Method for producing polyacetal
By employing a carbonate ester-diluted boron trifluoride catalyst, the method maintains catalyst activity and prevents precipitate formation, ensuring efficient and continuous polyacetal production.
Patent Information
- Application Number
- JP2023059378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing methods for producing polyacetal using boron trifluoride-based catalysts face challenges in maintaining catalyst activity when diluted with solvents, leading to reduced polymerization efficiency and the formation of precipitates like tar and scale, which can cause operational disruptions.
Using an organic solvent containing a carbonate ester with a boiling point of 150°C or less to dilute the boron trifluoride catalyst, ensuring the catalyst's activity is maintained while suppressing the formation of precipitates, allowing for continuous polymerization.
The method achieves high-yield production of polyacetal with controlled polydispersity and prevents the formation of tar and scale, enabling long-term continuous operation.
Smart Images

Figure 2024146467000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing polyacetal. [Background technology]
[0002] Polyacetal has an excellent balance of mechanical properties, chemical resistance, sliding properties, etc., and is easy to process, so it is widely used as a representative engineering plastic, mainly for electrical parts, electronic parts, automotive parts, and various other machine parts. As the range of its use expands in recent years, there is a tendency for increasingly high mechanical properties to be required.
[0003] A widely used method for producing polyacetal is cationic polymerization of cyclic ethers such as 1,3,5-trioxane (hereinafter sometimes simply referred to as trioxane).
[0004] In general, as a polymerization catalyst for trioxane, a boron trifluoride ether complex (e.g., boron trifluoride diethyl ether complex, boron trifluoride dibutyl ether complex) is often used, and in such a case, the polymerization catalyst is often used after being diluted with a solvent. For example, Patent Document 1 discloses a method for producing polyacetal using a cyclohexane solution of a boron trifluoride diethyl ether complex.
[0005] Moreover, Patent Document 2 discloses a method for producing polyacetal using a dibutyl ether solution of a boron trifluoride dibutyl ether complex.
[0006] Furthermore, Patent Document 3 discloses a method for producing polyacetal using a boron trifluoride di-n-butyl ether complex and a mixed liquid of cyclohexane and n-hexane, as an example of a method for suppressing scale generation inside a polymerization reactor and enabling long-term stable operation. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2022 / 085280 [Patent Document 2] International Publication No. 2020 / 137414 [Patent Document 3] JP 2017-82099 A Summary of the Invention [Problem to be solved by the invention]
[0008] For example, in order to obtain a polymer having a high molecular weight and a controlled polydispersity in a twin-shaft paddle type continuous polymerization reactor, it is essential to disperse the polymerization catalyst in a monomer (e.g., trioxane) in a highly active state and to carry out the polymerization as uniformly as possible in the polymerization reactor.
[0009] For this purpose, it is essential to design the reaction system so that the polymerization catalyst is diluted with a solvent and dispersed in the monomer, and polymerization is initiated by contact between the polymerization catalyst and the monomer after the polymerization catalyst is dispersed in the monomer.
[0010] However, when a highly reactive compound such as boron trifluoride or its ether complex is used as a polymerization catalyst, the solvent used for dilution may react with the polymerization catalyst, thereby reducing the activity of the polymerization catalyst.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing polyacetal which uses boron trifluoride or an ether complex thereof as a polymerization catalyst, and which is capable of producing polyacetal having a high molecular weight and a controlled polydispersity index without decreasing polymerization activity even when the polymerization catalyst is diluted with a solvent, and which further suppresses the formation of precipitates such as tar and scale, thereby enabling continuous operation over long periods of time. [Means for solving the problem]
[0012] The present inventors have conducted extensive investigations to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by using a polymerization catalyst containing boron trifluoride or an ether complex of boron trifluoride, and by supplying monomers such as trioxane to a polymerization reactor to carry out polymerization, and by using an organic solvent containing a carbonate ester as a diluent solvent, thereby completing the present invention.
[0013] That is, the present invention is as follows. [1] A method for producing polyacetal, the method comprising: A catalyst solution (a) containing a polymerization catalyst including boron trifluoride or an ether complex of boron trifluoride and an organic solvent; At least one cyclic ether and / or cyclic formal (b) containing trioxane, A polymerization step of supplying the mixture to a polymerization reactor and carrying out polymerization, The organic solvent contains a carbonate ester. A method for producing polyacetal. [2] The method for producing a polyacetal according to [1], wherein the standard boiling point of the carbonate ester is 150°C or lower. Effect of the Invention
[0014] According to the present invention, when using boron trifluoride or its ether complex as a polymerization catalyst, polyacetal can be produced in high yield without decreasing the polymerization activity even when the polymerization catalyst is diluted with a solvent. In addition, the formation of precipitates such as tar and scale is suppressed, making it possible to operate continuously for a long period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail.
[0016] The method for producing polyacetal of the present embodiment includes a polymerization step of supplying a catalyst solution (a) containing a polymerization catalyst including boron trifluoride or an ether complex of boron trifluoride and an organic solvent, and at least one cyclic ether and / or cyclic formal (b) including trioxane to a polymerization reactor to carry out polymerization, wherein the organic solvent includes a carbonate ester.
[0017] (Catalyst solution (a)) In this embodiment, a catalyst solution (a) containing a polymerization catalyst and an organic solvent is supplied to a polymerization reactor to carry out polymerization.
[0018] <Polymerization catalyst> The polymerization catalyst contained in the catalyst solution (a) used in this embodiment includes boron trifluoride or a boron trifluoride ether complex. Among them, boron trifluoride dialkyl ether complex is more preferred, and boron trifluoride diethyl ether complex or boron trifluoride di-n-butyl ether complex is even more preferred. Furthermore, boron trifluoride diethyl ether complex is particularly preferred because it has a large mole number per unit volume.
[0019] <Organic solvent> The organic solvent contained in the catalyst solution (a) used in this embodiment contains a carbonate ester.
[0020] In general, it is said that the boron trifluoride ether complex generates protons by reacting with water in the system, and these protons initiate the polymerization of monomers such as trioxane. According to the present invention, the yield is improved by the catalyst solution (a) containing a carbonate ester. The reason for this effect is not clear, but it is speculated that this is because the carbonate ester has an appropriate polarity, so that the ether compound dissociates appropriately from the boron trifluoride ether complex, and an appropriate amount of protons is generated by the reaction with water. In addition, the boron trifluoride ether complex may be denatured by impurities in the catalyst solution (a) to produce a tar-like precipitate. This tendency is particularly noticeable when an organic solvent with low polarity (e.g., an aliphatic hydrocarbon compound) is used, and the precipitate may cause problems such as clogging of the liquid delivery pump. However, by including a carbonate in the catalyst solution (a), it is possible to prevent such a precipitate from being produced.
[0021] In this embodiment, the term "carbonate ester" refers to R 1 -O-CO-OR 2 (In the formula, R 1 and R 2 R is a compound represented by the structural formula: 1 and R 2 Examples of the optional substituent represented by the formula (1) include a hydrocarbon group, a group in which a hydrogen atom constituting a carbon-hydrogen bond of a hydrocarbon group is substituted with a substituent (e.g., a halogen atom such as fluorine or chlorine, a hydroxyl group, an amino group, a cyano group), etc. Examples of the hydrocarbon group include, but are not limited to, an alkyl group which may have a branched structure and / or a ring structure, an aromatic ring-containing hydrocarbon group, etc. Examples of alkyl groups which may include branched and / or cyclic structures include, but are not limited to, methyl, ethyl, propyl (including isomers), butyl (including isomers), pentyl (including isomers), hexyl (including isomers), cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, methylcyclopropyl, methylcyclobutyl, methylcyclopentyl, methylcyclohexyl, ethylcyclopropyl, ethylcyclobutyl, ethylcyclopentyl, ethylcyclohexyl, cyclopropylmethyl, cyclobutylmethyl, cyclopentylmethyl, cyclohexylmethyl, cyclopropylethyl, cyclobutylethyl, cyclopentylethyl, cyclohexylethyl, and the like. Examples of aromatic ring-containing hydrocarbon groups include, but are not limited to, phenyl, methylphenyl, ethylphenyl, dimethylphenyl, methylethylphenyl, diethylphenyl, benzyl, phenethyl, biphenyl, naphthyl, methylnaphthyl, ethylnaphthyl, dimethylnaphthyl, methylethylnaphthyl, diethylnaphthyl, and the like. The carbonate ester in this embodiment is preferably a carbonate ester in which two hydrogen atoms of carbonic acid (HO-CO-OH) are substituted with a hydrocarbon group, more preferably a carbonate ester in which two hydrogen atoms of carbonic acid are substituted with an alkyl group which may have a branched structure and / or a ring structure, and even more preferably a carbonate ester in which two hydrogen atoms of carbonic acid are substituted with an alkyl group having 1 to 6 carbon atoms which may have a branched structure and / or a ring structure. More preferred examples of the carbonate ester include dimethyl carbonate, diethyl carbonate, and dipropyl carbonate (including isomers). The carbonate ester in this embodiment may also be a compound in which a hydrogen atom constituting a carbon-hydrogen bond of the carbonate ester exemplified above is substituted with a substituent (for example, a halogen atom such as fluorine or chlorine, a hydroxyl group, an amino group, or a cyano group).
[0022] The carbonate ester preferably has a normal boiling point of 150° C. or lower, from the viewpoint of easily volatilizing it so as not to remain in the produced polyacetal (and removing it if necessary).
[0023] <Other components of catalyst solution (a) and concentrations of each component in catalyst solution (a)> In this embodiment, the concentration of the carbonate ester in the catalyst solution (a) is preferably 80% by mass or more, more preferably 90% by mass or more, and more preferably 99.99% by mass or less, and more preferably 99.9% by mass or less. The concentration of the carbonate ester can be set within the above range by adjusting the amount of the carbonate ester used when preparing the catalyst solution (a). Alternatively, the prepared catalyst solution (a) can be analyzed by, for example, gas chromatography or the like. 1It is also possible to analyze the catalyst solution (a) by 1 H NMR or the like, and select one whose carbonate ester concentration is within the above range for use.
[0024] In this embodiment, the catalyst solution (a) may contain an organic solvent other than carbonate ester, for example, a hydroxy compound in which a hydroxy group is added to a hydrocarbon group, a hydroxy compound in which a hydrogen atom constituting a carbon-hydrogen bond is substituted with a substituent (for example, a halogen atom such as fluorine or chlorine, a hydroxyl group, an amino group, a cyano group), etc. In addition, within a range that does not deactivate the polymerization catalyst, it may contain an aliphatic ether compound in which two aliphatic groups are bonded together via an oxygen atom, an aromatic ether compound in which two aromatic groups are bonded together via an oxygen atom, an aromatic aliphatic ether compound in which an aromatic group and an aliphatic group are bonded together via an oxygen atom, an aliphatic ester compound in which two aliphatic groups are bonded together via an ester bond (-CO-O-), an aromatic ester compound in which two aromatic groups are bonded together via an ester bond, an aromatic aliphatic ester compound in which an aliphatic group and an aromatic group are bonded together via an ester bond, etc.
[0025] In this embodiment, the amount of the organic solvent having low polarity in the catalyst solution (a) is preferably as small as possible in order to ensure the solubility of the polymerization catalyst, and is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. Examples of the organic solvent having low polarity include aliphatic hydrocarbon compounds.
[0026] The concentration of the polymerization catalyst in the catalyst solution (a) is preferably 0.01% by mass or more and 20% by mass or less. If the concentration of the polymerization catalyst in the catalyst solution (a) is equal to or more than the lower limit, the polymerization reaction can be more reliably carried out, and if the concentration of the polymerization catalyst is equal to or less than the upper limit, a rapid reaction can be more suppressed and the polymerization can be more stably carried out.
[0027] (At least one cyclic ether and / or cyclic formal (b)) In this embodiment, at least one cyclic ether and / or cyclic formal (b) is used as a monomer component. The cyclic ether and / or cyclic formal (b) refers to a cyclic compound having at least one carbon-oxygen bond or carbon-oxygen-carbon bond, and also includes a formaldehyde polymer (trimer, tetramer, etc.). Examples of the cyclic ether and / or cyclic formal (b) include trioxane, tetraoxane, ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epibromohydrin, styrene oxide, oxatane, 1,3-dioxolane, ethylene glycol formal, propylene glycol formal, diethylene glycol formal, triethylene glycol formal, 1,4-butanediol formal, 1,5-pentanediol formal, 1,6-hexanediol formal, etc. The cyclic ether and / or cyclic formal (b) may be used alone or in combination of two or more kinds.
[0028] At least one kind of cyclic ether and / or cyclic formal (b) used in this embodiment must contain trioxane. Trioxane is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous solution of formalin in the presence of an acid catalyst. This trioxane may contain impurities such as water, methanol, formic acid, and methyl formate that cause chain transfer, so it is preferable to purify the trioxane in advance by a method such as distillation to remove these impurities.
[0029] When purifying trioxane as described above, the total amount of impurities to be chain-transferred is 1×10 per 1 mol of trioxane. -3 mol or less, and more preferably 0.5×10 -3 By reducing the amount of impurities to the above values, the polymerization reaction rate can be increased sufficiently for practical use, and various properties such as the thermal stability of the produced polymer can be improved.
[0030] The amount of trioxane in the at least one cyclic ether and / or cyclic formal (b) is preferably in the range of 80 to 100 mol%, more preferably 85 to 100 mol%, even more preferably 90 to 100 mol%, and still more preferably 95 to 100 mol%, based on the total number of moles of the cyclic ether and / or cyclic formal (b).
[0031] When trioxane and a cyclic ether and / or a cyclic formal other than trioxane are used in combination as the at least one cyclic ether and / or cyclic formal (b), the cyclic ether and / or cyclic formal other than trioxane is particularly preferably 1,3-dioxolane or 1,4-butanediol formal.
[0032] When trioxane and a cyclic ether and / or a cyclic formal other than trioxane are used in combination as the at least one cyclic ether and / or cyclic formal (b), the amount of the cyclic ether and / or the cyclic formal other than trioxane added is preferably in the range of 1 to 20 mol%, more preferably 1 to 15 mol%, even more preferably 1 to 10 mol%, and even more preferably 1 to 5 mol%, based on the number of moles of trioxane.
[0033] (Chain transfer agent) In the polymerization step of this embodiment, a chain transfer agent may be used in some cases for the purpose of controlling the molecular weight.
[0034] For example, the following general formula: R 3 O-(CH2-O) n -R 4 (In the formula, R 3 and R 4are each independently any one selected from the group consisting of hydrogen or a branched or linear alkyl group, and n is an integer of 1 to 20.) can also be used. In particular, by using an acetal having a molecular weight of 200 or less, preferably 60 to 170, the molecular weight of the finally obtained polyacetal can be well adjusted. Examples of low molecular weight acetals represented by the above general formula include, but are not limited to, methylal, methoxymethylal, dimethoxymethylal, trimethoxymethylal, etc. These may be used alone or in combination of two or more.
[0035] The amount of the low molecular weight acetal represented by the above general formula to be added is 0.1×10 per 1 mol of the total number of moles of trioxane, cyclic ether, and cyclic formal, from the viewpoint of controlling the molecular weight of the target polyacetal within a suitable range. -5 ~0.2×10 -2 The mol range is preferred, with 0.1×10 -5 ~0.2×10 -3 The mol range is more preferred, with 0.1×10 -5 ~0.1×10 -3 The molar range is more preferred.
[0036] (polymerization process) The polymerization step (polymerization) in this embodiment can be carried out by a known method, for example, by adding the catalyst solution (a) to at least one of the above-mentioned cyclic ether and / or cyclic formal (b) (hereinafter sometimes referred to as "monomer (b)"). The shape (structure) of the polymerization reactor used is not particularly limited, but for example, a polymerization reactor in which a heat medium can be passed through the jacket, more specifically a two-shaft paddle-type or screw-type stirring and mixing type polymerization reactor can be suitably used. Then, in this embodiment, polyacetal is obtained by the polymerization step.
[0037] As a polymerization method, for example, a method of supplying the catalyst solution (a), the monomer (b), and an arbitrary chain transfer agent to a polymerization reactor and polymerizing them can be mentioned. When supplying the catalyst solution (a) and the monomer (b) to the polymerization reactor, the catalyst solution (a) and the monomer (b) may be mixed in advance and then supplied to the polymerization reactor, or the catalyst solution (a) and the monomer (b) may be supplied to the polymerization reactor through separate lines and then mixed in the polymerization reactor, but it is preferable to supply the catalyst solution (a) and the monomer (b) to the polymerization reactor through separate lines. In particular, trioxane contained in the monomer (b) is often easily polymerized by a polymerization catalyst, so it is preferable not to supply it through the same line as the catalyst solution (a).
[0038] The amount of the polymerization catalyst contained in the catalyst solution (a) is not particularly limited as long as it is an amount that can polymerize most of the monomer (b) to produce polyacetal. However, the amount of the polymerization catalyst relative to the total mole number of the monomer (b) is preferably 1.0×10 -5 ~1.0×10 -3 In addition, when polyacetal is continuously produced, for example, by using a flow reactor or the like, it is preferable to adjust the molar ratio of the total amount of monomer (b) per unit time to the amount of polymerization catalyst supplied to be within the above range.
[0039] The upper limit of the more preferred range of the amount of the polymerization catalyst contained in the catalyst solution (a) is 2.0×10 -4 mol or less, whereas the lower limit of the more preferred range is 2.0 × 10 -5 mol or more.
[0040] The polymerization reaction temperature may be any temperature higher than the melting point and lower than the boiling point of the monomer (b) used. For example, when trioxane is used as the monomer (b), the temperature is preferably kept in the range of 63 to 135°C, more preferably in the range of 70 to 120°C, and even more preferably in the range of 70 to 100°C. The residence (reaction) time in the polymerization reactor is preferably 0.1 to 30 minutes, more preferably 0.1 to 25 minutes, and even more preferably 0.1 to 20 minutes. It is also preferable to set the residence (reaction) time so as to obtain a desired yield by appropriately sampling the polymer.
[0041] (Other processes) In this embodiment, the polymerization catalyst is used as a catalyst solution (a) containing an organic solvent as described above. Therefore, in this embodiment, it is preferable to further include a mixing step of mixing the polymerization catalyst containing boron trifluoride or an ether complex of boron trifluoride with an organic solvent before the polymerization step.
[0042] In this embodiment, after the polymerization step, the polyacetal obtained in the polymerization step may be subjected to removal of residual monomers and / or removal and deactivation of the catalyst (removal and deactivation step). For the removal and deactivation, a method proposed in the past may be used. Specifically, for example, the polyacetal discharged from the polymerization reactor may be introduced into an aqueous solution containing only water or at least one deactivator such as amines such as ammonia, triethylamine, and tri-n-butylamine, hydroxides of alkali metals or alkaline earth metals, inorganic salts, and organic acid salts for the purpose of efficiently deactivating the catalyst, and the monomers and catalyst remaining in the polyacetal may be removed and deactivated while being continuously stirred for several minutes to several hours at room temperature to 100°C or lower. In addition, from the viewpoint of increasing the efficiency of washing and removing the catalyst, it is also preferable to pulverize the polyacetal to make it fine, particularly when the polyacetal is in the form of a large block.
[0043] The polyacetal obtained by the above-mentioned polymerization process often has a hydroxyl group terminal that is likely to be the starting point of thermal decomposition. In such a case, for example, the hydroxyl group terminal can be reacted with an organic acid anhydride to stabilize it. In addition, in such a case, for example, the polyacetal can be heated before use as a product to decompose easily decomposed components and sites in advance.
[0044] The process of stabilizing the hydroxyl end by reacting the organic acid anhydride with the polyacetal will be described below. The organic acid anhydride is not particularly limited as long as it reacts with the unstable hydroxyl end of the polyacetal. Specific examples include propionic anhydride, benzoic anhydride, acetic anhydride, succinic anhydride, maleic anhydride, glutaric anhydride, and phthalic anhydride. Among these, the organic acid anhydride is preferably propionic anhydride and acetic anhydride, which become gas at or below the melting point of the polyacetal, from the viewpoint of being easily removed by high-temperature drying of the polyacetal after the reaction.
[0045] The reaction between the organic acid anhydride and the hydroxyl end may be in a liquid phase or a gas phase. For example, the polyacetal obtained in the polymerization step may be dispersed or dissolved in an organic solvent inert to the hydroxyl end of the polyacetal and the organic acid anhydride, and then reacted with the organic acid anhydride. Alternatively, for example, the polyacetal obtained in the polymerization step may be contacted with a gasified organic acid anhydride and reacted.
[0046] In the reaction between an organic acid anhydride and a hydroxyl terminal, the reaction temperature, reaction time (which may be contact time), and amount of the organic acid anhydride used can each be determined arbitrarily. The apparatus used in the reaction is not particularly limited, and known reactors and dryers can be used, such as stirring tanks, autoclaves, conical ribbon dryers, rotary dryers, paddle dryers, etc. The apparatus may also be equipped with any device necessary for carrying out the reaction.
[0047] Furthermore, the polyacetal obtained in the above-mentioned polymerization step often has thermally unstable terminal groups. Therefore, for example, after the removal / deactivation step, it is preferable to subject the unstable terminal groups to a stabilization treatment. Specific examples of the stabilization treatment include a treatment for blocking the unstable terminal groups by reacting them with an esterification agent or etherification agent in a liquid or gas phase, or a treatment for decomposing and removing the unstable terminals. These treatments are preferable in terms of suppressing the decomposition of the polyacetal during melt processing.
[0048] When the unstable terminals are decomposed and removed to stabilize the resulting polyacetal, the thermally unstable terminals [-(OCH2) n It is preferable to decompose and remove the --OH group using a decomposition treatment agent. The decomposition treatment agent is not particularly limited, and examples thereof include aliphatic amine compounds such as ammonia, triethylamine, and tributylamine; inorganic weak acid salts of alkali metals or alkaline earth metals such as hydroxides, carbonates, phosphates, silicates, and borates of alkali metals or alkaline earth metals such as sodium, potassium, magnesium, calcium, or barium; and organic acid salts of alkali metals or alkaline earth metals such as formates, acetates, stearates, palmitates, propionates, and oxalates. Among these, the decomposition treatment agent is preferably an aliphatic amine compound, and more preferably triethylamine.
[0049] The method for decomposing and removing the unstable terminals is not particularly limited, and examples thereof include a method of heat treating the polyacetal in a molten state in the presence of a decomposition agent such as triethylamine at a temperature not lower than the melting point of the polyacetal (e.g., not lower than 170° C.) and not higher than 260° C. An example of an apparatus used for the heat treatment is a single-screw or twin-screw extruder equipped with a vent pressure reducing device, and a twin-screw extruder is preferred.
[0050] The polyacetal obtained by the production method of this embodiment can be blended with commonly used known additives such as antioxidants, formic acid scavengers, weather (light) stabilizers, release (lubricant) agents, reinforcing agents, conductive agents, thermoplastic resins, thermoplastic elastomers, pigments, plasticizers, peroxide decomposers, basic assistants, antistatic agents, flame retardants, dyes, and fillers, as desired. Furthermore, the polyacetal obtained by this embodiment can be blended with other polymers within the range that does not impair its physical properties. The blending ratios of these blending agents and polymers can be appropriately selected.
[0051] The polyacetal obtained by the manufacturing method of this embodiment, and the composition containing the above-mentioned compounding agents, can be used for various purposes as molded products or parts through various moldings. Such uses are not particularly limited, but can be used as known polyacetal uses, such as electric and electronic parts and industrial parts such as gears, cams, sliders, levers, arms, clutches, pulleys, rollers, rollers, key stems, key tops, shafts, bearings, guides, etc. In addition, it can be used as automobile parts, and specific examples thereof include fuel-related parts such as gasoline tanks, fuel pump modules, valves, and gasoline tank flanges, door-related parts such as door locks, door handles, window regulators, and speaker grills, seat belt slip rings, seat belt peripheral parts such as press buttons, combination switch parts, and switches.
[0052] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment. The present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0053] The following examples are intended to illustrate the present embodiments without limiting them.
[0054] [Example 1] A catalyst solution was prepared by adding dimethyl carbonate to 0.50 mL (0.56 g) of boron trifluoride diethyl ether complex to make the solution volume 250 mL. The concentration of the boron trifluoride diethyl ether complex was 0.21 mass%.
[0055] A unidirectionally rotating twin-shaft paddle-type continuous polymerization reactor (Kurimoto Iron Works, Ltd., diameter 2B, L / D=14.8) set at 80°C was used as the polymerization reactor. To prevent oxygen contamination, 60 L of nitrogen was flowed per hour from near the feed port of the polymerization reactor. Trioxane (water concentration: 10 ppm) was fed at 3500 g / hr, 1,3-dioxolane at 120 g / hr, and methylal at 0.60 g / hr to this polymerization reactor. The boron trifluoride diethyl ether complex was added at a rate of 2.0 x 10 per mol of trioxane. -5 The catalyst solution was fed so that the amount of trioxane was 1.0 mol. The trioxane and the catalyst solution were fed through separate lines so that they could not come into contact with each other until they reached the paddle section installed in the polymerization reactor.
[0056] Thirty minutes after the start of the catalyst solution feed, the polyacetal discharged from the polymerization reactor was poured into a polyethylene tank containing water. The polymerization was carried out continuously for more than one hour.
[0057] Next, the polyacetal from which the polymerization catalyst had been washed off was filtered using a centrifuge, and then 1 part by mass of an aqueous solution containing triethylamine was added to 100 parts by mass of the polyacetal (polyacetal copolymer), mixed uniformly, and then dried at 120°C for 3 hours to obtain a polyacetal dry powder. The yield of the polyacetal dry powder was calculated to be 87% from the weight of the polyacetal dry powder and the value obtained by multiplying the time it took to collect the polyacetal in a plastic tank containing water by the supply rate of trioxane.
[0058] [Example 2] The same method as in Example 1 was carried out except that diethyl carbonate was used instead of dimethyl carbonate. The concentration of boron trifluoride diethyl ether in the catalyst solution was 0.23 mass%. The yield of polyacetal dry powder was 87%. In addition, the polymerization could be carried out continuously for more than one hour.
[0059] [Comparative Example 1] The same method as in Example 1 was carried out except that cyclohexane was used instead of dimethyl carbonate. Thirty minutes after starting the feed of the catalyst solution, the feed pump for the catalyst solution became clogged and could no longer operate.
[0060] [Comparative Example 2] The same procedure as in Example 1 was carried out except that di-n-butyl ether was used instead of dimethyl carbonate. The yield of the polyacetal dry powder was 82%. The polymerization could be carried out continuously for more than one hour.
[0061] [Comparative Example 3] The same method as in Example 1 was carried out, except that o-xylene was used instead of dimethyl carbonate. The yield of polyacetal dry powder was 78%. The polymerization could be carried out continuously for more than one hour.
[0062] The above results are shown in Table 1.
[0063] [Table 1]
[0064] As can be seen from Table 1, the continuous polymerization time was shorter in Comparative Example 1 than in Examples 1 and 2. In Examples 1 and 2, no precipitate such as tar or scale was observed in the vessel containing the catalyst solution after operation was stopped, whereas in Comparative Example 1, precipitate (tar-like substance) was observed at the bottom of the vessel containing the catalyst solution after operation was stopped. It is presumed that such precipitate caused clogging of the feed pump in Comparative Example 1, making operation impossible.
[0065] In addition, in Comparative Examples 2 and 3, polymerization could be carried out continuously for more than one hour compared to Examples 1 and 2, but the yield of polyacetal dry powder was low. This result is considered to be due to the influence of a decrease in polymerization activity. Therefore, it can be said that it is important to prepare a catalyst solution that does not decrease polymerization activity, as in Examples 1 and 2.
Claims
1. A method for producing polyacetal, the method comprising the steps of: A catalyst solution (a) containing a polymerization catalyst including boron trifluoride or an ether complex of boron trifluoride and an organic solvent; At least one cyclic ether and / or cyclic formal (b) containing trioxane, A polymerization step of supplying the mixture to a polymerization reactor and carrying out polymerization, The organic solvent contains a carbonate ester. A method for producing polyacetal.
2. 2. The method for producing a polyacetal according to claim 1, wherein the normal boiling point of the carbonate ester is 150° C. or lower.
Citation Information
Patent Citations
Termination of polymerization reaction
JP2000290334A
Termination of polymerization reaction
JP2000290336A
Polyacetal resin-based molded product
JP2004250555A
Method for producing polyoxymethylene
JP2008533265A
Manufacturing method of polyacetal copolymer
JP2017082099A