Nonaqueous electrolyte secondary battery separator, nonaqueous electrolyte secondary battery component, and nonaqueous electrolyte secondary battery

A polyolefin porous film separator with controlled void inclination angles addresses the issue of ion permeability loss in high-capacity batteries by maintaining effective ion flow despite compression from electrode expansion.

JP2024146678AInactive Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023104431
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High-capacity non-aqueous electrolyte secondary batteries, such as those with silicon electrodes, face issues with decreased ion permeability due to the expansion of the negative electrode during charging and discharging, leading to increased internal pressure that compresses the separator and closes its voids.

Method used

A separator for non-aqueous electrolyte secondary batteries is designed with a polyolefin porous film where the inclination angle of voids in the cross-section is maintained within a specific range, ensuring good ion permeability even after compression.

Benefits of technology

The separator effectively maintains ion permeability under pressure, preventing decreases in ion flow and internal short circuits, suitable for high-capacity batteries with expanding electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146678000005
    Figure 2024146678000005
  • Figure 2024146678000006
    Figure 2024146678000006
  • Figure 2024146678000001
    Figure 2024146678000001
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery separator capable of satisfactorily maintaining ion permeability even after being compressed.SOLUTION: The nonaqueous electrolyte secondary battery separator includes a polyolefin porous film in which an average of inclination angles of major axes of voids extracted from a two-dimensional image of a cross section of the film is 7.0 or more, the inclination angles being calculated from respective circumscribed rectangles of the voids, the two-dimensional image being obtained by use of the SEM, the cross section being formed by cutting the film in a direction perpendicular to a surface by a straight line that passes a center of the surface and is parallel to an MD or TD direction.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for a nonaqueous electrolyte secondary battery, a member for a nonaqueous electrolyte secondary battery, and a nonaqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries, such as lithium secondary batteries, are currently widely used as batteries for devices such as personal computers, mobile phones and personal digital assistants, or as on-board batteries for vehicles.

[0003] A porous film mainly composed of polyolefin is mainly used as a separator in such a nonaqueous electrolyte secondary battery. An example of the porous film mainly composed of polyolefin is a porous film produced by a method including a step of stretching a resin composition containing a polyolefin resin, as described in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-130900 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, development of high-capacity batteries has been promoted for use in applications such as electric vehicles (EVs) with longer driving distances. As the high-capacity batteries, for example, nonaqueous electrolyte secondary batteries having a silicon electrode as the negative electrode have been developed. However, it is known that the negative electrode in high-capacity batteries such as the silicon electrode expands during charging and discharging, and its volume changes, for example, to about four times that of conventional negative electrodes. As a result, the internal pressure inside the battery (cell) increases in the high-capacity batteries. In the high-capacity batteries, the separator is compressed during charging and discharging due to the increased internal pressure, and the voids (pores) inside the separator are blocked, resulting in a decrease in permeability of ions, which are charge carriers.

[0006] In order to solve the above problems, an object of one aspect of the present invention is to provide a separator for a non-aqueous electrolyte secondary battery that can maintain good ion permeability even after being compressed. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors discovered that a separator for a non-aqueous electrolyte secondary battery, comprising a polyolefin porous film in which the inclination of the voids in the cross section is within a specific range, can maintain good ion permeability even after being compressed, and thus arrived at the present invention.

[0008] One aspect of the present invention is a separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, wherein a two-dimensional image of a cross section of the polyolefin porous film is obtained using a scanning electron microscope, and the average inclination angle of the long axis calculated from the circumscribing rectangle of the void extracted from the two-dimensional image is 7.0° or more, and the cross section is formed by cutting the polyolefin porous film in a direction perpendicular to the surface by a straight line that passes through the center of the surface and is parallel to the MD or TD direction. Effect of the Invention

[0009] The separator for a non-aqueous electrolyte secondary battery according to one aspect of the present invention exhibits an effect of being able to maintain good ion permeability even after being compressed. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram showing a void portion inside a polyolefin porous film constituting a separator for a nonaqueous electrolyte secondary battery according to one embodiment of the present invention, and a circumscribed rectangle of the void portion. [Diagram 2] FIG. 1 is a schematic diagram showing the state of voids 3 inside a polyolefin porous film 1 having a low crystal orientation in the MD or TD direction of the polyolefin resin, and a schematic diagram showing the state of voids 3 inside a polyolefin porous film 2 having a high crystal orientation in the MD or TD direction of the polyolefin resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each of the configurations described below, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in different embodiments. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more, B or less."

[0012] In this specification, MD (machine direction) means the direction in which the sheet-shaped polyolefin resin composition and the porous film are conveyed in the manufacturing method of the porous film described later, and TD (transverse direction) means the direction parallel to the surface of the sheet-shaped polyolefin resin composition and the porous film, and perpendicular to the MD.

[0013] In addition, when the manufacturing method, i.e., the direction in which the raw material sheet-shaped polyolefin resin composition and porous film are transported, is unknown, the MD direction of the separator for nonaqueous electrolyte secondary batteries and the porous film constituting the separator for nonaqueous electrolyte secondary batteries means the longitudinal direction of the film (cylindrical type: winding direction, zigzag type: folding direction). In addition, the TD direction of the separator for nonaqueous electrolyte secondary batteries and the porous film means the direction parallel to the surface of the separator for nonaqueous electrolyte secondary batteries and the porous film and perpendicular to the MD direction.

[0014] [Embodiment 1: Separator for non-aqueous electrolyte secondary battery] The separator for a non-aqueous electrolyte secondary battery according to embodiment 1 of the present invention is a separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, wherein a two-dimensional image of a cross section of the polyolefin porous film is obtained using a scanning electron microscope, and the average inclination angle of the major axis calculated from the circumscribing rectangle of the void extracted from the two-dimensional image is 7.0° or more, and the cross section is formed by cutting the polyolefin porous film in a direction perpendicular to the surface by a straight line passing through the center of the surface and parallel to the MD or TD direction.

[0015] The separator for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention includes a polyolefin porous film. Hereinafter, the polyolefin porous film is also simply referred to as a "porous film." Hereinafter, the separator for a non-aqueous electrolyte secondary battery is also simply referred to as a "separator."

[0016] The separator according to one embodiment of the present invention may be a separator made of the porous film. The separator according to one embodiment of the present invention may be a laminate including the porous film and an insulating porous layer described later. Hereinafter, a separator that is a laminate including the porous film and an insulating porous layer described later is also referred to as a "laminated separator". Furthermore, the separator according to one embodiment of the present invention may include a known porous layer such as a heat-resistant layer, an adhesive layer, or a protective layer described later as a porous layer other than the insulating porous layer, as necessary.

[0017] In one embodiment of the present invention, the average value of the inclination angle is calculated as follows. First, a porous film is cut in a direction perpendicular to the surface by a straight line passing through the center of the surface of the porous film and parallel to the MD or TD direction to form a cross section. A two-dimensional image of the formed cross section is obtained using a scanning electron microscope (SEM), and a circumscribing rectangle of the voids extracted from the two-dimensional image is created. The inclination angle of the long axis calculated from the circumscribing rectangle is averaged for all voids included in the two-dimensional image to obtain the average inclination angle. Hereinafter, the inclination angle of the long axis is also simply referred to as the "inclination angle". The circumscribing rectangle is a rectangle that is in contact with the voids on the inside.

[0018] Specifically, the average value of the tilt angle is calculated, for example, by a method including the following steps (1) to (12). (1) A porous film is cut along a straight line that passes through the center of the surface of the porous film and is parallel to the MD or TD direction, in a direction perpendicular to the surface, to form a cross section. (2) A deposition film for SEM observation is formed on the cross section formed in step (1). (3) The cross section on which the deposition film was formed in step (2) is observed using an SEM with an accelerating voltage of 0.8 kV and a working distance of 3.0 mm to obtain a backscattered electron image of the cross section (film thickness direction: 960 pixels × MD or TD direction: 1280 pixels). (4) From the SEM image of the cross section obtained in step (3), an analysis area of ​​100 pixels in the film thickness direction × 1280 pixels in the MD or TD direction is extracted. At this time, the analysis area is extracted so that the entire cross-sectional area of ​​the porous film is included in the analysis area. In addition, in the analysis area, the x coordinate (x axis) is taken in the MD or TD direction, and the y coordinate (y axis) is taken in the film thickness direction. (5) Normalization of brightness values ​​is performed on the analysis area. (6) The analysis region obtained in step (5) and subjected to the normalization process of the brightness values ​​is subjected to an inversion process of the brightness values ​​in order to accurately identify voids when performing the binarization process described below. (7) The analysis region obtained in step (6) and subjected to the inversion process of the luminance value is binarized. (8) Blob processing is performed on the binarized analysis region obtained in step (7) to identify and extract voids. Specifically, the area of ​​the blobs constituting each void identified by the blob processing is calculated using the number of pixels, and blobs having an area of ​​10 pixels or more are extracted as voids. In the subsequent processing, the extracted voids are treated as voids, and voids consisting of blobs with an area of ​​less than 10 pixels are not treated as voids. (9) For each void portion extracted in step (8), a circumscribing rectangle is created as shown in Fig. 1. Here, Fig. 1 is a schematic diagram showing a void portion inside a porous film constituting a separator according to one embodiment of the present invention and a circumscribing rectangle for the void portion. In Fig. 1, the void portion is described as "void." The circumscribing rectangle is a rectangle that contacts the void portion on its inside. (10) For each of the circumscribing rectangles created from each void in step (9), the point with the smallest x-coordinate among the four vertices is designated as P1, and counterclockwise therefrom, P2, P3, and P4 are designated as P2, P3, and P4. Next, for each of the circumscribing rectangles, the straight line connecting P1 and P2 is designated as L12, the straight line connecting P1 and P4 is designated as L14, and the longer straight line of L12 and L14 is designated as the major axis. (11) For each of the circumscribing rectangles, the angle between the long axis and the x-axis is calculated, and the calculated value is set as the inclination angle θ of each gap, with 0°<θ<90°. (12) Calculate the average value of the inclination angles θ of each void calculated in step (11) for all voids. The calculated average value is set as the average value of the inclination angles.

[0019] In the step (1), a laminate separator having other layers such as an insulating porous layer in addition to the porous film may be used instead of the porous film. In that case, as shown in step (4), the analysis region is extracted so that the entire cross-sectional region of the porous film, which is the base material of the laminate separator, is included in the analysis region. In other words, the cross-sectional region of the other layer does not have to be included in the analysis region.

[0020] In the step (1), the method for cutting the porous film is not particularly limited, and a known method can be adopted. For example, an ion milling method can be adopted as the cutting method. In addition, in the step (1), the same cutting method as that for cutting the porous film can be adopted when cutting the laminated separator.

[0021] In the step (2), the vapor-deposited film may be a typical vapor-deposited film that can be used for observing a backscattered electron image using a SEM. For example, a vapor-deposited film made of osmium or the like may be used. A known method may be used to form the vapor-deposited film.

[0022] The magnification of the SEM used to obtain the SEM image in the step (3) is not particularly limited as long as the voids can be discerned. The magnification of the SEM may be, for example, 3000 to 7000 times.

[0023] The process from step (4) onwards corresponds to an image analysis process of the cross-sectional SEM image obtained in step (3). The image analysis process can be carried out, for example, by loading data of the cross-sectional SEM image in a JPEG file format into a computer using Python. The image analysis process can also be carried out using a commercially available program capable of carrying out the processes of steps (4) to (12).

[0024] In a non-aqueous electrolyte secondary battery, pressure is applied vertically from above to the surface of the separator and the porous film constituting the separator due to the expansion of an electrode (e.g., a negative electrode). FIG. 2 is a schematic diagram showing the state of voids 3 inside a polyolefin porous film 1 in which the crystalline orientation of the polyolefin resin in the MD or TD direction is small, and a schematic diagram showing the state of voids 3 inside a polyolefin porous film 2 in which the crystalline orientation of the polyolefin resin in the MD or TD direction is large. As shown in FIG. 2, the voids 3 inside the polyolefin porous film 1 in which the crystalline orientation in the MD or TD direction is small tend to be in a state in which each void is separated. On the other hand, the voids 3 inside the polyolefin porous film 2 in which the crystalline orientation in the MD or TD direction is large tend to be in a state in which multiple voids are overlapped and connected. Here, the multiple overlapping and connected voids are treated as one large void with a large inclination angle during the above-mentioned image analysis. Therefore, when the porous film has a configuration in which a plurality of the voids overlap and are connected in the MD or TD direction, the average value of the inclination angle becomes high.

[0025] From the above, in the separator according to one embodiment of the present invention, the average value of the inclination angle is as large as 7.0° or more, which reflects the occurrence of voids in the MD direction or TD direction that are overlapped and connected in the porous film. Therefore, in one embodiment of the present invention, the porous film has many voids in the form of one large void as described above. The pressure required to close multiple voids that function as large voids is larger, and they are less likely to be closed when pressure is applied. Therefore, the separator according to one embodiment of the present invention has the effect of maintaining good ion permeability even when compressed by including the porous film.

[0026] From the viewpoint of maintaining good ion permeability when compressed, the average value of the inclination angle is preferably 8.0° or more, and more preferably 8.7° or more. The average value of the inclination angle is preferably 20° or less, and more preferably 15° or less. When the average value of the inclination angle is 20° or less, short circuits can be effectively prevented. The standard deviation of the inclination angle θ in all voids is preferably 13.0 to 18.0, and more preferably 14.0 to 17.0.

[0027] In one embodiment of the present invention, both the average value of the inclination angle in the MD direction and the average value of the inclination angle in the TD direction are preferably 7.0° or more, and more preferably within the above-mentioned preferred range. In that case, there are more voids in the porous film that are treated as one large void as described above, and the separator according to one embodiment of the present invention can maintain ion permeability better when compressed. The "average value of the inclination angle in the MD direction" means the average value of the inclination angle calculated from a two-dimensional image of a cross section formed by cutting the polyolefin porous film in a direction perpendicular to the surface with a straight line passing through the center of the surface and parallel to the MD direction. The "average value of the inclination angle in the TD direction" means the average value of the inclination angle calculated from a two-dimensional image of a cross section formed by cutting the polyolefin porous film in a direction perpendicular to the surface with a straight line passing through the center of the surface and parallel to the TD direction. In the following, the term "average value of the inclination angle" simply means the average value of the inclination angle in the MD direction or the average value of the inclination angle in the TD direction.

[0028] The average area of ​​the voids extracted in the step (8) in the entire porous film (unit: μm 2 ) is 0.012 μm from the viewpoint that the ion permeability of the compressed porous film can be more suitably maintained. 2 ~0.03μm 2 It is preferable that the thickness is 0.015 μm. 2 ~0.025μm 2 The standard deviation of the area in all voids is preferably 0.018 to 0.030, and more preferably 0.019 to 0.029.

[0029] The average Feret diameter (unit: μm) of the voids in the entire porous film is preferably 0.18 μm to 0.28 μm, and more preferably 0.2 μm to 0.25 μm, from the viewpoint of more suitably maintaining the ion permeability of the compressed porous film. The standard deviation of the Feret diameter in all voids is preferably 0.120 to 0.200, and more preferably 0.140 to 0.190.

[0030] From the viewpoint of more suitably maintaining the ion permeability of the compressed porous film, the average value (unit: μm) of the circle equivalent diameter of the voids in the entire porous film is preferably 0.12 μm to 0.18 μm, more preferably 0.11 μm to 0.16 μm. The standard deviation of the circle equivalent diameter in all voids is preferably 0.060 to 0.080, more preferably 0.062 to 0.078.

[0031] The average circularity of the voids in the entire porous film (no unit) is preferably 0.2 or more, and more preferably 0.3 or more, from the viewpoint of more suitably maintaining the ion permeability of the compressed porous film. The average circularity of the voids is preferably 0.4 or less, and more preferably 0.37 or less. The closer the circularity is to 1, the closer the shape of the voids is to a circle. The standard deviation of the circularity in all voids is preferably 0.0171 to 0.0190, and more preferably 0.0172 to 0.0189.

[0032] The average value of the long / short ratio (L / S) of the long side length L (μm) to the short side length S (μm) calculated from the circumscribed rectangle of the voids in the entire porous film is preferably 5.0 or less, and more preferably 4.5 or less, from the viewpoint of more suitably maintaining the ion permeability of the compressed porous film. Moreover, the average value of the long / short ratio is 1.0 or more, preferably 2.0 or more, and preferably 3.5 or more. The standard deviation of the long / short ratio in all voids is preferably 1.9 to 2.8, and more preferably 2.0 to 2.7.

[0033] The average value and standard deviation of the area, Feret's diameter, circle equivalent diameter, circularity and length ratio of the void portion can be measured and calculated, for example, by the method described in the Examples below.

[0034] The porous film contains polyolefin resin, and generally is a porous film mainly composed of polyolefin resin. "Mainly composed of polyolefin resin" means that the ratio of polyolefin resin in the porous film is 50% by volume or more, preferably 90% by volume or more, more preferably 95% by volume or more of the total material constituting the porous film.

[0035] The porous film has a large number of interconnected pores inside, allowing gas or liquid to pass from one side to the other. The pores are synonymous with the voids.

[0036] The thickness of the porous film is 4 to 40 μm, and preferably 5 to 20 μm. If the thickness of the porous film is 4 μm or more, internal short circuit of the battery can be sufficiently prevented. On the other hand, if the thickness of the porous film is 40 μm or less, the nonaqueous electrolyte secondary battery can be prevented from becoming large.

[0037] The polyolefin resin has a weight average molecular weight of 5×10 5 ~15×10 6It is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more. In particular, it is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more, since the strength of the obtained porous film and the separator containing the porous film is improved.

[0038] The polyolefin resin is not particularly limited, but examples thereof include thermoplastic resins such as homopolymers or copolymers obtained by polymerizing monomers such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, and 1-hexene. Examples of the homopolymers include polyethylene, polypropylene, and polybutene. Examples of the copolymers include ethylene-propylene copolymers.

[0039] Among these, polyethylene is more preferred because it can prevent excessive current from flowing through the separator at a lower temperature. The prevention of excessive current from flowing is also called shutdown. Examples of the polyethylene include low-density polyethylene, high-density polyethylene, linear polyethylene (ethylene-α-olefin copolymer), and ultra-high molecular weight polyethylene having a weight-average molecular weight of 1 million or more. Among these, ultra-high molecular weight polyethylene having a weight-average molecular weight of 1 million or more is more preferred.

[0040] The polyolefin resin preferably has a number-average branch number of 0.5 or less, more preferably 0.2 or less. When the number-average branch number of the polyolefin resin is within the above-mentioned range, the crystalline orientation of the polyolefin resin in the MD and TD directions in the porous film is suitably improved. Here, as described later, when the crystalline orientation in the MD and TD directions is suitably improved, the voids in the porous film tend to be in a state in which multiple voids overlap and are connected, and as a result, the average value of the inclination angle is suitably improved. Therefore, by having the number-average branch number of the polyolefin resin within the above-mentioned range, the average value of the inclination angle can be suitably improved and controlled to the above-mentioned suitable range.

[0041] In this specification, the number-average branch number can be calculated, for example, from a conformation plot using GPC-MALS. Specifically, the number-average branch number of the polyolefin resin can be measured and calculated by the method described in the Examples below.

[0042] The weight per unit area of ​​the porous film, i.e., the weight per unit area, is usually 4 to 20 g / m2 so as to increase the weight energy density and volume energy density of the battery. 2 is preferably 5 to 12 g / m 2 It is more preferable that:

[0043] From the viewpoint of exhibiting sufficient ion permeability, the air permeability of the porous film is preferably 110 to 200 sec / 100 mL, and more preferably 110 to 190 sec / 100 mL, in terms of Gurley value.

[0044] The porosity of the porous film is preferably 20% by volume to 80% by volume, and more preferably 30% by volume to increase the amount of electrolyte retained and to provide the function of reliably preventing (shutting down) the flow of excessive current at a lower temperature.

[0045] Furthermore, from the viewpoint that the porous film and the separator containing the porous film have better ion permeability after compression, the porosity of the porous film is more preferably 35 volume % or more, and particularly preferably 50 volume % or more.

[0046] The pore size of the pores in the porous film is preferably 0.3 μm or less, and more preferably 0.14 μm or less, from the viewpoints of sufficient ion permeability and preventing the intrusion of particles constituting the electrode.

[0047] <Method of manufacturing porous film> The method for producing the porous film in one embodiment of the present invention is not particularly limited, but specifically includes, for example, a method including the following steps (A) to (C).

[0048] (A) a step of adding a polyolefin resin and, optionally, a pore-forming agent to a kneader and melt-kneading the mixture to obtain a polyolefin resin composition; (B) A step of stretching the obtained polyolefin resin composition in the MD direction while cooling it, and forming it into a sheet to obtain a primary sheet; (C) A step of stretching the primary sheet in the TD direction.

[0049] In step (A), the amount of the polyolefin resin used is preferably 6 wt % to 45 wt %, and more preferably 9 wt % to 36 wt %, based on 100 wt % of the weight of the resulting polyolefin resin composition.

[0050] The pore-forming agent is not particularly limited, but examples thereof include inorganic fillers and plasticizers. The inorganic fillers are not particularly limited, but examples thereof include inorganic fillers, specifically calcium carbonate, etc. The plasticizers are not particularly limited, but examples thereof include low molecular weight hydrocarbons such as liquid paraffin.

[0051] In addition to the pore-forming agent, the additives may include any known additives within the scope of the present invention, provided that the effects of the present invention are not impaired. Examples of the known additives include antioxidants, fillers, and dispersion aids. Examples of the fillers include alumina.

[0052] In the step (B), the method for obtaining the primary sheet is not particularly limited, and the primary sheet can be produced by a sheet forming method such as inflation processing, calendar processing, T-die extrusion processing, or skiff method.

[0053] For example, the sheet molding temperature in the sheet molding method, such as the T-die extrusion temperature in the T-die extrusion process, is preferably 200°C or higher and 280°C or lower, and more preferably 220°C or higher and 260°C or lower.

[0054] The stretching temperature in step (B) is preferably 120°C or higher and 160°C or lower, and more preferably 130°C or higher and 155°C or lower.

[0055] In the step (B), the polyolefin resin composition can be cooled by contacting it with a coolant such as cold air or cooling water, or by contacting it with a cooling roll, etc. The method of contacting it with a cooling roll is preferred.

[0056] When the polyolefin resin composition and the primary sheet contain a pore-forming agent, the method includes a step of washing the stretched sheet with a washing liquid to remove the pore-forming agent between steps (B) and (C) or after step (C).

[0057] The cleaning liquid is not particularly limited as long as it is a solvent capable of removing the pore-forming agent, and examples of the cleaning liquid include an aqueous hydrochloric acid solution, heptane, and dichloromethane.

[0058] The stretching temperature during stretching in the TD direction in step (C) is preferably 80°C or higher and 120°C or lower, and more preferably 80°C or higher and 115°C or lower.

[0059] The primary sheet stretched in the TD direction in step (C) may be heat-set at a specific temperature to obtain a porous film. The heat setting is preferably performed at a temperature of 110° C. or more and 130° C. or less, more preferably 115° C. or more and 128° C. or less. The heat setting is preferably performed for a period of 15 seconds or more and less than 20 minutes, more preferably 1 minute or more and 15 minutes or less.

[0060] In the method for producing a porous film, the average value of the inclination angle in the produced porous film can be controlled to a suitable range of 7.0 or more by appropriately adjusting the reaction conditions. One example of a method for controlling the average value of the inclination angle to a suitable range of 7.0 or more is a method for suitably improving the crystal orientation in the MD or TD direction of the polyolefin resin in the produced porous film. Here, as described above, when the crystal orientation in the MD or TD direction of the polyolefin resin in the porous film is high, voids tend to be generated in a form in which multiple overlaps and are connected. The multiple overlaps and are connected are treated as one large void with a large inclination angle. Therefore, by improving the crystal orientation in the MD or TD direction, the average value of the inclination angle can be controlled to a suitable range of 7.0 or more.

[0061] A specific method for suitably improving the crystal orientation in the MD direction of the polyolefin resin includes a method of controlling the stretching ratio in the MD direction in a specific range in step (B). From the viewpoint of suitably improving the crystal orientation in the MD direction, the stretching ratio in the MD direction is preferably high, specifically, preferably 1.55 times or more, more preferably 1.8 times or more. From the viewpoint of film formation stability, the stretching ratio in the MD direction is preferably 2.5 times or less, more preferably 2.2 times or less. By setting the stretching ratio in the MD direction within the above-mentioned range, particularly 1.55 times or more, the crystal orientation in the MD direction of the polyolefin resin can be suitably improved. As a result, the average value of the inclination angle in the MD direction of the produced porous film can be controlled to a suitable range of 7.0 or more.

[0062] A specific method for suitably improving the crystal orientation in the TD direction of the polyolefin resin includes a method of controlling the stretching ratio in the TD direction in a specific range in step (C). From the viewpoint of suitably improving the crystal orientation in the TD direction, the stretching ratio in the TD direction is preferably high, specifically, preferably 5 times or more, more preferably 7 times or more. From the viewpoint of film formation stability, the stretching ratio in the TD direction is preferably 12 times or less, more preferably 10 times or less. By setting the stretching ratio in the TD direction within the above-mentioned range, particularly 5 times or more, the crystal orientation in the TD direction of the polyolefin resin can be suitably improved. As a result, the average value of the inclination angle in the TD direction of the produced porous film can be controlled to a suitable range of 7.0 or more.

[0063] Therefore, by adjusting either the stretching ratio in the MD direction or the stretching ratio in the TD direction within the above-mentioned preferred range, the average value of the tilt angle can be improved and suitably controlled within the above-mentioned range. Also, by adjusting both the stretching ratio in the MD direction and the stretching ratio in the TD direction within the above-mentioned preferred range, both the average value of the tilt angle in the MD direction and the average value of the tilt angle in the TD direction can be improved and suitably controlled within the above-mentioned range.

[0064] In addition, by controlling the stretch ratio in the MD direction to within the above range, particularly 1.55 times or more, and / or controlling the stretch ratio in the TD direction to within the above range, particularly 5 times or more, and using a polyolefin resin that can achieve high crystal orientation as the raw material polyolefin resin, the average value of the inclination angle in the manufactured porous film can be more suitably improved and controlled to a more suitable range. Examples of polyolefin resins that can achieve high crystal orientation include polyolefin resins with few branches, specifically polyolefin resins with a number average branch number of 0.5 or less. In particular, when the stretch ratio in the MD direction is a small ratio close to 1.55 times within the above range, it is preferable to use a polyolefin resin with a number average branch number of 0.2 or less from the viewpoint of preventing insufficient improvement of the average value of the inclination angle in the MD direction only by controlling the stretch ratio in the MD direction. Similarly, when the stretch ratio in the TD direction is a small ratio close to 5 times within the above-mentioned range, it is preferable to use a polyolefin-based resin having a number-average branch number of 0.2 or less, from the viewpoint of preventing an insufficient improvement in the average tilt angle in the TD direction only by controlling the stretch ratio in the TD direction.

[0065] <Insulating porous layer> When the separator according to one embodiment of the present invention is a laminated separator, it preferably includes the porous film and an insulating porous layer laminated on the porous film.

[0066] The insulating porous layer is usually a resin layer containing a resin, and is preferably a heat-resistant layer or an adhesive layer. The resin constituting the insulating porous layer is preferably insoluble in the electrolyte of the battery and is electrochemically stable within the range of use of the battery. In the following, the insulating porous layer is also simply referred to as a "porous layer."

[0067] The porous layer is laminated on one or both sides of the porous film as necessary. When the porous layer is laminated on one side of the porous film, the porous layer is preferably laminated on the surface of the porous film facing the positive electrode when the porous film is used as a nonaqueous electrolyte secondary battery, and more preferably on the surface in contact with the positive electrode.

[0068] It is preferable that the resin is insoluble in the electrolyte of the battery and is electrochemically stable within the range of use of the battery.

[0069] Specific examples of the resin include polyolefins; (meth)acrylate resins; fluorine-containing resins; polyamide resins; polyimide resins; polyester resins; rubbers; resins having a melting point or glass transition temperature of 180°C or higher; water-soluble polymers; polycarbonate, polyacetal, polyether ether ketone, and the like.

[0070] Of the above-mentioned resins, polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins and water-soluble polymers are preferred.

[0071] As the polyolefin, polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, and the like are preferable.

[0072] Examples of fluorine-containing resins include polyvinylidene fluoride (PVDF), polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, and the like, as well as fluorine-containing rubbers having a glass transition temperature of 23° C. or lower among the above-mentioned fluorine-containing resins.

[0073] As the polyamide-based resin, aramid resins such as aromatic polyamides and wholly aromatic polyamides are preferred.

[0074] Specific examples of the aramid resin include poly(paraphenylene terephthalamide), poly(metaphenylene isophthalamide), poly(parabenzamide), poly(metabenzamide), poly(4,4'-benzanilide terephthalamide), poly(paraphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(metaphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(paraphenylene-2,6-naphthalene dicarboxylic acid amide), poly(metaphenylene-2,6-naphthalene dicarboxylic acid amide), poly(2-chloroparaphenylene terephthalamide), paraphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, metaphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, etc. Among these, poly(paraphenylene terephthalamide) is more preferable.

[0075] As the polyester-based resin, aromatic polyesters such as polyarylates and liquid crystal polyesters are preferred.

[0076] Examples of rubbers include styrene-butadiene copolymers and hydrogenated products thereof, methacrylate copolymers, acrylonitrile-acrylate copolymers, styrene-acrylate copolymers, ethylene propylene rubber, and polyvinyl acetate.

[0077] Examples of resins having a melting point or glass transition temperature of 180° C. or higher include polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, and polyetheramide.

[0078] Examples of the water-soluble polymer include polyvinyl alcohol, polyethylene glycol, cellulose ether, sodium alginate, polyacrylic acid, polyacrylamide, and polymethacrylic acid.

[0079] The resin used in the porous layer may be of one type alone or of two or more types in combination.

[0080] The porous layer may contain fine particles. In this specification, fine particles refer to organic fine particles or inorganic fine particles generally called fillers. Therefore, when the porous layer contains fine particles, the resin contained in the porous layer functions as a binder resin that binds the fine particles together and the fine particles and the porous film. In addition, the fine particles are preferably insulating fine particles.

[0081] The organic fine particles contained in the porous layer include fine particles made of resin. Specific examples of the inorganic fine particles contained in the porous layer include fillers made of inorganic substances such as calcium carbonate, talc, clay, kaolin, silica, hydrotalcite, diatomaceous earth, magnesium carbonate, barium carbonate, calcium sulfate, magnesium sulfate, barium sulfate, aluminum hydroxide, boehmite, magnesium hydroxide, calcium oxide, magnesium oxide, titanium oxide, titanium nitride, alumina (aluminum oxide), aluminum nitride, mica, zeolite, and glass. These inorganic fine particles are insulating fine particles. The fine particles may be used alone or in combination of two or more kinds.

[0082] Among the above-mentioned fine particles, fine particles made of an inorganic substance are preferred, and fine particles made of an inorganic oxide such as silica, calcium oxide, magnesium oxide, titanium oxide, alumina, mica, zeolite, aluminum hydroxide, or boehmite are more preferred, and fine particles of at least one type selected from the group consisting of silica, magnesium oxide, titanium oxide, aluminum hydroxide, boehmite, and alumina are even more preferred, with alumina being particularly preferred.

[0083] The content of the fine particles in the porous layer is preferably 1 to 99% by volume of the porous layer, and more preferably 5 to 95% by volume. By setting the content of the fine particles in the above range, the voids formed by the contact between the fine particles are less likely to be blocked by resin or the like. Therefore, sufficient ion permeability can be obtained, and the basis weight per unit area can be set to an appropriate value.

[0084] The fine particles may be used in combination of two or more types having different particle diameters or specific surface areas.

[0085] The thickness of the porous layer is preferably 0.5 to 15 μm per layer, more preferably 2 to 10 μm. If the thickness of the porous layer is 0.5 μm or more per layer, internal short circuit due to damage to the nonaqueous electrolyte secondary battery can be sufficiently suppressed, and the amount of electrolyte held in the porous layer becomes sufficient. On the other hand, if the thickness of the porous layer is 15 μm or less per layer, deterioration of rate characteristics or cycle characteristics can be suppressed.

[0086] The weight per unit area of ​​the porous layer, i.e., the basis weight per layer, is 1 to 20 g / m 2 It is preferable that the thickness is 4 to 10 g / m 2 It is more preferable that:

[0087] The volume of the porous layer constituents contained in one square meter of the porous layer is 0.5 to 20 cm per layer. 3 It is preferable that the thickness is 1 to 10 cm. 3 More preferably, it is 2 to 7 cm. 3 It is even more preferable that:

[0088] The porosity of the porous layer is preferably 20 to 90% by volume, more preferably 30 to 80% by volume, so that sufficient ion permeability can be obtained. Also, the pore size of the pores in the porous layer is preferably 3 μm or less, more preferably 1 μm or less, so that sufficient ion permeability can be obtained in the laminated separator.

[0089] <Laminated separator> The separator according to one embodiment of the present invention may be a laminated separator.

[0090] The thickness of the laminated separator is preferably 5.5 μm to 45 μm, and more preferably 6 μm to 25 μm.

[0091] The laminated separator preferably has an air permeability of 100 to 350 sec / 100 mL in Gurley value, and more preferably 100 to 300 sec / 100 mL.

[0092] The separator according to an embodiment of the present invention may include another porous layer other than the porous film and the porous layer, if necessary, within a range that does not impair the object of the present invention. Examples of the other porous layer include known porous layers such as a heat-resistant layer, an adhesive layer, and a protective layer.

[0093] The other porous layer may be provided on one or both sides of the laminate separator. When the laminate separator has an insulating porous layer on both sides of a porous film, the other porous layer may be provided on the insulating porous layer on both sides, or on the insulating porous layer on one side. When the laminate separator has an insulating porous layer on only one side of a porous film, the other porous layer may be provided on the insulating porous layer, or on the side of the porous film where the insulating porous layer is not provided. It can also be said that the other porous layer may be provided on the outermost layer of the laminate separator.

[0094] For example, the laminated separator further includes an adhesive layer in addition to the insulating porous layer. In this specification, the adhesive layer means a porous layer having adhesive properties. The adhesive layer may be provided on the surface of the laminated separator that contacts the electrode. Examples of components that contribute to adhesive properties contained in the adhesive layer include acrylic resin, PVDF, etc.

[0095] <Method of manufacturing porous layer and laminated separator> An example of a method for producing the insulating porous layer in one embodiment of the present invention and the laminated separator in one embodiment of the present invention is a method in which a coating liquid containing the resin contained in the porous layer is applied to one or both sides of the porous film and dried to precipitate a porous layer.

[0096] In addition, when a porous layer is deposited on both sides of the porous film, (a) the porous layer may be deposited simultaneously on both sides of the porous film, or (b) the coating liquid may be applied to one side of the porous film and dried to deposit a porous layer on one side of the porous film, and then the coating liquid may be applied to the other side of the porous film and dried to deposit a porous layer on the other side of the porous film.

[0097] Furthermore, before the coating liquid is applied to one or both sides of the porous film, the one or both sides of the porous film to be coated with the coating liquid may be subjected to a hydrophilization treatment, if necessary.

[0098] The coating liquid contains the resin contained in the porous layer. The coating liquid may also contain the fine particles described below that may be contained in the porous layer. The coating liquid may usually be prepared by dissolving the resin that may be contained in the porous layer in a solvent and dispersing the fine particles. Here, the solvent that dissolves the resin also serves as a dispersion medium that disperses the fine particles. The resin may also be made into an emulsion by the solvent.

[0099] The solvent is not particularly limited as long as it does not adversely affect the porous film, dissolves the resin uniformly and stably, and disperses the fine particles uniformly and stably.Specific examples of the solvent include water and organic solvents.The solvent may be used alone or in combination of two or more.

[0100] The coating liquid may be formed by any method as long as it satisfies the conditions such as the resin solid content (resin concentration) and the amount of fine particles required to obtain a desired porous layer. Specific examples of the method for forming the coating liquid include mechanical stirring, ultrasonic dispersion, high pressure dispersion, and media dispersion. The coating liquid may also contain additives such as dispersants, plasticizers, surfactants, and pH adjusters as components other than the resin and fine particles, as long as the object of the present invention is not impaired. The amount of additives added may be within a range that does not impair the object of the present invention.

[0101] The method of applying coating liquid to porous film, that is, the method of forming a porous layer on the surface of porous film, is not particularly limited.The method of forming a porous layer can be, for example, the method of applying coating liquid directly to the surface of porous film, and then removing the solvent; the method of applying coating liquid to a suitable support, removing the solvent to form a porous layer, and then pressing this porous layer and the porous film, and then peeling off the support; the method of applying coating liquid to a suitable support, pressing a porous film on the coating surface, and then peeling off the support, and then removing the solvent.

[0102] As a method for applying the coating liquid, a conventionally known method can be adopted, and specific examples thereof include a gravure coater method, a dip coater method, a bar coater method, and a die coater method.

[0103] The solvent is generally removed by drying, or the solvent contained in the coating liquid may be replaced with another solvent before drying.

[0104] [Embodiment 2: Nonaqueous electrolyte secondary battery member, Embodiment 3: Nonaqueous electrolyte secondary battery] The member for a nonaqueous electrolyte secondary battery according to the second embodiment of the present invention comprises a positive electrode, the separator for a nonaqueous electrolyte secondary battery according to the first embodiment of the present invention, and a negative electrode arranged in this order.

[0105] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention includes the separator for nonaqueous electrolyte secondary batteries according to the first embodiment of the present invention.

[0106] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention is, for example, a nonaqueous secondary battery that obtains electromotive force by doping and dedoping lithium, and may include a nonaqueous electrolyte secondary battery member in which a positive electrode, the separator according to the first embodiment of the present invention, and a negative electrode are laminated in this order. Note that the components of the nonaqueous electrolyte secondary battery other than the separator are not limited to the components described below.

[0107] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention usually has a structure in which a battery element in which a negative electrode and a positive electrode are opposed to each other through the separator according to the first embodiment of the present invention and an electrolyte is impregnated in the structure is sealed in an exterior material. The nonaqueous electrolyte secondary battery is preferably a lithium ion secondary battery. Note that the term "doping" refers to occlusion, support, adsorption, or insertion, and refers to a phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.

[0108] A nonaqueous electrolyte secondary battery member according to embodiment 2 of the present invention includes the separator according to embodiment 1 of the present invention. Thus, the nonaqueous electrolyte secondary battery member has an effect of suppressing deterioration of battery performance caused by internal pressure during repeated charging and discharging in a nonaqueous electrolyte secondary battery. A nonaqueous electrolyte secondary battery according to embodiment 3 of the present invention includes the separator according to embodiment 1 of the present invention. Thus, the nonaqueous electrolyte secondary battery has an effect of suppressing deterioration of battery performance caused by internal pressure during repeated charging and discharging.

[0109] <Positive electrode> The positive electrode in the nonaqueous electrolyte secondary battery member and the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is generally used as a positive electrode in a nonaqueous electrolyte secondary battery, but for example, a positive electrode sheet having a structure in which an active material layer containing a positive electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.

[0110] The positive electrode active material may be, for example, a material capable of doping and dedoping lithium ions, specifically, a lithium composite oxide containing at least one transition metal such as V, Mn, Fe, Co, or Ni.

[0111] Examples of the conductive agent include carbonaceous materials such as natural graphite, artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, and organic polymer compound sintered bodies. The conductive agent may be used alone or in combination of two or more kinds.

[0112] Examples of the binder include fluorine-based resins such as polyvinylidene fluoride, acrylic resins, and styrene-butadiene rubber. The binder also functions as a thickener.

[0113] Examples of the positive electrode current collector include conductors such as Al, Ni, stainless steel, etc. Among them, Al is more preferable because it is easy to process into a thin film and is inexpensive.

[0114] Examples of methods for producing a sheet-shaped positive electrode include a method of pressurizing and molding a positive electrode active material, a conductive agent, and a binder on a positive electrode current collector; a method of forming a paste of a positive electrode active material, a conductive agent, and a binder using an appropriate organic solvent, applying the paste to a positive electrode current collector, drying the paste, and then pressing the paste to adhere it to the positive electrode current collector; and the like.

[0115] <Negative electrode> The negative electrode in the nonaqueous electrolyte secondary battery member and the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is generally used as a negative electrode in a nonaqueous electrolyte secondary battery, but for example, a negative electrode sheet having a structure in which an active material layer containing a negative electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.

[0116] Examples of the negative electrode active material include materials capable of doping and dedoping lithium ions, lithium metal, lithium alloys, etc. Examples of the material include carbonaceous materials, etc. Examples of the carbonaceous materials include natural graphite, artificial graphite, cokes, carbon black, and pyrolytic carbons, etc.

[0117] The negative electrode current collector may be made of, for example, Cu, Ni, stainless steel, etc., and in particular, in a lithium ion secondary battery, Cu is more preferable because it is difficult to form an alloy with lithium and it is easy to process into a thin film.

[0118] Examples of methods for producing a sheet-shaped negative electrode include a method of pressurizing a negative electrode active material on a negative electrode current collector, a method of forming a paste of a negative electrode active material using an appropriate organic solvent, applying the paste to a negative electrode current collector, drying, and then pressing to fix the paste to the negative electrode current collector, etc. The paste preferably contains the conductive agent and the binder.

[0119] <Nonaqueous electrolyte> The nonaqueous electrolyte in the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is a nonaqueous electrolyte generally used in nonaqueous electrolyte secondary batteries, and for example, a nonaqueous electrolyte obtained by dissolving a lithium salt in an organic solvent can be used. As the lithium salt, for example, LiClO 4 , LiPF 6 , LiAsF 6 , LiSbF 6 , LiBF 4 , LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 , Li 2 B 10 Cl 10 , lithium salts of lower aliphatic carboxylic acids and LiAlCl 4 The lithium salts may be used alone or in combination of two or more.

[0120] Examples of the organic solvent constituting the nonaqueous electrolyte include carbonates, ethers, esters, nitriles, amides, carbamates, sulfur-containing compounds, and fluorine-containing organic solvents obtained by introducing a fluorine group into these organic solvents. The organic solvents may be used alone or in combination of two or more.

[0121] [summary] One embodiment of the present invention may include the following inventions [1] to [7]. [1] A separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, wherein a two-dimensional image of a cross section of the polyolefin porous film is obtained using a scanning electron microscope, and an average inclination angle of the long axis calculated from a circumscribing rectangle of a void extracted from the two-dimensional image is 7.0 or more, and the cross section is formed by cutting the polyolefin porous film in a direction perpendicular to the surface by a straight line passing through the center of the surface and parallel to the MD or TD direction. [2] The separator for a nonaqueous electrolyte secondary battery according to [1], further comprising an insulating porous layer containing a resin. [3] The separator for a non-aqueous electrolyte secondary battery according to [2], wherein the resin is at least one selected from the group consisting of polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins, and water-soluble polymers. [4] The separator for a nonaqueous electrolyte secondary battery according to [2] or [3], wherein the resin is an aramid resin. [5] The separator for a nonaqueous electrolyte secondary battery according to any one of [2] to [4], further comprising an adhesive layer in addition to the insulating porous layer. [6] A member for a non-aqueous electrolyte secondary battery, comprising a positive electrode, the separator for a non-aqueous electrolyte secondary battery according to any one of [1] to [5], and a negative electrode, arranged in this order.[7] [7] A non-aqueous electrolyte secondary battery comprising the separator for a non-aqueous electrolyte secondary battery according to any one of [1] to [5].

[0122] The scope of the nonaqueous electrolyte secondary battery separator, nonaqueous electrolyte secondary battery member, and nonaqueous electrolyte secondary battery according to one embodiment of the present invention may include any combination of the features described in the above-mentioned configurations within the scope of the claims. EXAMPLES

[0123] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0124] [Measurement method] The physical properties of the separators produced in Examples 1 to 3 and Comparative Examples 1 and 2 were measured by the following methods.

[0125] (Film thickness) The thickness of the separator was measured using a high-precision digital length measuring instrument (VL-50) manufactured by Mitutoyo Corporation.

[0126] (porosity) (a) Film thickness measurement The thickness of the separator was measured by the method described above in the section (Thickness). (b) Measurement of basis weight A square sample with a side length of 8 cm was cut from the separator, and the weight W (g) of the sample was measured. Then, the weight per unit area of ​​the separator was calculated according to the following formula (1).

[0127] Weight per unit area (g / m 2 )=W / (0.08×0.08) (1) (c) Measurement of true density The separator was cut into 4 mm to 6 mm squares and vacuum dried at 30° C. or less for 17 hours, after which the true density of the separator was measured by a helium gas substitution method using a dry automatic densitometer (Micromeritics AccuPyeII 1340). (d) Calculation of void ratio The membrane thickness [μm] and weight [g / m2] of the separator calculated and measured in the above steps (a) to (c)2 ] and true density [g / m 3 ], the porosity [%] of the separator was calculated based on the following formula (2).

[0128] (Porosity) = [1-(weight per unit area) / {(film thickness) x 10 -6 ×1[m 2 ]×(true density)}]×100 (2) (Various parameters that represent the void shape) <Acquisition of cross-sectional SEM images> The cross section of the separator was observed using an SEM according to the procedures (i) to (iii) below. (i) The separator was subjected to ion milling using a cross-sectional specimen preparation device IB-19520 manufactured by JEOL Ltd. to cut the separator to form a cross section. This cross section was obtained by cutting the separator along a straight line passing through the center and parallel to the MD in a direction perpendicular to the surface. (ii) Osmium deposition was carried out on the cross section formed in (i). (iii) A cross section on which the deposition film was formed in (ii) was observed with a scanning electron microscope (S-4800, Hitachi High-Tech Corporation) at a magnification of 5000 times to obtain a SEM image (film thickness direction: 960 pixels × MD direction: 1280 pixels) of the cross section. The observation conditions were an acceleration voltage of 0.8 kV and a working distance of 3.0 mm.

[0129] <Calculation of various parameters> Using the procedures shown in 1. to 17. below, image analysis of the cross-sectional SEM images was performed, and each parameter of the void shape (average area, average Feret diameter, average circle equivalent diameter, average circularity, average length-to-short ratio (L / S), and average inclination angle θ) was calculated. 1. Using Python, the image data file (JPEG file) of the SEM image of the cross section was read. From the image data read in 2.1, an analysis area of ​​100 pixels in the thickness direction × 1280 pixels in the MD direction was extracted. At this time, the analysis area was extracted so that the entire cross-sectional area of ​​the separator (porous film) was included in the analysis area. In addition, in the analysis area, the x coordinate (x axis) was taken in the MD direction, and the y coordinate (y axis) was taken in the thickness direction. The brightness values ​​of the analysis regions extracted in 3.2 were normalized. 4. In order to accurately identify voids during binarization, the analysis area in which the brightness values ​​were normalized in step 3 was inverted. The analysis area in which the brightness values ​​were inverted in 5.4 was normalized using a threshold value of 180, and the normalized analysis area was then binarized. Blob processing was performed on the analysis area binarized in 6.5 to identify voids. 7. The area of ​​each blob, i.e., each void identified in 6., was calculated from the number of pixels. In the analysis region in this example, 1 pixel is 394 μm 2 is equivalent to. 8. Among the identified gaps, gaps consisting of blobs with an area of ​​10 pixels or more were extracted. In the subsequent processing, the extracted gaps were treated as gaps, and gaps consisting of blobs with an area of ​​less than 10 pixels were not treated as gaps. For each void extracted in 9.8, the x-direction spread was measured as Dfx, and the y-direction spread as Dfy, as shown in Figure 1. Next, the weighted average of Dfx and Dfy for each void was calculated, and the calculated value was taken as the Feret's diameter for each void. 10. The area of ​​each void was calculated and this value was designated as A. For each void, the area was calculated by (4×A / π) 1 / 2 The value represented by the following formula was calculated, and the calculated value was taken as the circular equivalent diameter of each void portion. 11. The perimeter of each void was calculated and the value was designated as l. For each void, the calculated value of l and the area A of each void were used to calculate 4π×A / l 2 The calculated value was taken as the circularity of each void portion. 12. For each void, a circumscribing rectangle was created as shown in Figure 1. The circumscribing rectangle had the long side, short side, and inclination angle as parameters. For each of the bounding rectangles created in 13.12., the point with the smallest x coordinate among the four vertices of the bounding rectangle was designated P1, and then P2, P3, and P4 were designated in a counterclockwise direction from there. 14. For each of the circumscribing rectangles, the line connecting P1 and P2 is L12, and the line connecting P1 and P4 is L14. 15. For each of the circumscribed rectangles, the longer straight line of L12 or L14 was set as the major axis, and the shorter straight line was set as the minor axis. Then, the length of the major axis: L and the length of the minor axis: S were measured. The long / short ratio (L / S) of each gap was calculated using the measured values ​​of L and S. 16. For each of the circumscribing rectangles, the angle between the long axis and the x-axis was calculated, and the calculated value was taken as the inclination angle θ of each gap, with the range 0°<θ<90°. 17. The average values ​​of the parameters calculated in the above process (area, Feret diameter, circle equivalent diameter, circularity, long / short ratio (L / S) and inclination angle θ) for all voids were calculated. In addition, the standard deviations of the area, Feret diameter, circle equivalent diameter, circularity, long / short ratio (L / S) and inclination angle θ for each void were calculated.

[0130] (Difference in air permeability / film thickness before and after compression at 60MPa) The difference in air permeability / film thickness of the separator before and after compression at 60 MPa was measured by the methods shown in steps 1 to 5 below. Step 1: A 6 cm x 6 cm square sample was cut from the separator. Step 2: The air permeability of the sample cut out in step 1 was measured in accordance with JIS P8117. The measured air permeability was calculated as the air permeability of the separator when not compressed: AP 1 (Unit: sec / 100 mL). The thickness of the separator was measured using a high-precision digital length measuring machine (VL-50) manufactured by Mitutoyo Corporation. The measured thickness was defined as the thickness of the separator before compression: t 1 (Unit: μm). Step 3: The sample cut out in step 1 was sandwiched between aluminum plates and pressed using a hydraulic compression molding machine (compression molding machine NF-50, manufactured by Shinto Metal Industries Co., Ltd.) under the following pressing conditions: 60 MPa, 35° C., and 5 minutes. Step 4: For the sample pressed in step 3, the air permeability and film thickness were measured in the same manner as in step 2. The measured air permeability and film thickness were respectively defined as the air permeability of the separator after compression: AP 2 (unit: sec / 100mL) and the thickness of the separator after compression, t 2 (Unit: μm). Step 5: The AP obtained in Step 2 and Step 4 1 , AP 2 , t 1 and t 2 Using the above, the difference in air permeability / film thickness of the separator before and after compression at 60 MPa was calculated according to the following formula (3).

[0131] (Difference in air permeability / film thickness before and after compression at 60 MPa) (unit: sec / 100 mL / μm) = {(AP 2 ) / (t 2 )}-{(AP 1 ) / (t 1 )} (3) (number average branch number) The number average branch number of polyethylene, which is a polyolefin resin used in the examples and comparative examples, was calculated by the method shown in steps 1 to 4 below. Step 1: A standard sample was prepared, which was made of the same type of polyolefin as the polyolefin constituting the polyolefin resin, but was made of a linear polyolefin with no branching. Step 2: For the standard samples prepared in step 1, conformation plots based on GPC-MALS were generated using DAWN HELEOS II. Step 3: Using the same method as in step 2, a conformation plot was created based on GPC-MALS for the polyolefin resin. Step 4: From the conformation plots prepared in steps 2 and 3, the number average branch number of the polyolefin resin was calculated according to the following formula.

[0132]

number

[0133] (In the formula, R gL is the radius of gyration of the linear polyolefin resin, and R gb is the radius of gyration of the branched polyolefin resin, and g is the radius of gyration of the branched polyolefin resin at the same molecular weight (R gL / R gb ) 2 is the value of B n is the number of branches in a single chain.) [Example 1] 27.4 parts by weight of ultra-high molecular weight polyethylene powder (intrinsic viscosity: 21 dL / g, viscosity average molecular weight: 3 million, number average branch number: 0.1, manufactured by Tosoh Corporation), 6.9 parts by weight of polyethylene wax (Excelex 40800, manufactured by Mitsui Chemicals, Inc.) having a weight average molecular weight of 4000, and 3.0 parts by weight of alumina (product name AEROXIDE Alu65, manufactured by Nippon Aerosil Co., Ltd.) were prepared. The total of the ultra-high molecular weight polyethylene, polyethylene wax, and alumina was 100 parts by weight, and 0.3 parts by weight of antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of antioxidant (IRGAFOS 168, manufactured by BASF), 0.4 parts by weight of sodium stearate, and 0.6 parts by weight of dispersing aid (BYK-MAX P4102, manufactured by BYK) were added. Further, calcium carbonate (manufactured by Maruo Calcium Co., Ltd.) having an average particle size of 0.07 μm was added so that the amount was 38 volume % with respect to the total volume of the obtained mixture. These were mixed in powder form in a Henschel mixer, and then melt-kneaded in a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded in a single-screw extruder to obtain a resin sheet. The resin sheet was stretched in the MD direction by a pair of heated rolls to a stretch ratio of 2.07 times to obtain a sheet-like polyolefin resin composition. The obtained sheet-like polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (hydrochloric acid 4 mol / L, nonionic surfactant 0.5 wt %) to remove the calcium carbonate, thereby obtaining a primary sheet. Then, both ends in the TD direction of the obtained primary sheet were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretch ratio of 7.05 times to produce a porous film 1. The produced porous film 1 was used as a separator 1.

[0134] [Example 2] 70 parts by weight of ultra-high molecular weight polyethylene powder (GUR4032, number average branch number: 0.5, manufactured by Ticona) and 30 parts by weight of polyethylene wax (FNP-0115, manufactured by Nippon Seiro) having a weight average molecular weight of 1000 were prepared. The total of the ultra-high molecular weight polyethylene and the polyethylene wax was 100 parts by weight, and 0.4 parts by weight of an antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of an antioxidant (IRGAFOS 168, manufactured by BASF), and 1.3 parts by weight of sodium stearate were added. Furthermore, calcium carbonate having an average particle size of 0.1 μm (manufactured by Maruo Calcium Co., Ltd.) was added so that it was 38% by volume with respect to the total volume of the obtained mixture. These were mixed in powder form using a Henschel mixer, and then melt-kneaded using a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded using a single-screw extruder to form a resin sheet. The resin sheet was stretched in the MD direction by a pair of heated rolls to a stretch ratio of 2.04 times to obtain a sheet-like polyolefin resin composition. The obtained sheet-like polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (4 mol / L hydrochloric acid, 0.5 wt % nonionic surfactant) to remove the calcium carbonate to obtain a primary sheet. Then, both ends of the obtained primary sheet in the TD direction were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretch ratio of 7.05 times to produce a porous film 2. The produced porous film 2 was used as a separator 2.

[0135] [Example 3] 27.4 parts by weight of ultra-high molecular weight polyethylene powder (intrinsic viscosity: 21 dL / g, viscosity average molecular weight: 1.5 million, number average branch number: 0.1, manufactured by Tosoh Corporation) and 6.9 parts by weight of polyethylene wax (Excelex 40800, manufactured by Mitsui Chemicals, Inc.) having a weight average molecular weight of 4000 were prepared. The total of the ultra-high molecular weight polyethylene and the polyethylene wax was 100 parts by weight, and 0.3 parts by weight of an antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of an antioxidant (IRGAFOS 168, manufactured by BASF), and 0.4 parts by weight of sodium stearate were added. Furthermore, calcium carbonate having an average particle size of 0.07 μm (manufactured by Maruo Calcium Co., Ltd.) was added so that it was 38% by volume with respect to the total volume of the obtained mixture. These were mixed in powder form using a Henschel mixer, and then melt-kneaded using a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded using a single-screw extruder to form a resin sheet. The resin sheet was stretched in the MD direction by a pair of heated rolls to a stretch ratio of 1.56 times to obtain a sheet-like polyolefin resin composition. The obtained sheet-like polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (4 mol / L hydrochloric acid, 0.5 wt % nonionic surfactant) to remove the calcium carbonate to obtain a primary sheet. Then, both ends of the obtained primary sheet in the TD direction were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretch ratio of 7.05 times to produce a porous film 3. The produced porous film 3 was used as a separator 3.

[0136] [Comparative Example 1] A porous film C1 was produced by carrying out the same operation as in Example 2, except that the stretching ratio in the MD direction was changed to 1.49 times. The produced porous film C1 was used as a separator C1.

[0137] [Comparative Example 2] A commercially available porous film (Celgard, #2400) was used as separator C2.

[0138] [result] The physical properties of the separators 1 to 3 and the separators C1 and C2 obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were measured by the above-mentioned methods, and the results are shown in the following Tables 1 to 3.

[0139] [Table 1]

[0140] [Table 2]

[0141] [Table 3]

[0142] As shown in Table 1, separators 1 to 3 in Examples 1 to 3 include a porous film having an average tilt angle of 7.0 or more, and correspond to a separator according to one embodiment of the present invention. On the other hand, separators C1 and C2 in Comparative Examples 1 and 2 are made of a porous film having an average tilt angle of less than 7.0, and do not correspond to a separator according to one embodiment of the present invention. In addition, separators 1 to 3 have a smaller difference in air permeability / film thickness before and after compression at 60 MPa than separators C1 and C2, and the increase in air permeability, i.e., the decrease in ion permeability, before and after compression is smaller. Therefore, it was found that a separator according to one embodiment of the present invention can maintain good ion permeability even when compressed.

[0143] As shown in Tables 1 to 3, the average values ​​and standard deviations of the parameters of the void area, Feret diameter, circle equivalent diameter, circularity, and length ratio of the separators 1 to 3 are within the preferred ranges shown in the above-mentioned (Modes for carrying out the invention). On the other hand, the average values ​​and standard deviations of the parameters of the separators C1 and C2 are outside the above-mentioned preferred ranges. It has been shown that the separators 1 to 3 can maintain ion permeability better even when compressed than the separators C1 and C2. Therefore, it was found that the separator according to one embodiment of the present invention can maintain ion permeability better even when compressed because the average values ​​and standard deviations of the parameters are within the above-mentioned preferred ranges. [Industrial Applicability]

[0144] The separator according to one embodiment of the present invention can maintain good ion permeability even when compressed, and therefore can be used as a separator for a high-capacity non-aqueous electrolyte secondary battery having a high internal pressure. [Explanation of symbols]

[0145] 1. Polyolefin porous film with low crystal orientation in the MD or TD direction of polyolefin resin 2. Polyolefin porous film with high crystal orientation in the MD or TD direction of polyolefin resin 3 void

Claims

1. A separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, A two-dimensional image of a cross section of the polyolefin porous film is obtained using a scanning electron microscope, and the average inclination angle of the major axis calculated from the circumscribed rectangle of the void extracted from the two-dimensional image is 7.0 or more; The cross section is a cross section formed by cutting the polyolefin porous film in a direction perpendicular to the surface along a straight line passing through the center of the surface and parallel to the MD or TD direction.

2. The separator for a non-aqueous electrolyte secondary battery according to claim 1 , further comprising an insulating porous layer containing a resin.

3. 3. The separator for a non-aqueous electrolyte secondary battery according to claim 2, wherein the resin is at least one selected from the group consisting of polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins, and water-soluble polymers.

4. 3. The separator for a non-aqueous electrolyte secondary battery according to claim 2, wherein the resin is an aramid resin.

5. The separator for a non-aqueous electrolyte secondary battery according to claim 2 , further comprising an adhesive layer in addition to the insulating porous layer.

6. A member for a non-aqueous electrolyte secondary battery, comprising a positive electrode, the separator for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5, and a negative electrode, arranged in this order.

7. A non-aqueous electrolyte secondary battery comprising the separator for non-aqueous electrolyte secondary batteries according to any one of claims 1 to 5.