Silica-titania composite oxide powder, and resin composition
A silica-titania composite oxide powder with controlled refractive index and specific surface area is produced to address transparency and viscosity issues in silicone and epoxy resins, ensuring effective viscosity adjustment and transparency in optical applications.
Patent Information
- Application Number
- JP2023059025
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional silica-titania composite oxide powders used as additives for silicone and epoxy resins lack the appropriate refractive index, specific surface area, and transparency, leading to ineffective viscosity adjustment and transparency issues in optical applications.
A silica-titania composite oxide powder is produced by burning a mixed gas of siloxane and titanium alkoxide under controlled conditions, achieving a refractive index of 1.47 to 1.61, amorphous crystal type, and a specific surface area of 150 to 400 m²/g, ensuring strong interactions with the resin for effective viscosity adjustment.
The powder maintains transparency and exhibits high viscosity adjustment effects, such as thixotropy and thickening, when added to silicone and epoxy resins, making it suitable for optical applications.
Smart Images

Figure 2024146241000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel silica-titania composite oxide powder, specifically to a silica-titania composite oxide powder that is suitably used as an additive for adjusting viscosity characteristics while maintaining transparency of silicone resins, epoxy resins, etc. [Background technology]
[0002] Silicone resins and epoxy resins with a refractive index in the range of 1.47 to 1.61 are used as transparent encapsulants for optical elements such as LEDs after their viscosity characteristics, such as thixotropy and thickening, have been adjusted.
[0003] In adjusting the viscosity characteristics of resins, fumed silica powder is used as an additive, but the refractive index of fumed silica does not match that of the resin, and transparency cannot be maintained, making it unsuitable for optical applications.
[0004] As an additive whose refractive index matches that of the resin, there is a silica-titania composite oxide powder (Patent Documents 1 and 2). However, since the specific surface area of the conventional powder is small, the interaction between the particles constituting the powder and between the particles and the resin is weak, and there is a problem that the viscosity adjusting effect is not expressed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-036168 A [Patent Document 2] JP 2020-070223 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a silica-titania composite oxide powder that is suitable for use as an additive for silicone resins and epoxy resins, i.e., a silica-titania composite oxide powder that has an appropriate refractive index, crystal type and specific surface area and can both maintain the transparency of silicone resins and epoxy resins and adjust the viscosity characteristics. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result, have succeeded in obtaining a silica-titania composite oxide powder that solves the above problems by combusting a mixed gas of siloxane, which is an organosilicon compound, and titanium alkoxide, which is an organotitanium compound, under specific conditions, thereby completing the present invention.
[0008] That is, the present invention provides a silica-titania composite oxide powder that satisfies all of the following requirements: (1) Refractive index at a wavelength of 589 nm is 1.47 to 1.61 (2) The crystal form is amorphous (3) Specific surface area is 150 to 400 m 2 / g Effect of the Invention
[0009] The silica-titania composite oxide powder of the present invention has a refractive index of 1.47 to 1.61, which is within the range of silicone resins and epoxy resins used in optical applications, and has a uniform amorphous composition within the particles, so when added to these resins, it maintains the transparency of the resin and exhibits extremely high transparency as a composition. In addition, the specific surface area is 150 to 400 m 2 / g, the interaction between particles and between the particles and the resin is strong, and when added to a resin, a viscosity adjusting effect such as thixotropy and thickening is exhibited. In other words, the silica-titania composite oxide powder of the present invention is useful as an additive to resins for optical applications and as a resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The silica-titania composite oxide powder of the present invention is (1) Refractive index at a wavelength of 589 nm is 1.47 to 1.61 (2) The crystal form is amorphous (3) Specific surface area is 150 to 400 m 2 / g It is characterized in that all of the above is satisfied.
[0011] The silica-titania composite oxide powder of the present invention has a refractive index of 1.47 to 1.61 at a wavelength of 589 nm. Since the refractive index is within this range, when this powder is added to silicone resins or epoxy resins used in transparent sealing materials, the transparency of these resins is not impaired and these resins exhibit excellent performance.
[0012] The refractive index of the silica-titania composite oxide powder of the present invention at a wavelength of 589 nm is a value measured by a liquid immersion method. That is, a liquid whose temperature dependence of the refractive index is known is used as a dispersion medium, and the powder to be measured is dispersed in it. Then, the temperature dependence of the transparency (transmittance or absorbance) of the dispersion liquid at a wavelength of 589 nm is measured, and the dispersion liquid temperature at which the transparency is highest (absorbance is lowest) is determined. The refractive index of the dispersion medium at that temperature is then taken as the refractive index of the powder.
[0013] The silica-titania composite oxide powder of the present invention has an amorphous crystal type. The crystal type is identified by XRD measurement. A case where no peak is detected in the XRD pattern is amorphous. Examples of crystalline phases that can be generated in silica-titania composite oxide include anatase-type titania and rutile-type titania. The confirmation of a crystalline phase in silica-titania composite oxide powder means that the inside of the particles constituting the powder is phase-separated and the components are spatially non-uniform. This state is the same as a mixture of powders having different refractive indices, and even if the refractive index is within the above-mentioned range, the transparency effect is not exhibited. For the expression of transparency, it is an essential feature that the crystal type is amorphous, that is, that the crystal type is spatially uniform.
[0014] Furthermore, when titania separates and precipitates in the silica-titania composite oxide, the powder exhibits photocatalytic activity, and therefore, when added to a resin, this can cause the resin to deteriorate, making it unsuitable as an additive in that sense as well.
[0015] The silica-titania composite oxide of the present invention has a specific surface area of 150 to 400 m 2 / g. The specific surface area is measured by nitrogen adsorption BET 1 point. 2 If the specific surface area is less than 150 m / g, the interaction between the particles that make up the powder and between the particles and the resin is weak when the powder is added to the resin, and therefore the viscosity adjusting effect such as thixotropy or thickening is not achieved. 2 The primary particle size of powders with a specific surface area of less than 400 m2 is large, which tends to scatter light and is poor in transparency. 2 When the specific surface area is greater than 200 to 350 m / g, the particles that make up the powder are small and the curvature of the particle surface is large. If the curvature is large, the chemical bonds of the atoms that make up the surface are distorted, resulting in high surface reactivity and making the surface more susceptible to chemical reactions with resins, making the powder unsuitable as a viscosity adjusting additive. In terms of transparency and reactivity, a specific surface area of 200 to 350 m 2 / g is a more preferred embodiment.
[0016] From the viewpoint of transparency and viscosity adjustment, it is preferable that the powder is easily dispersible. That is, the dispersibility index n of the silica-titania composite oxide powder of the present invention is preferably 2.5 or more. Here, the dispersibility index n is the absorbance τ of a water suspension containing the powder at a concentration of 0.25 mass % for light with a wavelength of 460 nm. 460 and absorbance τ for light with a wavelength of 700 nm 700 Using n = ln(τ 460 / τ 700 ) / ln(700 / 460). The dispersibility index n is related to the dispersed particle size, and the smaller the dispersed particle size, the larger the dispersibility index n. Powders with a large dispersibility index n are easily dispersed as small particles in a medium, and are favorable in terms of transparency, thixotropy, and viscosity.
[0017] The chemical formula for the silica-titania composite oxide powder of the present invention is Si 1-x Ti x O2 (0≦x≦1). When x=0, it corresponds to silica, and when x=1, it corresponds to titania. x is the ratio of the number of moles of Ti to the sum of the number of moles of Si and the number of moles of Ti in the powder, that is, x=number of moles of Ti / (number of moles of Si+number of moles of Ti). In the present invention, this mol% expression is called Ti molar ratio (mol%). That is, Ti molar ratio (mol%)=100×number of moles of Ti / (number of moles of Si+number of moles of Ti). The Ti molar ratio can be determined by XRF measurement. The refractive index of the silica-titania composite oxide powder increases in proportion to the Ti molar ratio. For the silica-titania composite oxide powder of the present invention, the relationship of refractive index=1.46+0.06×Ti molar ratio (mol%) / 10 generally exists.
[0018] The method for producing the silica-titania composite oxide powder of the present invention is not particularly limited, but it can be produced by a method for burning a mixture of siloxane and titanium alkoxide, that is, a method for co-firing siloxane and titanium alkoxide.
[0019] Examples of the siloxane include hexamethyldisiloxane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and decamethylcyclopentasiloxane.
[0020] Examples of titanium alkoxides include tetramethoxytitanium, tetraethoxytitanium, tetra-i-propoxytitanium, tetra-n-propoxytitanium, tetra-n-butoxytitanium, tetra-s-butoxytitanium, and tetra-t-butoxytitanium.
[0021] One or more of the above siloxanes and one or more of the above titanium alkoxides can be used in combination.
[0022] In the co-firing method of siloxane and titanium alkoxide, the shape of the burner used is not particularly limited, but a concentric multi-tube burner is preferable in terms of ease of ignition, combustion stability, etc. The concentric multi-tube burner is composed of a center and a plurality of annular tubes extending concentrically from the center tube.
[0023] The method using a concentric quadruple tube burner consisting of a central tube and three annular tubes is described in detail below.
[0024] The gases introduced into the burner are outlined below. A gas containing both siloxane and titanium alkoxide is introduced into the central tube. A gas containing a flammable gas is introduced into the first annular tube outside the central tube. A combustion supporting gas is introduced into the second annular tube outside the first annular tube. A gas such as air is introduced into the third annular tube outside the second annular tube. The following describes in detail the central tube, first annular tube, second annular tube, and third annular tube in that order.
[0025] First, vaporized siloxane, titanium alkoxide, and oxygen are mixed in advance and introduced into the central tube. In this case, in addition to siloxane, titanium alkoxide, and oxygen, an inert gas such as nitrogen may be mixed. Air may also be used as an oxygen source.
[0026] The refractive index of the silica-titania composite oxide powder can be adjusted using the raw material Ti molar ratio calculated from the number of moles of Si and the number of moles of Ti contained in the raw materials of the powder, siloxane and titanium alkoxide, as an index. Here, the raw material Ti molar ratio is Raw material Ti molar ratio (mol%) = 100 x number of moles of Ti contained in raw material / (number of moles of Si contained in raw material + number of moles of Ti contained in raw material).
[0027] The above will be explained by taking as an example a case where octamethylcyclotetrasiloxane (abbreviated as D4) is used as the siloxane and tetra-i-propoxytitanium (abbreviated as TTPO) is used as the titanium alkoxide as the raw materials, that is, a method of co-firing D4 and TTPO.
[0028] The Si content per molecule of D4 is 4 atoms, and the Ti content is 0. The Si content per molecule of TTPO is 0 atoms, and the Ti content is 1 atom. From this, the raw material Ti molar ratio in the co-firing method of D4 and TTPO can be calculated as Raw material Ti molar ratio (mol%) = 100 × number of moles of TTPO supplied / (4 × number of moles of D4 supplied + number of moles of TTPO supplied).
[0029] In order to obtain a desired refractive index, the powder can be manufactured as follows. First, the raw material Ti molar ratio is set so that the desired refractive index = 1.46 + 0.06 × raw material Ti molar ratio (mol%) / 10 is satisfied. Next, using the set raw material Ti molar ratio, the D4 supply moles and TTPO supply moles are determined as manufacturing conditions so that the raw material Ti molar ratio (mol%) = 100 × TTPO supply moles / (4 × D4 supply moles + TTPO supply moles) is satisfied. Then, manufacturing is carried out under the determined conditions. After manufacturing, the refractive index of the obtained silica-titania composite oxide powder is measured, and if there is a deviation from the desired value, fine adjustment of the raw material Ti molar ratio by increasing or decreasing it according to the deviation may be repeated until the desired value is obtained.
[0030] The crystal type and specific surface area can be adjusted using the raw material concentration in the central tube as an index. The raw material concentration in the central tube can be calculated using only the moles of gas supplied to the central tube: Raw material concentration (mol%) = 100 x (moles of siloxane + moles of titanium alkoxide) / total moles of gas supplied to the central tube.
[0031] The lower the concentration of the raw material in the central tube, the higher the specific surface area, but the lower the flame temperature, making it difficult for the crystal form to become amorphous. On the other hand, the higher the concentration, the easier it is for the crystal form to become amorphous due to the high flame temperature, but the lower the specific surface area. In order to obtain the silica-titania composite oxide powder of the present invention, it is preferable that the raw material concentration in the central tube is in the range of 0.8 to 1.2 mol%. If the concentration is below 0.8 mol%, the flame temperature becomes too low, so that titania precipitates as a crystalline phase, and the inside of the particles constituting the powder becomes a separated phase structure containing crystals, and is no longer amorphous. Also, if the concentration exceeds 1.2 mol%, the specific surface area is increased to 150 m 2 In terms of achieving both the crystal type and the specific surface area, it is more preferable that the raw material concentration in the central tube is 0.9 to 1.2 mol %.
[0032] The refractive index, crystal type, and specific surface area are adjusted as described above. In addition, in order to produce the silica-titania composite oxide of the present invention, it is necessary to adjust the following two indices regarding the gas supplied to the central tube.
[0033] One is the O2 concentration in the central tube, where the O2 concentration in the central tube is O2 concentration (mol%) = 100 × number of moles of O2 supplied to the central tube / total number of moles of gases other than combustible gases supplied to the central tube.
[0034] The other is the RO of the central tube, where RO is the number of moles of O2 supplied to the central tube / the number of moles of O2 required for stoichiometric complete combustion of the combustible gas supplied to the central tube.
[0035] In particular, when D4, TTPO, pure oxygen, pure nitrogen, and air are supplied to the central tube, the formulas for calculating O2 concentration and RO are as follows: O2 concentration (mol%) = 100 x (number of moles of pure oxygen + 0.21 x number of moles of air) / (number of moles of pure oxygen + number of moles of pure nitrogen + number of moles of air), RO = (number of moles of pure oxygen + 0.21 x number of moles of air) / (16 x number of moles of D4 + 18 x number of moles of TTPO). Here, we use the fact that 16 moles of O2 are required for stoichiometric complete combustion of 1 mole of D4, and 18 moles of O2 are required for stoichiometric complete combustion of 1 mole of TTPO.
[0036] The O2 concentration must be 18 mol% or more. If it is less than 18 mol%, the combustion reaction rate is too slow, and the reaction does not proceed. Therefore, the combustion reaction is not complete, and the silica-titania composite oxide powder of the present invention cannot be obtained.
[0037] In addition, RO must be 0.2 or more. If it is less than 0.2, the raw materials siloxane and titanium alkoxide will burn incompletely, producing solid carbon or solid carbide, and the silica-titania composite oxide powder of the present invention cannot be obtained.
[0038] In the first annular tube located outside the central tube, a combustible gas such as hydrogen or a hydrocarbon is introduced to form a combustion supporting flame. Inert gas such as nitrogen and / or a combustion supporting gas such as air may be mixed in. The mixing ratio can be, for example, as follows: Combustible gas concentration (mol%) = 100 x total number of moles of combustible gas supplied to the first annular tube / total number of moles of gas supplied to the first annular tube.
[0039] The amount of combustible gas in the first annular pipe may be set appropriately as long as a flame can be formed, but in terms of facilitating the formation of a stable flame, it is desirable to set the auxiliary fuel ratio R1 in the range of 0.005 to 0.5. Here, R1 = the number of moles of O2 required for the combustible gas supplied to the first annular pipe to stoichiometrically burn completely / the number of moles of O2 required for the combustible gas supplied to the central pipe to stoichiometrically burn completely. If R1 is greater than 0.5, there is no particular effect and it is economically disadvantageous. If it is less than 0.005, the combustion becomes unstable and a flame is not formed. In addition, in order to prevent the generation of solid carbon or solid carbides, the type of combustible gas supplied to the first annular pipe is preferably a combustible gas such as hydrogen or ammonia that does not contain carbon atoms, and particularly preferably hydrogen.
[0040] In the second annular pipe, which is located outside the first annular pipe, a combustion support gas such as oxygen is introduced to form a combustion support flame. At this time, an inert gas such as nitrogen may be mixed. For example, the mixture ratio can be indicated as O2 concentration (mol%) = 100 x number of moles of O2 supplied to the second annular pipe / total number of moles of gas supplied to the second annular pipe.
[0041] The amount of combustion-supporting gas in the second annular pipe may be set appropriately as long as a flame can be formed, but it is preferable to supply it so that the combustion-supporting oxygen ratio R2 is 0.1 to 2.0. Here, R2 = number of moles of O2 supplied to the second annular pipe / number of moles of O2 required for stoichiometric complete combustion of the combustible gas supplied to the central pipe. If it is greater than 2.0, there is no particular effect and it is economically disadvantageous. If it is less than 0.1, the combustion becomes unstable and a flame is not formed.
[0042] In order to adjust the gas flow of the flame, pure oxygen, air, pure nitrogen, or a mixture of these gases is supplied to the third annular pipe. From the viewpoint of economy, the use of air is a preferred embodiment.
[0043] The silica-titania composite oxide produced as described above is separated from the combustion gas by filter separation using a metal filter, ceramic filter, bag filter or the like, or by centrifugal separation using a cyclone or the like, and is recovered and taken out as a powder.
[0044] The silica-titania composite oxide powder of the present invention can be used as a viscosity adjusting additive for transparent encapsulants for optical elements such as LEDs, which are based on silicone resins or epoxy resins, by utilizing its refractive index range, crystal type, and specific surface area range. EXAMPLES
[0045] EXAMPLES In the following, examples and comparative examples are shown to specifically explain the present invention, but the present invention is not limited to these examples.
[0046] In the following examples and comparative examples, various physical properties were measured by the following methods.
[0047] (1) Refractive index measurement Benzyl alcohol, 1-pentanol, and 1-bromonaphthalene were mixed in a predetermined mass ratio to prepare a mixed solvent for refractive index measurement.
[0048] 10 g of the mixed solvent was placed in a 20 ml glass container (AS ONE Labolan screw vial, model no. 5), and 0.2 g of silica-titania composite oxide powder, which had been dried overnight at 120°C, was then added to the mixed solvent. The powder-containing mixed solvent was then dispersed for 1 minute at 28% output using an ultrasonic cell disrupter (BRANSON Sonifier SFX250, probe: 1 / 4 inch). During dispersion, the powder-containing mixed solvent was cooled in an ice-water bath.
[0049] The refractive index of the mixed solvent without powder added at a wavelength of 589 nm was measured in the temperature range of 10 to 40°C using an Atago digital refractometer RX-7000i.
[0050] The absorbance of the mixed solvent containing the dispersed powder at a wavelength of 589 nm was measured at temperatures ranging from 10 to 40°C using a JASCO V-650 spectrophotometer equipped with a temperature control folder. The measurement sample was placed in a quartz cell with an optical path length of 10 mm. The refractive index of the mixed solvent without powder at the temperature showing the minimum absorbance was taken as the refractive index of the silica-titania composite oxide powder.
[0051] (2) Crystal type measurement (XRD measurement) The crystal type was measured using an X-ray diffractometer (Rigaku SmartLab). The measurement conditions were CuKα radiation, scan range 2θ = 10 to 90 °, scan speed 1 ° / min, and step width 0.02 °. Cases where no peaks were detected in the obtained X-ray diffraction pattern were determined to be amorphous.
[0052] (3) Specific surface area measurement The measurement was performed by the nitrogen adsorption BET one-point method using a BET specific surface area measuring device SA-1000 manufactured by Shibata Scientific Co., Ltd.
[0053] (4) Measurement of Ti molar ratio (XRF measurement) The Ti molar ratio was measured using a fluorescent X-ray analyzer (Rigaku ZSX Primus IV). Using the amounts of Si and Ti obtained by the analyzer, the Ti molar ratio was calculated as Ti molar ratio (mol%) = 100 × Ti amount / (Si amount + Ti amount). Note that the amounts of Si and Ti in the Ti molar ratio calculation formula are based on the amount of substance (number of moles).
[0054] (5) Dispersity index measurement A 0.25% by mass aqueous suspension of the powder to be measured was prepared as follows: 0.05 g of powder and 20 ml of distilled water were placed in a 30 ml glass container (AS ONE Lablan Sample Vial, Model No. 6), the glass container containing the sample was placed so that the bottom of the probe tip of an ultrasonic cell disrupter (BRANSON Sonifier II Model 250D, probe: 1 / 4 inch) was 15 mm below the water surface, and the powder was dispersed in distilled water at an output of 20 W and for a dispersion time of 3 minutes to prepare a 0.25% by mass aqueous suspension of the powder to be measured.
[0055] The absorbance τ of the resulting aqueous suspension at 460 nm 460 and absorbance τ for light with a wavelength of 700 nm 700 was measured using a spectrophotometer V-630 manufactured by JASCO Corp. The measurement sample was placed in a quartz cell with an optical path length of 10 mm.
[0056] The τ obtained above 460 and τ 700 Using this, we calculate the dispersion index n as n = ln(τ 460 / τ 700 ) / ln(700 / 460).
[0057] Examples 1 to 6, Comparative Examples 1 to 5 As shown below, D4 and TTPO were combusted in a concentric quadruple tube burner to produce silica-titania composite oxide powder. Two types of concentric quadruple tube burners were used, one with a ratio of the third annular tube outer diameter to the central tube diameter of 4.0 and the other with a ratio of 6.8. Other dimensions, such as the central tube diameter, the first annular tube, the second annular tube, and the third annular tube inner diameter, were the same for both.
[0058] Heated and vaporized D4, TTPO, pure oxygen, air, and pure nitrogen were supplied to the central tube. Hydrogen and pure nitrogen were supplied to the first annular tube. Pure oxygen or a mixture of pure oxygen and air was supplied to the second annular tube. Air was supplied to the third annular tube. The burner used, production conditions, physical properties of the obtained silica-titania composite oxide powder, and composition of the mixed solvent used in refractive index measurement are shown in Table 1.
[0059] [Table 1]
Claims
1. A silica-titania composite oxide powder characterized by satisfying all of the following conditions (1) to (3): (1) A refractive index at a wavelength of 589 nm is 1.47 to 1.
61. (2) The crystal form is amorphous. (3) Surface area is 150 to 400 m 2 / g
2. A resin composition comprising the silica-titania composite oxide powder according to claim 1.
Citation Information
Patent Citations
Curable composition and its cured body
JP1992225052A
Inorganic powder having low refractive index, its production and liquid detergent composition and transparent dentifrice composition using the same
JP1996012319A
Inorganic particle for dental material and method for producing the same
JP2003146822A
Aggregate of silica-based compound oxide particle and method for manufacturing the same
JP2008037700A
Silica-titania composite oxide particle and manufacturing method therefor
JP2017036168A