles in photosensitive resin compositions tend to aggregate over time, leading to defects and reduced resolution in the formed patterns, limiting the storage stability and coatability of the compositions.

Method used

A photosensitive resin composition containing silica particles derived from sodium silicate sol with an average particle diameter of 3 to 40 nm, along with specific ratios and components like carboxyl group-containing resins and photopolymerization initiators, is used to maintain high resolution and coatability even after extended storage.

Benefits of technology

The composition achieves high resolution and excellent coatability, preventing silica aggregation and maintaining film quality over time, thus ensuring stable film formation and pattern precision.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146161000001
    Figure 2024146161000001
  • Figure 2024146161000002
    Figure 2024146161000002
  • Figure 2024146161000003
    Figure 2024146161000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition that maintains high resolution even after a predetermined period has elapsed after preparation, while also exhibiting excellent coatability.SOLUTION: A photosensitive resin composition includes (A) a carboxyl group-containing resin, (B) an epoxy resin, (C) a photopolymerization initiator, and (D) silica, where the (D) silica includes particles composed of silica sol derived from sodium silicate, where the particles have an average particle size of 3-40 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition, a dry film, a cured product, and a printed wiring board. [Background technology]

[0002] In general, in a printed wiring board used in electronic devices, a solder resist layer is formed in an area other than a connection hole on a substrate on which a circuit pattern is formed, in order to prevent solder from adhering to unnecessary parts of the printed wiring board in a process such as solder reflow when mounting electronic components on the printed wiring board. The solder resist layer is mainly formed by applying a photosensitive resin composition to a substrate, drying it, exposing it to light, developing it to form a pattern, and then curing the patterned resin by heating or irradiating it with light, which is called a photo solder resist. It has also been proposed to form a solder resist layer using a photosensitive dry film without using the above-mentioned liquid photosensitive resin composition.

[0003] These photosensitive resin compositions and photosensitive dry films contain an alkali-soluble photosensitive resin component to enable exposure and development, and, if necessary, contain other photopolymerizable monomers and thermosetting components such as epoxy in consideration of heat resistance and substrate adhesion. In addition, inorganic fillers are sometimes blended into the photosensitive resin composition to reduce the linear expansion coefficient and suppress peeling of the solder resist layer and warping of the substrate (Patent Document 1, etc.). Among inorganic fillers, spherical silica in particular has excellent filling properties and a low thermal expansion coefficient, and is therefore widely used to improve the properties of solder resist.

[0004] In recent years, as electronic components are required to be smaller and have higher performance, printed wiring boards on which electronic components are mounted are also required to be smaller and more dense, and in order to manufacture highly integrated printed wiring boards, development of photosensitive resin compositions capable of forming solder resists with high resolution is underway. For example, it is known that light scattering can be effectively suppressed by dispersing silica with a maximum particle size of 1 μm or less as a filler in a photosensitive resin composition, making it possible to form fine opening patterns (Patent Document 2, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-72834 A [Patent Document 2] JP 2012-242592 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, small-diameter silica tends to aggregate over time. When small-diameter silica aggregates, it appears as particles in the photosensitive resin composition or dry film, which may cause defects when the film is coated. In addition, even if small-diameter silica is used, the resolution may be reduced due to silica aggregation. Therefore, when small-diameter silica is dispersed in the photosensitive resin composition to ensure high resolution, it cannot be stored for a long period of time, and it is necessary to coat and form a pattern quickly.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a photosensitive resin composition that has high resolution and excellent coatability even after a required period of time has passed since its preparation. [Means for solving the problem]

[0008] The present inventors have conducted research into the above-mentioned problems, and have found that if the silica fine particles are made of a specific silica sol, a photosensitive resin composition having high resolution and excellent coatability can be obtained even after a required period of time has passed since the preparation of the photosensitive resin composition. The present invention is based on this finding. That is, the gist of the present invention is as follows.

[0009] [1] A photosensitive resin composition comprising: (A) a carboxyl group-containing resin; (B) an epoxy resin; (C) a photopolymerization initiator; and (D) silica, The photosensitive resin composition, wherein the (D) silica contains particles made of a silica sol derived from sodium silicate, and the average particle size of the particles is 3 to 40 nm. [2] The photosensitive resin composition according to [1], wherein the (D) silica is contained in an amount of 5 to 70% by mass based on the total solid content of the photosensitive resin composition. [3] The photosensitive resin composition according to [1], further comprising a thermosetting catalyst. [4] A dry film comprising a first film and a resin layer formed by applying the photosensitive resin composition according to [1] to one side of the first film and drying the composition. [5] A cured product obtained by curing the photosensitive resin composition according to [1] or the resin layer of the dry film according to [4]. [6] A printed wiring board having a coating made of the cured product described in [5]. Effect of the Invention

[0010] The photosensitive resin composition of the present invention has high resolution and excellent coatability even after a required period of time has elapsed since its preparation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, any numerical range expressed using "~" is intended to include both ends of the range.

[0012] [Photosensitive resin composition] The photosensitive resin composition of the present invention contains (A) a carboxyl group-containing resin, (B) an epoxy resin, (C) a photopolymerization initiator, and (D) silica. Each component constituting the photosensitive resin composition will be described below.

[0013] <(A) Carboxyl group-containing resin> As the (A) carboxyl group-containing resin contained in the photosensitive resin composition according to the present invention, various conventionally known carboxyl group-containing resins having a carboxyl group in the molecule can be used. In particular, a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is preferred from the viewpoint of photocurability and development resistance. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. When using only a carboxyl group-containing resin without an ethylenically unsaturated double bond, it is necessary to use a compound having a plurality of ethylenically unsaturated groups in the molecule, i.e., a photopolymerizable monomer, which will be described later, in combination in order to make the composition photocurable. The (A) carboxyl group-containing resin may be used alone or in combination of two or more kinds.

[0014] Specific examples of the (A) carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers): In this specification, (meth)acrylate is a general term for acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0015] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.

[0016] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0017] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.

[0018] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).

[0019] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).

[0020] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.

[0021] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0022] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0023] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.

[0024] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0025] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0026] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).

[0027] The carboxyl group-containing resins are not limited to those listed above, and may be used alone or in combination. Among the above, the carboxyl group-containing resins synthesized using a compound having a phenolic hydroxyl group as a starting material, such as the carboxyl group-containing resins (10) and (11), are preferably used because of their excellent HAST resistance and PCT resistance.

[0028] The acid value of the (A) carboxyl group-containing resin is preferably 40 to 150 mgKOH / g. By making the (A) carboxyl group-containing resin have an acid value of 40 mgKOH / g or more, alkaline development becomes good. Also, by making the acid value 150 mgKOH / g or less, it becomes easy to draw a good resist pattern. More preferably, it is 50 to 130 mgKOH / g.

[0029] The weight average molecular weight of the (A) carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. By making the weight average molecular weight 2,000 or more, it is possible to improve tack-free performance and resolution. Furthermore, by making the weight average molecular weight 150,000 or less, it is possible to improve developability and storage stability. It is more preferably 5,000 to 15,000. The weight average molecular weight can be measured by gel permeation chromatography (GPC).

[0030] The amount of the (A) carboxyl group-containing resin in the photosensitive resin composition is preferably 10 to 50 mass % in terms of solid content. By making it 10 mass % or more, the coating strength can be improved. Also, by making it 50 mass % or less, the viscosity becomes appropriate and the printability is improved. More preferably, it is 10 to 40 mass %.

[0031] <(B) Epoxy resin> The photosensitive resin composition of the present invention contains (B) an epoxy resin.

[0032] Examples of the (B) epoxy resin include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like. These may be used alone or in combination of two or more.

[0033] (B) Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.

[0034] The equivalent weight of the epoxy group of the epoxy resin (B) in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to the equivalent weight of the carboxyl group of the carboxyl group-containing resin (A) of 1. By making it 0.5 equivalent weight or more, it is possible to prevent the carboxyl group from remaining in the cured product, and to obtain good heat resistance, alkali resistance, electrical insulation, etc. Also, by making the blending amount 2.5 equivalent weight or less, it is possible to prevent the low molecular weight cyclic (thio)ether group from remaining in the dried coating film, and to ensure good strength of the cured product, etc.

[0035] The photosensitive resin composition of the present invention may contain a thermosetting component other than the epoxy resin, as long as the effect of the present invention is not impaired. Examples of the thermosetting component include known and commonly used ones such as an isocyanate compound, a blocked isocyanate compound, an amino resin, a maleimide compound, a benzoxazine resin, a carbodiimide resin, a cyclocarbonate compound, an oxetane compound, and an episulfide resin.

[0036] <(C) Photopolymerization initiator> The photosensitive resin composition of the present invention contains (C) a photopolymerization initiator in order to photopolymerize the above-mentioned (A) carboxyl group-containing resin and the photopolymerizable monomer described below. As the photopolymerization initiator, a known one can be used, for example, an α-aminoacetophenone-based photopolymerization initiator such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morphonyl)phenyl]-1-butanone, or N,N-dimethylaminoacetophenone: 1-hydroxy-cyclohexylphenyl Ketones, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one and other hydroxyacetophenone-based photoinitiators; bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethyl phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylphenylphosphine oxide, acylphosphine oxide photopolymerization initiators such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphine acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphine acid isopropyl ester, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide;Benzoin-based photopolymerization initiators such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ether-based photopolymerization initiators; benzophenone-based photopolymerization initiators such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; acetophenone, 2,2-dimethoxy-2-phenylacetophenone acetophenone-based photopolymerization initiators such as 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanol; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chlorothioxanthone, and chlorothioxanthone; Anthraquinone-based photopolymerization initiators such as chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal-based photopolymerization initiators such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid ester-based photopolymerization initiators such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenyl)anthraquinone ... oxime ester photoinitiators such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium;These photopolymerization initiators may be used alone or in combination of two or more.

[0037] Commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad 819 manufactured by IGM Resins. Commercially available titanocene photopolymerization initiators include JMT-784 manufactured by Yueyang Kimoutain Sci-Tech Co., Ltd. and GR-FMT manufactured by Hubei Kimoutain Sci-Tech Co., Ltd.

[0038] In addition, a photopolymerization initiator having two oxime ester groups in the molecule can also be suitably used, and specific examples thereof include oxime ester compounds having a carbazole structure represented by the following general formula (I). [ka]

[0039] In the above formula, X represents a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), a naphthyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), and Y and Z each represent a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, Ar represents an alkylene having 1 to 10 carbon atoms, vinylene, phenylene, biphenylene, pyridylene, naphthylene, thiophene, anthrylene, thienylene, furylene, 2,5-pyrrole-diyl, 4,4'-stilbene-diyl, or 4,2'-styrene-diyl, and n is an integer of 0 or 1.

[0040] In particular, an oxime ester photopolymerization initiator in which, in the above formula, X1 and Y1 are respectively a methyl group or an ethyl group, Z is methyl or phenyl, n is 0, and Ar is phenylene, naphthylene, thiophene, or thienylene is preferred.

[0041] In addition to the above-mentioned photopolymerization initiators, benzoin compounds, acetophenone compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, xanthone compounds, and the like can be used as photopolymerization initiators. However, it is preferable to use these compounds as a photopolymerization initiation aid or a sensitizer in combination with the above-mentioned photopolymerization initiators rather than using them alone as a photopolymerization initiator. Among the above, from the viewpoint of deep section curing, thioxanthone compounds and tertiary amine compounds are preferred, and thioxanthone compounds are more preferred. Furthermore, two or more of the above compounds may be used in combination.

[0042] The amount of the photopolymerization initiator (C) in the photosensitive resin composition is preferably 1 to 50 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A) in terms of solid content, which can improve the curability in deep areas.

[0043] When the photosensitive resin composition contains the benzoin compound or the like as a photopolymerization initiator, the amount of the benzoin compound or the like is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin (A) in terms of solid content, which can improve the curability of the deeper portion.

[0044] <(D) Silica> The photosensitive resin composition of the present invention contains particles of silica sol derived from sodium silicate as (D) silica. The silica sol is obtained by neutralizing or ion-exchanging sodium silicate (Na2SiO3, also called "water glass") as a raw material. In the present invention, particles of the specific silica sol described above and having an average particle size of 3 to 40 nm are used. The average particle size of the particles is preferably 10 to 30 nm.

[0045] In the present invention, the average particle size of silica is the average particle size (D50) including not only the particle size of primary particles but also the particle size of secondary particles (aggregates), and can be determined by a laser diffraction particle size distribution measuring device and a measuring device by dynamic light scattering. For example, as a measuring device by laser diffraction, Microtrac MT3300EXII (measurement range: 0.02 to 2,000 μm) manufactured by Microtrac-Bell may be used, and when it is below the measurement range, Nanotrac Wave II UT151 (measurement range: 0.8 to 6,500 nm) manufactured by Microtrac-Bell may be used as a measuring device by dynamic light scattering.

[0046] In this way, by using particles having an average particle diameter of 3 to 40 nm made of a specific silica sol as silica, a photosensitive resin composition having high resolution and excellent coatability can be obtained even after a required period of time has passed since the preparation of the photosensitive resin composition (in other words, a photosensitive resin composition having excellent storage stability can be obtained). The reason for this is unclear, but it can be inferred as follows. That is, from the viewpoint of improving the resolution of the formed coating film, it is preferable to add small-diameter silica having an average particle diameter of 40 nm or less. However, as described above, if small-diameter silica is present in the photosensitive resin composition, the small-diameter silica will aggregate in the photosensitive resin composition and appear as particles in the photosensitive resin composition or in the dry film, which may cause defects when the film is coated, thereby deteriorating the coatability. In the present invention, by using particles made of silica sol derived from sodium silicate, aggregation in the photosensitive resin composition can be suppressed for a long period of time even for silica having an average particle diameter of 40 nm or less, so that a photosensitive resin composition having high resolution and excellent coatability can be obtained. This is because conventional silica particles using silica sol derived from silicon alkoxide contain organic groups in the raw material, and therefore require heating to burn off the organic groups, whereas the silica sol derived from sodium silicate as described above does not contain organic groups. It is presumed that the difference in the manufacturing process affects the aggregation of silica fine particles in the photosensitive resin composition.

[0047] The method for producing the above-mentioned particles made of silica sol is not particularly limited, but as an example, a sodium silicate aqueous solution (also called water glass) is prepared using sodium silicate as a raw material, and colloidal silica is obtained by adding an acid to the sodium silicate aqueous solution, and the colloidal silica is treated with an ion exchange resin, and then a base is added to adjust the pH to obtain silica sol. The average particle size of the particles made of silica sol can be adjusted by the concentration of the aqueous solution when preparing the colloidal silica. Specifically, particles made of silica sol having a desired average particle size can be obtained by a known method such as that described in JP-A-06-16414.

[0048] The particles made of silica sol derived from sodium silicate are preferably surface-treated. Here, the surface treatment refers to a treatment for improving compatibility with a resin component. In addition, a surface treatment capable of introducing a curable reactive group into the surface of silica may be performed. Here, the curable reactive group is not particularly limited as long as it is a group that undergoes a curing reaction with a curable compound such as (A) a carboxyl group-containing resin or (B) an epoxy resin, and may be a photocurable reactive group or a thermosetting reactive group. Examples of the photocurable reactive group include a methacryl group, an acrylic group, a vinyl group, and a styryl group, and examples of the thermosetting reactive group include an epoxy group, an amino group, a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. The method of introducing a curable reactive group into the surface of silica is not particularly limited, and it can be introduced using a known and commonly used method, and the surface of silica can be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group. As the coupling agent, a silane coupling agent, a titanium coupling agent, a zirconium coupling agent, an aluminum coupling agent, etc. can be used. In addition, as the surface-treated silica that does not have a curable reactive group, for example, silica-alumina surface treatment, titanate-based coupling agent treatment, aluminate-based coupling agent treatment, organic treatment, etc. can be mentioned.

[0049] The average particle size of the particles made of silica sol derived from sodium silicate can be adjusted by the conditions during production. In addition, as the particles made of silica sol derived from sodium silicate, a commercially available product having an average particle size within the above range may be used as it is. Specific examples include SNOWTEX (registered trademark) manufactured by Nissan Chemical Industries, Ltd.: (product numbers) ST-XS, ST-S, ST-30, ST-50-T, ST-UP, ST-PS-S, ST-PS-M, ST-OXS, ST-OS, ST-O, ST-O-40, ST-OUP, ST-PS-SO, ST-PS-MO, ST-NXS, ST-NS, ST-N, ST-N-40, ST-CXS, ST-C, ST-CM, ST-AK; and Organosilica sol manufactured by Nissan Chemical Industries, Ltd.: (product numbers) MA-ST-M, IPA- ST, IPA-ST-UP, NPC-ST-30, PGM-ST, PGM-ST-UP, DMAC-ST, NMP-ST, MEK-ST-40, MEK-ST-UP, MIBK-ST, CHO-ST-M, EAC-ST, PMA-ST, TOL -ST, MEK-AC-2140Z, PGM-AC-2140Y, PGM-AC-3140Y, MIBK-AC-2140Z, MEK-EC-2130Y, MEK-EC-2430Z, EP-M2130Y, EP-M2230Y, etc.

[0050] The particles made of silica sol derived from sodium silicate may be blended in a slurry state, which facilitates high dispersion and prevents aggregation, making it easy to handle as silica having an average particle size in the above-mentioned specific range.

[0051] The particles made of silica sol derived from sodium silicate may be used alone or in combination of two or more kinds.

[0052] The photosensitive resin composition of the present invention may contain, as the (D) silica, other silica than the particles made of silica sol derived from the above-mentioned sodium silicate, as long as the effect of the present invention is not impaired. Examples of other silica include fused silica, spherical silica, amorphous silica, crystalline silica, etc., and among them, spherical silica is preferred. The method for producing other silica is not particularly limited, but the sol-gel method is preferred because it can produce silica with a small average particle size.

[0053] The blending amount of (D) silica is preferably 5 to 70 mass % based on the total solid content of the photosensitive resin composition, more preferably 7 to 60 mass %, and further preferably 10 to 50 mass %. When the blending amount of (D) silica is within the above range, the resolution becomes better.

[0054] <Thermosetting catalyst> The photosensitive resin composition of the present invention may contain a heat curing catalyst for promoting the curing of the epoxy resin (B) and other heat curing components. Examples of the heat curing catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (trade name of dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.

[0055] The compounds are not limited to the above, and any compound that promotes the reaction between the epoxy group of the epoxy resin (B) and the carboxyl group of the carboxyl group-containing resin (A) may be used alone or in combination of two or more. In addition, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct may also be used, and preferably, these compounds that also function as adhesion-imparting agents may be used in combination with the heat curing catalyst.

[0056] The thermosetting catalyst may be used alone or in combination of two or more. From the viewpoint of the storage stability of the photosensitive resin composition and the heat resistance of the cured coating, the amount of the thermosetting catalyst is preferably 0.01 to 30 parts by mass, and more preferably 0.1 to 20 parts by mass, calculated as solid content per 100 parts by mass of the carboxyl group-containing resin (A).

[0057] <Inorganic filler> The photosensitive resin composition of the present invention may contain other inorganic fillers as fillers other than the above-mentioned (D) silica, within the scope of not impairing the effects of the present invention. As the inorganic filler, known ones can be used, and examples thereof include talc, mica, aluminum oxide, calcium oxide, magnesium oxide, zinc oxide, calcium carbonate, magnesium carbonate, fly ash, dewatered sludge, kaolin, clay, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, aluminum silicate, magnesium silicate, calcium silicate, wollastonite, potassium titanate, magnesium sulfate, calcium sulfate, magnesium phosphate, sepiolite, zonolite, boron nitride, aluminum borate, silica balloon, glass flake, glass balloon, iron slag, copper, iron, iron oxide, sendust, alnico magnet, various ferrites and other magnetic powders, cement, glass powder, Neuburg diatomaceous earth, diatomaceous earth, antimony trioxide, magnesium oxysulfate, aluminum hydrate, hydrated gypsum, alum, and barium sulfate. These inorganic fillers may be used alone or in combination of two or more. (D) Inorganic fillers other than silica may also be surface-treated like silica.

[0058] The inorganic filler other than silica (D) preferably has an average particle size (D50) of 0.1 to 700 nm, more preferably 0.1 to 400 nm, from the viewpoint of dispersibility, etc. The average particle size has the same definition as above.

[0059] The blending amount of the inorganic filler other than (D) silica in the photosensitive resin composition can be appropriately adjusted in relation to the blending amount of (D) silica, but is usually adjusted to be within the range of 0 to 20 mass %.

[0060] <Photopolymerizable monomer> The photosensitive resin composition of the present invention may contain a photopolymerizable monomer. The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric alcohols such as polyhydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; glycidyl ether acrylates such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and acrylates obtained by directly acrylate or urethane acrylate of polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadiene, and polyester polyols, as well as melamine acrylates and at least one of the methacrylates corresponding to the acrylates, can be appropriately selected and used. Such photopolymerizable monomers can also be used as reactive diluents.

[0061] The photopolymerizable monomer may be used alone or in combination of two or more. The amount of the photopolymerizable monomer is preferably 0.5 to 50 parts by mass, calculated as solid content, per 100 parts by mass of the (A) carboxyl group-containing resin. When the amount is 0.5 parts by mass or more, the photocurability is good, and pattern formation is easy in alkaline development after irradiation with active energy rays. When the amount is 50 parts by mass or less, halation is unlikely to occur and good resolution can be obtained.

[0062] <Other ingredients> In addition to the above-mentioned components, the photosensitive resin composition according to the present invention may contain, if necessary, components such as colorants, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.

[0063] The photosensitive resin composition of the present invention may contain an organic solvent from the viewpoints of ease of preparation and coatability. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents can be used alone or in combination of two or more.

[0064] The amount of the organic solvent in the photosensitive resin composition can be appropriately changed depending on the materials constituting the photosensitive resin composition, and can be, for example, 30 to 300 parts by mass in terms of solid content per 100 parts by mass of the (A) carboxyl group-containing resin.

[0065] The photosensitive resin composition of the present invention may be used in the form of a dry film or in the form of a liquid. When used in the form of a liquid, the composition may be one-component or two or more-component.

[0066] <Dry film> The photosensitive resin composition of the present invention can also be in the form of a dry film comprising a first film and a resin layer made of the photosensitive resin composition formed on the first film. The first film in the dry film according to the present invention refers to a film that is at least adhered to the resin layer when the film is laminated by heating or the like onto a substrate such as a board so that the resin layer made of the photosensitive resin composition formed on the dry film is in contact with the substrate and integrally molded. The first film may be peeled off from the resin layer in a step after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a step after exposure.

[0067] To prepare a dry film, the photosensitive resin composition of the present invention is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then coated onto a first film in a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and typically dried for 1 to 30 minutes at a temperature of 50 to 130° C. to obtain a film. There are no particular limitations on the coating film thickness, but it is generally appropriately selected within the range of 1 to 150 μm, preferably 5 to 60 μm, in terms of the film thickness after drying.

[0068] As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.

[0069] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.

[0070] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0071] After forming a resin layer of the photosensitive resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer, etc. The second film in the dry film of the present invention refers to a film that is peeled off from the resin layer before lamination when the dry film is laminated by heating or the like so that the resin layer side of the dry film is in contact with a base material such as a substrate to be integrally molded.

[0072] The second film that can be peeled off from the resin layer may be, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc., as long as the adhesive strength between the resin layer and the second film is smaller than the adhesive strength between the resin layer and the first film when the second film is peeled off.

[0073] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0074] <Cured product> The cured product of the present invention is obtained by curing the above-mentioned photosensitive resin composition or the resin layer of the above-mentioned dry film.

[0075] <Printed wiring board> The printed wiring board of the present invention has a cured product obtained from the resin layer of the photosensitive resin composition or dry film of the present invention. As a method for producing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100 ° C. to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.

[0076] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards on which circuits have already been formed using copper or the like, as well as materials such as copper-clad laminates for high-frequency circuits made from paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.

[0077] In the case of a dry film form, the lamination onto the substrate is preferably performed under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the circuit substrate is uneven, the dry film adheres to the circuit substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.

[0078] When the photosensitive resin composition of the present invention contains an organic solvent, it is preferable to apply the photosensitive resin composition to the surface of a substrate and then perform volatilization drying. The volatilization drying can be performed using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of countercurrent contact of hot air in a dryer using a heat source of an air heating method using steam, or a method of spraying the hot air from a nozzle onto the substrate).

[0079] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed portion is developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. In addition, in the case of a dry film form, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed, as long as the characteristics are not impaired. Furthermore, a cured coating excellent in various properties such as adhesion and hardness can be formed by irradiating the cured product with active energy rays and then heat curing (e.g., 100 to 220°C), or irradiating active energy rays after heat curing, or by heat curing only to perform final finish curing (main curing).

[0080] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:

[0081] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.

[0082] After the cured coating is formed on the substrate as described above, components such as electronic elements are mounted on the substrate by solder reflow treatment. The solder reflow treatment can be performed by a conventionally known method. In general, the solder reflow treatment is performed under treatment conditions of, for example, 245 to 260°C for 5 to 10 seconds.

[0083] The photosensitive resin composition or dry film of the present invention is preferably used for manufacturing electronic parts such as printed wiring boards, and more preferably used to form a permanent coating. In this case, the photosensitive resin composition or dry film of the present invention is used to form a cured product by the above-mentioned method or the like. When the resin layer of the photosensitive resin composition or dry film of the present invention is insulating, it is preferably used to form a solder resist, a coverlay, or an interlayer insulating layer. In particular, it can be preferably used for forming a permanent coating film such as a solder resist used in a package substrate. The photosensitive resin composition of the present invention may also be used to form a solder dam. EXAMPLES

[0084] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0085] <Synthesis Example 1 (Synthesis of Carboxyl Group-Containing Resin A)> Into an autoclave equipped with a thermometer, a nitrogen introduction device, an alkylene oxide introduction device, and a stirrer, 119.4 parts by mass of a novolac cresol resin (trade name "Shounol CRG951", manufactured by Aica Kogyo Co., Ltd., OH equivalent: 119.4), 1.19 parts by mass of potassium hydroxide, and 119.4 parts by mass of toluene were introduced, and the system was replaced with nitrogen while stirring, and the temperature was raised. Next, 63.8 parts by mass of propylene oxide was gradually added dropwise, and the mixture was heated to 125-132°C and 0-4.8 kg / cm. 2 The mixture was reacted at 100° C. for 16 hours. After that, the mixture was cooled to room temperature, and 1.56 parts by mass of 89% phosphoric acid was added to the reaction solution and mixed to neutralize the potassium hydroxide, to obtain a propylene oxide reaction solution of a novolac cresol resin [solid content: 62.1%; hydroxyl value: 182.2 mg KOH / g (307.9 g / eq.)]. This propylene oxide reaction solution had an average of 1.08 moles of propylene oxide added per equivalent of phenolic hydroxyl group. 293.0 parts by mass of the resulting propylene oxide reaction solution of the novolac cresol resin, 43.2 parts by mass of acrylic acid, 11.53 parts by mass of methanesulfonic acid, 0.18 parts by mass of methyl hydroquinone, and 252.9 parts by mass of toluene were introduced into a reactor equipped with a stirrer, a thermometer, and an air blowing tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10 ml / min and stirring. 12.6 parts by mass of water produced by the reaction were distilled off as an azeotropic mixture with toluene. The mixture was then cooled to room temperature, and the resulting reaction solution was neutralized with 35.35 parts by mass of a 15% aqueous sodium hydroxide solution, and then washed with water. The mixture was then distilled off while replacing the toluene with 118.1 parts by mass of diethylene glycol monoethyl ether acetate in an evaporator, to obtain a novolac acrylate resin solution. Next, 332.5 parts by mass of the obtained novolac type acrylate resin solution and 1.22 parts by mass of triphenylphosphine were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and air was blown in at a rate of 10 ml / min. While stirring, 60.8 parts by mass of tetrahydrophthalic anhydride was gradually added, and the mixture was reacted at 95 to 101°C for 6 hours, cooled, and then removed. In this way, a solution of carboxyl group-containing resin A (solid content: 65% by mass, acid value of solid content: 87.7 mgKOH / g) was obtained.

[0086] <Preparation of Photosensitive Resin Composition> The components shown in Table 1 below were mixed and mixed at room temperature using a three-roll mill to obtain the photosensitive resin compositions shown in the table. Each value in the table indicates parts by mass (solid content equivalent).

[0087] In addition, each component *1 to *11 in Table 1 below is as follows. *1: Novolac epoxy resin (Dow Chemical, 176g / eq) *2: Phenol novolac type epoxy resin (DIC Corporation, diethylene glycol monoethyl ether acetate diluted solution, solid content 75% by mass) *3: Oxime ester photoinitiator (manufactured by BASF Japan Ltd.) *4: Acylphosphine oxide photoinitiator (Omnirad 819, IGM Resins) *5: Particles made of silica sol derived from sodium silicate (Nissan Chemical Co., Ltd., average particle size 12 nm, diluted with propylene glycol monomethyl ether acetate, solid content 42% by mass) *6: Particles made of silica sol derived from sodium silicate (Nissan Chemical Co., Ltd., average particle size 22 nm, diluted with propylene glycol monomethyl ether acetate, solid content 40% by mass) *7: Particles made of silica sol derived from sodium silicate (Nissan Chemical Co., Ltd., average particle size 45 nm, diluted with propylene glycol monomethyl ether acetate, solid content 30% by mass) *8: Spherical silica (manufactured by Admatechs Co., Ltd., average particle size 50 nm, methacrylsilane treatment, diluted with propylene glycol monomethyl ether acetate, solid content 60% by mass) *9: Fumed silica (manufactured by Nippon Aerosil Co., Ltd., average particle size 12 nm) *10: Dipentaerythritol hexaacrylate *11:Dicyandiamide

[0088] [Table 1]

[0089] <Evaluation of dispersion stability> For each of the photosensitive resin compositions of Examples 1-2 and Comparative Examples 1-3, the degree of dispersion was confirmed by the granular method using a grind gauge with a width of 90 mm, a length of 240 mm, and a maximum depth of 25 μm in accordance with JIS K5101 and JIS K5600. The degree of dispersion was evaluated from the distance of the section where 20 or more particles were confirmed (dense particle value). The above evaluation was performed immediately after the preparation of each photosensitive resin composition (initial stage) and after storing it for one month in a room temperature environment (25° C. in a dark place) (one month later).

[0090] The thus obtained degrees of dispersion (crowded particle value) were compared, and the dispersion stability was evaluated according to the following evaluation criteria. 〇: Dense grain value after one month is 12.5 or less △: Dense grain value after one month is greater than 12.5 and less than 20 ×: Dense grain value after 1 month is greater than 20 The evaluation results are shown in Table 2 below.

[0091] <Evaluation of film-forming properties> Immediately after preparing each photosensitive resin composition as described above, the composition was applied to the surface of a polyethylene terephthalate film (T-60, manufactured by Toray Industries, Inc., thickness 38 μm) as a first film using an applicator so that the film thickness after drying would be 15 μm, and the composition was dried at 80° C. for 30 minutes to prepare a dry film (initial). In addition, each of the prepared photosensitive resin compositions was allowed to stand for one month in a room temperature environment (25° C. in a dark place), and then a dry film (after one month) was produced in the same manner as above.

[0092] For the dry films obtained as described above, initially and after one month, a 1 cm x 1 cm square area of ​​each dried coating surface was observed using an optical microscope at 1000x magnification to check for the presence or absence of defects such as pinholes, and the film formability was evaluated according to the following evaluation criteria. ○: No defects such as pinholes ×: Defects such as pinholes are present The evaluation results are shown in Table 2 below.

[0093] <Evaluation of resolution> A copper substrate pretreated with CZ-8100 manufactured by MEC Co., Ltd. was heat-laminated using a vacuum laminator with dry films prepared in the same manner as in the above <Evaluation of film formability> except that the film thickness after drying was 20 μm. This substrate was exposed to light through a step tablet (Photec 41 steps) using a projection exposure machine, after which the first film was peeled off and a 1 wt% Na2CO3 aqueous solution at 30°C was sprayed at a pressure of 2 kg / cm. 2 The substrate was then exposed to a UV conveyor oven for 60 seconds at an integrated exposure of 2000 mJ / cm. 2 After irradiating with ultraviolet light under the conditions above, the film was heat cured for 60 minutes at 150° C. Of the resulting cured film, the openings showing a sensitivity of 10 steps on a step tablet were observed by SEM, and the resolution was evaluated according to the following criteria. ○…Good aperture diameter at φ50um △…Good aperture diameter at φ60um ×…No good aperture diameter can be obtained with an aperture diameter of φ60um The evaluation results are shown in Table 2 below.

[0094] [Table 2]

[0095] As is clear from Table 2, the photosensitive resin compositions (Examples 1 and 2) containing particles of silica sol derived from sodium silicate as silica have good dispersion stability of silica in the composition and have excellent coatability (film-forming property) even one month after the composition was prepared. In addition, since the photosensitive resin compositions of Examples 1 and 2 have an average particle size of 3 to 40 nm made of silica sol derived from sodium silicate, it is understood that the compositions have high resolution even one month after preparation.

[0096] On the other hand, the photosensitive resin composition of Comparative Example 1 has good dispersibility and film-forming properties because it contains particles of silica sol derived from sodium silicate as silica. However, since the average particle size exceeds 40 nm, it is understood that the resolution is somewhat decreased one month after the preparation of the composition. In addition, since the photosensitive resin composition of Comparative Example 2 contains spherical silica having an average particle diameter of 50 nm, it is found that the dispersion stability is poor, and the film-forming property and resolution are reduced one month after the composition is prepared. In addition, since the photosensitive resin composition of Comparative Example 3 contains fumed silica having an average particle size of 12 nm as silica, it is somewhat inferior in dispersion stability, and it is found that the film-forming property and the resolution decrease one month after the composition is prepared.

Claims

1. A photosensitive resin composition comprising (A) a carboxyl group-containing resin, (B) an epoxy resin, (C) a photopolymerization initiator, and (D) silica, The photosensitive resin composition, wherein the (D) silica contains particles made of a silica sol derived from sodium silicate, and the average particle size of the particles is 3 to 40 nm.

2. 2. The photosensitive resin composition according to claim 1, wherein the (D) silica is contained in an amount of 5 to 70% by mass based on the total solid content of the photosensitive resin composition.

3. The photosensitive resin composition according to claim 1 , further comprising a thermal curing catalyst.

4. 13. A dry film comprising: a first film; and a resin layer formed by applying the photosensitive resin composition according to claim 1 to one surface of the first film and drying the composition.

5. A cured product obtained by curing the photosensitive resin composition according to claim 1 or the resin layer of the dry film according to claim 4.

6. A printed wiring board having a coating made of the cured product according to claim 5.

Citation Information

Patent Citations

  • Photosensitive resin composition, dry film, printed wiring board and production method of photosensitive resin composition

    JP2017129736A

  • Manufacturing method of interlayer insulating film and interlayer insulating film

    JP2022079201A

  • Photosensitive resin composition, dry film, cured product and printed wiring board

    JP2022107466A

  • Laminated curable resin structure, dry film, cured product and electronic component

    JP2022159249A

  • Photosensitive resin composition, dry film, and printed wiring board