Solid electrolyte and all-solid battery

A solid electrolyte compound with specific elemental composition and peak intensity ratio enhances both ionic conductivity and thermal stability in all-solid-state batteries, addressing the limitations of existing electrolytes.

JP2024146206APending Publication Date: 2024-10-15TDK CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023058975
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing solid electrolytes in all-solid-state batteries have lower ionic conductivity compared to organic electrolytes and lack sufficient thermal stability.

Method used

A solid electrolyte compound containing Li, one or more elements from Group 3 to Group 15, and a halogen, specifically with a peak intensity ratio R1 (Ra/Rb) of 0.041 > R1 > 0.011, as determined by TOF-SIMS, is used to enhance both ionic conductivity and thermal stability.

Benefits of technology

The proposed solid electrolyte achieves high ionic conductivity and high thermal stability, reducing internal resistance and ensuring stable battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146206000003
    Figure 2024146206000003
  • Figure 2024146206000001
    Figure 2024146206000001
  • Figure 2024146206000002
    Figure 2024146206000002
Patent Text Reader

Abstract

To provide a solid electrolyte which achieves both high ionic conductivity and high thermal stability.SOLUTION: There is provided a solid electrolyte which is a compound containing Li, one or more elements selected from Group 3 to Group 15 elements, and halogen, wherein the halogen includes Cl, a peak of LiCl2 is detected in the negative ion analysis by time-of-flight secondary ion mass spectrometry of the compound and the peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of the LiCl2 to the peak intensity Rb of all ions satisfies 0.041>R1>0.011.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid electrolyte and an all-solid-state battery.

Background Art

[0002] In recent years, all-solid-state batteries have attracted attention from the viewpoints of improving safety and increasing output power. One of the characteristics of all-solid-state batteries is that a solid is used as the electrolyte. Here, the required properties of the solid electrolyte include ion conductivity, oxidation-reduction resistance, moldability, and the like. One of the problems is to improve the ion conductivity compared with conventional organic electrolytes. Generally, many solid electrolytes have lower conductivity than organic electrolytes.

[0003] Patent Document 1 discloses a solid electrolyte represented by the following compositional formula (i) (where 0 < z < 2 and X is Cl or Br). Li 6-3z Y z X6 ··· Formula (i)

[0004] Patent Document 2 discloses a solid electrolyte composed of a compound represented by the following formula (ii) (where A is at least one element selected from the group consisting of Li, Cs, and Ca, and X is at least one element selected from the group consisting of F, Cl, Br, and I). AaEbGcXd ··· (ii)

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Non-Patent Documents

[0006]

Non-Patent Document 1

[0007] According to Non-Patent Document 1, halide-based solid electrolytes have attracted attention due to their high ionic conductivity and high chemical and electrochemical stability among solid electrolytes, but their thermal stability needs to be improved.

[0008] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and provides a solid electrolyte and an all-solid-state battery that achieve both high ionic conductivity and high thermal stability. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides the following means.

[0010] A first aspect of the present invention is a solid electrolyte comprising a compound containing Li, one or more elements selected from the group consisting of Group 3 to Group 15 elements, and a halogen, the halogen including Cl, a peak of LiCl2 is detected in negative ion analysis of the compound by time-of-flight secondary ion mass spectrometry, and a peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of LiCl2 to the peak intensity Rb of all ions satisfies 0.041>R1>0.011.

[0011] A second aspect of the present invention is the solid electrolyte of the first aspect, wherein R1 (Ra / Rb) satisfies 0.030>R1>0.019.

[0012] A third aspect of the present invention is the solid electrolyte of the first aspect, wherein the compound is represented by the following formula (1): LiaEbGcCldXe···(1) (In formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides, and G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , SiO 18 , PO3, PO4, P2O7, P3O 10 , SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, C H3COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-CO O, C6H5SO3, OOC-CH=CH-COO, C(OH)(CH2COOH)2COO, AsO4, BiO4, CrO4, MnO4, PtF6, PtCl6, PtBr6, PtI6, SbO4, SeO4, TeO4, HCOO, O, and X is one or more elements selected from the group consisting of F, Br, and I, and 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1、0≦e<6.1である。)

[0013] A fourth aspect of the present invention is the solid electrolyte of the first aspect, wherein the compound is represented by the following formula (2): LiqMrPsOtCluSv···(2) (In formula (2), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, and Cl is chlorine. q, r, s, t, u, and v are 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×stu / 2, respectively.)

[0014] A fifth aspect of the present invention relates to the solid electrolyte of the first aspect, in which the compound is one or more of the compounds represented by the following formulae (3) to (6). Li2ZrCl6···(3) Li2ZrOCl4 (4) Li2ZrSO4Cl4 (5) Li3ZrPO4Cl4 (6)

[0015] A sixth aspect of the present invention is an all-solid-state battery in which a positive electrode and a negative electrode face each other via a solid electrolyte layer, and at least one of the solid electrolyte layer, the positive electrode, and the negative electrode contains a solid electrolyte according to any one of the first to fifth aspects. Effect of the Invention

[0016] According to the solid electrolyte of the present invention, it is possible to provide a solid electrolyte that has both high ionic conductivity and high thermal stability. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.

[0019] "Solid electrolyte" A solid electrolyte is a material that can move ions when an external electric field is applied. If the ionic conductivity of a solid electrolyte is high, the exchange of ions in the solid-state battery becomes smoother, and the internal resistance becomes smaller.

[0020] The solid electrolyte according to this embodiment is a compound containing Li, one or more elements selected from the group 3 to group 15 elements, and a halogen, the halogen including Cl, a LiCl2 peak is detected in negative ion analysis of the compound by time-of-flight secondary ion mass spectrometry, and the peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of LiCl2 to the peak intensity Rb of all ions satisfies 0.041>R1>0.011. When R1 (Ra / Rb) satisfies 0.041>R1>0.011, high ionic conductivity and high thermal stability can be achieved at the same time.

[0021] From the viewpoint of achieving both high ionic conductivity and high thermal stability, it is preferable that R1 (Ra / Rb) satisfies 0.030>R1>0.019.

[0022] The solid electrolyte according to the present embodiment may be in the form of a powder (particles) or in the form of a sintered body obtained by sintering the powder. The solid electrolyte may be a compact obtained by compressing and molding the powder, a compact obtained by molding a mixture of the powder and a binder, or a coating film formed by applying a coating material containing the powder, a binder, and a solvent, and then removing the solvent by heating. The main structure of the solid electrolyte may be amorphous or crystalline.

[0023] (Negative ion analysis by time-of-flight secondary ion mass spectrometry) Time-of-Flight Secondary Ion Mass Spectrometry (TOF-SIMS) is a technique in which an ion beam (primary ions) is irradiated onto the surface of a solid sample, and the ions (secondary ions) emitted from the surface are mass-separated by utilizing the difference in their flight times (the flight time is proportional to the square root of the ion's mass). When measured, TOF-SIMS spectral data has the horizontal axis representing time and the vertical axis representing the ion count (intensity), but by converting the time axis into mass number, the horizontal axis becomes mass number, and the mass distribution of secondary ions, i.e., the mass spectrum, is obtained.

[0024] "Peak intensity of all ions" refers to the count number of all ions (total count), and "peak intensity of LiCl2" refers to the count number of LiCl2 ions (negative ions). Therefore, the peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of LiCl2 to the peak intensity Rb of all ions refers to the count number of LiCl2 ions in the count number of all ions (total count).

[0025] In the solid electrolyte according to this embodiment, the peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of LiCl2 to the peak intensity Rb of all ions satisfies 0.041>R1>0.011.

[0026] The generation of LiCl is thought to be the cause of the detection of LiCl2 peaks in the TOF-SIMS mass spectrum. LiCl is generated when the solid electrolyte decomposes due to a reaction caused by heating or a change in potential in electrochemical measurements of the solid electrolyte. LiCl has high thermal stability, so its generation on the surface of the solid electrolyte improves its thermal stability. When there is little LiCl, i.e. when the peak intensity ratio R1 (Ra / Rb) is 0.011 or less, the effect of improving thermal stability cannot be fully obtained. On the other hand, LiCl has low ionic conductivity, so when there is a large amount of LiCl, that is, when the peak intensity ratio R1 (Ra / Rb) is 0.041 or more, the ionic conductivity decreases.

[0027] In the present invention, it has been clarified that the peak intensity ratio R1 (Ra / Rb) of the peak intensity Ra of LiCl2 to the peak intensity Rb of all ions by TOF-SIMS can be used as an index of thermal stability.

[0028] In the solid electrolyte according to the present embodiment, the compound may be represented by the following formula (1): LiaEbGcCldXe···(1) (In formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids, and G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 、Si6O 18 、PO3、PO4、P2O7、P3O 10 、SO3、SO4、SO5、S2O3、S2O4、S2O5、S2O6、S2O7、S2O8、BF4、PF6、BOB、(COO)2、N、AlCl4、CF3SO3、CH3COO、CF3COO、OOC-(CH2)2-COO、OOC-CH2-COO、OOC-CH(OH)-CH(OH)-COO、OOC-CH(OH)-CH2-COO、C6H5SO3、OOC-CH=CH-COO、C(OH)(CH2COOH)2COO、AsO4、BiO4、CrO4、MnO4、PtF6、PtCl6、PtBr6、PtI6、SbO4、SeO4、TeO4、HCOO、O, and is one or more groups selected from the group consisting of X is one or more elements selected from the group consisting of F, Br, and I, and 0.5 ≦ a < 6, 0 < b < 2, 0 ≦ c ≦ 6, 0 < d ≦ 6.1, 0 ≦ e < 6.1.)

[0029] In formula (1), when E is Al, Sc, Y, or a lanthanoid, a is preferably 2.0 ≦ a ≦ 4.0, more preferably 2.5 ≦ a ≦ 3.5. When E is Zr or Hf, a is preferably 1.0 ≦ a ≦ 3.0, more preferably 1.5 ≦ a ≦ 2.5. In the compound represented by formula (1), if 0.5 ≦ a < 6, the content of Li contained in the compound becomes appropriate and the ionic conductivity of the solid electrolyte layer 10 increases.)

[0030] In formula (1), E is an essential component and is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. E improves the ionic conductivity of the solid electrolyte. b is 0 < b < 2. Since the effect of including E can be obtained more effectively, b is preferably 0.6 ≦ b. Further, E is an element that forms the skeleton of the solid electrolyte. b is more preferably b ≦ 1.)

[0031] In formula (1), G may include at least one group selected from the group consisting of anions, for example, the anions OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, and Si4O 11 , SiO 18 , PO3, PO4, P2O7, P3O 10 , SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, CH3 COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-COO, C6 and at least one group selected from the group consisting of HSO, OOC-CH=CH-COO, C(OH)(CHCOOH)COO, AsO, BiO, CrO, MnO, PtF, PtCl, PtBr, PtI, SbO, SeO, TeO, HCOO, and O (BOB is bisoxalatoborate, OOC-(CH)-COO is succinate, OOC-CH-COO is malonate, OOC-CH(OH)-CH(OH)-COO is tartrate, OOC-CH(OH)-CH-COO is malate, CHSO is benzenesulfonate, OOC-CH=CH-COO is fumarate, OOC-CH=CH-COO is maleate, and C(OH)(CHCOOH)COO is citrate). By selecting one of the above groups for the anion, high ionic conductivity is obtained and reduction resistance is improved.

[0032] c satisfies 0≦c≦6. c is preferably 0.5≦c because the effect of widening the potential window on the reduction side by including G is more pronounced. c is preferably c≦3 so that a decrease in the ionic conductivity of the solid electrolyte caused by an excessively high G content does not occur.

[0033] X may contain at least one selected from the group consisting of F, Br, and I. X is preferably at least one selected from the group consisting of Br and I in order to increase the ionic conductivity of the solid electrolyte, preferably contains Br and / or I, and particularly preferably contains I. When X contains F, since X becomes a solid electrolyte with high ionic conductivity, it is preferable to contain F and two or more selected from the group consisting of Br and I.

[0034] When X is F, it becomes a solid electrolyte with sufficiently high ionic conductivity and excellent oxidation resistance. When X is Br, it becomes a solid electrolyte with sufficiently high ionic conductivity and a good balance between oxidation resistance and reduction resistance. When X is I, it becomes a solid electrolyte with high ionic conductivity.

[0035] d satisfies 0 < d ≤ 6.1. It is preferable that 1 ≤ d. When 1 ≤ d, when the solid electrolyte is pressure-molded into a pellet shape, the strength of the pellet increases. Also, when 1 ≤ d, the ionic conductivity of the solid electrolyte increases. Also, it is preferable that d ≤ 5 so that the potential window of the solid electrolyte does not become narrow due to an excessive Cl content causing a shortage of G.

[0036] e satisfies 0 ≤ e < 6.1. At this time, e satisfies 0 ≤ (e - d) < 6.1.

[0037] In the solid electrolyte, the compound can be one or more represented by the following formulas (3) to (6); Li2ZrCl6 ··· (3) Li2ZrOCl4 ··· (4) Li2ZrSO4Cl4 ··· (5) Li3ZrPO4Cl4 ··· (6)

[0038] The compound may be represented by the following formula (2). LiqMrPsOtCluSv ··· (2) (In formula (2), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, and Cl is chlorine. q, r, s, t, u, and v are 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×stu / 2, respectively.)

[0039] "All-solid-state battery" FIG. 1 is a schematic cross-sectional view of an all-solid-state battery 100 according to this embodiment. The all-solid-state battery 100 shown in FIG. 1 includes a power generating element 40 and an exterior body 50. The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside through a pair of terminals 60, 62 that are connected to each other. Although a laminated type battery is shown in FIG. 1, a wound type battery may also be used. The all-solid-state battery 100 is used, for example, in laminate batteries, square batteries, cylindrical batteries, coin batteries, button batteries, and the like.

[0040] <Power generation element> The power generating element 40 includes a solid electrolyte layer 10, a positive electrode 20, and a negative electrode 30. The power generating element 40 is charged or discharged by the exchange of ions between the positive electrode 20 and the negative electrode 30 via the solid electrolyte layer 10 and the exchange of electrons via an external circuit. The all-solid-state battery 100 according to this embodiment contains the solid electrolyte according to the above embodiment in at least one of the solid electrolyte layer 10, the positive electrode 20, and the negative electrode 30.

[0041] (Solid electrolyte layer) The solid electrolyte layer 10 may be a layer containing the solid electrolyte according to the above embodiment. The solid electrolyte layer 10 may be only the solid electrolyte according to the above embodiment, but may be used together with a support such as a binder or nonwoven fabric. The binder may be the same as that used for the electrodes. The ratio of the binder to the solid electrolyte is preferably 10% or less by volume. The support such as nonwoven fabric may be any insulating material such as resin, ceramics, or glass used as the binder, and preferably has an aperture ratio of 70% or more. The solid electrolyte layer 10 is sandwiched between a positive electrode 20 and a negative electrode 30. The solid electrolyte layer 10 includes a solid electrolyte that can move ions by an externally applied voltage. For example, the solid electrolyte conducts lithium ions and inhibits the movement of electrons.

[0042] The solid electrolyte layer 10 is, for example, a halide-based solid electrolyte. The solid electrolyte layer 10 includes, for example, the above-mentioned solid electrolyte. When the above-mentioned solid electrolyte is included in the positive electrode 20 or the negative electrode 30, the solid electrolyte included in the solid electrolyte layer 10 does not have to be the above-mentioned one.

[0043] (positive electrode) 1, the positive electrode 20 has a plate-shaped (foil-shaped) positive electrode current collector 22 and a positive electrode mixture layer 24. The positive electrode mixture layer 24 is in contact with at least one surface of the positive electrode current collector 22.

[0044] The positive electrode current collector 22 may be made of any material as long as it is an electronically conductive material that is resistant to oxidation during charging and is not easily corroded. The positive electrode current collector 22 is, for example, a metal such as aluminum, stainless steel, nickel, or titanium, a conductive resin, etc. The positive electrode current collector 22 may be in any of the following forms: powder, foil, punching, and expandable.

[0045] The positive electrode mixture layer 24 contains a positive electrode active material, and optionally a solid electrolyte, a binder, and a conductive assistant.

[0046] The positive electrode active material is not particularly limited as long as it can reversibly absorb and release, and insert and remove (intercalate and deintercalate) lithium ions, and any positive electrode active material used in known all-solid-state batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.

[0047] Examples of lithium-containing metal oxides include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and composite metal oxides represented by the general formula: LiNixCoyMnzO2 (x+y+z=1), lithium vanadium compounds (LiVOPO4, Li3V2(PO4)3), olivine-type LiMPO4 (wherein M represents at least one selected from Co, Ni, Mn, and Fe), and lithium titanate (Li4Ti5O 12 ) etc.

[0048] The positive electrode active material may not contain lithium. Examples of such positive electrode active materials include non-lithium-containing metal oxides (MnO2, V2O5, etc.), non-lithium-containing metal sulfides (MoS2, etc.), and non-lithium-containing fluorides (FeF3, VF3, etc.). When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.

[0049] The solid electrolyte contained in the positive electrode 20 is, for example, the solid electrolyte according to the above embodiment. The solid electrolyte contained in the positive electrode 20 may be a halide-based solid electrolyte other than the solid electrolyte according to the above embodiment.

[0050] The content of the solid electrolyte in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1 mass % to 50 mass %, and more preferably 5 mass % to 30 mass %, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive assistant, and the binder.

[0051] The binder bonds the positive electrode active material, the solid electrolyte, and the conductive assistant to one another in the positive electrode mixture layer 24, and also firmly bonds the positive electrode mixture layer 24 to the positive electrode current collector 22. The positive electrode mixture layer 24 preferably contains a binder. The binder preferably has oxidation resistance and good adhesiveness.

[0052] Examples of the binder used in the positive electrode mixture layer 24 include polyvinylidene fluoride (PVDF) or its copolymer, polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid (PA) and its copolymer, metal ion crosslinked polyacrylic acid (PA) and its copolymer, polypropylene (PP) grafted with maleic anhydride, polyethylene (PE) grafted with maleic anhydride, and mixtures thereof. Among these, it is particularly preferable to use PVDF as the binder.

[0053] The content of the binder in the positive electrode mixture layer 24 is not particularly limited, but is preferably 0.1% by mass to 10% by mass, and more preferably 0.1% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive assistant, and binder. If the amount of binder is too small, it tends not to be possible to form a positive electrode 20 with sufficient adhesive strength. Conversely, if the amount of binder is too large, it tends to be difficult to obtain sufficient volume or mass energy density, since general binders are electrochemically inactive and do not contribute to discharge capacity.

[0054] The conductive assistant improves the electronic conductivity of the positive electrode mixture layer 24. Known conductive assistants can be used. Examples of the conductive assistant include carbon materials such as carbon black, graphite, carbon nanotubes, and graphene, metals such as aluminum, copper, nickel, stainless steel, iron, and amorphous metals, conductive oxides such as ITO, and mixtures thereof. The conductive assistant may be in the form of powder or fiber.

[0055] There is no particular limitation on the content of the conductive assistant in the positive electrode mixture layer 24. When the conductive assistant is added, the mass ratio of the conductive assistant is preferably 0.5 mass % to 20 mass %, and more preferably 1 mass % to 5 mass %, based on the total mass of the positive electrode active material, solid electrolyte, conductive assistant, and binder.

[0056] (Negative electrode) 1, the negative electrode 30 has a negative electrode current collector 32 and a negative electrode mixture layer 34. The negative electrode mixture layer 34 is in contact with the negative electrode current collector 32.

[0057] The negative electrode current collector 32 may have electronic conductivity. The negative electrode current collector 32 is made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 32 may be in the form of a powder, a foil, a punching, or an expandable material.

[0058] The negative electrode mixture layer 34 contains a negative electrode active material, and, if necessary, a solid electrolyte, a binder, and a conductive assistant.

[0059] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. The negative electrode active material may be any negative electrode active material used in known all-solid-state batteries.

[0060] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies, Si, SiO x Metals that can combine with lithium, such as Sn and aluminum, their alloys, composites of these metals and carbon materials, lithium titanate (Li4Ti5O 12 ), titanium niobium oxide (TiNb2O7), oxides such as SnO2, metallic lithium, etc. The negative electrode active material is preferably natural graphite.

[0061] The solid electrolyte contained in the negative electrode 30 is, for example, the solid electrolyte according to the above embodiment. The solid electrolyte contained in the negative electrode 30 may be a halide-based solid electrolyte other than the solid electrolyte according to the above embodiment.

[0062] The binder and conductive assistant contained in the negative electrode 30 are the same as the binder and conductive assistant contained in the positive electrode 20 .

[0063] <Exterior body> The exterior body 50 houses the power generating element 40 therein. The exterior body 50 prevents moisture and the like from entering from the outside to the inside. As shown in Fig. 1, for example, the exterior body 50 has a metal foil 52 and a resin layer 54 laminated on each side of the metal foil 52. The exterior body 50 is a metal laminate film in which the metal foil 52 is coated with the resin layer 54 from both sides.

[0064] The metal foil 52 is, for example, an aluminum foil or a stainless steel foil. The resin layer 54 can be, for example, a resin film such as polypropylene. The materials constituting the resin layer 54 may be different between the inside and outside. For example, the outside material can be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inside material can be polyethylene (PE) or polypropylene (PP).

[0065] <Terminal> The terminals 60 and 62 are connected to the positive electrode 20 and the negative electrode 30, respectively. The terminal 62 connected to the positive electrode 20 is a positive electrode terminal, and the terminal 60 connected to the negative electrode 30 is a negative electrode terminal. The terminals 60 and 62 are responsible for electrical connection to the outside. The terminals 60 and 62 are made of a conductive material such as aluminum, nickel, or copper. The connection method may be welding or screwing. The terminals 60 and 62 are preferably protected with insulating tape to prevent short circuits.

[0066] [Manufacturing method of all-solid-state batteries] Next, a method for producing the all-solid-state battery according to the present embodiment will be described. The all-solid-state battery according to the present embodiment contains the solid electrolyte according to the above embodiment in at least one of the solid electrolyte layer, the positive electrode, and the negative electrode. First, a solid electrolyte is prepared. The solid electrolyte can be produced, for example, by mixing raw material powders containing predetermined elements in a predetermined molar ratio and subjecting them to a mechanochemical reaction. When the mechanochemical reaction is carried out, the unreacted raw materials are adjusted so as to remain in the solid electrolyte. Specifically, the rotation speed, revolution speed, synthesis time, and state of the raw material powder at the time of input of the planetary ball mill can be changed to allow the unreacted components of the raw materials to remain. In the synthesis of the solid electrolyte according to the above embodiment, the ratio R1 of the peak intensity of LiCl2 detected by TOF-SIMS can be adjusted by first mixing the raw materials other than a part of LiCl, and then adding and mixing the remaining LiCl after a predetermined time, or by first mixing the raw materials other than LiCl, and then adding and mixing LiCl after a predetermined time. Specifically, for example, in Example 1, half of LiCl and ZrCl4 are mixed first, and then the remaining LiCl is added and mixed two hours after the start of synthesis. In Example 3, Zr(SO4)2 and ZrCl4 are mixed first, and then LiCl is added and mixed one hour after the start of synthesis.

[0067] When the raw material powder contains a halide raw material, the halide raw material is likely to evaporate when the temperature is increased. For this reason, halogen gas may be made to coexist in the atmosphere during sintering to supplement the halogen. In addition, when the raw material powder contains a halide raw material, sintering may be performed by a hot press method using a mold with high airtightness. In this case, since the mold has high airtightness, evaporation of the halide raw material due to sintering can be suppressed. By sintering in this manner, a solid electrolyte in the form of a sintered body made of a compound having a predetermined composition is obtained.

[0068] Next, the positive electrode 20 is prepared. The positive electrode is manufactured by applying a paste containing a positive electrode active material onto a positive electrode current collector 22 and drying it to form a positive electrode mixture layer 24. The above-mentioned solid electrolyte may be added to the paste containing the positive electrode active material.

[0069] Next, the negative electrode 30 is prepared. The negative electrode is manufactured by applying a paste containing a negative electrode active material onto a negative electrode current collector 32 and drying it to form a negative electrode mixture layer 34. The above-mentioned solid electrolyte may be added to the paste containing the negative electrode active material.

[0070] The power generating element 40 can be produced, for example, by powder molding. A guide with a hole is placed on the positive electrode 20, and the guide is filled with a solid electrolyte. The surface of the solid electrolyte is then smoothed, and the negative electrode 30 is placed on top of the solid electrolyte. This sandwiches the solid electrolyte between the positive electrode 20 and the negative electrode 30. Pressure is then applied to the positive electrode 20 and the negative electrode 30 to pressure mold the solid electrolyte. By pressure molding, a laminate is obtained in which the positive electrode 20, the solid electrolyte layer 10, and the negative electrode 30 are stacked in this order.

[0071] Next, external terminals are welded to the positive electrode current collector 22 of the positive electrode 20 and the negative electrode current collector 32 of the negative electrode 30, which form the laminate, by a known method, to electrically connect the positive electrode current collector 22 or the negative electrode current collector 32 to the external terminal. Thereafter, the laminate connected to the external terminal is housed in an exterior body 50, and the opening of the exterior body 50 is heat-sealed to seal it. Through the above steps, the all-solid-state battery 100 of this embodiment is obtained.

[0072] The all-solid-state battery 100 according to this embodiment contains the above-mentioned solid electrolyte, and therefore has smooth Li-ion conduction and low internal resistance.

[0073] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES

[0074] "Example 1" (Preparation of solid electrolyte) In a glove box with a dew point of approximately -75°C, raw material powders of lithium chloride (LiCl) and zirconium chloride (ZrCl4) were weighed so that their molar ratio was 2:1. First, half of the lithium chloride (LiCl) and all of the zirconium chloride (ZrCl4) were put into a hermetically sealed zirconia container for a planetary ball mill that already contained zirconia balls. Next, the hermetically sealed container was covered with a lid, the lid was screwed onto the container body, and further, the space between the lid and the container was sealed with a polyimide tape. The polyimide tape has the effect of blocking moisture. Next, the hermetically sealed zirconia container was set in the planetary ball mill. The rotation speed of the rotation around its own axis was set at 300 rpm, the revolution speed was set at 300 rpm, and the rotation direction of the rotation around its own axis and the revolution direction were set to be opposite, and the mechanochemical reaction was started. After the start of the synthesis, the remaining half of the lithium chloride (LiCl) was added in 2 hours (2h), and the mechanochemical reaction was further carried out for 22 hours (22h) to synthesize a solid electrolyte (Li2ZrCl6).

[0075] The planetary ball mill is usually installed in an ordinary atmosphere (air). The hermetically sealed zirconia container for the planetary ball mill is screwed and further sealed with a polyimide tape. When the hermetically sealed zirconia container is set in the planetary ball mill, since the hermetically sealed zirconia container is firmly pressed and fixed, it is considered that there is almost no moisture intrusion from the air into the hermetically sealed zirconia container even in an ordinary atmosphere.

[0076] <Measurement of mass spectrum by TOF-SIMS> For the solid electrolyte (Li2ZrCl6) of Example 1, the mass spectrum was measured by time-of-flight secondary ion mass spectrometry, and the peak intensity ratio R1 (Ra / Rb) of the peak intensity of LiCl2 to the peak intensity Rb of all ions was obtained.

[0077] The measurement was carried out with the following apparatus and conditions for TOF-SIMS. (1) Apparatus: TOF-SIMS5 manufactured by ION-TOF (2) Measurement conditions Measurement mode: Spectrometry Primary ion: Bi3 ++ Acceleration voltage: 25 kV Measurement area: 40000μm 2 (200μm×200μm) Measurement ion species: Negative Electronic neutralization: Yes

[0078] <Measurement of ionic conductivity (before storage test at 80℃)> Next, in a glove box with argon gas circulating at a dew point of approximately -70°C, the obtained solid electrolyte (Li2ZrCl6) powder was filled into a pressure molding die and pressure molded with a load of approximately 30 KN to prepare a measurement cell for ionic conductivity.

[0079] The pressure molding die is composed of a PEEK (polyether ether ketone) cylinder with a diameter of 10 mm, and upper and lower punches made of SKD11 material with a diameter of 9.99 mm.

[0080] After that, a stainless steel disk and a Teflon (registered trademark) disk, both 50 mm in diameter and 5 mm thick with four screw holes, were prepared and the pressure molding die was set as follows. They were loaded in the following order: stainless steel disk / Teflon (registered trademark) disk / pressure molding die / Teflon (registered trademark) disk / stainless steel disk, and the four screws were tightened with a torque of approximately 3 N m. Screws were also inserted into the screw holes on the sides of the upper and lower punches to serve as external connection terminals.

[0081] The external connection terminal was connected to a potentiostat (VersaSTAT3 manufactured by Princeton Applied Research) equipped with a frequency response analyzer, and the ionic conductivity was measured using an impedance measurement method. Measurements were performed at a measurement frequency range of 1 MHz to 0.1 Hz, an amplitude of 10 mV, and a temperature of 25°C. The ionic conductivity of the solid electrolyte (Li2ZrCl6) of Example 1 was 2.0×10 -3 S / cm. At this time, the internal resistance at a temperature of 25°C was obtained.

[0082] <Measurement of ionic conductivity (after storage test at 80℃)> In the same manner as described above, a measurement cell for ionic conductivity was prepared and kept in a thermostatic chamber maintained at 80° C. for 24 hours. Thereafter, the ambient temperature was returned to 25° C., and the ionic conductivity was measured in the same manner as described above. The ionic conductivity of the solid electrolyte (Li2ZrCl6) of Example 1 was 1.9×10 -3 It was S / cm. At this time, the rate of increase in internal resistance after storage at 80°C relative to the internal resistance at 25°C (the ratio of the internal resistance after storage at 80°C to the internal resistance at 25°C taken as 100%) was obtained.

[0083] (Production of all-solid-state batteries) The solid-state battery was fabricated in a glove box with a dew point of approximately -70°C. The solid-state battery was fabricated using a pellet fabrication jig. The pellet fabrication jig has a PEEK (polyether ether ketone) holder with an inner diameter of 10 mm, and upper and lower punches with diameters of 9.99 mm. The material of the upper and lower punches is die steel (SKD11 material).

[0084] A lower punch was inserted into a PEEK holder of a pellet making jig, and 50 mg of the solid electrolyte (Li2ZrCl6) of Example 1 was placed on the lower punch. Next, the resin holder was vibrated to smooth the surface of the solid electrolyte, and then an upper punch was inserted on the solid electrolyte and pressed with a load of about 4 KN using a press machine.

[0085] Next, the lower punch was removed, and 10 mg of the negative electrode mixture was placed on the solid electrolyte. Next, the PEEK holder was vibrated to level the surface of the negative electrode mixture, and then the lower punch was inserted on the negative electrode mixture and pressed with a press machine under a load of 3KN. The negative electrode mixture consisted of the negative electrode active material, the auxiliary carbon and binder, and the above-mentioned solid electrolyte, and the negative electrode active material was lithium titanate (LTO). Next, the upper punch was removed, and 10 mg of the positive electrode mixture was placed on the solid electrolyte layer. Next, the PEEK holder was vibrated to level the surface of the positive electrode mixture, and then the upper punch was inserted on the positive electrode mixture and pressed with a load of 3KN using a press machine. The positive electrode mixture consisted of the positive electrode active material, the conductive auxiliary carbon and binder, and the above-mentioned solid electrolyte, and the positive electrode active material was lithium cobalt oxide (LCO). In this manner, an all-solid-state battery was produced in which the negative electrode mixture layer, the solid electrolyte layer, and the positive electrode mixture layer were laminated in this order.

[0086] In addition, two stainless steel plates with a diameter of 50 mm and a thickness of 5 mm and two Bakelite (registered trademark) plates with a diameter of 50 mm and a thickness of 2 mm were prepared. Next, four holes for passing screws were provided in each of the two stainless steel plates and the two Bakelite (registered trademark) plates. The holes for passing screws were provided in positions where the two stainless steel plates and the two Bakelite (registered trademark) plates overlap in plan view when the electrochemical cell, the two stainless steel plates, and the two Bakelite (registered trademark) plates are stacked, but do not overlap with the electrochemical cell in plan view.

[0087] Then, a stainless steel plate, a Bakelite® plate, an all-solid-state battery, a Bakelite® plate, and a stainless steel plate were stacked in this order, and screws were inserted into the screw holes and tightened with a torque of 1 N m. In this way, an all-solid-state battery was obtained in which the upper and lower punches of the electrochemical cell were insulated by the Bakelite® plate.

[0088] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0089] "Example 2" The solid electrolyte (Li2ZrOCl4) of Example 2 was synthesized by starting the synthesis with half of the LiCl and ZrOCl2, adding the remaining half of LiCl 2 hours after the start of the synthesis, and synthesizing Li2ZrOCl4 by further allowing the mechanochemical reaction for 22 hours. The solid electrolyte of Example 2 was synthesized in the same manner as Example 1 except that the raw materials were different.

[0090] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0091] "Example 3" The solid electrolyte (Li2ZrSO4Cl4) of Example 3 was synthesized by starting the synthesis with Zr(SO4)2 and ZrCl4, adding LiCl after a predetermined time after the start of the synthesis, and further carrying out a mechanochemical reaction so that the synthesis time including the predetermined time was 24 hours, to synthesize Li2ZrSO4Cl4. Specifically, the synthesis was started with Zr(SO4)2 and ZrCl4, LiCl was added 1 hour after the start of the synthesis, and the mechanochemical reaction was carried out for a further 23 hours to synthesize Li2ZrSO4Cl4. The solid electrolyte of Example 3 was synthesized in the same manner as Example 1, except that the raw materials were different, and the synthesis was started with Zr(SO4)2 and ZrCl4, and LiCl was added 1 hour after the start of the synthesis.

[0092] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0093] "Example 4" The solid electrolyte (Li3ZrPO4Cl4) of Example 4 was synthesized by starting the synthesis with Zr3(PO4)4 and ZrCl4, adding LiCl 2 hours after the start of the synthesis, and further carrying out a mechanochemical reaction for 22 hours to synthesize Li3ZrPO4Cl4. The solid electrolyte of Example 4 was synthesized in the same manner as in Example 1, except that the raw materials were different, and the synthesis was started with Zr3(PO4)4 and ZrCl4, and LiCl was added 2 hours after the start of the synthesis.

[0094] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0095] "Examples 5 and 6" The solid electrolytes (Li2ZrCl6) of Examples 5 and 6 were synthesized in the same manner as the solid electrolyte of Example 1, except that the remaining half of LiCl was added after a predetermined time from the start of synthesis, and the mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, thereby synthesizing Li2ZrCl6. Specifically, in Example 5, synthesis was started with half of the LiCl and ZrCl4, and the remaining half of LiCl was added 1 hour after the start of synthesis, and the mechanochemical reaction was continued for another 23 hours to synthesize Li2ZrCl6. The solid electrolyte of Example 5 was synthesized in the same manner as in Example 1, except for the time from the start of synthesis until the remaining half of LiCl was added. In Example 6, synthesis was started with half the amount of LiCl and ZrCl4, and the remaining half of LiCl was added 3 hours after the start of synthesis, and the mechanochemical reaction was continued for another 21 hours to synthesize Li2ZrCl6. The solid electrolyte of Example 6 was synthesized in the same manner as in Example 1, except for the time from the start of synthesis until the remaining half of LiCl was added.

[0096] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0097] "Examples 7 and 8" The solid electrolytes (Li2ZrOCl4) of Examples 7 and 8 were synthesized in the same manner as the solid electrolyte of Example 2, except that the remaining half of LiCl was added after a predetermined time from the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, to synthesize Li2ZrOCl4. Specifically, in Example 7, synthesis was started with half of the LiCl and ZrOCl2, and the remaining half of LiCl was added 1 hour after the start of synthesis, and the mechanochemical reaction was continued for another 23 hours to synthesize Li2ZrOCl4. The solid electrolyte of Example 7 was synthesized in the same manner as in Example 2, except for the time from the start of synthesis until the remaining half of LiCl was added. In Example 8, synthesis was started with half the amount of LiCl and ZrOCl2, and the remaining half of LiCl was added 3 hours after the start of synthesis, and the mechanochemical reaction was continued for another 21 hours to synthesize Li2ZrOCl4. The solid electrolyte of Example 8 was synthesized in the same manner as in Example 2, except for the time from the start of synthesis until the remaining half of LiCl was added.

[0098] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0099] "Examples 9 and 10" The solid electrolytes (Li2ZrSO4Cl4) of Examples 9 and 10 were prepared in the same manner as the solid electrolyte of Example 3, except that LiCl was added a predetermined time after the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, to synthesize Li2ZrSO4Cl4. Specifically, in Example 9, synthesis was started with Zr(SO4)2 and ZrCl4, LiCl was added 2 hours after the start of synthesis, and the mechanochemical reaction was continued for another 22 hours to synthesize Li2ZrSO4Cl4. The solid electrolyte of Example 9 was synthesized in the same manner as in Example 3, except for the time from the start of synthesis until the addition of LiCl. In Example 10, synthesis was started with Zr(SO4)2 and ZrCl4, LiCl was added 3 hours after the start of synthesis, and the mechanochemical reaction was continued for another 21 hours to synthesize Li2ZrSO4Cl4. The solid electrolyte of Example 10 was synthesized in the same manner as in Example 3, except for the time from the start of synthesis until the addition of LiCl.

[0100] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0101] "Examples 11 and 12" The solid electrolytes (Li3ZrPO4Cl4) of Examples 11 and 12 were prepared in the same manner as the solid electrolyte of Example 4, except that LiCl was added a predetermined time after the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, to synthesize Li3ZrPO4Cl4. Specifically, in Example 11, synthesis was started with Zr3(PO4)4 and ZrCl4, LiCl was added 3 hours after the start of synthesis, and the mechanochemical reaction was continued for another 21 hours to synthesize Li3ZrPO4Cl4. The solid electrolyte of Example 11 was synthesized in the same manner as in Example 4, except for the time from the start of synthesis until the addition of LiCl. In Example 12, synthesis was started with Zr3(PO4)4 and ZrCl4, LiCl was added 1 hour after the start of synthesis, and the mechanochemical reaction was continued for another 23 hours to synthesize Li3ZrPO4Cl4. The solid electrolyte of Example 12 was synthesized in the same manner as in Example 4, except for the time from the start of synthesis until the addition of LiCl.

[0102] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0103] "Example 13" The solid electrolyte (Li6PS5Cl) of Example 13 was synthesized in the same manner as in Example 1, except that all the raw materials were added at the same time. Specifically, the raw material powders of lithium sulfide (Li2S), phosphorus sulfide (P2S5), and lithium chloride (LiCl) were weighed out so that the molar ratio was 5:1:2, respectively, and were added to a closed vessel made of zirconia, and were subjected to a mechanochemical reaction for 24 hours to synthesize the solid electrolyte (Li6PS5Cl).

[0104] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0105] "Example 14" The solid electrolyte of Example 14 (Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 ) was synthesized in the same manner as in Example 1, except that all the raw materials were added at the same time. Specifically, the raw material powders of lithium sulfide (Li2S), silicon sulfide (Si2S), phosphorus sulfide (P2S5), and lithium chloride (LiCl) were weighed out to have a molar ratio of 4.62:1.74:0.72:0.3, respectively, and were added to a closed vessel made of zirconia and subjected to a mechanochemical reaction for 24 hours to produce a solid electrolyte (Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 ) was synthesized.

[0106] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0107] "Comparative Example 1" The solid electrolyte of Comparative Example 1 (Li2ZrSO4Cl) was prepared in the same manner as the solid electrolyte of Example 3, except that LiCl was added a predetermined time after the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, to synthesize Li2ZrSO4Cl4. Specifically, synthesis was started with Zr(SO4)2 and ZrCl4, LiCl was added 0.5 hours after the start of synthesis, and the mechanochemical reaction was continued for another 23.5 hours to synthesize Li2ZrSO4Cl4. The solid electrolyte of Comparative Example 1 was synthesized in the same manner as in Example 3, except for the time from the start of synthesis until the addition of LiCl.

[0108] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0109] "Comparative Example 2" The solid electrolyte of Comparative Example 2 (Li2ZrOCl4) was synthesized in the same manner as the solid electrolyte of Example 2, except that the remaining half of LiCl was added after a predetermined time from the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, thereby synthesizing Li2ZrOCl4. Specifically, synthesis was started with half of LiCl and ZrOCl2, and the remaining half of LiCl was added 0.5 hours after the start of synthesis, and the mechanochemical reaction was continued for another 23.5 hours to synthesize Li2ZrOCl4. The solid electrolyte of Comparative Example 2 was synthesized in the same manner as in Example 2, except for the time from the start of synthesis until the remaining half of LiCl was added.

[0110] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0111] "Comparative Example 3" The solid electrolyte of Comparative Example 3 (Li3ZrPO4Cl4) was prepared in the same manner as the solid electrolyte of Example 4, except that LiCl was added a predetermined time after the start of synthesis, and a mechanochemical reaction was further carried out so that the synthesis time, including the predetermined time, was 24 hours, to synthesize Li3ZrPO4Cl4. Specifically, synthesis was started with Zr3(PO4)4 and ZrCl4, and the remaining half of LiCl was added 0.5 hours after the start of synthesis, and the mechanochemical reaction was continued for another 23.5 hours to synthesize Li3ZrPO4Cl4. The solid electrolyte of Example 11 was synthesized in the same manner as in Example 4, except for the time from the start of synthesis until the addition of LiCl.

[0112] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0113] "Comparative Example 4" The solid electrolyte (Li2ZrSO4FCl3) of Comparative Example 4 was synthesized in the same manner as in Example 1, except that all the raw materials were added at the same time. Specifically, the raw material powders of lithium chloride (LiCl), lithium fluoride (LiF), zirconium sulfate (Zr(SO4)2), and zirconium chloride (ZrCl4) were weighed out to have a molar ratio of 2:2:1:1, and were added to a closed zirconia container and subjected to a mechanochemical reaction for 24 hours to synthesize the solid electrolyte (Li2ZrSO4FCl3).

[0114] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0115] "Comparative Example 5" The solid electrolyte (Li2ZrSO4Cl3Br) of Comparative Example 5 was synthesized in the same manner as in Example 1, except that all the raw materials were added at the same time. Specifically, the raw material powders of lithium chloride (LiCl), lithium bromide (LiBr), zirconium sulfate (Zr(SO4)2), and zirconium chloride (ZrCl4) were weighed out to have a molar ratio of 2:2:1:1, and were added to a closed zirconia container and subjected to a mechanochemical reaction for 24 hours to synthesize the solid electrolyte (Li2ZrSO4Cl3Br).

[0116] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0117] "Comparative Example 6" The solid electrolyte (Li2ZrSO4Cl3I) of Comparative Example 6 was synthesized in the same manner as in Example 1, except that all the raw materials were added at the same time. Specifically, the raw material powders of lithium chloride (LiCl), lithium iodide (LiI), zirconium sulfate (Zr(SO4)2), and zirconium chloride (ZrCl4) were weighed out to have a molar ratio of 2:2:1:1, and were added to a closed zirconia container and subjected to a mechanochemical reaction for 24 hours to synthesize the solid electrolyte (Li2ZrSO4Cl3I).

[0118] The combination of raw materials (composition and molar ratio), as well as the synthesis time and characteristics of the synthesis process, are summarized in the following Table 1. In addition, the measurement results of the properties of the solid electrolyte are summarized in the following Table 2.

[0119] [Table 1]

[0120] [Table 2]

[0121] For the solid electrolytes of Examples 1, 2, 4, 7 to 14, the ionic conductivity before the 80°C storage test was 1×10 -3 [S / cm] or more, and the ionic conductivity after storage test at 80°C is also 1×10 -3 [S / cm] or higher, achieving both high ionic conductivity and high thermal stability. In addition, the solid electrolytes of Examples 5 and 6 also had an ionic conductivity of 7×10 -4 [S / cm] or more, and the ionic conductivity after storage test at 80°C is also 6×10 -4 [S / cm] or more, and high ionic conductivity close to the solid electrolytes of Examples 1, 2, 4, and 7 to 14 and high thermal stability are both achieved. Furthermore, the solid electrolyte of Example 3 also had an ionic conductivity of 3.1 × 10 before the 80°C storage test. -4 [S / cm] or more, and the ionic conductivity after storage test at 80°C is also 2.8×10 -4[S / cm] or higher, achieving both high ionic conductivity and high thermal stability.

[0122] The solid electrolytes in Examples 1, 5, and 6 have the same composition (Li2ZrCl6), but differ in ionic conductivity. The ionic conductivity of Example 1 is 2.0×10 -3 [S / cm], and the ionic conductivity of Example 5 is 7.5×10 -4 [S / cm], and the ionic conductivity of Example 6 is 9.0×10 -4 [S / cm]. This difference is considered to be mainly due to the difference in structure and crystallinity (degree of amorphousness). This difference in structure and crystallinity is considered to be due to the difference in the conditions of the synthesis process. That is, the time from the start of synthesis to the addition of the remaining half of LiCl was 2 hours, 1 hour, and 3 hours in Examples 1, 5, and 6, respectively. The decrease in ionic conductivity before and after the 80°C storage test (the ratio of "difference in ionic conductivity before and after the 80°C storage test / ionic conductivity before the 80°C storage test") was 5%, 15%, and 3% in Examples 1, 5, and 6, respectively. Furthermore, the resistance increase rates due to storage at 80° C. were 5%, 17%, and 3% in Examples 1, 5, and 6, respectively, which were lower than those of the comparative example. As described above, even with the same composition, it was possible to achieve both high ionic conductivity and high thermal stability by adjusting the conditions of the synthesis process.

[0123] The solid electrolytes of Examples 2, 7, and 8 have the same composition (Li2ZrOCl4), but differ in ionic conductivity. The ionic conductivity of Example 2 is 2.8×10 -3 [S / cm], and the ionic conductivity of Example 7 is 2.5×10 -3 [S / cm] [S / cm], and the ionic conductivity of Example 8 is 2.0 × 10 -3 [S / cm]. This difference is considered to be mainly due to the difference in structure and crystallinity (degree of amorphousness). This difference in structure and crystallinity is considered to be due to the difference in the conditions of the synthesis process. That is, the time from the start of synthesis to the addition of the remaining half of LiCl was 2 hours, 1 hour, and 3 hours in Examples 2, 7, and 8, respectively. On the other hand, the solid electrolyte of Comparative Example 2 has the same composition (Li2ZrOCl4) as Examples 2, 7, and 8, but the ionic conductivity (before the 80°C storage test) is lower than those of Examples 2, 7, and 8, being 1.0×10 -3 [S / cm], and after the 80°C storage test, it was 6.8×10 -4 The decrease in ionic conductivity before and after the 80° C. storage test was 32%, whereas it was 8%, 5%, and 7% for Examples 2, 7, and 8, respectively. Moreover, the resistance increase rates due to storage at 80° C. were 9%, 5% and 8% in Examples 2, 7 and 8, respectively, which were lower than Comparative Example 2, which was 48%. As described above, even with the same composition, it is possible to achieve both high ionic conductivity and high thermal stability by adjusting the conditions of the synthesis process.

[0124] The solid electrolytes of Examples 3, 9, and 10 have the same composition (Li2ZrSO4Cl4), but have different ionic conductivities. The ionic conductivity of Example 3 is 3.1×10 -4 [S / cm], and the ionic conductivity of Example 9 is 2.5×10 -3 [S / cm] [S / cm], and the ionic conductivity of Example 10 is 2.3 × 10 -3 [S / cm]. This difference is considered to be mainly due to the difference in structure and crystallinity (degree of amorphousness). This difference in structure and crystallinity is considered to be due to the difference in the conditions of the synthesis process. That is, the time from the start of synthesis to the addition of the remaining half of LiCl was 1 hour, 2 hours, and 3 hours in Examples 3, 9, and 10, respectively. On the other hand, the solid electrolyte of Comparative Example 1 also had the same composition (Li2ZrSO4Cl4) as Examples 3, 9, and 10, but the ionic conductivity (before the 80°C storage test) was lower than those of Examples 3, 9, and 10, at 2.0 × 10 -3 [S / cm], and after the 80°C storage test, it was 1.5×10 -3 The decrease in ionic conductivity before and after the 80° C. storage test was 27%, whereas it was 8%, 7%, and 6% in Examples 3, 9, and 10, respectively. Moreover, the resistance increase rates due to storage at 80° C. were 9%, 7% and 6% in Examples 3, 9 and 10, respectively, which were lower than Comparative Example 1, which was 37%. As described above, even with the same composition, it is possible to achieve both high ionic conductivity and high thermal stability by adjusting the conditions of the synthesis process.

[0125] The solid electrolytes of Examples 4, 11, and 12 have the same composition (Li3ZrPO4Cl4), but have different ionic conductivities. The ionic conductivity of Example 4 is 2.2×10 -3 [S / cm], and the ionic conductivity of Example 11 is 2.1×10 -3 [S / cm] [S / cm], and the ionic conductivity of Example 12 is 1.8 × 10 -3 [S / cm]. This difference is considered to be mainly due to the difference in structure and crystallinity (degree of amorphousness). This difference in structure and crystallinity is considered to be due to the difference in the conditions of the synthesis process. That is, the time from the start of synthesis to the addition of the remaining half of LiCl was 2 hours, 3 hours, and 1 hour in Examples 4, 11, and 12, respectively. On the other hand, the solid electrolyte of Comparative Example 3 has the same composition (Li3ZrPO4Cl4) as Examples 4, 11, and 12, but the ionic conductivity (before the 80°C storage test) is lower than those of Examples 4, 11, and 12, being 1.8 × 10 -3 [S / cm], and after the 80°C storage test, it was 1.3×10 -3 The decrease in ionic conductivity before and after the 80° C. storage test was 25%, whereas it was 15%, 10%, and 16% in Examples 4, 11, and 12, respectively. Moreover, the resistance increase rates due to storage at 80° C. were 17%, 11% and 19% in Examples 3, 9 and 10, respectively, which were lower than Comparative Example 3, which was 33%. As described above, even with the same composition, it is possible to achieve both high ionic conductivity and high thermal stability by adjusting the conditions of the synthesis process. [Explanation of symbols]

[0126] 10...solid electrolyte layer, 20...positive electrode, 22...positive electrode current collector, 24...positive electrode mixture layer, 30...negative electrode, 32 ... negative electrode current collector, 34 ... negative electrode mixture layer, 40 ... power generating element, 50 ... exterior body, 52 ... metal foil, 54...resin layer, 60,62...terminal, 100...all-solid battery

Claims

1. A compound containing Li, one or more elements selected from the group consisting of elements in groups 3 to 15, and a halogen, The halogen includes Cl; The negative ion analysis of the compound by time-of-flight secondary ion mass spectrometry revealed that LiCl 2 The peak is detected, The LiCl relative to the peak intensity Rb of all ions 2 A solid electrolyte, wherein a peak intensity ratio R1 (Ra / Rb) to a peak intensity Ra of the solid electrolyte satisfies 0.041>R1>0.

011.

2. The solid electrolyte according to claim 1 , wherein R1 (Ra / Rb) satisfies 0.030>R1>0.

019.

3. The solid electrolyte according to claim 1 , wherein the compound is represented by the following formula (1): LiaEbGcCldXe...(1) In formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids, and G is OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , P.O. 3 , P.O. 4 , P 2 O 7 , P 3 O 10 , S.O. 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , B.F. 4 , P.F. 6 ,BOB,(COO) 2 , N, AlCl 4 , C.F. 3 SO 3 , C.H. 3 COO, CF 3 COO,OOC-(CH 2 ) 2 -COO,OOC-CH 2 -COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH 2 -COO, C 6 H 5 SO 3 , OOC-CH=CH-COO, C(OH)(CH 2 COOH) 2 COO, A.S.O. 4 , BiO 4 , CrO 4 , MnO 4 , PtF 6 , PtCl 6 , PtBr 6 , PtI 6 , SbO 4 , SeO 4 , TeO 4 , HCOO, and O; X is one or more elements selected from the group consisting of F, Br, and I; and 0.5≦a<6, 0<b<2, 0≦c≦6, 0<d≦6.1, and 0≦e<6.

1.

4. The solid electrolyte according to claim 1 , wherein the compound is represented by the following formula (2): LiqMrPsOtCluSv...(2) (In formula (2), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, and Cl is chlorine. q, r, s, t, u, and v are each 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×s−t−u / 2.)

5. The solid electrolyte according to claim 1, wherein the compound is one or more of the compounds represented by the following formulas (3) to (6): Li 2 Black 6 ・・・(3) Li 2 Black 4 ・・・(4) <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> 25O<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> Cl<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr">・・・(5) Li 3 ZrPO 4 Cl 4 ・・・(6)

6. The positive electrode and the negative electrode face each other via a solid electrolyte layer, An all-solid-state battery comprising the solid electrolyte according to any one of claims 1 to 5 in at least one of the solid electrolyte layer, the positive electrode, and the negative electrode.

Citation Information

Patent Citations

  • Solid electrolyte, solid electrolyte layer, and solid electrolyte battery

    JP2021163522A

  • Positive electrode active material, positive electrode active material layer, and all-solid-state battery

    JP2022139663A

  • Solid electrolyte material and all-solid state battery

    JP2022151964A

  • Solid electrolyte material and battery using same

    WO2020137153A1

  • Solid electrolyte material and battery using same

    WO2020137155A1