Composite material for manufacturing inductor, inductor, and method for manufacturing inductor

The composite material and structured manufacturing process enhance inductor performance by ensuring high density and stability, improving inductance and reducing deformation, thus enhancing magnetic sensing efficiency.

JP2024146717AActive Publication Date: 2024-10-15ZHONGSHAN SKCOIL ELECTRONICS CO LTD +3

Patent Information

Application Number
JP2023181007
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-10-20
Publication Date
2024-10-15
Estimated Expiration
2043-10-20

AI Technical Summary

Technical Problem

Conventional inductors face issues with low powder density, coil deformation, and poor magnetic sensing performance due to uneven density distribution and compression during press molding.

Method used

A composite material comprising carbonyl iron powder, amorphous powder, epoxy resin, coupling agent, and zinc stearate is used to manufacture T-core and U-core structures, followed by specific cold and hot press forming processes to create an inductor with high molding density and improved coil stability.

Benefits of technology

The inductor achieves high inductance performance, low loss, and high conversion efficiency with reduced risk of product cracking through peak baking, addressing the issues of coil deformation and uneven density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146717000001_ABST
    Figure 2024146717000001_ABST
Patent Text Reader

Abstract

To provide a composite material for manufacturing an inductor, an inductor, and a method for manufacturing an inductor.SOLUTION: The present invention provides a composite material for manufacturing an inductor, an inductor, and a manufacturing method thereof. The composite material includes the following components in mass percentage: 70 to 75% carbonyl iron powder, 20 to 25% amorphous powder, 2 to 5% epoxy resin, 0.3 to 0.5% coupling agent, and 0.1 to 1.5% zinc stearate. The composite material according to the present invention can be combined with a specific inductor manufacturing process to produce an inductor with excellent performance.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of inductor technology, and more particularly to a composite material for the manufacture of an inductor, an inductor, and a method for the manufacture thereof. [Background technology]

[0002] An inductor is a device that can convert electric power into magnetic force and store it. The structure of an inductor is similar to that of a transformer, but it only has one winding. An inductor has a certain inductance and only inhibits changes in electric current. When no current is passing through a circuit, an inductor will inhibit the current flowing there when the circuit is connected, and when no current is passing through a circuit, an inductor will maintain the current unchanged. Inductors are also called chokes, reactors, and dynamic reactors.

[0003] The integrally molded inductor in the prior art includes a compression-molded metal magnetic powder block and a coil, the coil includes a coil body and two terminals, the coil body is made of a metal-coated wire and embedded in the metal magnetic powder block, the terminals are located on both sides of the metal magnetic powder block, and the coil body has a bidirectional spiral structure.

[0004] Currently, integrally molded inductors have several different structures as follows. As shown in Figure 2, for A-series inductors, a coil is first wound, then the coil is placed in a mold, and then filled with a uniform composite material and cold-pressed in one go. As shown in Figure 4, for B-series inductors, a coil is first wound, then the coil is placed in a mold, and then filled with a uniform composite material and hot-pressed in one go. As shown in Figure 4, for C-series inductors, a T-core is first cold-pressed, and then a coil is wound on the protruding base of the T-core, which is then placed in a mold, and then filled with a uniform composite material and hot-pressed in one go.

[0005] The above A and B series inductors are affected by the coil, and the molding density at the center of the coil is low, so that the coil is compressed during press molding and is easy to deform, which affects the magnetic induction effect and thus the performance of the inductor. The above C series inductors have a convex base structure with a T-core at the center of the coil, and the density is not low, but the density outside the T-core is not high. During press molding, the coil is still compressed and deformed, which affects the magnetic induction effect and thus the performance of the inductor. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2023-120748 A Summary of the Invention [Problem to be solved by the invention]

[0007] Based on the above technical problems existing in the prior art, the present invention provides a composite material for manufacturing an inductor, and the inductor manufactured by combining said material with a specific process has excellent performance. [Means for solving the problem]

[0008] In order to achieve the above objectives, the technical solution of the present invention is as follows: A composite material for manufacturing an inductor, comprising the following components based on mass percentage: Carbonyl iron powder 70~75% Amorphous powder 20~25% Epoxy resin: 2~5% Coupling agent: 0.3~0.5% Zinc stearate 0.1~1.5%

[0009] In some embodiments, the amorphous powder comprises the following components: Silicon 1.8~3.8% B 2~4% C 0.2~1.0% P 0.02~0.2% S 0.01~0.03% The rest is Fe.

[0010] Moreover, the present invention further provides a method for manufacturing an inductor, the method including the following steps. S1. Coil production: Use a winding machine to wind a flat copper wire to obtain a coil with two parallel leads in the horizontal direction, bend the two leads in the same direction so that they are perpendicular to the winding part, and peel off the lead part. S2, a T-core and a U-core are respectively manufactured using the composite material according to claim 1 or 2. Specifically, the method includes the following steps: The epoxy resin and coupling agent are added to a solvent to obtain a first mixture. Next, the carbonyl iron powder and amorphous powder are added to the first mixture and mixed uniformly to obtain a second mixture. The second mixture is granulated to form particles. The zinc stearate is added to the particles and mixed uniformly to obtain a third mixture. The third mixture is filled into a mold and cold press molded to obtain a T-core and a U-core, respectively. The T-core includes a base and a convex portion disposed on the base, and the convex portion fits into the space of the coil. The U-core has a groove inside, and the groove fits into the coil. S3, the coil obtained in step S1 is placed in the groove of the U-core, and the lead wire is extended to the outside of the groove. S4: Place a T-core in the coil space, and the base covers the groove mouth and bends the lead wire. S5: The assembled U-core, coil, and T-core are hot-pressed to obtain a formed part. S6: Sinter the molded member. S7: After firing, the molded member is subjected to roll spraying and paint stripping treatment to obtain an inductor. S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated from the inside to the outside in the order of a copper layer, a nickel layer, and a tin layer to obtain the final inductor product.

[0011] In some embodiments, in step S2, the molding pressure is 3.5 to 4.0 T / cm 2 It is.

[0012] In some embodiments, in step S2, the cold pressing time is 1 to 2 s.

[0013] In some embodiments, in step S4, the bend angle of the lead wire is 45 to 90°, and more preferably, in step S4, the bend angle of the lead wire is 55 to 60°, so that the lead wire forms an angle of 30 to 35° with the surface of the base, facilitating hot press molding in step S5, and further bending the lead wire to the surface of the base.

[0014] In some embodiments, the hot pressing temperature is 160 to 180°C in step S5.

[0015] In some embodiments, in step S5, the hot pressing pressure is 5.0 to 6.0 T / cm 2 It is.

[0016] In some embodiments, in step S5, the hot pressing time is 50 to 80 s.

[0017] In some embodiments, in step S6, the firing process is performed by first firing at a stepwise increased temperature and then firing at a stepwise decreased temperature. First stage, baking temperature 80±5℃, baking time 30±3min; Second stage, baking temperature 100±5℃, baking time 30±3min; Third stage, baking temperature 120±5℃, baking time 30±3min; Fourth stage, baking temperature 140±5℃, baking time 30±3min; 5th stage, baking temperature 160±5℃, baking time 120±3min; 6th stage, baking temperature 140±5℃, baking time 15±3min; 7th stage, baking temperature 120±5℃, baking time 15±3min; Step 8: baking temperature 100±5℃, baking time 15±3min.

[0018] In some embodiments, in step S7, a roll spray applies the insulating paint evenly to the surface of the molding member.

[0019] In some embodiments, in step S7, paint removal is performed by removing the paint from the copper wire of the lead wire portion of the molded member after roll spraying, to expose the copper wire to the surface.

[0020] In some embodiments, in step S8, the copper layer has a thickness of 2-4 μm, the nickel layer has a thickness of 1-3 μm, and the tin layer has a thickness of 6-8 μm.

[0021] In some embodiments, the position at which the composite layer is plated on the side surface is 1 / 6 of the way down from the top surface of the inductor to the side surface.

[0022] In some embodiments, the solvent is acetone and / or ethanol.

[0023] The present invention further provides an inductor obtained by the manufacturing method according to any one of the above embodiments.

[0024] In some embodiments, the inductor includes a molded part formed of a U-core, a coil, and a T-core, the U-core has a groove that fits the coil, the T-core includes a base and a protrusion placed on the base, the protrusion fits the inner diameter of the coil, the coil is provided with two parallel lead wires, the coil is disposed within the groove and the lead wires are located outside the groove, the protrusion of the T-core is disposed within the space of the coil, the base fits into the groove mouth, the lead wires are bent onto the surface of the base, an insulating paint layer is applied to the surface of the molded part other than the lead wires, and a copper layer, a nickel layer, and a tin layer are applied to the surface of the lead wires in order from the inside to the outside.

[0025] In some embodiments, the base of the T-core has notches at two corners through which the coil leads pass. Effect of the Invention

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention uses a specific composite material to manufacture a magnetic body and combines specific processes to manufacture an inductor, thereby obtaining an inductor with excellent electrical performance. Specifically, a specific composite material is used, and a specific cold press molding process is used to manufacture a T-core and a U-core with a specific structure, and then a coil is placed in the groove of the U-core, the T-core is placed in the space of the coil, and the base directly covers the groove mouth of the U-core, and a specific hot press molding process is used to manufacture a molded part. This effectively solves the problems of low powder density, deterioration of inductance performance due to deformation of the coil, and high loss of the conventional inductor, and the inductor manufactured by the present invention has a high molding density, a coil that is not easily deformed, excellent inductance performance, high conversion efficiency, and low loss. In addition, the present invention adopts peak baking (step-by-step baking) to effectively reduce the risk of cracking of the product and reduce the problem of thermal expansion caused by sudden high-temperature solidification. [Brief description of the drawings]

[0027] [Figure 1] 1 is a structural diagram and a manufacturing flowchart of an inductor according to the present invention. [Diagram 2] 13 is an explanatory diagram of A-series inductors of conventional comparative examples 4 to 6. FIG. [Diagram 3] 13 is an explanatory diagram of B-series inductors according to conventional comparative examples 4 to 6. FIG. [Figure 4] 13 is an explanatory diagram of conventional C-series inductors according to comparative examples 4 to 6. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] In the following, the technical solutions in the embodiments of the present invention will be clearly and completely described by combining specific embodiments of the present invention. However, the embodiments described herein are only some of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without requiring creative efforts all fall within the scope of protection of the present invention.

[0029] In the following examples and comparative examples, the following materials are used: Epoxy resin: Epoxy resin with model number NF552 manufactured by Eiko Chemical Co., Ltd. Coupling agent: A silane coupling agent, model number KH-550, manufactured by Tenyo Co., Ltd. Zinc stearate: A product of Cenova New Materials Co., Ltd.

[0030] In the following examples and comparative examples, the dimensions of the coils used are the same. The inductors are manufactured in two sizes, as follows: Size 1: length x width x height is 5.1 mm x 5.3 mm x 3.0 mm; Size 2: length x width x height is 6.0 mm x 6.0 mm x 3.1 mm. In comparative examples 4 to 6, the dimensions are adjusted due to differences in structure, the height remains the same, and the length and width are each increased by 0.3 mm.

[0031] Example 1: As shown in FIG. 1, the manufacturing method of an inductor includes the following steps. S1. Coil production: A coil winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction. The two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and a laser device is used to remove the paint from the lead wire (31) section in three directions.

[0032] S2. The composite material is used to manufacture a T-core and a U-core, which contain the following components in mass percentage of the composite material: Carbonyl iron powder: 70% Amorphous powder: 25% Epoxy resin: 4% Silane coupling agent: 0.3% Zinc stearate: 0.7% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0033] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to form a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, forming a gel-like second mixture. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours. After the materials are mixed uniformly, they are put into a mold and cold-pressed to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The base (21) is rectangular with notches at two corners to facilitate passage of the lead wire (31) of the coil (3). The protrusion (22) fits into the space of the coil (3). The U-core (1) has a groove (11) inside, which fits into the coil (3). Here, the cold press pressure is 3.5 T / cm. 2The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0034] S3: The coil (3) obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0035] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0036] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 180°C, and the hot-pressing pressure is 5.5 T / cm. 2 and the hot pressing time is 50 s.

[0037] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0038] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0039] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated from the inside to the outside in the order of copper layer, nickel layer, and tin layer to obtain the final inductor product. The thickness of the copper layer is 3 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 7 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0040] As shown in FIG. 1, the specific structure of the inductor obtained by the method of this embodiment is as follows. The inductor includes a molded member consisting of a U-core (1), a coil (3), and a T-core (2), the U-core (1) having a groove (11) that fits the coil (3), the T-core (2) having a base (21) and a protrusion (22) placed on the base (21), the protrusion (22) fits into the space of the coil (3), the coil (3) has two parallel lead wires (31), the coil (3) is disposed within the groove (11) and the lead wires (31) are located outside the groove (11), the protrusion (22) of the T-core (2) is located in the space of the coil (3), and the base (21) fits into the groove opening, and the lead wires (31) are bent onto the surface of the base (21). An insulating paint is applied to the surface of the molded part other than the surface of the lead wire (31), and the surface of the lead wire (31) is coated with a copper layer, a nickel layer, and a tin layer in that order from the inside to the outside. The base (21) of the T-shaped iron core (T-core) (2) has notches at two corners, so that the lead wire (31) of the coil (3) can pass through the notches.

[0041] Example 2: As shown in FIG. 1, the manufacturing method of an inductor includes the following steps: S1. Coil production: A coil winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction. The two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and a laser device is used to remove the paint from the lead wire (31) section in three directions.

[0042] S2. A T-core (2) and a U-core (1) are manufactured using a composite material, and the composite material contains the following components by mass percentage: Carbonyl iron powder: 75% Amorphous powder: 20% Epoxy resin: 4% Silane coupling agent: 0.3% Zinc stearate: 0.7% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0043] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to prepare a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, and a gel-like second mixture is prepared. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours to mix the materials uniformly, and then put into a mold and cold press molded to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The protrusion 22 fits into the space of the coil 3. A groove 11 is provided inside the U-core 1, and the groove 11 fits into the coil 3. Here, the cold press pressure is 3.5 T / cm. 2 The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0044] S3: The coil obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0045] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0046] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 180°C, and the hot-pressing pressure is 5.5 T / cm. 2 and the hot pressing time is 50 s.

[0047] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0048] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0049] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated from the inside to the outside in the order of copper layer, nickel layer, and tin layer to obtain the final inductor product. The thickness of the copper layer is 3 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 7 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0050] The structure of the inductor of this embodiment is the same as that of the first embodiment.

[0051] Example 3: As shown in FIG. 1, the manufacturing method of an inductor includes the following steps: S1. Coil production: A coil winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction. The two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and a laser device is used to remove the paint from the lead wire (31) section in three directions.

[0052] S2. A T-core (2) and a U-core (1) are manufactured using a composite material, and the composite material contains the following components by mass percentage: Carbonyl iron powder: 73% Amorphous powder: 23% Epoxy resin: 3% Silane coupling agent: 0.3% Zinc stearate: 0.7% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0053] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to prepare a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, and a gel-like second mixture is prepared. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours to mix the materials uniformly, and then put into a mold and cold press molded to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The protrusion 22 fits into the space of the coil 3. A groove 11 is provided inside the U-core 1, and the groove 11 fits into the coil 3. Here, the cold press pressure is 3.5 T / cm. 2 The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0054] S3: The coil (3) obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0055] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0056] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 180°C, and the hot-pressing pressure is 5.5 T / cm. 2 and the hot pressing time is 50 s.

[0057] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0058] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0059] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated from the inside to the outside in the order of copper layer, nickel layer, and tin layer to obtain the final inductor product. The thickness of the copper layer is 3 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 7 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0060] The structure of the inductor of this embodiment is the same as that of the first embodiment.

[0061] Comparative Example 1: As shown in FIG. 1, the manufacturing method of the coil includes the following steps: S1. Coil production: A coil winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction. The two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and a laser device is used to remove the paint from the lead wire (31) section in three directions.

[0062] S2. The composite material is used to manufacture a T-core and a U-core, which contain the following components in mass percentage of the composite material: Carbonyl iron powder: 70% Amorphous powder: 25% Epoxy resin: 4% Silane coupling agent: 0.3% Zinc stearate: 0.7% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0063] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to prepare a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, and a gel-like second mixture is prepared. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours to mix the materials uniformly, and then put into a mold and cold press molded to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The protrusion 22 fits into the space of the coil 3. A groove 11 is provided inside the U-core 1, and the groove 11 fits into the coil 3. Here, the cold press pressure is 3.5 T / cm. 2 The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0064] S3: The coil (3) obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0065] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0066] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 180°C, and the hot-pressing pressure is 5.5 T / cm. 2 and the hot pressing time is 50 s.

[0067] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0068] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0069] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated in the order of copper layer, nickel layer, and tin layer from the inside to the outside to obtain the final inductor product. The thickness of the copper layer is 4 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 6 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0070] The structure of the inductor of this comparative example is the same as that of the first embodiment.

[0071] Comparative Example 2: As shown in FIG. 1, the manufacturing method of an inductor includes the following steps:

[0072] S1. Coil production: A coil winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction. The two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and a laser device is used to remove the paint from the lead wire (31) section in three directions.

[0073] S2. The composite material is used to manufacture a T-core and a U-core, which contain the following components in mass percentage of the composite material: Carbonyl iron powder: 70% Amorphous powder: 25% Epoxy resin: 3% Silane coupling agent: 1% Zinc stearate: 1% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0074] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to prepare a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, and a gel-like second mixture is prepared. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours to mix the materials uniformly, and then put into a mold and cold press molded to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The protrusion 22 fits into the space of the coil 3. A groove 11 is provided inside the U-core 1, and the groove 11 fits into the coil 3. Here, the cold press pressure is 3.5 T / cm. 2 The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0075] S3: The coil (3) obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0076] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0077] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 180°C, and the hot-pressing pressure is 5.5 T / cm. 2 and the hot pressing time is 50 s.

[0078] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0079] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0080] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated in the order of copper layer, nickel layer, and tin layer from the inside to the outside to obtain the final inductor product. The thickness of the copper layer is 4 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 6 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0081] The structure of the inductor of this comparative example is the same as that of the first embodiment.

[0082] Comparative Example 3: As shown in Figure 1, the method for manufacturing an inductor includes the following steps: S1, coil fabrication: A winding machine is used to wind a flat copper wire to obtain a coil (3) having two parallel lead wires (31) in the horizontal direction, the two lead wires (31) are bent in the same direction to be perpendicular to the winding section, and the lead wires (31) are subjected to three-way paint stripping using a laser device.

[0083] S2. The composite material is used to manufacture a T-core and a U-core, which contain the following components in mass percentage of the composite material: Carbonyl iron powder: 70% Amorphous powder: 25% Epoxy resin: 4% Silane coupling agent: 0.3% Zinc stearate: 0.7% The elemental composition of the amorphous powder is as follows: Silicon 3.0% B 4.0% C 1.0% P 0.03% S 0.01% The rest is Fe

[0084] The specific manufacturing procedures for the U-core (1) and the T-core (2) are as follows: Epoxy resin and coupling agent are added to ethanol to prepare a first mixture, then carbonyl iron powder and amorphous powder are added to the first mixture, and the mixture is stirred uniformly to evaporate the ethanol, and a gel-like second mixture is prepared. The second mixture is put into a granulator (screen mesh is 100 mesh) to granulate it into particles, heated at 45°C for 2 hours, then sieved (screen mesh is 100 mesh), zinc stearate is added to the fine particles, and stirred at a rotation speed of 100 r / min for 0.5 hours to mix the materials uniformly, and then put into a mold and cold press molded to obtain a T-core (2) and a U-core (1). The T-core (2) includes a base (21) and a protrusion (22) placed on the base (21). The protrusion 22 fits into the space of the coil 3. A groove 11 is provided inside the U-core 1, and the groove 11 fits into the coil 3. Here, the cold press pressure is 3.5 T / cm. 2 The cold pressing time is 2 s, and the cold pressing is performed at room temperature. The amount of the solvent added is 25% of the total mass of the epoxy resin, the coupling agent, the carbonyl iron powder, and the amorphous powder.

[0085] S3: The coil obtained in step S1 is placed in the groove (11) of the U-shaped iron core (U-core) (1), and the lead wire (31) is extended to the outside of the groove.

[0086] S4: A T-shaped iron core (T-core) (2) is placed in the space of the coil (3), the base (21) covers the mouth of the groove (11), the lead wire (31) is bent at 55°, and the angle between the lead wire and the surface of the base (21) is set to 35°.

[0087] S5. The assembled U-core (1), coil (3), and T-core (2) are hot-pressed to obtain a molded part. The hot-pressing temperature is 160°C, and the hot-pressing pressure is 7.0 T / cm. 2 and the hot pressing time is 80 s.

[0088] S6: The molded part is placed in an oven, and the temperature is first raised stepwise to be fired, and then lowered stepwise to be fired. First stage, baking temperature 80℃, baking time 30min; Second stage, baking temperature 100℃, baking time 30min; Third stage, baking temperature 120℃, baking time 30min; 4th stage, baking temperature 140℃, baking time 30min; 5th stage, baking temperature 160℃, baking time 120min; 6th stage, baking temperature 140℃, baking time 15min; 7th stage, baking temperature 120℃, baking time 15min; Step 8: baking temperature 100℃, baking time 15min.

[0089] S7: Roll spray and paint stripping are performed on the molded part to obtain an inductor. The roll spray is specifically as follows: insulating paint is evenly applied to the surface of the molded part. Paint stripping is performed on the copper wire of the lead wire part of the molded part after roll spraying to expose the copper wire on the surface.

[0090] S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor, and the composite layer is laminated in the order of copper layer, nickel layer, and tin layer from the inside to the outside to obtain the final inductor product. The thickness of the copper layer is 4 μm, the thickness of the nickel layer is 2 μm, and the thickness of the tin layer is 6 μm. The position where the composite layer is plated on the side is 1 / 6 from top to bottom from the surface of the inductor.

[0091] The structure of the inductor of this comparative example is the same as that of the first embodiment.

[0092] Comparative Example 4: In this comparative example, the raw material composition of the composite material used to manufacture the magnet is as follows, in mass percentages: Alloy powder 95% Epoxy resin 4% Silane coupling agent: 0.3% Zinc stearate 0.7% Here, the alloy powder is a typical commercial product, for example, FeSiCr-C soft magnetic alloy powder from Antai Co., Ltd.

[0093] The structure of the inductor of this comparative example is as shown in the structure of the A series inductor in Figure 2, and is manufactured by a conventional method. Specifically, it is as follows.

[0094] According to the method of Example 1, the composite material is first mixed uniformly, then the coil is placed in the mold, the uniformly mixed composite material is filled, and cold press molding is performed at one time, and the cold press pressure is 6.0 T / cm 2 and the time is 3s.

[0095] Comparative Example 5: In this comparative example, the raw material composition of the composite material used to manufacture the magnet is, in mass percentages, as follows: Carbonyl iron powder 95% Epoxy resin 4% Silane coupling agent: 0.3% Zinc stearate 0.7%

[0096] The structure of the inductor of this comparative example is as shown in the structure of the B series inductor in Figure 3, and is manufactured by a conventional method. Specifically, it is as follows.

[0097] According to the method of Example 1, the composite material is mixed uniformly, then the coil is placed in the mold, filled with the uniformly mixed composite material, and hot press molding is carried out at one time, and the hot press temperature is 160°C / cm 2 , the pressure is 5.0 T, and the time is 8 s.

[0098] Comparative Example 6: In this comparative example, the raw material composition of the composite material used to manufacture the magnet is, in mass percentages, as follows: Carbonyl iron powder 95% Epoxy resin 4% Silane coupling agent: 0.3% Zinc stearate 0.7%

[0099] The inductor structure of this comparative example is as shown in the structure of a C-series inductor in Figure 4, and is manufactured by a conventional method. Specifically, it is as follows.

[0100] According to the method of Example 1, the composite material was first mixed uniformly, and then cold pressed to obtain a T-core. The cold pressing temperature was room temperature and the pressure was 4.0 T / cm. 2 The time is 2s. Next, the coil is wound on the protruding part of the T-core, which is then placed in a mold, filled with the homogeneously mixed composite material, and hot-pressed at once. The hot-press temperature is 160°C, and the pressure is 5.0T / cm. 2 and the time is 60s.

[0101] The relevant performance tests were carried out with reference to the inductors of Examples 1-3 and Comparative Examples 1-6, and the specific measurement methods are as follows.

[0102] Inductor and current measurement: The sample was tested using an LCR tester, and the parameters were set to frequency: 1 MHz, bias current (initial energization), and the inductance and current values ​​were measured.

[0103] Loss: Using a CHROMA1810 tester, the test parameters were set to 100mT, frequency: 100KHz.

[0104] The test results are shown in Table 1. Table 1. Related performance test results for each inductor [Table 1]

[0105] Each of the technical features of the above embodiments may be combined in any combination, and for the sake of conciseness, not all possible combinations of each of the technical features of the above embodiments are described, but any combination of these technical features should be considered to be within the scope described in this specification unless they are inconsistent.

[0106] The above examples are provided to illustrate the technical methods of the present invention, and are not limiting. The present invention is described in detail with reference to the preferred embodiments. Those skilled in the art should understand that any modification or equivalent replacement of the technical solution of the present invention falls within the protection scope of the present invention, as long as it does not deviate from the spirit and scope of the technical solution. [Explanation of symbols]

[0107] 1. U-core 11 Groove 2 T-core 21 Base 22 Convex 3 Coil 31 Lead Wire

Claims

1. As a percentage by mass, Carbonyl iron powder 70-75%, Amorphous powder 20-25%, Epoxy resin 2-5%, Coupling agent: 0.3 to 0.5% Zinc stearate 0.1 to 1.5%, A composite material for producing an inductor, comprising the components:

2. In mass percentage, the amorphous powder comprises: Si 1.8-3.8%, B 2-4%, C 0.2-1.0%, P 0.02-0.20%, S 0.01-0.03%, The remainder is Fe, 2. The composite material for manufacturing an inductor according to claim 1, comprising the following components:

3. A method for manufacturing an inductor, comprising the steps of: S1, Coil production: Use a winding machine to wind a copper flat wire to obtain a coil with two parallel leads in the horizontal direction, bend the two leads in the same direction to be perpendicular to the winding part, and peel off the lead part; S2. Using the composite material according to claim 1 or 2, a T-core and a U-core are manufactured, respectively; adding the epoxy resin and a coupling agent to a solvent to obtain a first mixture; then adding the carbonyl iron powder and the amorphous powder to the first mixture and uniformly mixing to obtain a second mixture; granulating the second mixture to form particles; adding the zinc stearate to the particles and uniformly mixing to obtain a third mixture; filling the third mixture into a mold and cold press molding to obtain a T-core and a U-core, respectively; the T-core includes a base and a protrusion disposed on the base, the protrusion fits into the space of the coil; the U-core has a recess inside, the recess fits into the coil; S3: The coil obtained in step S1 is placed in a groove of a U-core, and the lead wire is extended to the outside of the groove; S4. Place a T-core in the coil space, cover the groove with the base, and bend the lead wire. S5: The assembled U-core, coil, and T-core are hot-pressed to obtain a formed part. S6: Sintering the molded member; S7: After firing, the molded member is subjected to roll spraying and paint stripping treatment to obtain an inductor. S8, Surface treatment: A composite layer is plated on the paint peeling position on the surface of the inductor and on the two sides parallel to the lead wire of the inductor. The composite layer is laminated from the inside to the outside in the order of a copper layer, a nickel layer, and a tin layer to obtain the final inductor product.

4. In step S5, the hot pressing temperature is 160-180° C. and / or the hot pressing pressure is 5.0-6.0 T / cm 2 and / or the hot pressing time is 50 to 80 seconds.

5. In step S2, the pressure of the cold press is 3.5 to 4.0 T / cm 2 and / or the cold pressing time is 1 to 2 s.

6. 4. The method for manufacturing an inductor according to claim 3, wherein in step S8, the copper layer has a thickness of 2-4 μm, the nickel layer has a thickness of 1-3 μm, and the tin layer has a thickness of 6-8 μm.

7. In step S6, the firing process is performed by first increasing the temperature stepwise and then decreasing the temperature stepwise. Specifically, First stage, baking temperature 80±5°C, baking time 30±3 min; second stage, baking temperature 100±5°C, baking time 30±3min; Third stage, baking temperature 120±5°C, baking time 30±3min; fourth stage, baking temperature 140±5°C, baking time 30±3min; 5th stage, baking temperature 160±5°C, baking time 120±3min; Stage 6, baking temperature 140±5°C, baking time 15±3min; seventh stage, baking temperature 120±5°C, baking time 15±3min; Stage 8, baking temperature 100±5°C, baking time 15±3min; 4. The method for manufacturing an inductor according to claim 3,

8. An inductor manufactured by the manufacturing method according to any one of claims 3 to 7.

9. 9. The inductor according to claim 8, comprising a molded member formed of a U-core, a coil, and a T-core, the U-core having a groove that fits the coil, the T-core having a base and a protrusion disposed on the base, the protrusion fitting the inner diameter of the coil, the coil having two parallel lead wires, the coil being disposed within the groove and the lead wires being located outside the groove, the protrusion of the T-core being disposed within the space of the coil, the base fitting the opening of the groove, the lead wires being bent onto a surface of the base, an insulating paint layer being applied to a portion of the surface of the molded member other than the lead wires, and a copper layer, a nickel layer, and a tin layer being applied to a surface of the lead wires in this order from the inside to the outside.

10. 10. The inductor according to claim 9, wherein the base of the T-core has notches at two corners, and the leads of the coil pass through the notches.

Citation Information

Patent Citations

  • Composite dust core material and its production

    JP1995034183A

  • Surface mounted type choke coil

    JP1999307357A

  • Composite magnetic material, core using the same, and magnetic element

    JP2004197218A

  • Choke coil

    JP2004281777A

  • Dust core, method of producing the dust core, electrical / electronic component including the dust core, and electrical / electronic equipment including the electrical / electronic component mounted thereon

    JP2018170304A

Cited By

  • Surface-mount device power inductor for usb-type charger and method for manufacturing the same

    KR103007281B1