Composition for polishing and method for manufacturing magnetic disk substrate
A polishing composition with silica particles and specific additives addresses the issue of scratches on magnetic disk substrates, enhancing surface quality for higher recording densities.
Patent Information
- Application Number
- JP2023059203
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Conventional polishing compositions for magnetic disk substrates fail to effectively reduce scratches, which hinders the achievement of higher recording densities due to surface defects.
A polishing composition containing silica particles with specific particle size distributions and additives like sulfuric ester containing polyalkylene oxide and naphthalene sulfonic acid formaldehyde condensate, along with controlled pH and oxidizing agents, is used to minimize scratches during the polishing process.
The composition significantly reduces scratches on magnetic disk substrates, enabling high-quality surface finishes suitable for higher recording densities.
Smart Images

Figure 2024146357000001 
Figure 2024146357000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition and a method for producing a magnetic disk substrate using the polishing composition. [Background technology]
[0002] Conventionally, the manufacturing process of a substrate that requires a highly accurate surface includes a step of polishing the substrate, which is the raw material of the substrate, using a polishing liquid. For example, in the manufacture of a nickel-phosphorus-plated magnetic disk substrate (hereinafter also referred to as Ni-P substrate), polishing that places emphasis on polishing efficiency (primary polishing) and final polishing (finish polishing) that is performed to achieve the surface accuracy of the final product are generally performed. Patent Document 1 is an example of a technical document related to a polishing composition used for polishing a magnetic disk substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-174009 A Summary of the Invention [Problem to be solved by the invention]
[0004] In response to recent demands for higher recording density of magnetic disk drives, etc., polishing compositions used for polishing magnetic disk substrates are required to have the ability to reduce defects (e.g., scratches) that occur on the surface of the magnetic disk substrate when the magnetic disk substrate is polished with the polishing composition. If a polishing composition having practical processability and excellent defect reduction performance is provided, it is useful because it can be used to productively produce magnetic disk substrates having high-quality surfaces that lead to higher recording density of magnetic disk drives.
[0005] The present invention has been made in view of the above circumstances, and aims to provide a polishing composition that can be used to polish Ni-P substrates and reduce scratches. Another related aim is to provide a method for producing Ni-P substrates using such a polishing composition. [Means for solving the problem]
[0006] According to the present specification, a polishing composition is provided for polishing a magnetic disk substrate (Ni-P substrate) having a nickel phosphorus plating layer. The polishing composition contains silica particles as abrasive grains and water. The abrasive grains have a number ratio of particles with a particle diameter of less than 10 nm based on observation with a transmission electron microscope of 10% or less, and a cumulative 95% particle diameter D95 in a number-based cumulative particle size distribution from the small diameter side of 55 nm or less. When the abrasive grains have a cumulative 95% particle diameter D95 of less than the above upper limit and the number ratio of particles with a particle diameter of less than 10 nm contained in the abrasive grains is within the above range, the abrasive grains are used for polishing Ni-P substrates and tend to reduce scratches on the surface after polishing.
[0007] In some preferred embodiments, the abrasive grains have a number ratio of particles having a particle diameter of less than 10 nm based on observation with a transmission electron microscope of 6% or less, more preferably 2% or less. When the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains is within the above range, the above-mentioned scratch reduction effect can be more effectively exhibited.
[0008] In some embodiments, the polishing composition further contains one or more defect-reducing agents selected from the group consisting of sulfuric acid esters containing polyalkylene oxide and naphthalene sulfonic acid formaldehyde condensates. In the polishing composition disclosed herein, the sulfuric acid esters containing polyalkylene oxide and naphthalene sulfonic acid formaldehyde condensates tend to contribute to improving the effect of reducing scratches on the surface after polishing. A polishing composition containing such a defect-reducing agent can more effectively reduce scratches. From the viewpoint of reducing scratches, in some preferred embodiments, the number of oxyalkylene units (e.g., the number of oxyethylene units) of the sulfuric acid esters containing polyalkylene oxide (e.g., polyethylene oxide) is 2 or more and 13 or less.
[0009] In some embodiments, the abrasive grains exhibit a multimodal particle size distribution. In some embodiments, the abrasive grains exhibit a particle size distribution obtained by plotting particle size on the horizontal axis and number frequency (%) on the vertical axis based on transmission electron microscopy, in which there are two or more particle sizes that exhibit a maximum number frequency within a number frequency range of 0.50% or more, and the largest of the particle sizes that exhibit the maximum number frequency is designated as particle size D L The smallest one is the particle diameter D S When the particle size ratio (D L / D S ) is 1.40 or more. When such abrasive grains are used, the effect of obtaining good polishing workability while suppressing the generation of scratches is easily exhibited.
[0010] In some embodiments, the polishing composition further contains an acid. By containing an acid, good processability is easily obtained.
[0011] In some embodiments, the polishing composition further comprises an oxidizing agent. By including an oxidizing agent, good processability is easily obtained.
[0012] In some embodiments, the polishing composition further comprises a chelating agent. By including a chelating agent, the occurrence of defects on the polished surface after polishing is likely to be suppressed.
[0013] In some embodiments, the pH of the polishing composition is within the range of 1 to 4. When the polishing composition has such a pH, the effects of the technology disclosed herein are preferably exhibited.
[0014] In some embodiments, the polishing composition is used in the final polishing step.The polishing composition disclosed herein is easy to reduce scratches on the surface after polishing, so it is particularly suitable for the final polishing that requires high surface quality after polishing.The polishing composition disclosed herein can reduce scratches in the final polishing of Ni-P substrate.
[0015] In some embodiments, the above-mentioned polishing composition is stored before use in a plurality of parts, including part A containing abrasive grains and part B containing at least a part of components other than abrasive grains, and is prepared by mixing the above-mentioned plurality of parts when used.The polishing composition is easy to improve the dispersion stability of the polishing composition.When mixing, for example, acid, oxidizing agent, etc. can be further mixed.
[0016] This specification also provides a method for producing a magnetic disk substrate. The method includes a step of polishing a substrate to be polished with any one of the polishing compositions disclosed herein. This method can efficiently produce a magnetic disk substrate (Ni-P substrate) having a high-quality surface with few scratches. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field.
[0018] <Polishing composition> (Abrasive grain) The polishing composition disclosed herein contains abrasive grains. The abrasive grains have a particle diameter of less than 10 nm in number ratio of 10% or less based on transmission electron microscope observation, and a cumulative 95% particle diameter D95 in the cumulative particle size distribution based on the number from the small diameter side (cumulative number distribution from the small diameter side) is 55 nm or less. Here, the number ratio of particles with a particle diameter of less than 10 nm indicates the ratio of the number of particles with a particle diameter of less than 10 nm to the total number of all particles contained in the abrasive grains. In addition, the cumulative number distribution is typically represented by a curve that extends from the end (lower left) of cumulative 0% and the small diameter side of the particle diameter to the upper right and reaches the end (upper right) of cumulative 100% and the large diameter side of the particle diameter in a graph with the horizontal axis being the particle diameter and the vertical axis being the cumulative number (%). The abrasive grains disclosed herein have a number ratio of particles having a relatively small particle diameter of less than 10 nm of 10% or less, and a cumulative 95% particle diameter D95 in the cumulative particle size distribution of 55 nm or less, thereby effectively reducing scratches on the surface after polishing with a polishing composition containing the abrasive grains.
[0019] The reason why the above-mentioned effect is obtained is not particularly limited, but is considered to be, for example, as follows. That is, among the particles contained in the polishing composition, so-called fine particles with a small particle diameter may promote particle aggregation and become a factor in the formation of coarse foreign matter that causes scratches. The polishing composition disclosed here has a number ratio of particles with a particle diameter of less than 10 nm contained in the composition of a certain value or less, so that the formation of coarse foreign matter is suppressed and scratches after polishing tend to be reduced. In addition, the cumulative 95% particle diameter D95 is a certain value or less, and the inclusion of particles with a large particle diameter is suppressed, which is also considered to contribute to the reduction of scratches.
[0020] From the viewpoint of reducing scratches, it is considered advantageous that the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains is small. In some preferred embodiments, the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains is 8% or less, more preferably 6% or less, even more preferably 4% or less, and particularly preferably 2% or less (e.g., 1.8% or less). In some embodiments, the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains may be 1.5% or less, or may be 1% or less. When the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains is within the above range, the above-mentioned scratch reduction effect can be more effectively exhibited. The lower limit of the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains is not particularly limited. From the viewpoint of availability of abrasive grains, in some embodiments, the number ratio of particles having a particle diameter of less than 10 nm contained in the abrasive grains may be 0.1% or more, 0.2% or more, 0.5% or more, or 0.7% or more.
[0021] From the viewpoint of reducing scratches, in some embodiments, the cumulative 95% particle diameter D95 in the cumulative particle size distribution of the abrasive grains is 50 nm or less, may be 45 nm or less, may be 40 nm or less, or may be 38 nm or less. The lower limit of the cumulative 95% particle diameter D95 is not particularly limited, but from the viewpoint of processability, in some embodiments, the cumulative 95% particle diameter D95 is 15 nm or more, may be 20 nm or more, may be 25 nm or more, may be 30 nm or more, or may be 32 nm or more.
[0022] In the technology disclosed herein, the particle size distribution of the abrasive grains is not particularly limited as long as the number ratio of particles with a particle diameter of less than 10 nm and the cumulative 95% particle diameter D95 satisfy the respective predetermined conditions. In some embodiments, the cumulative 90% particle diameter D90 in the cumulative particle size distribution of the abrasive grains is 50 nm or less, may be 43 nm or less, may be 38 nm or less, or may be 36 nm or less. In some embodiments, the cumulative 90% particle diameter D90 is 13 nm or more, may be 18 nm or more, may be 23 nm or more, may be 28 nm or more, or may be 30 nm or more. When the cumulative 90% particle diameter D90 is in the above range, scratches tend to be reduced while maintaining processability.
[0023] In some embodiments, the cumulative 50% particle diameter D50 in the cumulative particle size distribution of the abrasive grains is 40 nm or less, may be 30 nm or less, may be 25 nm or less, may be 20 nm or less, or may be 16 nm or less. In some embodiments, the cumulative 50% particle diameter D50 is 10 nm or more, may be 11 nm or more, may be 12 nm or more, or may be 13 nm or more. When the cumulative 50% particle diameter D50 is in the above range, scratches tend to be reduced.
[0024] In some embodiments, the cumulative 10% particle diameter D10 in the cumulative particle size distribution of the abrasive grains is 35 nm or less, may be 30 nm or less, may be 23 nm or less, may be 18 nm or less, or may be 14 nm or less. In some embodiments, the cumulative 10% particle diameter D10 is 10 nm or more, may be 11 nm or more. When the cumulative 10% particle diameter D10 is in the above range, scratches tend to be reduced.
[0025] In some embodiments, the cumulative 5% particle diameter D5 in the cumulative particle size distribution of the abrasive grains is 30 nm or less, may be 25 nm or less, may be 20 nm or less, may be 15 nm or less, or may be 13 nm or less. In some embodiments, the cumulative 5% particle diameter D5 is 10 nm or more. When the cumulative 5% particle diameter D5 is in the above range, scratches tend to be reduced.
[0026] In this specification, the number ratio of particles with a particle diameter of less than 10 nm, cumulative 5% particle diameter D5, cumulative 10% particle diameter D10, cumulative 50% particle diameter D50, cumulative 90% particle diameter D90, and cumulative 95% particle diameter D95 are specifically determined by the following method. That is, using a transmission electron microscope (TEM, Hitachi High-Technologies Corporation STEM HD-2700), 10,000 or more particles observable by TEM contained in the abrasive grain to be measured (which may be one type of abrasive grain or a mixture of two or more types of abrasive grain) are photographed at a magnification (for example, 200,000 times to 400,000 times) at which about 100 particles can be observed in one field of view, and a TEM image is obtained. Then, the area of each particle is calculated from the image of each particle, and the diameter of an ideal circle (perfect circle) having the same area as the calculated area is calculated as the particle diameter of each particle. By detecting the number of particles with a particle diameter of less than 10 nm and the number of particles with a particle diameter of 10 nm or more in the acquired TEM image, the ratio of the number of particles with a particle diameter of less than 10 nm to the total number of abrasive grains to be measured is calculated. The cumulative particle size distribution of the abrasive grains to be measured is obtained by plotting the calculated particle diameters of each particle constituting the abrasive grain on the horizontal axis and the cumulative number (%) on the vertical axis. The cumulative 5% particle diameter D5, cumulative 10% particle diameter D10, cumulative 50% particle diameter D50, cumulative 90% particle diameter D90, and cumulative 95% particle diameter D95 are calculated based on the cumulative particle size distribution. The TEM image can be analyzed using MacView, an image analysis software manufactured by Mountech Co., Ltd. The same applies to the examples described later.
[0027] (Particle size ratio (D L / D S )) In some embodiments, the abrasive grains exhibit a multimodal grain size distribution. Specifically, in some embodiments, the abrasive grains have two or more grain sizes whose number frequency shows a maximum value in a range of 0.50% or more in a grain size number distribution obtained by plotting the particle size on the horizontal axis and the number frequency (%) on the vertical axis based on transmission electron microscope observation. The abrasive grains exhibiting such a multimodal grain size distribution may be realized by combining two or more types of silica particles (products), or may be realized by one type of silica particle (product). In some preferred embodiments, the abrasive grains contain a combination of two or more types of silica particles.
[0028] The particle size relationship of the particle sizes showing the maximum number frequency is not particularly limited. In some embodiments, the particle size having the maximum number frequency is referred to as the particle size D L The smallest particle diameter is called particle diameter D S Then, the particle diameter D S Particle size D L The ratio of particle size (hereinafter referred to as "particle size ratio (D L / D S The particle size ratio (D L / D S ) is a certain value or more, a multi-modal particle size distribution is used, which tends to improve workability.
[0029] In some preferred embodiments, the grain size ratio of the abrasive grains (D L / D S ) is 1.5 or more, more preferably 1.7 or more, may be 1.9 or more, may be 2.0 or more, may be 2.1 or more, or may be 2.2 or more. From the viewpoint of suppressing the occurrence of defects (e.g., scratches), the large-small particle diameter ratio (D L / D S ) is preferably 4.5 or less, may be 4.0 or less, may be 3.5 or less, may be 3.0 or less, or may be 2.5 or less.
[0030] The particle size ratio (D L / D S) is specifically obtained by the following method. That is, using a transmission electron microscope (TEM, Hitachi High-Technologies Corporation STEM HD-2700), 10,000 or more particles observable by TEM contained in the abrasive grain to be measured are photographed at a magnification (e.g., 200,000 to 400,000 times) at which about 100 particles can be observed in one field of view, and a TEM image is obtained. Then, the area of each particle is calculated from the image of each particle, and the diameter of an ideal circle (perfect circle) having the same area as the calculated area is calculated as the particle size of each particle. A particle size number distribution is obtained by plotting the calculated particle size of each particle constituting the abrasive grain to be measured on the horizontal axis and the number frequency (%) on the vertical axis. In the particle size number distribution, a particle size showing a maximum (peak) in the number frequency range of 0.50% or more is obtained. When there are multiple particle sizes showing the maximum number frequency, the particle size D L and the smallest particle diameter D S By calculating the ratio of the particle size (D L / D S The above TEM images can be analyzed using image analysis software MacView manufactured by Mountech Co., Ltd. The same applies to the examples described later.
[0031] (Silica particles) The polishing composition disclosed herein contains silica particles as abrasive grains. Examples of the silica particles include colloidal silica. Colloidal silica has the function of mechanically polishing the surface of a Ni-P substrate. As the colloidal silica, it is preferable to use colloidal silica synthesized through particle growth in an aqueous phase, such as sodium silicate method silica or alkoxide method silica. This type of colloidal silica can suitably achieve high processability and good surface accuracy. The colloidal silica may be used alone or in combination with two or more types having different manufacturing conditions and / or physical properties. The colloidal silica may also be surface-modified. Examples of surface modification include chemical modification such as introduction of functional groups and metal modification.
[0032] The particle shape of silica particles is not particularly limited, and may be, for example, spherical or non-spherical.When the polishing composition disclosed herein is used for the finish polishing process of Ni-P substrate, the shape is preferably close to spherical.
[0033] Although not particularly limited, the average aspect ratio of silica particles is 1.0 or more in principle, and may be, for example, 1.03 or more, 1.06 or more, or 1.08 or more from the viewpoint of processability. In addition, from the viewpoint of efficiently increasing surface precision, in some embodiments, the average aspect ratio is suitably 1.30 or less. By reducing the average aspect ratio of silica particles, the silica particles can be easily rolled and moved, and the polishing resistance can be reduced, so that processing can be stabilized and scratches can be more preferably reduced. From such a viewpoint, the average aspect ratio of silica particles is preferably 1.28 or less, more preferably 1.25 or less (for example, 1.2 or less). Here, the average aspect ratio of silica particles refers to the average value of the major axis / minor axis ratio of each particle constituting the silica particles, that is, the number-average aspect ratio. Hereinafter, unless otherwise specified, the average aspect ratio in this specification means the number-average aspect ratio.
[0034] Specifically, the average aspect ratio of silica particles is determined by the following method. That is, using a transmission electron microscope (TEM, Hitachi High-Technologies Corporation's STEM HD-2700), 10,000 or more particles observable by TEM contained in the colloidal silica to be measured are photographed at a magnification (for example, 200,000 to 400,000 times) at which about 100 particles can be observed in one field of view, and a TEM image is obtained. Then, for the smallest rectangle circumscribing each particle image, the value obtained by dividing the length of its long side (long axis value) by the length of its short side (short axis value) is calculated as the long axis / short axis ratio (aspect ratio) of each particle. The above aspect ratio can be determined using image analysis software MacView manufactured by Mountech Co., Ltd.
[0035] In some preferred embodiments, the polishing composition contains substantially only silica particles as abrasive grains. Here, "contains substantially only silica particles" means that the proportion of silica particles in the total solid content of the polishing composition is 99% by weight or more, more preferably 99.5% by weight or more, and even more preferably 99.9% by weight or more. In such an embodiment, while maintaining high processability, it can achieve better surface accuracy (for example, a surface with reduced number of scratches).
[0036] In some preferred embodiments, the polishing composition contains substantially only colloidal silica as abrasive grains. Here, "contains substantially only colloidal silica" means that the proportion of colloidal silica in the total solid content of the polishing composition is 99% by weight or more, more preferably 99.5% by weight or more, and even more preferably 99.9% by weight or more. In such an embodiment, while maintaining high processability, better surface precision (for example, a surface with reduced number of scratches) can be achieved.
[0037] The polishing composition disclosed herein may contain silica particles other than the colloidal silica (e.g., fumed silica, precipitated silica, etc.) to the extent that the effect of the present invention is not significantly impaired. In addition, particles other than silica particles, i.e., non-silica particles, may be contained to the extent that the effect of the present invention is not significantly impaired, but the polishing composition disclosed herein can be preferably implemented in an embodiment that does not substantially contain particles other than colloidal silica, i.e., non-colloidal silica particles. Here, "substantially not containing non-colloidal silica particles" means that the ratio of non-colloidal silica particles to the total solid content contained in the polishing composition is 1% by weight or less, more preferably 0.5% by weight or less, and even more preferably 0.1% by weight or less. In such an embodiment, the application effect of the technology disclosed herein can be suitably exhibited.
[0038] The polishing composition disclosed herein is preferably implemented in an embodiment that does not substantially contain alumina particles. Examples of alumina particles include α-alumina particles. Such a polishing composition prevents quality degradation caused by the use of alumina particles. Examples of quality degradation include the occurrence of scratches and dents, alumina residue, and puncture defects. In this specification, "substantially free of a specific abrasive, for example, alumina particles," means that the proportion of the abrasive particles in the total solid content contained in the polishing composition is 1% by weight or less, more preferably 0.5% by weight or less, and typically 0.1% by weight or less. A polishing composition with a proportion of 0% by weight of alumina particles, that is, a polishing composition that does not contain alumina particles, is particularly preferred. In addition, the polishing composition disclosed herein can be preferably implemented in an embodiment that does not substantially contain α-alumina particles.
[0039] The content of silica particles in the polishing composition is not particularly limited, and is, for example, 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 1% by weight or more, and even more preferably 3% by weight or more. When the silica particles contain multiple types of silica particles, the above content is the total content of them. By increasing the content of silica particles, higher processability tends to be realized. From the viewpoint of the surface smoothness of the substrate after polishing and the dispersion stability of the particles, the above content is usually 25% by weight or less, preferably 20% by weight or less, more preferably 15% by weight or less, and even more preferably 10% by weight or less, for example 8% by weight or less, and may be 6% by weight or less.
[0040] (water) The polishing composition disclosed herein contains water. As the water, ion-exchanged water, pure water, ultrapure water, distilled water, etc. can be preferably used. The ion-exchanged water may be deionized water.
[0041] (Defect reduction agent) In some embodiments, the polishing composition contains a defect-reducing agent. The defect-reducing agent has the function of suppressing the occurrence of defects (typically scratches) during polishing of a Ni-P substrate. The defect-reducing agent is not particularly limited as long as it can exhibit the above-mentioned function. The defect-reducing agent can be used alone or in combination of two or more.
[0042] In some embodiments, a sulfuric acid ester containing polyalkylene oxide is used as the defect reducing agent. The concept of sulfuric acid ester here includes sulfuric acid ester and its salt. Specific examples of sulfuric acid ester containing polyalkylene oxide include polyoxyethylene alkyl sulfate, polyoxyethylene naphthyl sulfate, polyoxyethylene alkyl sulfate, polyoxyethylene naphthyl ether sulfate, etc. Specific examples of polyoxyethylene alkyl sulfate include polyoxyethylene lauryl sulfate. Among them, polyoxyethylene alkyl sulfate (e.g., polyoxyethylene lauryl sulfate) and polyoxyethylene naphthyl ether sulfate are preferred. The above-mentioned sulfuric acid ester containing polyalkylene oxide can be used alone or in combination of two or more.
[0043] The number of oxyalkylene units (e.g., the number of oxyethylene units) in the sulfate containing polyalkylene oxide (e.g., polyethylene oxide) is not particularly limited. In some embodiments, the number of oxyalkylene units (e.g., the number of oxyethylene units) in the sulfate containing polyalkylene oxide (e.g., polyethylene oxide) is 2 or more and 25 or less. From the viewpoint of reducing defects, in some preferred embodiments, the number of oxyalkylene units (e.g., the number of oxyethylene units) in the sulfate containing polyalkylene oxide (e.g., polyethylene oxide) is 20 or less, more preferably 13 or less, and may be 10 or less, or may be 6 or less. The number of oxyalkylene units means the average number of oxyalkylene units in a mixture having different numbers of oxyalkylene units.
[0044] In some other embodiments, the defect reducing agent may be selected from organic compounds such as sulfonic acid compounds, etc. The concept of sulfonic acid compounds herein includes sulfonic acid compounds and their salts. Specifically, the sulfonic acid may be selected from polyalkylarylsulfonic acid compounds such as naphthalenesulfonic acid formaldehyde condensates, methylnaphthalenesulfonic acid formaldehyde condensates, anthracenesulfonic acid formaldehyde condensates, and benzenesulfonic acid formaldehyde condensates; melamine formalin resin sulfonic acid compounds such as melamine sulfonic acid formaldehyde condensates; ligninsulfonic acid compounds such as ligninsulfonic acid and modified ligninsulfonic acid; aromatic aminosulfonic acid compounds such as aminoarylsulfonic acid-phenol-formaldehyde condensates; and sulfonic acid compounds such as polyisoprenesulfonic acid, polyvinylsulfonic acid, polyallylsulfonic acid, and polyisoamylenesulfonic acid, and salts thereof (e.g., alkali metal salts such as sodium salts and potassium salts). Of these, naphthalenesulfonic acid compounds such as naphthalenesulfonic acid formaldehyde condensates and methylnaphthalenesulfonic acid formaldehyde condensates and salts thereof are preferred, with naphthalenesulfonic acid formaldehyde condensates and salts thereof being more preferred.
[0045] In some embodiments, the polishing composition comprises one or more selected from the group consisting of sulfuric acid ester containing polyalkylene oxide and naphthalene sulfonic acid formaldehyde condensate.The polishing composition comprising such defect additive can more effectively exhibit scratch reduction effect.
[0046] The content of the defect reducing agent in the polishing composition is not particularly limited, and may be, for example, 0.0003% by weight or more, or 0.0005% by weight or more. In some preferred embodiments, the content of the defect reducing agent is 0.001% by weight or more, may be 0.003% by weight or more, or may be 0.005% by weight or more. In addition, the content of the defect reducing agent in the polishing composition can be 0.1% by weight or less (for example, less than 0.1% by weight), or may be 0.05% by weight or less. In some preferred embodiments, the content of the defect reducing agent is 0.03% by weight or less, or may be 0.02% by weight or less. By limiting the amount of the defect reducing agent used within the above range, the processability tends to be easily maintained.
[0047] The amount of the defect reducing agent contained in the polishing composition can also be specified by the relative relationship with the abrasive grain contained in the polishing composition.The content of the defect reducing agent relative to 100 parts by weight of the abrasive grain contained in the polishing composition is, for example, appropriate to be 0.005 parts by weight or more, and from the viewpoint of scratch reduction, it is preferably 0.01 parts by weight or more, more preferably 0.03 parts by weight or more, and even more preferably 0.05 parts by weight or more.In addition, the content of the defect reducing agent relative to 100 parts by weight of the abrasive grain is appropriate to be approximately 3 parts by weight or less, and from the viewpoint of maintaining processability, it is preferably 1 part by weight or less, more preferably 0.7 parts by weight or less, and may be 0.6 parts by weight or less.
[0048] (acid) In some embodiments, the polishing composition contains an acid. The acid acts to chemically polish the Ni-P substrate. The acid can be either an inorganic acid or an organic acid. The acid can be used alone or in combination of two or more.
[0049] Specific examples of inorganic acids include phosphoric acid (orthophosphoric acid), nitric acid, sulfuric acid, hydrochloric acid, boric acid, sulfamic acid, phosphinic acid, phosphonic acid, pyrophosphoric acid, tripolyphosphoric acid, tetrapolyphosphoric acid, hexametaphosphoric acid, carbonic acid, hydrofluoric acid, sulfurous acid, thiosulfuric acid, chloric acid, perchloric acid, chlorous acid, hydroiodic acid, periodic acid, iodic acid, hydrobromic acid, perbromic acid, bromic acid, chromic acid, and nitrous acid.
[0050] Examples of the organic acid include organic carboxylic acid, organic phosphonic acid, organic sulfonic acid, amino acid, etc. The number of carbon atoms contained in these organic acids is typically about 1 to 18, and preferably about 1 to 10, for example. Specific examples of organic acids include malonic acid, citric acid, isocitric acid, 1,2,4-butanetricarboxylic acid, maleic acid, malic acid, glycolic acid, succinic acid, itaconic acid, iminodiacetic acid, gluconic acid, lactic acid, mandelic acid, tartaric acid, formic acid, acetic acid, propionic acid, butyric acid, adipic acid, oxalic acid, valeric acid, enanthic acid, caproic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, cyclohexanecarboxylic acid, phenylacetic acid, and benzoic acid. Organic carboxylic acids such as crotonic acid, oleic acid, linoleic acid, linolenic acid, ricinoleic acid, methacrylic acid, glutaric acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, tartronic acid, glyceric acid, hydroxybutyric acid, hydroxyacetic acid, hydroxybenzoic acid, salicylic acid, methylenesuccinic acid, gallic acid, ascorbic acid, nitroacetic acid, oxaloacetic acid, chloroacetic acid, dichloroacetic acid, trichloroacetic acid, pyridine carboxylic acids such as nicotinic acid and picolinic acid; methyl acid phosphate, ethyl ester ... Chill acid phosphate, ethyl glycol acid phosphate, isopropyl acid phosphate, phytic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethanehydroxy-1,1,2-triphosphonic acid organic phosphonic acids such as ethanesulfonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, α-methylphosphonosuccinic acid, aminopoly(methylenephosphonic acid); organic sulfonic acids such as ethanesulfonic acid, aminoethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, 2-naphthalenesulfonic acid, sulfosuccinic acid, 10-camphorsulfonic acid, taurine;Amino acids such as glycine, alanine, glutamic acid, aspartic acid, valine, leucine, isoleucine, serine, threonine, cysteine, methionine, phenylalanine, tryptophan, tyrosine, proline, cystine, glutamine, asparagine, lysine, and arginine;
[0051] Examples of preferred acids from the viewpoint of processability include phosphoric acid, phosphonic acid, malonic acid, citric acid, maleic acid, hydrochloric acid, nitric acid, sulfuric acid, sulfamic acid, phytic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, etc. Among these, preferred acids include phosphoric acid, phosphonic acid, malonic acid, citric acid, and maleic acid.
[0052] The acid may be used in the form of a salt of the acid. Examples of the salt include metal salts, ammonium salts, alkanolamine salts, etc. of the above-mentioned inorganic acids and organic acids. Examples of the metal salts include alkali metal salts such as lithium salts, sodium salts, and potassium salts. Examples of the ammonium salts include quaternary ammonium salts such as tetramethylammonium salts and tetraethylammonium salts. Examples of the alkanolamine salts include monoethanolamine salts, diethanolamine salts, and triethanolamine salts.
[0053] Specific examples of salts that can be contained in the polishing composition disclosed herein include alkali metal phosphates and alkali metal hydrogen phosphates such as tripotassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, trisodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate; alkali metal salts of the organic acids exemplified above; and, in addition, alkali metal salts of glutamic acid diacetate, alkali metal salts of diethylenetriaminepentaacetate, alkali metal salts of hydroxyethylethylenediaminetriacetate, and alkali metal salts of triethylenetetraminehexaacetate. The alkali metal in these alkali metal salts can be, for example, lithium, sodium, potassium, etc.
[0054] In some embodiments, the salt may be an inorganic acid salt such as an alkali metal salt or an ammonium salt of an inorganic acid. For example, in addition to the above-mentioned alkali metal phosphates and alkali metal hydrogen phosphates, potassium chloride, sodium chloride, ammonium chloride, potassium nitrate, sodium nitrate, ammonium nitrate, etc. may be used.
[0055] The content of the acid in the polishing composition is not particularly limited. The content of the acid is usually 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 0.8% by weight or more, for example 1.2% by weight or more. By increasing the concentration of the acid, the processability tends to improve. The content of the acid is usually 15% by weight or less, preferably 10% by weight or less, more preferably 5% by weight or less, for example 3% by weight or less. By limiting the content of the acid, the surface accuracy of the substrate (Ni-P substrate) after polishing is likely to improve.
[0056] (Oxidizing agent) The polishing composition disclosed herein can contain an oxidizing agent as necessary.Examples of the oxidizing agent include, but are not limited to, peroxide, nitric acid or its salt, periodic acid or its salt, peroxo acid or its salt, permanganic acid or its salt, chromic acid or its salt, oxygen acid or its salt, metal salts, sulfuric acid, etc.The oxidizing agent can be used alone or in combination of two or more. Specific examples of the oxidizing agent include hydrogen peroxide, sodium peroxide, barium peroxide, nitric acid, iron nitrate, aluminum nitrate, ammonium nitrate, peroxomonosulfuric acid, ammonium peroxomonosulfate, metal peroxomonosulfate, peroxodisulfate, ammonium peroxodisulfate, metal peroxodisulfate, peroxolinic acid, peroxosulfuric acid, sodium peroxoborate, performic acid, peracetic acid, perbenzoic acid, perphthalic acid, hypobromous acid, hypoiodous acid, chloric acid, bromic acid, iodic acid, periodic acid, perchloric acid, hypochlorous acid, sodium hypochlorite, calcium hypochlorite, potassium permanganate, metal chromate, metal dichromate, iron chloride, iron sulfate, iron citrate, ammonium iron sulfate, etc. Preferred examples of the oxidizing agent include hydrogen peroxide, iron nitrate, periodic acid, peroxomonosulfuric acid, peroxodisulfuric acid, and nitric acid. It preferably contains at least hydrogen peroxide, and more preferably consists of hydrogen peroxide.
[0057] The content of the oxidizing agent in the polishing composition is preferably 0.01% by weight or more based on the amount of active ingredient, more preferably 0.05% by weight or more, even more preferably 0.1% by weight or more, and may be 0.2% by weight or more, or may be 0.3% by weight or more, in consideration of the rate of oxidation of the object to be polished and therefore the processability. Also, in view of improving the surface accuracy of the object to be polished, the content of the oxidizing agent in the polishing composition is preferably 5% by weight or less based on the amount of active ingredient, more preferably 1% by weight or less.
[0058] (Basic compounds) The polishing composition may contain a basic compound as necessary for the purpose of pH adjustment, etc. Here, the basic compound refers to a compound that has the function of increasing the pH of the polishing composition by being added to the composition. Examples of basic compounds include alkali metal hydroxides such as potassium hydroxide and sodium hydroxide, quaternary ammonium compounds such as quaternary ammonium hydroxide, ammonia, amines, etc. The basic compounds may be used alone or in combination of two or more.
[0059] (chelating agent) The polishing composition disclosed herein may contain a chelating agent as necessary. By including a chelating agent, the occurrence of defects on the polished surface after polishing can be suppressed. Examples of the chelating agent include aminocarboxylic acid-based chelating agents and organic phosphonic acid-based chelating agents. Examples of the aminocarboxylic acid-based chelating agent include ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, nitrilotriacetic acid, sodium nitrilotriacetate, ammonium nitrilotriacetate, glutamic acid diacetic acid, hydroxyethylethylenediaminetriacetic acid, sodium hydroxyethylethylenediaminetriacetate, diethylenetriaminepentaacetic acid, sodium diethylenetriaminepentaacetate, triethylenetetraminehexaacetic acid, and sodium triethylenetetraminehexaacetate. Examples of organic phosphonic acid chelating agents include 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetrakis(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1,2-triphosphonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, and α-methylphosphonosuccinic acid. Among them, preferred are glutamic acid diacetate, 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetrakis(methylenephosphonic acid) and diethylenetriaminepenta(methylenephosphonic acid). Particularly preferred chelating agents are glutamic acid diacetate and 1-hydroxyethylidene-1,1-diphosphonic acid. The chelating agents can be used alone or in combination of two or more.
[0060] The content of the chelating agent in the polishing composition is not particularly limited. The content of the chelating agent is usually 0.005% by weight or more, and may be 0.01% by weight or more, 0.1% by weight or more, or 0.5% by weight or more. The content of the chelating agent is usually 5% by weight or less, and may be 3% by weight or less, 2% by weight or less, or 1% by weight or less.
[0061] (Other Ingredients) The polishing composition disclosed herein may further contain, as necessary, known additives that can be used in polishing compositions (for example, polishing compositions for magnetic disk substrates such as Ni-P substrates), such as water-soluble polymers, surfactants, preservatives, and antifungal agents, within the scope that does not significantly impair the effects of the present invention. For example, examples of preservatives and antifungal agents include isothiazoline preservatives such as 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one, paraoxybenzoic acid esters, phenoxyethanol, and the like, but are not limited thereto.
[0062] (pH) The pH of the polishing composition disclosed herein is not particularly limited, and may be selected, for example, from the range of 0.5 to 6.5. From the viewpoint of processability, etc., in some preferred embodiments, the pH of the polishing composition is 4.0 or less, more preferably 3.7 or less, even more preferably 3.5 or less, may be 3.2 or less, may be 3.0 or less, may be 2.5 or less, or may be 2.2 or less. In addition, the pH of the polishing composition is preferably higher than 1.0, and from the viewpoint of suppressing roughness of the substrate surface after polishing, it is preferably 1.2 or more, more preferably 1.5 or more (e.g., more than 1.5), and may be 1.7 or more. The technology disclosed herein can be preferably implemented in an embodiment in which the pH of the polishing composition is 1 or more and 4 or less (e.g., 1.5 or more and 3.7 or less). The above-mentioned pH can be particularly preferably applied to a polishing composition for finish polishing of Ni-P substrates.
[0063] In the technique disclosed herein, the pH of the polishing composition can be determined by performing three-point calibration using a pH meter, then inserting a glass electrode into the composition to be measured. The standard solutions are, for example, oxalate pH standard solution: pH 1.68 (25°C), phthalate pH standard solution: pH 4.01 (25°C), neutral phosphate pH standard solution: pH 6.86 (25°C), and carbonate pH standard solution: pH 10.01 (25°C).
[0064] <Concentrate> The polishing composition disclosed herein may be in a concentrated form (i.e., in the form of a concentrated polishing liquid) before being supplied to a polishing object (e.g., a magnetic disk substrate). Such a concentrated polishing composition (concentrate) is advantageous from the viewpoints of convenience and cost reduction during production, distribution, storage, etc. The concentration ratio can be, for example, about 1.5 to 20 times in terms of volume. From the viewpoint of storage stability of the concentrate, etc., a concentration ratio of about 2 to 10 times is usually appropriate. Such a concentrated liquid can be used in a form in which a polishing composition (polishing liquid) is prepared by diluting it at a desired timing and the polishing liquid is supplied to a polishing object. The dilution can typically be performed by adding water to the concentrated liquid and mixing it.
[0065] <Multi-component polishing composition> The polishing composition disclosed herein may be a one-component type or a multi-component type, including a two-component type. For example, the polishing composition may be configured so that a part A containing some of the components (typically components other than water) of the polishing composition and a part B containing the remaining components are mixed and used for polishing an object to be polished. Some preferred embodiments of the multi-component polishing composition are configured to contain a part A containing abrasive grains (colloidal silica) (typically a dispersion liquid further containing a dispersion medium for colloidal silica) and a part B containing at least a part of the components other than the abrasive grains (e.g., an acid, a defect reducing agent, etc.). Usually, these are stored separately before use, and can be mixed at the time of use to prepare a one-component polishing composition. When mixed, an oxidizing agent such as hydrogen peroxide, water for dilution, etc. can be further mixed.
[0066] <Polishing process> The polishing composition disclosed herein can be suitably used for polishing an object to be polished (here, a Ni-P substrate) in an embodiment including the following operations, for example. A preferred embodiment of the method for polishing an object to be polished using the polishing composition disclosed herein will be described below. That is, a polishing liquid (working slurry) containing any of the polishing compositions disclosed herein is prepared. The preparation of the polishing liquid may include adjusting the concentration (e.g., diluting) or adjusting the pH of the polishing composition to prepare the polishing liquid. Alternatively, the polishing composition may be used as it is as the polishing liquid.
[0067] Next, the polishing liquid is supplied to the object to be polished, and polished in a conventional manner. For example, the object to be polished is set in a general polishing device, and the polishing liquid is supplied to the surface of the object to be polished (the surface to be polished) through the polishing pad of the polishing device. Typically, the polishing liquid is continuously supplied, and the polishing pad is pressed against the surface of the object to be polished, and the two are moved relatively (for example, rotated).
[0068] Thereafter, an alkaline cleaning step is carried out to clean the object to be polished with an alkaline cleaning solution. The alkaline cleaning step typically involves contacting at least the surface of the object to be polished with an alkaline cleaning solution. For example, the surface of the object to be polished can be brought into contact with the alkaline cleaning solution by immersing the object to be polished in the alkaline cleaning solution. An ultrasonic treatment may be carried out to apply ultrasonic waves to the object to be polished immersed in the alkaline cleaning solution. In addition to or instead of applying ultrasonic waves, scrubbing may be carried out using a polyvinyl alcohol sponge, a nonwoven fabric, a nylon brush, or the like. The pH of the alkaline cleaning solution used in the alkaline cleaning step may be, for example, 7.5 or more, and from the viewpoint of improving cleaning properties, it is preferably 8.0 or more, more preferably 8.5 or more, for example 8.8 or more. In addition, from the viewpoint of preventing roughening of the substrate surface due to cleaning, the pH of the alkaline cleaning solution is usually 11 or less, preferably 10 or less, and more preferably 9.5 or less. As the alkaline cleaning solution, an aqueous solution containing one or more of the above-mentioned basic compounds can be used. Among them, an aqueous solution of an alkali metal hydroxide is preferred, and for example, an aqueous solution of potassium hydroxide can be preferably used. The alkaline cleaning step may be performed using a commercially available alkaline cleaning solution.
[0069] After the polishing using the polishing liquid is completed, the object to be polished may be washed with a non-alkaline rinse liquid before proceeding to the alkaline washing step. The rinse liquid may be water such as pure water or ion-exchanged water, or an acidic aqueous solution (e.g., an aqueous solution with a composition obtained by removing abrasive grains from the polishing liquid).
[0070] <Application> The polishing composition disclosed herein can be used for polishing a nickel-phosphorus-plated magnetic disk substrate (Ni-P substrate) and can effectively reduce the number of defects on the surface of the Ni-P substrate. The Ni-P substrate is typically a magnetic disk substrate having a nickel-phosphorus plating layer on the surface of the substrate. The material of the substrate can be, for example, an aluminum alloy, glass, glassy carbon, etc. The polishing composition disclosed herein can be preferably used for polishing a Ni-P substrate having a nickel-phosphorus plating layer on an aluminum alloy substrate, for example. According to this specification, there can be provided a method for producing a Ni-P substrate, which includes a polishing step using the polishing composition disclosed herein and an alkaline cleaning step performed after the polishing step, and a Ni-P substrate produced by this method.
[0071] The polishing composition disclosed herein can highly reduce defects on the surface of a Ni-P substrate, and therefore can be particularly preferably used in the final polishing step (finish polishing step) of the Ni-P substrate. According to this specification, a method for producing a Ni-P substrate, comprising a final polishing step using the polishing composition disclosed herein and an alkaline washing step performed after the final polishing step, and a Ni-P substrate produced by the method can be provided. Note that the final polishing step refers to the last polishing step in the manufacturing process of the target object (i.e., a step after which no further polishing is performed). The manufacturing method of the substrate can further include a rough polishing step or a preliminary polishing step performed before the polishing step.
[0072] The polishing composition disclosed herein may be used in a polishing step upstream of the final polishing. Here, the polishing step upstream of the final polishing refers to a preliminary polishing step between the rough polishing step and the final polishing step. The preliminary polishing step typically includes at least a first polishing step, and may further include a second, third, etc. polishing step. The above-mentioned polishing composition can be used in any of the polishing steps, and the same or different polishing compositions can be used in these polishing steps. The polishing composition disclosed herein may be used, for example, in a polishing step performed immediately before the final polishing.
[0073] The polishing composition disclosed herein can be preferably used, for example, for polishing Ni-P substrates adjusted to a surface roughness of 20 Å or less by an upstream process. Here, the surface roughness refers to the surface roughness (arithmetic mean roughness (Ra)) measured by a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System. It is particularly preferable to apply the composition to polishing Ni-P substrates adjusted to a surface roughness of 10 Å or less. This allows Ni-P substrates with high quality surfaces to be produced with good productivity.
[0074] The matters disclosed in this specification include the following. [1] A polishing composition used for polishing a magnetic disk substrate having a nickel-phosphorus plating layer, comprising: The method includes the steps of: (a) preparing a powder containing colloidal silica as an abrasive grain; and (b) preparing water; The abrasive grains are a polishing composition in which the number ratio of particles having a particle diameter of less than 10 nm is 10% or less based on observation with a transmission electron microscope, and the cumulative 95% particle diameter D95 in the number-based cumulative particle size distribution from the small diameter side is 55 nm or less. [2] The polishing composition according to [1] above, further comprising one or more defect-reducing agents selected from the group consisting of sulfuric acid esters containing polyalkylene oxides and naphthalenesulfonic acid formaldehyde condensates. [3] The polishing composition according to [2] above, wherein the sulfuric acid ester containing a polyalkylene oxide has an oxyalkylene unit number of 2 or more and 13 or less. [4] The abrasive grains are In the particle size number distribution obtained by plotting particle size on the horizontal axis and number frequency (%) on the vertical axis based on transmission electron microscope observation, there are two or more particle sizes showing a maximum number frequency in the range of number frequency of 0.50% or more, The largest particle size among the particle sizes showing the maximum number frequency above is particle size D L The smallest particle diameter is called particle diameter D S When the particle size ratio (D L / D S ) is 1.40 or more. [5] The polishing composition according to any one of the above [1] to [4], further comprising an acid. [6] The polishing composition according to any one of the above [1] to [5], further comprising an oxidizing agent. [7] The polishing composition according to any one of the above [1] to [6], further comprising a chelating agent. [8] The polishing composition according to any one of the above [1] to [7], which has a pH within the range of 1 to 4. [9] The polishing composition according to any one of the above [1] to [8], which is used in a finish polishing step.
[10] The polishing composition according to any one of [1] to [9] above, which is stored before use in a state in which it is divided into a plurality of parts including a part A containing an abrasive grain and a part B containing at least a portion of components other than the abrasive grain, and which is prepared by mixing the plurality of parts when used.
[11] A method for producing a magnetic disk substrate, comprising supplying the polishing composition according to any one of [1] to
[10] above to a substrate to be polished, and polishing the substrate. EXAMPLES
[0075] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.
[0076] <Preparation of Polishing Composition> Example 1 Several kinds of colloidal silica with different average particle sizes were prepared. Abrasive grains containing these colloidal silicas alone or in combination with phosphoric acid, a chelating agent, a defect reducing agent, hydrogen peroxide as an oxidizing agent, and deionized water were mixed to adjust the pH. A polishing composition was prepared containing 3.5% by weight of abrasive grains, 2.0% by weight of phosphoric acid, 0.5% by weight of a chelating agent, 0.005% by weight of a defect reducing agent, and 0.6% by weight of hydrogen peroxide, and having a pH of 1.6. Tetrasodium L-glutamic acid diacetate (GLDA·4Na) was used as the chelating agent. Polyoxyethylene-β-naphthyl ether sulfate (POE(2)β-naphthyl ether sulfate), which has two oxyethylene units, was used as the defect reducing agent. The pH was adjusted using phosphoric acid and potassium hydroxide.
[0077] Here, the cumulative 5% particle diameter D5, cumulative 10% particle diameter D10, cumulative 50% particle diameter D50, cumulative 90% particle diameter D90, and cumulative 95% particle diameter D95 in the cumulative particle size distribution based on number based on TEM observation of the above abrasive grains are as shown in the corresponding columns in Table 1. In addition, the number ratio (content) of particles with a particle diameter of less than 10 nm in the entire abrasive grains based on TEM observation was 1.4%, and the particle diameter ratio (D L / D S) was 2.50.
[0078] (Examples 2 to 41, Comparative Examples 1 to 11) Except that the type and total content of abrasive grains, the type of chelating agent, and the type and content of defect reducing agent were as shown in Table 1 or 2, polishing compositions of Examples 2 to 41 and Comparative Examples 1 to 11 were prepared in the same manner as in Example 1. In addition, the description of "-" in the item of "defect reducing agent" in Tables 1 and 2 means that no defect reducing agent was used. Also, in Tables 1 and 2, "n" in "POE(n)β-naphthyl ether sulfate" and "POE(n) lauryl sulfate ester" represents the number of ethylene oxide units.
[0079] The cumulative 5% particle size D5, cumulative 10% particle size D10, cumulative 50% particle size D50, cumulative 90% particle size D90, and cumulative 95% particle size D95 of the abrasive grains used in each example, the number ratio of particles with a particle size of less than 10 nm, and the particle size ratio (D L / D S ) were as shown in the corresponding columns of Tables 1 and 2, respectively.
[0080] <Polishing of Ni-P Substrate> The polishing composition according to each example was used as it was in the polishing liquid, and the polishing object was polished under the following conditions. The polishing object was an aluminum substrate for hard disks having an electroless nickel phosphorus plating layer on the surface, which was pre-polished so that the surface roughness (arithmetic mean roughness (Ra)) measured by a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System was 6 Å. The diameter of the polishing object was 3.5 inches (a doughnut shape with an outer diameter of about 95 mm and an inner diameter of about 25 mm) and the thickness was 1.27 mm. In Comparative Examples 4 and 8, the platen was vibrated, and polishing could not be continued.
[0081] (polishing conditions) Polishing equipment: SpeedFam double-sided polishing machine, model "9B-5P" Polishing pad: Suede non-buff type Number of substrates to be polished: 10 ((2 substrates / carrier) x 5 carriers x 1 batch)) Polishing fluid supply rate: 56mL / min Polishing load: 140g / cm 2 Lower surface plate rotation speed: 31rpm Polishing time: 5 minutes
[0082] <Cleaning> The polished Ni-P substrate was immersed in pure water and subjected to ultrasonic treatment at a frequency of 170 kHz, then immersed in an alkaline cleaning solution (a cleaning solution "CSC-102B" available from Speedfam Co., Ltd., diluted 200 times by volume) and scrubbed with a polyvinyl alcohol sponge while applying ultrasonic waves at a frequency of 170 kHz. The substrate was then immersed in pure water and subjected to ultrasonic treatment at a frequency of 950 kHz, and then pulled out into an isopropyl alcohol atmosphere and dried.
[0083] <Scratch evaluation> A total of five substrates were randomly selected from the substrates obtained by polishing and cleaning with the polishing composition according to each example, and scratches on both sides of each substrate were detected under the following conditions. The total number of scratches on the five substrates (total of 10 sides) was divided by 10 to calculate the number of scratches per side of the substrate (number of scratches / side). If the number of scratches was less than 20 / side, it was evaluated as "AA (excellent)", if it was 20 or more / side but less than 30 / side, it was evaluated as "A (excellent)", if it was 30 or more / side but less than 40 / side, it was evaluated as "B+ (good)", if it was 40 or more / side but less than 50 / side, it was evaluated as "B (fair)", and if it was 50 or more / side, it was evaluated as "C (poor)". For Comparative Examples 4 and 8, in which polishing could not proceed due to vibration of the surface plate, "-" was entered in the corresponding column.
[0084] (Scratch detection conditions) Measurement equipment: Candela OSA7100 manufactured by KLA-Tencor Corporation Spindle speed: 10,000 rpm Measurement range: 17000-47000μm Step size: 4μm Encoder multiplier:×16 Detection channel: P-Sc channel
[0085] <Polishing speed> From the substrates obtained by polishing and cleaning with the polishing composition according to each example, 6 substrates (3 substrates / 1 batch) are randomly selected, and the weight loss of each substrate is measured by polishing to calculate the polishing speed, and the polishing speed of each example is calculated by averaging the weight loss.Specifically, the polishing speed is calculated based on the following formula: Polishing rate [μm / min] = weight loss of substrate due to polishing [g] / (substrate surface area [cm 2 ] × density of nickel phosphorus plating [g / cm 3 ] x polishing time [min] x 10 4 Here, the surface area of one side of the board is 66 cm 2 , the density of nickel phosphorus plating is 7.9g / cm 3The polishing rate was calculated as follows: If the polishing rate was 0.15 μm / min or more, it was evaluated as "AA (excellent)", if it was 0.10 μm / min or more and less than 0.15 μm / min, it was evaluated as "A (excellent)", if it was 0.05 μm / min or more and less than 0.10 μm / min, it was evaluated as "B (good)", and if it was less than 0.05 μm / min, it was evaluated as "C (poor)", and these were recorded in the corresponding columns in Tables 1 and 2. For Comparative Examples 4 and 8, in which polishing could not proceed due to vibration of the surface plate, "-" was recorded in the corresponding column.
[0086] [Table 1]
[0087] [Table 2]
[0088] As shown in Tables 1 and 2, in polishing a Ni-P substrate, in Examples 1 to 41, which used a polishing composition containing abrasive grains with a particle diameter of less than 10 nm being 10% or less and a cumulative 95% particle diameter D95 of 55 nm or less and water, scratches on the substrate after polishing were clearly reduced compared to Comparative Examples 1 to 3, 5 to 7, 10 and 11, which used a polishing composition using abrasive grains with a particle diameter of less than 10 nm being more than 10%. In addition, it was confirmed that Comparative Example 9, which used a polishing composition using abrasive grains with a cumulative 95% particle diameter D95 of more than 55 nm, was inferior in scratch reduction performance compared to Examples 1 to 41.
[0089] Furthermore, a comparison between Examples 1 to 8 and Example 12 and a comparison between Examples 9 to 11 and Example 13 confirmed that the addition of the defect reducing agent tends to reduce scratches.
[0090] Furthermore, for example, in Examples 14 to 22, Examples 21 and 22 used abrasive grains containing only one type of silica grain, and the grain size ratio (D L / D S ) was used in Examples 19 and 20, which used abrasive grains with a relatively small grain size ratio (D L / DS It was confirmed that in Examples 14 to 18, which used abrasive grains with a relatively large diameter, the polishing rate increased and good processability was exhibited. A similar tendency was observed in Examples 23 to 31.
[0091] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.
Claims
1. A polishing composition used for polishing a magnetic disk substrate having a nickel-phosphorus plating layer, comprising: The method includes the steps of: The abrasive grains are a polishing composition in which the number ratio of particles having a particle diameter of less than 10 nm is 10% or less based on observation with a transmission electron microscope, and the cumulative 95% particle diameter D95 in the number-based cumulative particle size distribution from the small diameter side is 55 nm or less.
2. 2. The polishing composition according to claim 1, further comprising, as a defect reducing agent, one or more selected from the group consisting of a sulfuric acid ester containing a polyalkylene oxide and a naphthalenesulfonic acid formaldehyde condensate.
3. The polishing composition according to claim 2 , wherein the sulfuric acid ester containing polyalkylene oxide has 2 or more and 13 or less oxyalkylene units.
4. The abrasive grains are In a particle size number distribution obtained by plotting particle size on the horizontal axis and number frequency (%) on the vertical axis based on observation with a transmission electron microscope, there are two or more particle sizes showing a maximum number frequency in a range of number frequency of 0.50% or more, The largest particle diameter among the particle diameters showing the maximum number frequency is the particle diameter D L The smallest particle diameter is called particle diameter D S When the particle size ratio (D L / D S 3. The polishing composition according to claim 1, wherein the polishing composition has a surface roughness of 1.40 or more.
5. The polishing composition according to claim 1 or 2, further comprising an acid.
6. The polishing composition according to claim 1 or 2, further comprising an oxidizing agent.
7. The polishing composition according to claim 1 or 2, further comprising a chelating agent.
8. 3. The polishing composition according to claim 1, having a pH in the range of 1 to 4.
9. The polishing composition according to claim 1 or 2, which is used in a finish polishing step.
10. 3. A method for producing a magnetic disk substrate, comprising supplying the polishing composition according to claim 1 or 2 to a substrate to be polished, and polishing the substrate.
Citation Information
Patent Citations
Polishing composition
JP2004259421A
Polishing liquid composition for magnetic disk substrate
JP2009172709A
Electronic material polishing liquid
JP2014127217A
Polishing composition, manufacturing method for magnetic disk substrate, and polishing method for magnetic disk