Electrolyte and lithium metal secondary battery
The use of lithium bis(fluorosulfonyl)imide and alkaline earth metal salts in the electrolytic solution of lithium metal secondary batteries addresses the efficiency decline issue, enhancing capacity retention and cycle life.
Patent Information
- Application Number
- JP2023059645
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Lithium metal secondary batteries face a decrease in coulombic efficiency and capacity retention rate due to repeated charging and discharging, leading to low energy efficiency.
An electrolytic solution containing lithium bis(fluorosulfonyl)imide (LiFSI) and an alkaline earth metal salt, such as calcium bis(fluorosulfonyl)imide (Ca(FSI), within specific concentration ranges, along with organic solvents like chain ethers, is used to enhance capacity retention.
The solution significantly improves the capacity retention rate and cycle life of lithium metal secondary batteries by maintaining high coulombic efficiency even after repeated charging and discharging.
Smart Images

Figure 2024146624000001 
Figure 2024146624000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte and a lithium metal secondary battery. [Background technology]
[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency in order to ensure that many people have access to affordable, reliable, sustainable, and advanced energy. As a secondary battery, for example, a lithium metal secondary battery is known that includes a positive electrode having a positive electrode current collector and a positive electrode mixture layer containing a lithium composite oxide, a negative electrode having a negative electrode current collector and a lithium metal layer, and a separator impregnated with an electrolyte.
[0003] As the electrolyte, for example, a non-aqueous electrolyte in which an electrolyte salt is dissolved in a non-aqueous solvent is known. Here, the electrolyte salt includes at least one first lithium salt selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(SO2CF3)2 and LiN(SO2C2F5)2, and at least one second lithium salt selected from lithium salts having an oxalic acid skeleton, lithium salts having a phosphoric acid skeleton and lithium salts having an S=O group. The first lithium salt and the second lithium salt are four or more in total. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 009994 Summary of the Invention [Problem to be solved by the invention]
[0005] In the technology of secondary batteries, the issues are to improve the capacity and cycle life. The capacity of lithium metal secondary batteries is improved because the negative electrode active material is lithium metal. However, the lithium metal secondary batteries have a problem that the coulomb efficiency decreases when they are repeatedly charged and discharged, resulting in a low capacity retention rate.
[0006] In order to solve the above problems, the present application aims to provide an electrolyte solution that can increase the capacity retention rate of a lithium metal secondary battery even after repeated charging and discharging, thereby contributing to improved energy efficiency. [Means for solving the problem]
[0007] The present inventors have found that the above-mentioned problems can be solved by adding a predetermined amount of an alkaline earth metal salt to an electrolyte solution containing an organic solvent and lithium bis(fluorosulfonyl)imide [LiFSI:(LiN(SO2F)2)], and have completed the present invention. Therefore, the present invention provides the following.
[0008] (1) An electrolyte solution comprising an organic solvent, lithium bis(fluorosulfonyl)imide, and an alkaline earth metal salt, the alkaline earth metal salt being one or both of an alkaline earth metal salt of bis(fluorosulfonyl)imide and an alkaline earth metal salt of bis(trifluoromethane)sulfonimide, the content of the alkaline earth metal salt being within the range of 0.1% by mass or more and 1.0% by mass or less.
[0009] The electrolyte (1) contains the alkaline earth metal salt in the above range, and therefore can increase the capacity retention rate of the lithium metal secondary battery even after repeated charging and discharging.
[0010] (2) The electrolyte solution according to (1), wherein the organic solvent is an ether-based solvent. (3) The electrolyte solution according to (2), wherein the ether-based solvent contains a chain ether containing two oxygen atoms per solvent molecule and a hydrofluoroether.
[0011] (3) The electrolyte, which contains a chain ether containing two oxygen atoms per solvent molecule, has a stable coordination structure, which improves durability.
[0012] (4) The electrolyte solution according to (3), wherein the content of the chain ether and the lithium bis(fluorosulfonyl)imide is in the range of 1:2.0 to 2.7 in terms of molar ratio.
[0013] Since the electrolyte solution (4) has a content of the chain ether and the lithium bis(fluorosulfonyl)imide within the above range, it is possible to increase the capacity retention rate of the lithium metal secondary battery even after repeated charging and discharging.
[0014] (5) The electrolyte solution according to any one of (1) to (4), wherein the concentration of the lithium bis(fluorosulfonyl)imide is in the range of 2.0 mol / L to 3.0 mol / L.
[0015] (5) The electrolyte solution has a high concentration of lithium bis(fluorosulfonyl)imide and improves the Coulombic efficiency, making it possible to further increase the capacity retention rate of lithium metal secondary batteries.
[0016] (6) The electrolyte solution according to any one of (1) to (5), further comprising at least one compound selected from the group consisting of an oxalate complex compound, a carbonate compound, a sulfone compound, and a sulfoxide compound, the content of the compound being within the range of 0.1% by mass or more and 1.0% by mass or less.
[0017] The electrolyte (6) further contains the above-mentioned compound within the above-mentioned range, so that it is possible to further increase the capacity retention rate of the lithium metal secondary battery.
[0018] (7) A lithium metal secondary battery comprising the electrolyte solution according to any one of (1) to (6).
[0019] The lithium metal secondary battery (7) has the above-mentioned electrolyte, and therefore has a high capacity retention rate even after repeated charging and discharging, thereby improving the capacity and cycle life of the lithium metal secondary battery (7). Effect of the Invention
[0020] According to the present invention, it is possible to provide an electrolyte solution that can increase the capacity retention rate of a lithium metal secondary battery even after repeated charging and discharging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described.
[0022] [Electrolyte] The electrolyte of the present embodiment includes an organic solvent, lithium bis(fluorosulfonyl)imide [LiFSI:(LiN(SO2F)2)], and an alkaline earth metal salt, which is one or both of an alkaline earth metal salt of bis(fluorosulfonyl)imide and an alkaline earth metal salt of bis(trifluoromethane)sulfonimide.
[0023] The concentration of LiFSI in the electrolyte may be, for example, in the range of 2.0 mol / L to 3.0 mol / L, or in the range of 2.2 mol / L to 2.8 mol / L.
[0024] The alkaline earth metal salt may be a magnesium salt, a calcium salt, a strontium salt, or a barium salt, or may be a magnesium salt or a calcium salt. The alkaline earth metal salt may be, for example, magnesium bis(fluorosulfonyl)imide {Mg(FSI)2:Mg[N(SO2F)2]2}, magnesium bis(trifluoromethane)sulfonimide {Mg(TFSI)2:Mg[N(SO2CF3)2]2}, calcium bis(fluorosulfonyl)imide {Ca(FSI)2:Ca[N(SO2F)2]2}, or calcium bis(trifluoromethane)sulfonimide {Ca(TFSI)2:Ca[N(SO2CF3)2]2}. The alkaline earth metal salt may be used alone or in combination of two or more. The content of the alkaline earth metal salt in the electrolyte is set to be within a range of 0.1% by mass to 1.0% by mass. The content of the alkaline earth metal salt is the content of the alkaline earth metal salt relative to the total amount of the electrolyte (content of the alkaline earth metal salt / total amount of the electrolyte x 100). The content of the alkaline earth metal salt may be in the range of 0.3% by mass to 0.7% by mass.
[0025] The organic solvent is not particularly limited as long as it can dissolve the lithium salt. For example, an ether solvent, a carbonate solvent, an ester solvent, a sulfone, or a nitrile can be used as the organic solvent. The organic solvent may be used alone or in combination of two or more kinds.
[0026] The ether solvent may be a chain ether, a hydrofluoroether, a cyclic ether, an aromatic ether, or a mixture thereof. The chain ether may contain one or two oxygen atoms per molecule. The chain ether containing one oxygen atom may be a dialkyl ether. The chain ether containing two oxygen atoms may be a dialkoxyalkane represented by the following general formula (1). R 1 OL-OR 2 (1) In formula (1), R 1 and R2 each independently represents an alkyl group having 1 to 2 carbon atoms, and L represents an alkylene group having 1 to 3 carbon atoms. A part or all of the hydrogen atoms of the alkyl group may be substituted with fluorine.
[0027] An example of a dialkyl ether is diethyl ether. An example of a dialkoxyalkane is 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, etc. An example of a hydrofluoroether is 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl)ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, etc. An example of a cyclic ether is tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl1,3-dioxolane, etc. An example of an aromatic ether is anisole.
[0028] The ether solvent may be, for example, a mixture of an ether having a boiling point of 80°C or more and an ether having a boiling point of less than 80°C. The ether having a boiling point of less than 80°C may have a boiling point in the range of 50 to 75°C. The ether solvent may be a mixture of a chain ether and a hydrofluoroether, a mixture of a chain ether containing two oxygen atoms per molecule and a hydrofluoroether, or a mixture of 1,2-dimethoxyethane and a hydrofluoroether. The mixing ratio of the dialkoxyalkane and the hydrofluoroether may be in the range of 50:50 to 80:20 in molar ratio. The content of the chain ether containing two oxygen atoms per molecule and LiFSI may be in the range of 1:2.0 to 2.7 in molar ratio.
[0029] The carbonate-based solvent may be a cyclic carbonate, a chain carbonate, or a mixture thereof. Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, vinylene carbonate, and fluoroethylene carbonate. Examples of the chain carbonate include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. The ester-based solvent may be a cyclic ester, a chain carboxylic acid ester, or a mixture thereof. Examples of the cyclic ester include γ-butyrolactone. Examples of the chain carboxylic acid ester include acetate, butyrate, and propionate. Examples of the sulfone include sulfolane and methylsulfolane. Examples of the nitrile include acetonitrile and propionitrile.
[0030] The electrolyte of the present embodiment may contain only the organic solvent, LiFSI, and alkaline earth metal salt. The electrolyte of the present embodiment may further contain an additive. The organic solvent may be a compound in which hydrogen is partially replaced by fluorine, chlorine, bromine, or the like.
[0031] As the additive, an oxalate complex compound, a carbonate compound, a sulfone compound, and a sulfoxide compound can be used. The oxalate complex compound and the carbonate compound have the effect of facilitating the generation of an alkaline earth metal carbonate. The sulfone compound and the sulfoxide compound have the effect of facilitating the formation of an alkaline earth metal sulfate. The formation of an alkaline earth metal carbonate or sulfate inhibits the deposition of alkaline earth metal ions on the negative electrode during charging of the battery, and facilitates the uniform deposition reaction on the lithium of the negative electrode during charging of the battery. The content of these additives is, for example, in the range of 0.1% by mass or more and 1.0% by mass or less. The content of the additive is the content of the additive relative to the total amount of the electrolyte (content of the carbide / total amount of the electrolyte x 100). The content of the additive may be in the range of 50% by mass or more and 200% by mass or less as the content relative to the alkaline earth metal salt (content of the additive in the electrolyte / content of the alkaline earth metal salt x 100).
[0032] An example of the oxalato complex compound is difluoro(oxalato)boric acid. A cyclic carbonate or a chain carbonate can be used as the carbonate compound. An example of the cyclic carbonate is ethylene carbonate, propylene carbonate, vinylene carbonate, fluoroethylene carbonate, etc. An example of the chain carbonate is dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, etc. An example of the sulfone compound is ethyl methyl sulfone. An example of the sulfoxide compound is dimethyl sulfoxide.
[0033] According to the electrolyte solution of the present embodiment having the above-mentioned configuration, since the above-mentioned alkaline earth metal is contained in the above-mentioned range, it is possible to increase the capacity retention rate of the lithium metal secondary battery even after repeated charging and discharging.
[0034] In the electrolytic solution of the present embodiment, when the organic solvent is an ether-based solvent, the reduction resistance is improved, so that the capacity retention rate of the lithium metal secondary battery can be increased even after repeated charging and discharging. When the ether-based solvent contains 1,2-dimethoxyethane and hydrofluoroether, the capacity retention rate of the lithium metal secondary battery can be increased more reliably even after repeated charging and discharging.
[0035] In the electrolyte of the present embodiment, when the concentration of lithium bis(fluorosulfonyl)imide is within the above range, the coulombic efficiency is improved, so that the capacity retention rate of the lithium metal secondary battery can be further increased. Furthermore, when the electrolyte contains compounds such as oxalate complex compounds, carbonate compounds, sulfone compounds, and sulfoxide compounds within the above range, the capacity retention rate of the lithium metal secondary battery can be further increased.
[0036] [Lithium metal secondary battery] In the lithium metal secondary battery of this embodiment, a separator impregnated with an electrolyte is disposed between a positive electrode and a negative electrode. The positive electrode has a positive electrode current collector and a positive electrode mixture layer containing a lithium composite oxide. The negative electrode has a negative electrode current collector and a lithium metal layer.
[0037] That is, in the lithium metal secondary battery of this embodiment, lithium metal is precipitated on the negative electrode when the battery is charged, and lithium ions are eluted from the negative electrode when the battery is discharged. Therefore, in the lithium metal secondary battery of this embodiment, the negative electrode does not need to have a lithium metal layer in the initial state. In this case, before using the lithium metal secondary battery, the lithium metal is precipitated on the negative electrode current collector by charging the lithium metal secondary battery, and a lithium metal layer is formed.
[0038] The positive electrode current collector is not particularly limited, but may be, for example, aluminum foil.
[0039] The positive electrode mixture layer contains a lithium composite oxide, and may further contain other components.
[0040] The lithium composite oxide is not particularly limited, but examples thereof include LiCoO2, Li(Ni 5 / 10 Co 2 / 10 Mn 3 / 10 )O 2、 Li(Ni) 6 / 10 Co 2 / 10 Mn 2 / 10 )O 2、 Li(Ni) 8 / 10 Co 1 / 10 Mn 1 / 10 )O 2、 Li(Ni) 0.8 Co 0.15 Al 0.05 )O 2、 Li(Ni) 1 / 6 Co 4 / 6 Mn 1 / 6 )O 2、 Li(Ni) 1 / 3 Co 1 / 3 Mn 1 / 3 )O 2、Examples of the material include LiCoO4, LiMn2O4, LiNiO2, and LiFePO4, and two or more of them may be used in combination.
[0041] Examples of other components include a positive electrode active material other than the lithium composite oxide, a conductive assistant, a binder, and the like.
[0042] The negative electrode current collector is not particularly limited, but may be, for example, copper foil.
[0043] The material constituting the separator is not particularly limited, but examples thereof include polyolefins such as polyethylene and polypropylene, aramid, polyimide, fluororesin, glass fiber, and cellulose fiber.
[0044] The lithium metal secondary battery of this embodiment can be manufactured by using a known method.
[0045] The lithium metal secondary battery of the present embodiment configured as described above contains the above-mentioned electrolyte, and therefore has a high capacity retention rate even after repeated charging and discharging, thereby improving the capacity and cycle life of the lithium metal secondary battery of the present embodiment. EXAMPLES
[0046] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0047] [Example 1] As an organic solvent, an ether-based solvent was prepared by mixing DME (1,2-dimethoxyethane) and HFE (1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether) in a molar ratio of 65:35. LiFSI [lithium bis(fluorosulfonyl)imide] and Ca(FSI)2 [calcium bis(fluorosulfonyl)imide] were added to this ether-based solvent and stirred to dissolve LiFSI and Ca(FSI)2 to obtain an electrolyte. The concentration of LiFSI in the obtained electrolyte was 2.35 mol / L, and the content of Ca(FSI)2 relative to LiFSI was 0.5 mass%. The composition of the obtained electrolyte is shown in Table 1 below.
[0048] [Examples 2 to 3, Comparative Examples 2 to 4] An electrolyte solution was obtained in the same manner as in Example 1, except that the amount of Ca(FSI)2 added to the ether-based solvent was changed so that the content of Ca(FSI)2 relative to LiFSI was the content shown in Table 1 below.
[0049] [Comparative Example 5] An electrolyte solution was obtained in the same manner as in Example 3, except that Ca(FSI)2 was replaced with Li(FSI)2.
[0050] [Examples 4 to 6] An electrolyte solution was obtained in the same manner as in Example 1, except that Ca(TFSI)2 [calcium bis(trifluoromethane)sulfonimide] (Example 4), Mg(FSI)2 [magnesium bis(fluorosulfonyl)imide] (Example 5), or Mg(TFSI)2 [magnesium bis(trifluorosulfonyl)imide] (Example 6) was used instead of Ca(FSI)2 in the same amount as Ca(FSI)2.
[0051] [Examples 7 to 10] An electrolyte solution was obtained in the same manner as in Example 1, except that FOB [difluoro(oxalato)boric acid] (Example 7), FEC (fluoroethylene carbonate) (Example 8), VC (vinylene carbonate) (Example 9), and DMC (dimethyl carbonate) (Example 10) were added to the ether solvent together with LiFSI and Ca(FSI)2 in amounts such that the content of each relative to LiFSI was 0.5 mass%.
[0052] [Comparative Example 1] An electrolyte solution was obtained in the same manner as in Example 1, except that Ca(FSI)2 was not added.
[0053] [Table 1]
[0054] [Preparation of lithium metal secondary battery] Lithium-nickel-cobalt-manganese composite oxide (Li(Ni 8 / 10 Co 1 / 10 Mn 1 / 10 )O2) was mixed with acetylene black as a conductive additive and polyvinylidene fluoride as a binder to obtain a coating solution for a positive electrode mixture layer.
[0055] As a positive electrode current collector, the area is 12 cm 2 The coating solution for the positive electrode composite layer was applied to an Al foil having a thickness of 15 μm, dried, and then the coating solution was applied to a thickness of 20 mg / cm 2 After forming the positive electrode mixture layer, the layer was rolled to obtain a positive electrode.
[0056] The negative electrode current collector and separator each had an area of 12 cm 2 , an 8 μm thick Cu foil and a 20 μm thick porous polyolefin film were used.
[0057] The positive electrode (positive electrode mixture layer, positive electrode current collector), separator and negative electrode current collector were laminated in this order, the separator was impregnated with an electrolyte solution, and then the resultant was sealed with a laminate film to obtain a lithium metal secondary battery.
[0058] [Charge and discharge test of lithium metal secondary battery] The discharge capacity per unit area of lithium metal is 3mAh / cm 2 The charge / discharge test was carried out under the following conditions. The lithium metal secondary battery was assembled in a jig, restrained at a restraining pressure of 0.05 MPa, and then left at the measurement temperature (25°C) for 1 hour. Next, a constant current charge was carried out at 0.2 C. The termination condition for the constant current charge was when the specified capacity (3 mAh / cm 2 ) or 5 hours have elapsed since the start of constant current charging, or the voltage has reached 3.3V. At this time, a negative electrode was used in which a 20 μm thick lithium foil was attached to one side of an 8 μm Cu foil. Next, the battery was charged at 0.1 C, and CCCV charging was performed at 4.3 V until it reached 0.05 C, and then constant current discharging was performed at 0.33 C until it reached 2.65 V. Then, the battery was charged at 0.33 C, and CCCV charging was started at 4.3 V for 10 minutes, after which it was paused for 5 minutes. Constant current discharging was performed up to 2.65 V, and then it was paused for 5 minutes. After this, CCCV charging was performed at 0.33 to 3.86 V to adjust to about SOC 50%. A constant current discharge of 4.5 C was performed from 3.86 V for 10 seconds, the voltage value after 10 seconds was measured, and the direct current resistance (DCR) was calculated from the slope of the current value and the voltage value after 10 seconds. After that, constant current charging at 0.33 C and CV charging at 4.3 V were performed, followed by a 5-minute pause. Then, constant current discharging at 0.33 C was performed up to 2.65 V. After this, a 5-minute pause was performed. This was repeated 100 times.
[0059] In addition, the current value at which the lithium metal battery can be completely discharged in one hour was defined as 1C, relative to the discharge capacity of the battery.
[0060] formula Capacity retention rate (%) = (Capacity at 50th cycle) / (Capacity at 1st cycle) x 100 The capacity retention rate was calculated based on the above. Next, the formula Specific resistance (Ω cm 2 ) = Cell resistance ÷ Positive electrode area The resistivity was calculated by the above.
[0061] The evaluation results of resistivity and capacity retention are shown in Table 2. The capacity retention is shown as the initial value (1st cycle), the 10th cycle, the 50th cycle, and the 100th cycle.
[0062] [Table 2]
[0063] From Table 2, it can be seen that when the electrolyte solutions of Examples 1 to 10 containing the predetermined alkaline earth metal salts in the predetermined ranges according to the present invention are used, the initial resistivity of the lithium metal secondary battery is 20 to 25 Ω cm 2 It can be seen that the capacity retention rate is high and the cycle life is long. In particular, it can be seen that the capacity retention rate of the lithium metal secondary battery is higher when the electrolyte solutions of Examples 7 to 10 containing the specified additive compound together with the specified alkaline earth metal salt are used. In contrast, the electrolyte solution of Comparative Example 1 does not contain an alkaline earth metal salt, and the electrolyte solutions of Comparative Examples 2 to 4 have alkaline earth metal salt contents outside the range of the present invention, so that the lithium metal secondary batteries using these electrolyte solutions have low capacity retention rates.
Claims
1. comprising an organic solvent, lithium bis(fluorosulfonyl)imide, and an alkaline earth metal salt; the alkaline earth metal salt is one or both of an alkaline earth metal salt of bis(fluorosulfonyl)imide and an alkaline earth metal salt of bis(trifluoromethane)sulfonimide; The electrolyte solution has an alkaline earth metal salt content in the range of 0.1% by mass or more and 1.0% by mass or less.
2. The electrolyte according to claim 1 , wherein the organic solvent is an ether solvent.
3. The electrolyte solution according to claim 2 , wherein the ether-based solvent comprises a chain ether containing two oxygen atoms per solvent molecule and a hydrofluoroether.
4. 4. The electrolyte solution according to claim 3, wherein the molar ratio of the chain ether to the lithium bis(fluorosulfonyl)imide is in the range of 1:2.0 to 1:2.
7.
5. The electrolyte solution according to claim 1, wherein the concentration of the lithium bis(fluorosulfonyl)imide is in the range of 2.0 mol / L to 3.0 mol / L.
6. Further, the composition contains at least one compound selected from the group consisting of an oxalate complex compound, a carbonate compound, a sulfone compound, and a sulfoxide compound, The electrolyte solution according to claim 1 , wherein the content of the compound is in the range of 0.1% by mass to 1.0% by mass.
7. A lithium metal secondary battery comprising the electrolyte solution according to any one of claims 1 to 5.
Citation Information
Patent Citations
Micropocket of index table and micropocket processing method of index table using laser
KR102412081B1
battery
WO2017047019A1
Secondary battery
WO2020195092A1
Non-aqueous electrolyte solution and electricity storage device in which same is used
WO2016009994A1
Cited By
Decorative member
US12290158B2
Lithium secondary battery
WO2026177165A1
Non-aqueous electrolyte secondary battery
WO2026181656A1
Lithium-ion secondary battery electrolyte solution and lithium-ion secondary battery
WO2026203200A1