Production method of thermal conductive sheet
By laminating and slicing composite sheets with controlled properties, the method addresses adhesion and curling issues in thermally conductive sheets, resulting in a stable and effective heat transfer solution.
Patent Information
- Application Number
- JP2023059335
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Thermally conductive sheets face issues with adhesion and curling during manufacturing due to their soft nature, leading to collapse and reduced effectiveness in heat dissipation applications.
A method involving laminating or folding primary composite sheets with low tensile strength and specific storage modulus, followed by slicing at controlled angles and temperatures to produce a thermally conductive sheet with improved adhesiveness and reduced curling.
The method results in a thermally conductive sheet with enhanced collapse resistance, minimal curling, and superior adhesiveness, ensuring effective heat transfer and stability during production.
Smart Images

Figure 2024146439000002 
Figure 2024146439000003 
Figure 2024146439000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a thermally conductive sheet. [Background technology]
[0002] In recent years, the amount of heat generated by electronic components such as plasma display panels (PDPs) and integrated circuit (IC) chips has increased as their performance has improved. As a result, it has become necessary to take measures to prevent malfunctions caused by temperature rises in electronic devices that use these components.
[0003] As a countermeasure against functional failures caused by temperature rises in electronic components, a method is generally adopted in which a heat sink, a heat sink plate, a heat sink fin, or other heat sink made of metal is attached to the heat generating body of the electronic component to promote heat dissipation. When using a heat sink, the heat generating body and the heat sink are usually attached in close contact with each other through a sheet-like member with high thermal conductivity (thermal conductive sheet) in between in order to efficiently transfer heat from the heat generating body to the heat sink.
[0004] Conventionally, various attempts have been made to improve the thermal conductivity of thermally conductive sheets. For example, Patent Document 1 proposes a thermally conductive sheet with smooth main surfaces and excellent thickness accuracy. More specifically, Patent Document 1 proposes a thermally conductive sheet containing a resin and a particulate filler, in which the standard deviation of the thickness is set to a predetermined value or less, the thermal conductivity in the thickness direction is set to a predetermined value or more, and the surface roughness Sa of both main surfaces is set to a predetermined value or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-140982 A Summary of the Invention [Problem to be solved by the invention]
[0006] Here, in recent years, from the viewpoint of increasing the adhesion to the adherend and improving the thermal conductivity, the thermal conductive sheet is also required to have excellent adhesiveness. However, the composition capable of imparting adhesiveness to the thermal conductive sheet also has an aspect of being "soft", and the intended thermal conductive sheet may collapse during production, or the produced thermal conductive sheet may curl.
[0007] Therefore, an object of the present invention is to provide a method for producing a thermally conductive sheet that has excellent resistance to collapse, is less likely to curl, and has excellent adhesiveness during production. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. The present inventors have discovered that when a primary composite sheet having a tensile strength of 1.00 MPa or less is laminated, folded, or wound to obtain a laminate, and then sliced at an angle of 45° or less to the lamination direction using a plane-type slicer, the storage modulus of the primary composite sheet at a frequency of 1 Hz is 0.90×10 8 Pa or more 8.00×10 8 The inventors have newly discovered that performing the heat treatment within a temperature range where the thermal conductive sheet has a thermal conductivity of 0.1 Pa or less suppresses collapse and curling of the thermal conductive sheet during production and furthermore, the thermal conductive sheet obtained has excellent adhesiveness, thereby completing the present invention. The primary composite sheet used is a primary composite sheet obtained by pressing a composite material containing a resin and a thermal conductive filler into a sheet shape.
[0009] That is, the present invention has an object to advantageously solve the above-mentioned problems, and [1] a method for producing a thermally conductive sheet of the present invention is a method for producing a thermally conductive sheet containing a resin and a thermally conductive filler, wherein the resin contains at least one resin that is liquid at room temperature and normal pressure, and the method includes the steps of: pressing a composite material containing the resin and the thermally conductive filler into a sheet shape to obtain a primary composite sheet; laminating a plurality of the primary composite sheets in a thickness direction, or folding or rolling the primary composite sheet to obtain a laminate; and slicing the laminate obtained in the laminate-obtaining step at an angle of 45° or less with respect to the lamination direction using a plane-type slicer to obtain a thermally conductive sheet of a predetermined thickness, wherein the primary composite sheet has a tensile strength of 1.00 MPa or less at 23° C., and the primary composite sheet has a storage modulus of 0.90×10 at a frequency of 1 Hz in the slicing step. 8 Pa or more 8.00×10 8 The slicing process is carried out in a temperature range where the thermal conductivity is 0.1 Pa or less. According to this method for producing a thermally conductive sheet, collapse and curling of the thermally conductive sheet during production are suppressed, and further, the obtained thermally conductive sheet has excellent adhesion. In this specification, "room temperature" refers to 23°C, and "normal pressure" refers to 1 atm (absolute pressure). The "tensile strength of the primary composite sheet at 23°C" and the "storage modulus of the primary composite sheet at a frequency of 1 Hz" can be measured according to the method described in the examples of this specification.
[0010] [2] In the method for producing a thermally conductive sheet according to the above [1], the resin that is liquid at room temperature and normal pressure preferably contains at least one type of acrylic resin. According to this method for producing a thermally conductive sheet, the adhesiveness of the obtained thermally conductive sheet can be further improved.
[0011] [3] In the method for producing a thermally conductive sheet according to [2] above, the weight-average molecular weight of the acrylic resin is preferably 20,000 or less. If the weight-average molecular weight of the acrylic resin is 20,000 or less, the adhesiveness of the obtained thermally conductive sheet can be further improved. The weight-average molecular weight of the acrylic resin can be measured by the method described in the examples of this specification.
[0012] [4] Furthermore, in the method for producing a thermally conductive sheet according to the above [2] or [3], the content of the acrylic resin in the resin is preferably 20% by mass or more and 70% by mass or less. This method can more effectively prevent the thermally conductive sheet from collapsing and curling during production, and can further increase the adhesiveness of the resulting thermally conductive sheet. Effect of the Invention
[0013] According to the present invention, it is possible to provide a method for producing a thermally conductive sheet that has excellent resistance to collapse, is less prone to curling during production, and has excellent adhesiveness. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a diagram for explaining a method for evaluating curl of a thermally conductive sheet in an example of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a method for evaluating curl of a thermally conductive sheet in an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail. The thermally conductive sheet obtained according to the method for producing a thermally conductive sheet of the present invention can be used, for example, by being sandwiched between a heat generating body and a heat sink when attaching the heat sink to the heat generating body. That is, the thermally conductive sheet obtained according to the method for producing a thermally conductive sheet of the present invention can be used as a heat dissipating member to constitute a heat dissipating device together with a heat sink, a heat sink plate, a heat sink fin, or other heat sink.
[0016] (Method of manufacturing thermal conductive sheet) The method for producing a thermally conductive sheet of the present invention is a method for producing a thermally conductive sheet containing a resin and a thermally conductive filler. Here, the resin contains at least one type of resin that is liquid at room temperature and normal pressure. The method for producing a thermally conductive sheet of the present invention includes a step of pressing a composite material containing a resin and a thermally conductive filler into a sheet shape to obtain a primary composite sheet having a tensile strength of 1.00 MPa or less at 23°C (primary composite sheet forming step), a step of laminating a plurality of primary composite sheets in the thickness direction or folding or rolling the primary composite sheet to obtain a laminate (laminate forming step), and a slicing step of slicing the laminate obtained in the laminate forming step at an angle of 45° or less with respect to the lamination direction using a plane-type slicer to obtain a thermally conductive sheet of a predetermined thickness. Here, in the slicing step, the storage modulus of the primary composite sheet at a frequency of 1 Hz is 0.90×10 8 Pa or more 8.00×10 8 The slicing process is characterized in that the slicing process is carried out in a temperature range where the storage modulus at a frequency of 1 Hz of the primary composite sheet is 0.90×10 or less. First, a thermally conductive sheet including a primary composite sheet that contains a resin that is liquid at room temperature and normal pressure and has a tensile strength of 1.00 MPa or less at 23°C has excellent adhesiveness and can enhance adhesion to an adherend. However, due to its softness, such a thermally conductive sheet is prone to collapse during production and curling immediately after slicing. Therefore, the present inventors have investigated various slicing conditions and found that the storage modulus of the primary composite sheet at a frequency of 1 Hz is 0.90×10 8 Pa or more 8.00×10 8 It was found that by performing the slicing process in a temperature range of 0.1 Pa or less, the occurrence of collapse and curling can be effectively suppressed.
[0017] Here, the thermally conductive sheet obtained according to the method for producing a thermally conductive sheet of the present invention may be formed by joining a plurality of strips (primary composite sheets) in parallel. In this case, each strip contains a resin and a thermally conductive filler that are liquid at room temperature and normal pressure, and the thermally conductive filler is oriented in the thickness direction of the thermally conductive sheet in each strip. Here, "orientation" means that the orientation angle of the thermally conductive filler with respect to the main surface of the thermally conductive sheet is 60° or more and 90° or less. The orientation angle can be measured according to the method described in the examples of this specification.
[0018] <Resin> The thermally conductive sheet obtained by the method for producing a thermally conductive sheet of the present invention contains a resin. The resin contains at least one resin that is liquid at room temperature and normal pressure, and may optionally contain a resin that is solid at room temperature and normal pressure.
[0019] <<Resin that is liquid under normal temperature and pressure>> Examples of resins that are liquid at room temperature and normal pressure include fluororesins, silicone resins, acrylic resins, and epoxy resins. These may be used alone or in combination of two or more. Among them, the resins that are liquid at room temperature and normal pressure preferably contain at least one of acrylic resins and fluororesins, and more preferably contain acrylic resins from the viewpoint of further increasing the adhesiveness of the resulting thermal conductive sheet.
[0020] Here, as the acrylic resin that is liquid under normal temperature and normal pressure, a known one can be used. Here, the term "acrylic resin" refers to a polymer containing a repeating unit of a (meth)acrylic acid ester monomer unit and, optionally, a repeating unit other than the (meth)acrylic acid ester monomer unit (hereinafter referred to as "other repeating units"). In this specification, "(meth)acrylic" means acrylic and / or methacrylic. As the acrylic resin that is liquid under normal temperature and normal pressure, one having a molecular weight of a predetermined value or less can be suitably used. The weight average molecular weight of the acrylic resin is preferably 20,000 or less, more preferably 10,000 or less, even more preferably 9,000 or less, even more preferably 8,000 or less, and particularly preferably 7,000 or less. By using such an acrylic resin with a low weight average molecular weight as the acrylic resin that is liquid under normal temperature and normal pressure, the adhesiveness of the thermal conductive sheet can be sufficiently increased. The weight average molecular weight of the acrylic resin that is liquid at room temperature and normal pressure may be, for example, 200 or more, preferably 500 or more, more preferably 700 or more, even more preferably 1,000 or more, still more preferably 1,500 or more, still more preferably 2,000 or more, and still more preferably 2,500 or more.
[0021] Examples of commercially available acrylic resins that are liquid at room temperature and pressure include "ARUFON UP-1000", "ARUFON UP-1010", "ARUFON UP-1020", "ARUFON UP-1021", "ARUFON UP-1061", "ARUFON UP-1080", "ARUFON UP-1110", "ARUFON UP-1170", "ARUFON UP-1190", "ARUFON UP-1500", "ARUFON UH-2000", "ARUFON UH-2041", "ARUFON UH-2190", "ARUFON UC-3510", "ARUFON UG-4010", "ARUFON US-6100", and "ARUFON US-6170" manufactured by Toagosei Co., Ltd.; UT-1001, UMM-1001, etc.
[0022] Examples of fluororesins that are liquid at room temperature and normal pressure include thermoplastic fluororesins that are liquid at room temperature and normal pressure, such as vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropentene-tetrafluoroethylene ternary copolymer, perfluoropropene oxide polymer, tetrafluoroethylene-propylene-vinylidene fluoride copolymer, etc. These may be used alone or in combination of two or more. In addition, examples of commercially available thermoplastic fluororesins that are liquid at room temperature and normal pressure include Viton (registered trademark) LM manufactured by DuPont Co., Ltd., Daiel (registered trademark) G-101 manufactured by Daikin Industries, Ltd., Dyneon (registered trademark) FC2210 manufactured by 3M Ltd., and the SIFEL series manufactured by Shin-Etsu Chemical Co., Ltd.
[0023] <<Resin that is solid at room temperature and pressure>> Here, the thermally conductive sheet may optionally contain a resin other than the resin that is liquid at room temperature and normal pressure. Such a resin may be a resin that is solid at room temperature and normal pressure. Such a resin may be, for example, a fluororesin that is solid at room temperature and normal pressure. Examples of fluororesins that are solid at room temperature and normal pressure include elastomers obtained by polymerizing fluorine-containing monomers, such as vinylidene fluoride-based fluororesins, tetrafluoroethylene-propylene-based fluororesins, and tetrafluoroethylene-purovinyl ether-based fluororesins. More specifically, examples of the thermoplastic fluororesins that are solid at room temperature and normal pressure include polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers, tetrafluoroethylene-hexafluoropropylene copolymers, tetrafluoroethylene-ethylene copolymers, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymers, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymers, polychlorotrifluoroethylene, ethylene-chlorofluoroethylene copolymers, tetrafluoroethylene-perfluorodioxole copolymers, polyvinyl fluoride, tetrafluoroethylene-propylene copolymers, acrylic modified polytetrafluoroethylene, ester modified polytetrafluoroethylene, epoxy modified polytetrafluoroethylene, and silane modified polytetrafluoroethylene. These may be used alone or in combination of two or more. In addition, examples of commercially available thermoplastic fluororesins that are solid at room temperature and normal pressure include Dai-el (registered trademark) G-300 series / G-700 series / G-7000 series (polyol vulcanized vinylidene fluoride-hexafluoropropylene binary copolymers), Dai-el G-550 series / G-600 series (polyol vulcanized vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymers), Dai-el G-800 series (peroxide vulcanized vinylidene fluoride-hexafluoropropylene binary copolymers), Dai-el G-900 series (peroxide vulcanized vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymers), and KYNAR (registered trademark) series (vinylidene fluoride-based fluororesin) and KYNAR (registered trademark) series (vinylidene fluoride-based fluororesin) manufactured by ALKEMA. Examples of such copolymers include the FLEX (registered trademark) series (vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymers); and A-100 (vinylidene fluoride-hexafluoropropylene binary copolymers) manufactured by Chemours.
[0024] <<Resin composition>> The content of the resin in the thermal conductive sheet that is liquid at room temperature and normal pressure is not particularly limited, and is preferably 50% by mass or more, more preferably 70% by mass or more, and preferably 85% by mass or less, based on 100% by mass of the entire resin. If the content of the resin in the liquid state at room temperature and normal pressure is equal to or more than the lower limit, the flexibility of the thermal conductive sheet can be effectively increased, so that the adhesion to the adherend can be improved and higher thermal conductivity can be exhibited. If the content of the resin in the liquid state at room temperature and normal pressure is equal to or less than the upper limit, the thermal conductivity of the thermal conductive sheet can be sufficiently increased by including a sufficient amount of thermally conductive filler.
[0025] In addition, the content of the acrylic resin in the resin contained in the thermal conductive sheet is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, and preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. If the content of the acrylic resin is equal to or more than the lower limit, the adhesiveness of the obtained thermal conductive sheet can be further improved. If the content of the acrylic resin is equal to or less than the upper limit, the collapse and curling of the thermal conductive sheet during production can be further suppressed.
[0026] [Thermal conductive filler] The thermally conductive filler imparts excellent thermal conductivity to the thermally conductive sheet. The thermally conductive filler is not particularly limited, and known thermally conductive fillers such as metal fillers and carbon fillers can be used. Among them, it is preferable to use carbon materials such as particulate carbon materials and fibrous carbon materials as the thermally conductive filler, and it is more preferable to use particulate carbon materials.
[0027] Here, the particulate carbon material is not particularly limited, and examples thereof include graphite such as artificial graphite, scaly graphite, exfoliated graphite, natural graphite, acid-treated graphite, expandable graphite, and expanded graphite; carbon black; etc. These may be used alone or in combination of two or more kinds. Among these, it is preferable to use expanded graphite as the particulate carbon material, because the use of expanded graphite can further improve the thermal conductivity of the thermally conductive sheet.
[0028] The expanded graphite can be obtained by, for example, chemically treating graphite such as flake graphite with sulfuric acid to obtain expandable graphite, expanding the graphite by heat treatment, and then pulverizing the expanded graphite. Examples of the expanded graphite include EC1500, EC1000, EC500, EC300, EC100, and EC50 (all trade names) manufactured by Ito Graphite Industries Co., Ltd.
[0029] The volume average particle diameter of the particulate carbon material is preferably 10 μm or more, more preferably 30 μm or more, and preferably 300 μm or less, and more preferably 200 μm or less. If the average particle diameter of the particulate carbon material is equal to or greater than the above lower limit, the heat transfer path of the particulate carbon material can be better formed in the heat conductive sheet, and the heat conductive sheet can exhibit excellent thermal conductivity. If the average particle diameter of the particulate carbon material is equal to or less than the above upper limit, a heat conductive sheet having a smooth surface and excellent thermal conductivity can be obtained. In the present invention, the "volume average particle diameter" refers to the maximum value (mode diameter) in the volume-based particle diameter distribution measured using a laser diffraction method. The measurement of the volume average particle diameter of the particulate carbon material is not particularly limited, and can be performed by taking out the particulate carbon material from the heat conductive sheet using any method, such as dissolving the resin using a good solvent for the resin contained in the heat conductive sheet.
[0030] The aspect ratio (major axis / minor axis) of the particulate carbon material is preferably 1 or more and 10 or less, and more preferably 1 or more and 5 or less. In the present invention, the "aspect ratio of a particulate carbon material" can be determined by observing a cross section of a strip in the thickness direction with a SEM (scanning electron microscope), measuring the maximum diameter (long diameter) and the particle diameter (short diameter) in a direction perpendicular to the maximum diameter for any 50 pieces of particulate carbon material, and calculating the average value of the ratio of the long diameter to the short diameter (long diameter / short diameter).
[0031] Furthermore, the fibrous carbon material that may be contained in the thermal conductive sheet is not particularly limited, and may be, for example, carbon nanotubes, vapor-grown carbon fibers, carbon fibers obtained by carbonizing organic fibers, cut products thereof, etc. These may be used alone or in combination of two or more.
[0032] Among the above, it is preferable to use a fibrous carbon nanostructure such as a carbon nanotube (hereinafter sometimes referred to as "CNT") as the fibrous carbon material, and it is more preferable to use a fibrous carbon nanostructure containing CNT.
[0033] Here, the fibrous carbon nanostructure containing CNT that can be suitably used as the fibrous carbon material may consist of CNT alone, or may be a mixture of CNT and fibrous carbon nanostructures other than CNT. The CNTs in the fibrous carbon nanostructure are not particularly limited, and single-walled carbon nanotubes and / or multi-walled carbon nanotubes can be used. However, the CNTs are preferably single-walled to five-walled carbon nanotubes, and more preferably single-walled carbon nanotubes.
[0034] The aspect ratio (major axis / minor axis) of the fibrous carbon material is preferably more than 10. In the present invention, the "aspect ratio of the fibrous carbon material" can be determined by using a TEM (transmission electron microscope) to measure the maximum diameter (long diameter) and the outer diameter (short diameter) in a direction perpendicular to the maximum diameter of 100 randomly selected fibrous carbon material fibers, and calculating the average value of the ratio of the long diameter to the short diameter (long diameter / short diameter).
[0035] The average diameter (Av) of the fibrous carbon material is preferably 0.5 nm or more, more preferably 1 nm or more, and preferably 15 nm or less, more preferably 10 nm or less. If the average diameter (Av) of the fibrous carbon material is equal to or more than the lower limit, the aggregation of the fibrous carbon material can be suppressed and the dispersibility of the fibrous carbon material can be improved. If the average diameter (Av) of the fibrous carbon material is 15 nm or less, the thermal conductivity and strength of the thermal conductive sheet can be sufficiently improved. The "average diameter (Av) of the fibrous carbon material" can be determined by measuring the diameter (outer diameter) of 100 randomly selected fibrous carbon material fibers using a TEM (transmission electron microscope).
[0036] Furthermore, the average length of the fibrous carbon material is preferably 0.1 μm or more, more preferably 1 μm or more, and is preferably 5000 μm or less. In the present invention, the "average length of the fibrous carbon material" can be determined by measuring the maximum diameter (long diameter) of 100 randomly selected fibrous carbon material fibers using a TEM (transmission electron microscope) and calculating the average value.
[0037] The BET specific surface area of the fibrous carbon material is 400m 2 / g or more, and 2 / g or more is more preferable, and 2500m 2 / g or less. When the BET specific surface area of the fibrous carbon material is equal to or more than the above lower limit, the thermal conductivity and strength of the thermal conductive sheet can be sufficiently increased. When the BET specific surface area of the fibrous carbon material is equal to or less than the above upper limit, the aggregation of the fibrous carbon material can be suppressed.
[0038] Furthermore, the fibrous carbon material having the above-mentioned properties is not particularly limited, and it is preferable to use a fibrous carbon nanostructure containing CNTs manufactured in accordance with a method (super-growth method; see International Publication No. 2006 / 011655) in which a trace amount of oxidant (catalyst activation material) is made present in the system when a raw material compound and a carrier gas are supplied onto a substrate having a catalyst layer for CNT production on the surface thereof to synthesize CNTs by chemical vapor deposition (CVD) to dramatically improve the catalytic activity of the catalyst layer. Note that, hereinafter, carbon nanotubes obtained by the super-growth method may be referred to as "SGCNTs". Here, the fibrous carbon nanostructure containing SGCNTs produced by the super-growth method may be composed only of SGCNTs, or may contain, in addition to SGCNTs, other carbon nanostructures such as non-cylindrical carbon nanostructures.
[0039] The content of the thermally conductive filler in the thermally conductive sheet is not particularly limited, and is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 60% by mass or less, and more preferably 50% by mass or less. If the content of the thermally conductive filler is equal to or greater than the lower limit, the thermally conductive filler can be sufficiently contained to sufficiently increase the thermal conductivity of the thermally conductive sheet. If the content of the thermally conductive filler is equal to or less than the upper limit, the adhesiveness of the thermally conductive sheet can be further increased, and therefore the adhesion of the thermally conductive sheet to the adherend can be increased.
[0040] Hereinafter, each step included in the method for producing a thermally conductive sheet of the present invention, which can efficiently produce the thermally conductive sheet as described above, will be described in order.
[0041] <Primary composite sheet forming process> In the primary composite sheet forming step, a composite material containing a resin and a thermally conductive filler is pressed into a sheet shape to obtain a primary composite sheet having a tensile strength at 23° C. of 1.00 MPa or less.
[0042] [Composite materials] Here, the composite material can be prepared by mixing all the components forming the thermally conductive sheet, i.e., the above-mentioned resin, the thermally conductive filler, and optionally other components. The above-mentioned components can be mixed using a known mixing device such as a kneader, a roll, or a mixer, without any particular limitation. The mixing may be optionally performed in the presence of a solvent such as an organic solvent. The mixing time can be, for example, 5 minutes or more and 60 minutes or less. The mixing temperature can be, for example, 5°C or more and 150°C or less.
[0043] [Molding of composite materials] The composite material prepared as described above can be optionally degassed, optionally removed from the solvent, and crushed, and then pressed (primary pressing) to form it into a sheet. Here, the composite material can be molded into a sheet shape using known molding methods such as press molding, rolling molding, and extrusion molding, without any particular limitation, as long as the molding method involves the application of pressure. Among these, the composite material is preferably formed into a sheet shape by rolling molding, and more preferably molded into a sheet shape by passing the composite material between rolls while sandwiched between protective films. The protective film is not particularly limited, and a polyethylene terephthalate (PET) film that has been subjected to a sandblasting treatment can be used. The roll temperature can be 5°C or higher and 150°C or lower.
[0044] [Properties of primary composite sheet] The thickness of the primary composite sheet obtained by pressing the composite material into a sheet shape is not particularly limited, and can be, for example, 0.05 mm or more and 2 mm or less. The primary composite sheet must have a tensile strength of 1.00 MPa or less. The tensile strength of the primary composite sheet is preferably 0.80 MPa or less, more preferably 0.60 MPa or less, and preferably 0.20 MPa or more. If the tensile strength of the primary composite sheet is equal to or less than the upper limit, the adhesion of the resulting thermally conductive sheet to the adherend can be improved. If the tensile strength of the primary composite sheet is equal to or more than the lower limit, the collapse resistance of the resulting thermally conductive sheet can be further reduced. Here, the tensile strength can be controlled according to the type of resin used, the amount of thermally conductive filler blended, and the like.
[0045] <Laminate formation process> In the laminate formation step, a laminate is obtained by laminating a plurality of primary composite sheets in the thickness direction, or by folding or rolling the primary composite sheet.
[0046] Here, in order to further increase the adhesive strength between the surfaces of the primary composite sheets in the laminate obtained in the laminate formation process and sufficiently suppress delamination of the laminate, the laminate formation process may be carried out with the surface of the primary composite sheet slightly dissolved in a solvent, or with an adhesive applied to the surface of the primary composite sheet or with an adhesive layer provided on the surface of the primary composite sheet, or the laminate in which the primary composite sheets are stacked may be further hot pressed (secondary pressure) in the stacking direction.
[0047] From the viewpoint of efficiently suppressing delamination, it is preferable to subject the obtained laminate to secondary pressure in the lamination direction. The conditions for secondary pressure are not particularly limited, and the pressure in the lamination direction can be 0.05 MPa or more and 2.5 MPa or less at a temperature of 20°C or more and 170°C or less for 10 seconds to 90 minutes.
[0048] In the laminate obtained by stacking, folding or rolling the primary sheet, the thermally conductive filler is presumably oriented in a direction substantially perpendicular to the stacking direction. For example, when the thermally conductive filler is a particulate carbon material and has a scale-like shape, the direction of the major axis of the main surface of the scale-like shape is presumably substantially perpendicular to the stacking direction.
[0049] <Slicing process> In the slicing process, the laminate obtained in the laminate forming process is sliced at an angle of 45° or less to the lamination direction using a plane-type slicer to obtain a thermally conductive sheet of a predetermined thickness consisting of slices of the laminate. The thermally conductive sheet obtained through the slicing process usually has a configuration in which strips containing resin and thermally conductive filler (slices of the primary composite sheet that constituted the laminate) are joined in parallel to each other.
[0050] Here, from the viewpoint of increasing the thermal conductivity of the thermal conduction sheet, the angle at which the laminate is sliced is preferably 30° or less with respect to the stacking direction, more preferably 15° or less with respect to the stacking direction, and preferably approximately 0° with respect to the stacking direction (i.e., in the direction along the stacking direction).
[0051] In order to prevent the collapse of the laminate during slicing and to prevent curling of the resulting thermally conductive sheet, the storage modulus of the primary composite sheet at a frequency of 1 Hz is set to 0.90 × 10 8 Pa or more 8.00×10 8 It is necessary to perform the slicing step in a temperature range where the storage modulus of the primary composite sheet at a frequency of 1 Hz is within the following range, i.e., 1.10×10 8 The range of 5.00×10 Pa or more is preferable. 8 The range of 4.00×10 Pa or less is preferable. 8 It is more preferable that the storage modulus is in the range of 0.1 to 1.0 Pa or less. Under conditions where the storage modulus is equal to or greater than the above lower limit, collapse of the laminate can be more effectively suppressed. Also, under conditions where the storage modulus is equal to or less than the above upper limit, curling can be more effectively suppressed. The storage modulus of the laminate in the slicing step can be set to the appropriate range by appropriately controlling the temperature conditions in the processing space where slicing is performed.
[0052] Furthermore, from the viewpoint of suppressing collapse of the laminate during slicing and suppressing curling of the resulting thermally conductive sheet, it is preferable to slice the laminate while applying pressure in a direction perpendicular to the stacking direction, and it is more preferable to slice the laminate while applying a pressure of 0.1 MPa or more and 0.5 MPa or less in the direction perpendicular to the stacking direction.
[0053] In the thermally conductive sheet obtained through the various processes described above, the thermally conductive filler is well oriented in the thickness direction. For example, when the thermally conductive filler is a particulate carbon material and has a scale shape, the direction of the major axis of the main surface of the scale shape approximately coincides with the thickness direction of the secondary sheet. EXAMPLES
[0054] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the examples and comparative examples, various measurements and evaluations were carried out as follows.
[0055] <Weight average molecular weight of acrylic resin> The weight-average molecular weight of the acrylic resin used as the raw material was measured by gel permeation chromatography (GPC) under the following conditions. Measurements by GPC were performed using a GPC system (Tosoh Corporation, HLC-8220) with two H-type columns (Tosoh Corporation, HZ-M) connected in series, tetrahydrofuran as the solvent, and a column temperature of 40°C. A differential refractometer (Tosoh Corporation, RI-8320) was used as the detector.
[0056] <Tensile strength of primary composite sheet> The primary composite sheets produced in the Examples and Comparative Examples were punched out using a dumbbell No. 2 (dumbbell shape, width 3 mm, length 70 mm) conforming to JIS K7113 to prepare samples. Using a tensile testing machine (manufactured by Shimadzu Corporation, product name "AG-IS20kN"), the breaking strength (tensile strength) was measured under the following conditions: load cell: 50 N, chuck distance: 35 mm, speed: 50 mm / min, temperature: 23° C. The average value of the measurements for the five sample pieces was taken as the tensile strength of each primary composite sheet.
[0057] <Orientation angle of thermally conductive filler> The thermally conductive sheets manufactured in the examples and comparative examples were cut into a square and the cross section was observed with a scanning electron microscope (SEM, Hitachi High-Technologies Corporation's "SU-3500") at a magnification that allowed the sheet to be viewed from top to bottom. The magnification was 700x. 50 lines were drawn along the long axis of the graphite particles in this cross section, and the average angle of the long axis with respect to the main surface of the thermally conductive sheet was calculated. If the angle was 90° or more, a supplementary angle was used. This was performed on four surfaces, and the average value of the filler orientation angles on the four surfaces was taken as the orientation angle of the filler. The closer the orientation angle of the thermally conductive filler is to 90°, the higher the thermal conductivity of the thermally conductive sheet. In all examples and comparative examples, it was confirmed that the orientation angle was 60° or more.
[0058] <Volume average particle size of thermally conductive filler> The particle size of the thermally conductive filler (expanded graphite) contained in the suspension was measured using a laser diffraction / scattering type particle size distribution analyzer (Horiba, Ltd., model "LA-960"), and a volumetric particle size distribution curve was obtained with the horizontal axis representing the particle size and the vertical axis representing the volume of the thermally conductive filler, and the particle size at the maximum value (mode diameter) was calculated as the volume average particle size of the thermally conductive filler.
[0059] <Storage modulus of primary composite sheet> The primary composite sheets prepared in the examples and comparative examples were cut to a size of 12.7 x 50.0 mm to prepare samples. The storage modulus was measured using a rotational rheometer (TA Instruments, model "ARES-G2") under the following conditions: temperature: -40°C to 40°C, heating rate: 2°C / min, frequency: 1 Hz, strain: 0.25%. The average value of the measurements of the three sample pieces was taken as the storage modulus of each primary composite sheet.
[0060] <Collapse resistance of thermal conductive sheet> The dimensional change of the surface of the laminate that rubbed against the slicer stage in the slicing process was measured before and after slicing with a vernier caliper (standard ABS digital caliper, manufactured by Mitutoyo Corporation). Measurements were taken before and after slicing at four locations: one on each side, 1 cm from the end face of the laminate in the direction parallel to the lamination direction of the pre-thermal conductive sheet, and one on each side, 1 cm from the end face of the laminate in the direction perpendicular to the lamination direction of the pre-thermal conductive sheet. The measurements were then evaluated along with the appearance of the obtained thermal conductive sheet according to the following criteria. The dimensional change rate was calculated as follows. Dimensional change rate (%) = (average of four dimensions after slicing ÷ average of four dimensions before slicing - 1) × 100 A: The dimensional change rate is 2% or less, and no cracks are observed. B: The dimensional change rate exceeds 2%, but no cracking is observed. C: The dimensional change rate exceeds 2% and cracks are observed.
[0061] <Curling of the thermal conductive sheet> The evaluation of the curl of the thermal conductive sheet was carried out in two steps: 1) visually checking for the presence of curl; and 2) measuring using a ruler. First, 1) visually checking for the presence of curl, and if no curl was found, it was rated as good (A). Next, for those that were found to have curl, 2) measuring using a ruler was carried out as follows to evaluate them. A method for evaluating the curl of a thermally conductive sheet in step 2) above will be described with reference to Figs. 1 and 2. Figs. 1 and 2 show schematic diagrams of exemplary thermally conductive sheets 10 and 20 to be evaluated for curl. The thermally conductive sheets 10 and 20 include curl generation regions 11 and 21, respectively. In a thermally conductive sheet that requires surface accuracy, the curl generation regions 11 and 21 are regions that may become surplus portions when the sheet is manufactured. Therefore, the smaller the area of the curl generation regions 11 and 21, the higher the product yield, which is preferable. Here, the thermally conductive sheet product may be rectangular. For this reason, it is preferable to obtain a thermally conductive sheet from which such a rectangular thermally conductive sheet product can be cut out with as large an area as possible. In the thermally conductive sheet 10 shown in Fig. 1, the maximum rectangular region is R 1 and such a region R 1 The short side of is L1. The same applies to Figure 2. 1 , R 2 Define the long side (short side L 1 , L 2 It was judged whether the length of the short side L (the side perpendicular to each of the long sides) of the thermal conductive sheets 10 and 20 obtained through the slicing process was about 85% or more of the length of one side of the thermal conductive sheets 10 and 20 themselves (i.e., 130 mm or more, which is greater than 127.5 mm, which is 85% of 150 mm). If the result was less than 85%, the sheet was not evaluated, but there were no samples in this embodiment or comparative example that met this criteria. Furthermore, for samples whose long side was 130 mm or more, the short side L 1 ,L 2The length of each was measured and it was judged whether it was 40% or more of the length of one side of the thermal conductive sheets 10 and 20 obtained through the slicing process (i.e., 60 mm or more, which is 40% of 150 mm). If this was met, the curl evaluation was rated as B, and if not, it was rated as C.
[0062] <Tackiness> The adhesion of the thermally conductive sheet was measured using a probe tack tester (manufactured by Rhesca Corporation, product name "TAC1000") in an atmosphere at 25°C. The thermally conductive sheet punched out to φ4 mm was attached with double-sided tape to the tip of a flat circular probe with φ5 mm on a lid placed on a stage, and the probe was pressed with a pressure of 0.5 MPa for 10 seconds on the lid, and the force required to pull the probe with the thermally conductive sheet attached from the lid was measured. The measured adhesion value is an index of the adhesion of the thermally conductive sheet to an adherend, such as metal, and the higher the measured value, the better the adhesion to an adherend such as metal.
[0063] Example 1 <Preparation of composite material> 36 parts of a thermoplastic fluororesin (manufactured by Daikin Industries, Ltd., trade name "Daiel G-101") that is liquid at room temperature and normal pressure as a resin that is liquid at room temperature and normal pressure, 22 parts of a thermoplastic fluororesin (manufactured by 3M Japan Ltd., trade name "Dyneon FC2211") that is solid at room temperature and normal pressure, 42 parts of a hydroxyl-containing liquid acrylic polymer (manufactured by Toagosei Co., Ltd., trade name "ARUFON (registered trademark) UH-2190") that is liquid at room temperature and normal pressure as a resin that is liquid at room temperature and normal pressure, and 90 parts of expanded graphite (manufactured by Ito Graphite Industries Co., Ltd., trade name "EC-300", volume average particle size: 50 μm) as a thermally conductive filler were stirred and mixed for 5 minutes using a Hobart mixer (manufactured by Kodaira Manufacturing Co., Ltd., trade name "ACM-5LVT type"). The resulting mixture was vacuum degassed for 30 minutes to obtain a composition that is a composite material. The resulting composition was then put into a crusher and crushed for 10 seconds. <Formation of primary composite sheet> Next, 1 kg of the crushed composition was sandwiched between sandblasted PET films (protective films) having a thickness of 50 μm, and rolled (primary pressing) under the conditions of a roll gap of 600 μm, a roll temperature of 50° C., a roll linear pressure of 50 kg / cm, and a roll speed of 1 m / min to obtain a primary composite sheet having a thickness of 0.8 mm. The tensile strength of the obtained primary composite sheet was measured as described above. <Formation of Laminate> Next, the obtained primary composite sheet was cut to a size of 150 mm length x 150 mm width x 0.8 mm thickness, and 190 sheets were stacked in the thickness direction of the primary composite sheet. Further, the sheet was pressed (secondary pressurization) in the stacking direction at a temperature of 25°C and a pressure of 0.1 MPa for 3 minutes to obtain a laminate with a height of approximately 150 mm. <Formation of thermal conductive sheet by slicing process> Then, while pressing the laminated side of the secondarily pressed laminate with a pressure of 0.3 MPa, a woodworking slicer (manufactured by Marunaka Iron Works Co., Ltd., product name ``Super Finishing Planer Super Mecha S'') was used to slice at an angle of 0 degrees to the lamination direction (in other words, in the normal direction to the main surface of the laminated primary composite sheet) with the temperature in the processing space of the slicer at 15°C, to obtain a thermally conductive sheet of 150 mm in length x 150 mm in width x 0.15 mm in thickness. The sliced laminate and the resulting thermally conductive sheet were then subjected to various measurements and evaluations according to the methods described above. The results are shown in Table 1.
[0064] Example 2 A thermally conductive sheet was produced in the same manner as in Example 1, except that the temperature in the processing space of the slicer in the slicing step was set to 0° C. Then, various measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0065] Example 3 A thermally conductive sheet was produced in the same manner as in Example 1, except that the temperature in the processing space of the slicer in the slicing step was set to 18° C. Then, various measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0066] Example 4 In preparing the composite material, the amounts of the thermoplastic fluororesin that is liquid at room temperature and normal pressure used in Example 1 were changed to 85 parts, the thermoplastic fluororesin that is solid at room temperature and normal pressure used in Example 1 to 15 parts, the amount of the acrylic polymer used in Example 1 to 0 parts, and the amount of the expanded graphite used in Example 1 to 70 parts, and the temperature in the processing space of the slicer in the slicing step was changed to 23° C., and other than these, various operations, measurements, and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.
[0067] Example 5 In preparing the composite material, the amounts of the thermoplastic fluororesin that is liquid at room temperature and normal pressure used in Example 1 were changed to 55 parts, the thermoplastic fluororesin that is solid at room temperature and normal pressure used in Example 1 was changed to 20 parts, and the amount of the acrylic polymer used in Example 1 was changed to 25 parts, respectively. Various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0068] Example 6 In preparing the composite material, various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that a hydroxyl-containing liquid acrylic polymer having a weight average molecular weight of 11,000 (manufactured by Toagosei Co., Ltd., product name "ARUFON (registered trademark) UH-2000") was used as the acrylic polymer instead of the acrylic polymer used in Example 1. The results are shown in Table 1.
[0069] Comparative Example 1 A thermally conductive sheet was produced in the same manner as in Example 1, except that the temperature in the processing space of the slicer in the slicing step was set to 23° C. Then, various measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0070] Comparative Example 2 A thermally conductive sheet was produced in the same manner as in Example 1, except that the temperature in the processing space of the slicer in the slicing step was set to -10°C. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.
[0071] Comparative Example 3 In preparing the composite material, the amount of the thermoplastic fluororesin that is liquid at room temperature and normal pressure used in Example 1 was changed to 70 parts, the amount of the thermoplastic fluororesin that is solid at room temperature and normal pressure used in Example 1 was changed to 30 parts, the amount of the acrylic polymer used in Example 1 was changed to 0 part, and the temperature in the processing space of the slicer in the slicing step was changed to 23° C., but other than that, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.
[0072] [Table 1]
[0073] From Table 1, a slice of a laminate formed using a primary composite sheet with a tensile strength of 1.00 MPa or less was prepared by dividing the slice into two pieces by the storage modulus of the primary composite sheet at a frequency of 1 Hz of 0.90 × 10 8 Pa or more 8.00×10 8 It can be seen that the thermally conductive sheets obtained in Examples 1 to 6, which were obtained in a temperature range of 0.1 MPa or less, had high levels of collapse resistance, curl suppression, and adhesion. On the other hand, it can be seen that the thermally conductive sheets obtained in Comparative Examples 1 and 2, in which the slicing process conditions did not satisfy the above-mentioned conditions regarding the storage modulus, and in Comparative Example 3, in which the tensile strength exceeded 1.00 MPa, did not achieve effects comparable to those of the Examples. [Industrial Applicability]
[0074] According to the present invention, it is possible to provide a method for producing a thermally conductive sheet that has excellent resistance to collapse, is less prone to curling during production, and has excellent adhesiveness. [Explanation of symbols]
[0075] 10,20 Thermal conductive sheet 11,21 Curl area R 1 , R 2 rectangular area L 1 ,L 2 Short Side
Claims
1. A method for producing a thermally conductive sheet containing a resin and a thermally conductive filler, comprising the steps of: The resin includes at least one resin that is liquid under normal temperature and pressure, a step of pressing the composite material containing the resin and the thermally conductive filler into a sheet shape to obtain a primary composite sheet; a step of laminating a plurality of the primary composite sheets in a thickness direction, or folding or rolling the primary composite sheet to obtain a laminate; and a slicing step of slicing the laminate obtained in the step of obtaining the laminate with a plane-type slicer at an angle of 45° or less with respect to the lamination direction to obtain a thermally conductive sheet of a predetermined thickness. The primary composite sheet has a tensile strength of 1.00 MPa or less at 23°C, In the slicing step, the storage modulus of the primary composite sheet at a frequency of 1 Hz is 0.90×10 8 Pa or more 8.00×10 8 The slicing process is performed in a temperature range of 0.1 Pa or less. A method for manufacturing a thermally conductive sheet.
2. The method for producing a thermal conductive sheet according to claim 1 , wherein the resin that is liquid at room temperature and normal pressure contains at least one type of acrylic resin.
3. The method for producing a thermal conductive sheet according to claim 2 , wherein the weight average molecular weight of the acrylic resin is 20,000 or less.
4. The method for producing a thermal conductive sheet according to claim 2 or 3, wherein a content of the acrylic resin in the resin is 20% by mass or more and 70% by mass or less.
Citation Information
Patent Citations
Heat conductive sheet and method of manufacturing the same
JP2020140982A