Non-aqueous electrolyte secondary battery separator, non-aqueous electrolyte secondary battery member, and non-aqueous electrolyte secondary battery

A polyolefin porous film separator for non-aqueous electrolyte secondary batteries maintains ion permeability by expanding void regions in stages, addressing the issue of pore closure due to electrode expansion and ensuring consistent performance in high-capacity batteries.

JP2024146846AActive Publication Date: 2024-10-15エスエスエルエム株式会社
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024050176
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-15
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

High-capacity non-aqueous electrolyte secondary batteries, such as those with silicon electrodes, experience decreased ion permeability due to the expansion and contraction of the negative electrode, leading to increased internal pressure and closure of pores in the separator, which impedes ion flow.

Method used

A polyolefin porous film separator is designed with a method to maintain ion permeability by expanding void regions in stages, using a scanning electron microscope to analyze the film's cross-section and performing adaptive histogram flattening and brightness inversion to determine the number of stages required to fill the resin area, ensuring uniform and dense void distribution.

Benefits of technology

The separator maintains good ion permeability even after compression, preventing pore closure and ensuring consistent performance in high-capacity batteries with fluctuating internal pressures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146846000003
    Figure 2024146846000003
  • Figure 2024146846000001
    Figure 2024146846000001
  • Figure 2024146846000002
    Figure 2024146846000002
Patent Text Reader

Abstract

To provide a non-aqueous electrolyte secondary battery separator capable of excellently maintaining ion permeability even after being compressed.SOLUTION: The present invention relates to a non-aqueous electrolyte secondary battery separator that includes a polyolefin porous film, wherein the number of stages required until a resin part region other than a cavity part region is filled with a cavity part region is 20 or less when an SEM is used to repeat processing to expand each of respective object pixels constituting the cavity part region for one stage by one pixel toward pixels adjoining four sides of the object pixel from a cross section on a two-dimensional image obtained under a condition that one pixel is 19.8×19.8 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for a nonaqueous electrolyte secondary battery, a member for a nonaqueous electrolyte secondary battery, and a nonaqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries, such as lithium secondary batteries, are currently widely used as batteries for devices such as personal computers, mobile phones and personal digital assistants, or as on-board batteries for vehicles.

[0003] A porous film mainly composed of polyolefin is mainly used as a separator in such a nonaqueous electrolyte secondary battery. An example of the porous film mainly composed of polyolefin is a porous film produced by a method including a step of stretching a resin composition containing a polyolefin resin, as described in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-130900 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, development of high-capacity batteries has been promoted for use in applications such as electric vehicles (EVs) with longer driving distances. As the high-capacity batteries, for example, nonaqueous electrolyte secondary batteries having a silicon electrode as the negative electrode have been developed. However, it is known that the negative electrode in high-capacity batteries such as the silicon electrode expands during charging and discharging, and its volume changes, for example, to about four times that of conventional negative electrodes. As a result, the internal pressure inside the battery (cell) increases in the high-capacity batteries. In the high-capacity batteries, the separator is compressed during charging and discharging due to the increased internal pressure, and the voids (pores) inside the separator are blocked, resulting in a decrease in permeability of ions, which are charge carriers.

[0006] In order to solve the above problems, an object of one aspect of the present invention is to provide a separator for a non-aqueous electrolyte secondary battery that can maintain good ion permeability even after being compressed. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that a separator for a non-aqueous electrolyte secondary battery containing a polyolefin porous film with a small gap distance can maintain good ion permeability even after compression. The present inventors have also found that when a process for expanding the size of the gap portion of a cross section of a polyolefin porous film under predetermined conditions is repeated, the gap distance can be evaluated using the number of repetitions until the portion other than the gap can no longer be observed. The present inventors have arrived at the present invention based on the above-mentioned matters.

[0008] One aspect of the present invention is a separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, wherein a two-dimensional image of 960 pixels in the film thickness direction and 1280 pixels in the MD direction, obtained from a cross section of the polyolefin porous film using a scanning electron microscope under conditions of a magnification of 5000 times and 1 pixel being 19.8 μm × 19.8 μm, is binarized into a void region and a resin region to obtain a binarized image, and then, when the binarized image is subjected to a process of gradually expanding the void region, the number of stages required until the resin region is completely filled with the expanded void region is 20 stages or less, and the process of gradually expanding is a process of repeating an operation of expanding each target pixel constituting the void region by one pixel in the pixel directions adjacent to the four sides of each target pixel per stage, A separator for a non-aqueous electrolyte secondary battery, characterized in that a process for expanding the void region in stages is carried out and the required number of stages is calculated using any of the following methods (1) to (9). (1) An analysis region of 100 pixels in the thickness direction × 1280 pixels in the MD direction is extracted from the two-dimensional image. (2) An adaptive histogram equalization process of the luminance values ​​is performed on the analysis region extracted in (1). (3) The analysis region, whose brightness values ​​have been subjected to adaptive histogram equalization processing in (2), is subjected to brightness value inversion processing. (4) All pixels constituting the analysis area whose brightness values ​​have been inverted in (3) are divided into pixels whose brightness values ​​are equal to or less than a threshold value of 180 within the brightness range of 0 to 255 and pixels whose brightness values ​​exceed the threshold value of 180, and binarized. (5) In the analysis region binarized in (4), a region consisting of pixels whose brightness value exceeds a threshold value of 180 is identified as a void region. (6) For each of the void regions identified in (5) in the analysis region, an operation is performed to expand four neighboring pixels constituting the boundary of each void region outward by one pixel. (7) The area other than the void area after the expansion operation in (6) is regarded as a resin area, and the resin area is subjected to blob processing to count the number of pixels constituting the resin area. The number of pixels thus counted is regarded as the number of resin areas. Then, it is confirmed whether the number of resin areas thus counted is 0. (8) If the number of resin part areas measured in (7) is 0, the process of calculating the required number of stages is terminated. If the number of resin part areas is not 0, the processes described in (6) and (7) are repeated until the number of resin part areas becomes 0, and the process of calculating the required number of stages is terminated at the point when the number of resin part areas becomes 0. (9) In (8), the number of times the processes described in (6) and (7) are repeated until the process of calculating the required number of stages is completed is calculated, and the calculated number is set as the required number of stages. Effect of the Invention

[0009] The separator for a non-aqueous electrolyte secondary battery according to one aspect of the present invention exhibits an effect of being able to maintain good ion permeability even after being compressed. [Brief description of the drawings]

[0010] [Figure 1] 3A to 3C are schematic diagrams illustrating a process for gradually expanding a void region in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each of the configurations described below, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in different embodiments. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more, B or less."

[0012] In this specification, MD (machine direction) means the direction in which the sheet-shaped polyolefin resin composition and the porous film are conveyed in the manufacturing method of the porous film described later, and TD (transverse direction) means the direction parallel to the surface of the sheet-shaped polyolefin resin composition and the porous film, and perpendicular to the MD.

[0013] In addition, when the manufacturing method, i.e., the direction in which the raw material sheet-shaped polyolefin resin composition and porous film are transported, is unknown, the MD direction of the separator for nonaqueous electrolyte secondary batteries and the porous film constituting the separator for nonaqueous electrolyte secondary batteries means the longitudinal direction of the film (cylindrical type: winding direction, zigzag type: folding direction). In addition, the TD direction of the separator for nonaqueous electrolyte secondary batteries and the porous film means the direction parallel to the surface of the separator for nonaqueous electrolyte secondary batteries and the porous film and perpendicular to the MD direction.

[0014] [Embodiment 1: Separator for non-aqueous electrolyte secondary battery] A separator for a non-aqueous electrolyte secondary battery according to a first embodiment of the present invention is a separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, wherein a two-dimensional image of 960 pixels in the film thickness direction and 1280 pixels in the MD direction, obtained from a cross section of the polyolefin porous film using a scanning electron microscope under conditions of a magnification of 5000 times and 1 pixel being 19.8 μm×19.8 μm, is binarized into a void region and a resin region to obtain a binarized image, and then, when the binarized image is subjected to a process of gradually expanding the void region, the number of stages required until the resin region is completely filled with the expanded void region is 20 stages or less, and the process of gradually expanding is a process of repeatedly expanding each target pixel constituting the void region by one pixel in the pixel directions adjacent to the four sides of each target pixel per stage, The method of performing the process of expanding the void region stepwise and calculating the required number of steps is the following methods (1) to (9). (1) An analysis region of 100 pixels in the thickness direction × 1280 pixels in the MD direction is extracted from the two-dimensional image. (2) An adaptive histogram equalization process of the luminance values ​​is performed on the analysis region extracted in (1). (3) The analysis region, whose brightness values ​​have been subjected to adaptive histogram equalization processing in (2), is subjected to brightness value inversion processing. (4) All pixels constituting the analysis area whose brightness values ​​have been inverted in (3) are divided into pixels whose brightness values ​​are equal to or less than a threshold value of 180 within the brightness range of 0 to 255 and pixels whose brightness values ​​exceed the threshold value of 180, and binarized. (5) In the analysis region binarized in (4), a region consisting of pixels whose brightness value exceeds a threshold value of 180 is identified as a void region. (6) For each of the void regions identified in (5) in the analysis region, an operation is performed to expand four neighboring pixels constituting the boundary of each void region outward by one pixel. (7) The area other than the void area after the expansion operation in (6) is regarded as a resin area, and the resin area is subjected to blob processing to count the number of pixels constituting the resin area. The number of pixels thus counted is regarded as the number of resin areas. Then, it is confirmed whether the number of resin areas thus counted is 0. (8) If the number of resin part areas measured in (7) is 0, the process of calculating the required number of stages is terminated. If the number of resin part areas is not 0, the processes described in (6) and (7) are repeated until the number of resin part areas becomes 0, and the process of calculating the required number of stages is terminated at the point when the number of resin part areas becomes 0. (9) In (8), the number of times the processes described in (6) and (7) are repeated until the process of calculating the required number of stages is completed is calculated, and the calculated number is set as the required number of stages.

[0015] The separator for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention includes a polyolefin porous film. Hereinafter, the polyolefin porous film is also simply referred to as a "porous film." Hereinafter, the separator for a non-aqueous electrolyte secondary battery is also simply referred to as a "separator."

[0016] The separator according to one embodiment of the present invention may be a separator made of the porous film. The separator according to one embodiment of the present invention may be a laminate including the porous film and an insulating porous layer described later. Hereinafter, a separator that is a laminate including the porous film and an insulating porous layer described later is also referred to as a "laminated separator". Furthermore, the separator according to one embodiment of the present invention may include a known porous layer such as a heat-resistant layer, an adhesive layer, or a protective layer described later as a porous layer other than the insulating porous layer, as necessary.

[0017] In one embodiment of the present invention, the number of required stages is the number of stages until the resin region is completely filled with the expanded void region when a binarization process is performed on a two-dimensional image of 960 pixels in the film thickness direction and 1280 pixels in the MD direction, obtained from the cross section of the porous film under the conditions of a magnification of 5000 times and 1 pixel being 19.8 μm × 19.8 μm, using a scanning electron microscope (SEM), to obtain a binarized image, and then, by repeating the operation of expanding each target pixel constituting the void region by 1 pixel in the pixel direction adjacent to the four sides of each target pixel for each step, the resin region is expanded in stages. Here, when each target pixel constituting the void region is expanded by 1 pixel in the pixel direction adjacent to the four sides of each target pixel, the void region as a whole is expanded by 1 pixel outward in the four neighborhoods of the pixel constituting the outer periphery of the void region. The cross section is a cross section formed by cutting the porous film in an arbitrary direction.

[0018] The method of performing the process of expanding the void region stepwise and calculating the required number of steps is the following methods (1) to (9). (1) An analysis region of 100 pixels in the thickness direction × 1280 pixels in the MD direction is extracted from the two-dimensional image. (2) An adaptive histogram equalization process of the luminance values ​​is performed on the analysis region extracted in (1). (3) The analysis region, whose brightness values ​​have been subjected to adaptive histogram equalization processing in (2), is subjected to brightness value inversion processing. (4) All pixels constituting the analysis area whose brightness values ​​have been inverted in (3) are divided into pixels whose brightness values ​​are equal to or less than a threshold value of 180 within the brightness range of 0 to 255 and pixels whose brightness values ​​exceed the threshold value of 180, and binarized. (5) In the analysis region binarized in (4), a region consisting of pixels whose brightness value exceeds a threshold value of 180 is identified as a void region. (6) For each of the void regions identified in (5) in the analysis region, an operation is performed to expand four neighboring pixels constituting the boundary of each void region outward by one pixel. (7) The area other than the void area after the expansion operation in (6) is regarded as a resin area, and the resin area is subjected to blob processing to count the number of pixels constituting the resin area. The number of pixels thus counted is regarded as the number of resin areas. Then, it is confirmed whether the number of resin areas thus counted is 0. (8) If the number of resin part areas measured in (7) is 0, the process of calculating the required number of stages is terminated. If the number of resin part areas is not 0, the processes described in (6) and (7) are repeated until the number of resin part areas becomes 0, and the process of calculating the required number of stages is terminated at the point when the number of resin part areas becomes 0. (9) In (8), the number of times the processes described in (6) and (7) are repeated until the process of calculating the required number of stages is completed is calculated, and the calculated number is set as the required number of stages.

[0019] The luminance value was measured by setting the luminance value of the darkest pixel in the analysis region to 0 and the luminance value of the brightest pixel in the analysis region to 255, and then measuring the luminance value of each pixel in 256 steps from 0 to 255. Thus, the luminance value of each pixel in the analysis region is defined as any numerical value from 0 to 255.

[0020] In general, it is difficult to achieve uniform illumination conditions over the entire area of ​​a two-dimensional image obtained by photographing using an SEM. Due to this, the brightness of the two-dimensional image and the analysis area extracted from the two-dimensional image may vary slightly depending on the location. Therefore, the two-dimensional image may be, for example, an image in which the center of the image is relatively bright and the periphery is gradually darker. In that case, if the analysis area extracted from the two-dimensional image is binarized directly using a uniform threshold value, the void portion may be smaller than the actual size or may be extracted larger depending on the location. Therefore, it becomes impossible to correctly divide the analysis area into the void portion area and the resin portion area and to accurately binarize the analysis area. Therefore, a method that uses binarization using a fixed threshold value, such as the method for measuring the required number of stages, makes it impossible to accurately measure the required number of stages.

[0021] On the other hand, the adaptive histogram flattening process is, specifically, as shown in the embodiment, adaptively, that is, dividing the analysis area into a plurality of areas, for example, 8 pixels vertically by 8 pixels horizontally, and flattening the histogram in each of the plurality of areas. The flattening process of the histogram is a process of expanding the histogram of the image to the entire area (0 to 255 because 1 pixel is 8 bits). The adaptive histogram flattening process makes the brightness of the entire analysis area uniform, and binarizes it with a uniform threshold value. Therefore, even if there is unevenness in brightness depending on the location in the analysis area, the unevenness is eliminated in the analysis area after the adaptive histogram flattening process is performed (hereinafter, also referred to as the "analysis area after the adaptive histogram flattening process"). As a result, in the entire analysis area after the adaptive histogram flattening process, each of the plurality of void areas is represented by the same brightness value, and each of the plurality of resin part areas having the same structure is represented by the same brightness value. Therefore, the analysis region after the adaptive histogram equalization process can be correctly divided into the void region and the resin region based on the luminance value, and can be accurately binarized. Therefore, the method for measuring the required number of stages using binarization with a fixed threshold value makes it possible to accurately measure the required number of stages.

[0022] Here, the adaptive histogram equalization process is a process that is generally performed when binarizing an analysis region consisting of a predetermined number of pixels based on brightness values, and can be performed by a person skilled in the art using a program available as open source. An example of the program available as open source is "OpenCV: cv::CLAHE Class Reference" used in the examples. When the adaptive histogram equalization process is performed using the program available as open source, the adaptive histogram equalization process is usually performed automatically, and there is no need to input parameters, etc.

[0023] The above methods (1) to (9) are specifically carried out, for example, by a method including the following steps (1a) to (8a). (1a) The porous film is cut in an arbitrary direction to form a cross section. (2a) A deposition film for SEM observation is formed on the cross section formed in step (1a). (3a) A cross section on which a vapor-deposited film is formed in step (2a) is observed using an SEM with a backscattered electron image under conditions of an acceleration voltage of 0.8 kV, a working distance of 3.0 mm, 1 pixel: 19.8 μm × 19.8 μm, and a magnification of 5000 times to obtain an SEM image (two-dimensional image) of the cross section. (4a) An analysis area of ​​a predetermined size (film thickness direction: 100 pixels × MD direction: 1280 pixels) is extracted from the SEM image of the cross section obtained in step (3a). (5a) Adaptive histogram equalization of luminance values ​​is performed on the analysis region extracted in step (4a). (6a) For the analysis region obtained in step (5a) and subjected to adaptive histogram equalization of brightness values, a brightness inversion process is performed in order to accurately identify voids when performing binarization, which will be described later. (7a) The analysis region obtained in step (6a) and subjected to the inversion process of the brightness values ​​is binarized at a threshold value of 180 within a brightness value range of 0 to 255, and the analysis region is divided into a void region consisting of pixels whose brightness values ​​exceed the threshold value of 180 and a resin region consisting of pixels whose brightness values ​​are equal to or less than the threshold value of 180. Note that the resin region means a region other than the void region. For example, when the porous film contains components other than resin, such as a filler, the region consisting of the other components is also treated as the resin region. (8a) For the binarized analysis region obtained in step (7a), an operation of expanding each target pixel constituting the void region by one pixel per stage in the pixel direction adjacent to the four sides of each target pixel is repeated until the resin part region is completely filled with the expanded void region. The number of times the operation is repeated is calculated as the required number of stages. Note that the resin part region being completely filled with the expanded void region means that the entire analysis region is occupied only by the expanded void region, and the number of pixels constituting the resin part region becomes zero.

[0024] In the step (1a), the cross section is not particularly limited, and may be, for example, a cross section formed by cutting the porous film in a direction perpendicular to the surface along a straight line passing through the center of the surface of the porous film and parallel to the MD or TD direction.

[0025] In the step (1a), a laminate separator including other layers such as an insulating porous layer in addition to a porous film, such as the laminate separator, may be used in place of the porous film.

[0026] In the step (1a), the method for cutting the porous film is not particularly limited, and a known method can be adopted. For example, an ion milling method can be adopted as the cutting method. In addition, in the step (1a), the same cutting method as that for cutting the porous film can be adopted when cutting the laminated separator.

[0027] In the step (2a), the deposited film may be a typical deposited film that can be used for observing a backscattered electron image using a SEM. For example, a deposited film made of osmium or the like may be used. A known method may be used to form the deposited film.

[0028] In the step (4a), an analysis region including the entire cross section of the porous film may be extracted as the analysis region, or multiple analysis regions of a predetermined size may be extracted from any location on the cross section of the porous film. When multiple analysis regions are extracted, the required number of stages is calculated from each of the multiple analysis regions by the method described in steps (5a) to (8a). Then, the average value of the multiple required numbers of stages calculated from the multiple analysis regions is defined as the required number of stages in the present invention. Note that, when a laminated separator including the other layer is to be cut, the analysis region may include all or a part of the cross section of the porous film. In other words, the cross-sectional area of ​​the other layer does not have to be included in the analysis region.

[0029] When extracting a plurality of the analysis regions, the extraction conditions are preferably such that three or more of the analysis regions are extracted, and more preferably such that five or more of the analysis regions are extracted. The area of ​​one of the plurality of extracted analysis regions is preferably 20% or more, and more preferably 40% or more, of the entire cross-sectional area of ​​the porous film. Furthermore, it is preferable that each of the plurality of extracted analysis regions is extracted from a non-overlapping area in the cross-section of the porous film. When the extraction conditions for the plurality of analysis regions satisfy the above-mentioned preferable conditions, the overall aspect of the porous film can be suitably evaluated.

[0030] With reference to FIG. 1, the process of repeating the operation of expanding the void region in the step (8a), that is, the process of expanding the void region stepwise, will be described. FIG. 1 is a schematic diagram showing the process of expanding the void region stepwise. Here, the analysis region obtained in step (7a) and subjected to binarization corresponds to the image represented by the 0th generation in FIG. 1. Moreover, the analysis region after the operation of expanding the void region is repeated n times corresponds to the image represented by the nth generation in FIG. 1. The regions other than the void region 1, such as region A and region B, in FIG. 1 are the resin region. As shown in FIG. 1, as n in the nth generation increases, the resin region, for example, region A and region B, shrinks. Therefore, it can be seen that the resin region eventually disappears as n increases. And, n when the resin region finally disappears is defined as the number of required stages in this specification. In FIG. 1, the image represented by the 19th generation has the resin region remaining on the outside. On the other hand, when the resin part region finally disappears, the entire analysis region is occupied by the void region 1, that is, the image shown in Fig. 1 is occupied by black color representing the void region 1. The number of steps required for the entire analysis region to be occupied by the void region is defined as the required number of steps.

[0031] In the separator according to one embodiment of the present invention, the required number of steps is as small as 20 or less. The required number of steps is a parameter that represents the distance between adjacent voids in the entire porous film, and when the required number of steps is small, the distance between adjacent voids is small. Therefore, the required number of steps being small means that the voids are distributed uniformly and densely in the entire porous film.

[0032] In a non-aqueous electrolyte secondary battery, pressure is applied vertically from above to the surfaces of the separator and the porous film constituting the separator due to the expansion of an electrode (e.g., a negative electrode). A porous film having pores distributed uniformly and densely has high strength of the pores themselves, and the pressure is not concentrated at one point, so that the pores are unlikely to deform or close due to the pressure. Therefore, the separator according to one embodiment of the present invention has the required number of stages of 20 or less, and includes a porous film having pores distributed uniformly and densely, thereby achieving the effect that the pores are unlikely to close even after compression, and good ion permeability can be maintained.

[0033] From the viewpoint of maintaining good ion permeability even after the above-mentioned compression, the required number of stages is preferably small. Specifically, the upper limit of the required number of stages is preferably 19 or less, more preferably 18 or less. The lower limit of the required number of stages is usually 10 or more, preferably 12 or more.

[0034] The porous film contains polyolefin resin, and generally is a porous film mainly composed of polyolefin resin. "Mainly composed of polyolefin resin" means that the ratio of polyolefin resin in the porous film is 50% by volume or more, preferably 90% by volume or more, more preferably 95% by volume or more of the total material constituting the porous film.

[0035] The porous film has a large number of interconnected pores inside, allowing gas or liquid to pass from one side to the other. The pores are synonymous with the voids.

[0036] The AC resistance of the porous film is 3.5 Ω cm 2 Preferably, it is 3.4 Ω cm or less. 2 It is more preferable that the AC resistance of the porous film is 3.5 Ω cm or less. 2If the lower limit is less than 0.1 Ω cm, the pores formed by the resin have excellent interconnectivity in the thickness direction, and the number of paths for Li ions increases, so that an increase in air permeability after compression can be suppressed. 2 The AC resistance of the porous film may be 0.1 Ω cm or more. 2 More than 3.5Ω cm 2 It may be the following.

[0037] The thickness of the porous film is 4 to 40 μm, and preferably 5 to 20 μm. If the thickness of the porous film is 4 μm or more, internal short circuit of the battery can be sufficiently prevented. On the other hand, if the thickness of the porous film is 40 μm or less, the nonaqueous electrolyte secondary battery can be prevented from becoming large.

[0038] The polyolefin resin has a weight average molecular weight of 5×10 5 ~15×10 6 It is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more. In particular, it is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more, since the strength of the obtained porous film and the separator containing the porous film is improved.

[0039] The polyolefin resin is not particularly limited, and examples thereof include thermoplastic resins such as homopolymers or copolymers obtained by polymerizing monomers such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, and 1-hexene. Examples of the homopolymers include polyethylene, polypropylene, and polybutene. Examples of the copolymers include ethylene-propylene copolymers.

[0040] Among these, polyethylene is more preferred because it can prevent excessive current from flowing through the separator at a lower temperature. The prevention of excessive current from flowing is also called shutdown. Examples of the polyethylene include low-density polyethylene, high-density polyethylene, linear polyethylene (ethylene-α-olefin copolymer), and ultra-high molecular weight polyethylene having a weight-average molecular weight of 1 million or more. Among these, ultra-high molecular weight polyethylene having a weight-average molecular weight of 1 million or more is more preferred.

[0041] The weight per unit area of ​​the porous film, i.e., the weight per unit area, is usually 4 to 20 g / m2 so as to increase the weight energy density and volume energy density of the battery. 2 is preferably 5 to 12 g / m 2 It is more preferable that:

[0042] From the viewpoint of exhibiting sufficient ion permeability, the air permeability of the porous film is preferably 110 to 200 sec / 100 mL, and more preferably 110 to 190 sec / 100 mL, in terms of Gurley value.

[0043] The porosity of the porous film is preferably 20% by volume to 80% by volume, and more preferably 30% by volume to increase the amount of electrolyte retained and to provide the function of reliably preventing (shutting down) the flow of excessive current at a lower temperature.

[0044] Furthermore, from the viewpoint that the porous film and the separator containing the porous film have better ion permeability after compression, the porosity of the porous film is more preferably 35 volume % or more, and particularly preferably 50 volume % or more.

[0045] The pore size of the pores in the porous film is preferably 0.3 μm or less, and more preferably 0.14 μm or less, from the viewpoints of sufficient ion permeability and preventing the intrusion of particles constituting the electrode.

[0046] <Method of manufacturing porous film> The method for producing the porous film according to an embodiment of the present invention is not particularly limited, and specifically includes, for example, a method including the steps (A) to (D) shown below: (A) a step of adding a polyolefin resin and, optionally, a pore-forming agent to a kneader and melt-kneading them to obtain a polyolefin resin composition; (B) A step of stretching the obtained polyolefin resin composition in the MD direction while cooling it, and forming it into a sheet to obtain a primary sheet; (C) stretching the obtained primary sheet in the TD direction; (D) A process in which the primary sheet stretched in the TD direction is heat-treated at a specific temperature for a specific time to perform heat setting, thereby obtaining a porous film.

[0047] In step (A), the amount of the polyolefin resin used is preferably 6 wt % to 45 wt %, and more preferably 9 wt % to 36 wt %, based on 100 wt % of the weight of the resulting polyolefin resin composition.

[0048] The pore-forming agent is not particularly limited, and examples thereof include inorganic fillers and plasticizers. The inorganic fillers are not particularly limited, and examples thereof include inorganic fillers, specifically calcium carbonate. The plasticizers are not particularly limited, and examples thereof include low molecular weight hydrocarbons such as liquid paraffin.

[0049] In addition to the pore-forming agent, the additives may include any known additives within the scope of the present invention, provided that the effects of the present invention are not impaired. Examples of the known additives include antioxidants, fillers, and dispersion aids. Examples of the fillers include alumina.

[0050] In the step (B), the method for obtaining the primary sheet is not particularly limited, and the primary sheet can be produced by a sheet forming method such as inflation processing, calendar processing, T-die extrusion processing, or skiff method.

[0051] For example, the sheet molding temperature in the sheet molding method, such as the T-die extrusion temperature in the T-die extrusion process, is preferably 200°C or higher and 280°C or lower, and more preferably 220°C or higher and 260°C or lower.

[0052] The stretching temperature in step (B) is preferably 120°C or higher and 160°C or lower, and more preferably 130°C or higher and 155°C or lower.

[0053] In the step (B), the polyolefin resin composition can be cooled by contacting it with a cooling medium such as cold air or cooling water, by contacting it with a cooling roll, etc. The cooling method is preferably the method of contacting it with a cooling roll.

[0054] When the polyolefin resin composition and the primary sheet contain a pore-forming agent, the method includes a step of washing the primary sheet or the stretched primary sheet with a washing liquid to remove the pore-forming agent between steps (B) and (C) or after step (C).

[0055] The cleaning liquid is not particularly limited as long as it is a solvent capable of removing the pore-forming agent, and examples of the cleaning liquid include an aqueous hydrochloric acid solution, heptane, and dichloromethane.

[0056] The stretching temperature in the TD stretching in step (C) is preferably 80° C. or more and 120° C. or less, and more preferably 80° C. or more and 115° C. or less. The stretching ratio in the TD stretching in step (C) is preferably 2 times or more and 12 times or less, and more preferably 4 times or more and 10 times or less.

[0057] In step (C), the upper limit of the stretching speed in the TD direction is preferably 12 m / min or less, more preferably 10 m / min or less. The lower limit of the stretching speed is preferably 0.5 m / min or more, more preferably 1 m / min or more. By stretching at a stretching speed within the above range, the primary sheet is more likely to be stretched uniformly during stretching, and anisotropy is less likely to occur in the pores, so that a porous film in which pores are distributed more uniformly and more densely can be produced.

[0058] The heat setting in the step (D) is preferably performed at a temperature of 110° C. or more and 140° C. or less, more preferably 115° C. or more and 135° C. or less. The heat setting is preferably performed for a time period of 20 seconds or more and less than 20 minutes, more preferably 21 seconds or more and 15 minutes or less. By performing the heat setting for a long time period of 20 seconds or more in the step (D), a porous film in which voids are distributed more uniformly and more densely can be produced.

[0059] In the present invention, the required number of steps can be controlled to a preferred range of 20 or less by controlling the stretching speed in the TD stretching in the step (C) to a preferred range of 12 m / min or less and controlling the heat setting time in the step (D) to a preferred range of 20 seconds or more. In addition, the AC resistance of the separator can be controlled to 3.5 Ω cm by the above control method. 2 It can be controlled within the following preferred ranges. From the viewpoint of controlling the required number of stages and the AC resistance of the separator within the preferred ranges, it is preferable not to perform a relaxation operation in the MD direction in the stretching step before heat setting. The relaxation operation bends the fibrils that form the pores, making the pores more likely to become non-uniform, and therefore the required number of stages of the separator is likely to increase. In addition, the relaxation operation increases the probability that the resin components overlap in the film thickness direction, and the interconnectivity of the pores decreases, reducing the number of paths for Li ions, which tends to increase the AC resistance of the separator.

[0060] <Insulating porous layer> When the separator according to one embodiment of the present invention is a laminated separator, it preferably includes the porous film and an insulating porous layer laminated on the porous film.

[0061] The insulating porous layer is usually a resin layer containing a resin, and is preferably a heat-resistant layer or an adhesive layer. The resin constituting the insulating porous layer is preferably insoluble in the electrolyte of the battery and is electrochemically stable within the range of use of the battery. In the following, the insulating porous layer is also simply referred to as a "porous layer."

[0062] The porous layer is laminated on one or both sides of the porous film as necessary. When the porous layer is laminated on one side of the porous film, the porous layer is preferably laminated on the surface of the porous film facing the positive electrode when the porous film is used as a nonaqueous electrolyte secondary battery, and more preferably on the surface in contact with the positive electrode.

[0063] It is preferable that the resin is insoluble in the electrolyte of the battery and is electrochemically stable within the range of use of the battery.

[0064] Specific examples of the resin include polyolefins; (meth)acrylate resins; fluorine-containing resins; polyamide resins; polyimide resins; polyester resins; rubbers; resins having a melting point or glass transition temperature of 180°C or higher; water-soluble polymers; polycarbonate, polyacetal, polyether ether ketone, and the like.

[0065] Of the above-mentioned resins, polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins and water-soluble polymers are preferred.

[0066] The polyolefin is preferably polyethylene, polypropylene, polybutene, an ethylene-propylene copolymer, or the like.

[0067] Examples of the fluorine-containing resin include polyvinylidene fluoride (PVDF), polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, and the like, and among the fluorine-containing resins, fluorine-containing rubbers having a glass transition temperature of 23° C. or lower can be mentioned.

[0068] As the polyamide-based resin, aramid resins such as aromatic polyamides and wholly aromatic polyamides are preferable.

[0069] Specific examples of the aramid resin include poly(paraphenylene terephthalamide), poly(metaphenylene isophthalamide), poly(parabenzamide), poly(metabenzamide), poly(4,4'-benzanilide terephthalamide), poly(paraphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(metaphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(paraphenylene-2,6-naphthalene dicarboxylic acid amide), poly(metaphenylene-2,6-naphthalene dicarboxylic acid amide), poly(2-chloroparaphenylene terephthalamide), paraphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, metaphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, etc. Among these, poly(paraphenylene terephthalamide) is more preferable.

[0070] As the polyester-based resin, aromatic polyesters such as polyarylates and liquid crystal polyesters are preferred.

[0071] Examples of the rubbers include styrene-butadiene copolymers and hydrogenated products thereof, methacrylic acid ester copolymers, acrylonitrile-acrylic acid ester copolymers, styrene-acrylic acid ester copolymers, ethylene propylene rubber, and polyvinyl acetate.

[0072] Examples of the resin having a melting point or glass transition temperature of 180° C. or higher include polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, and polyetheramide.

[0073] Examples of the water-soluble polymer include polyvinyl alcohol, polyethylene glycol, cellulose ether, sodium alginate, polyacrylic acid, polyacrylamide, and polymethacrylic acid.

[0074] The resin used in the porous layer may be of one type alone or of two or more types in combination.

[0075] The porous layer may contain fine particles. In this specification, fine particles refer to organic fine particles or inorganic fine particles generally called fillers. Therefore, when the porous layer contains fine particles, the resin contained in the porous layer functions as a binder resin that binds the fine particles together and the fine particles and the porous film. In addition, the fine particles are preferably insulating fine particles.

[0076] The organic fine particles contained in the porous layer include fine particles made of resin. Specific examples of the inorganic fine particles contained in the porous layer include fillers made of inorganic substances such as calcium carbonate, talc, clay, kaolin, silica, hydrotalcite, diatomaceous earth, magnesium carbonate, barium carbonate, calcium sulfate, magnesium sulfate, barium sulfate, aluminum hydroxide, boehmite, magnesium hydroxide, calcium oxide, magnesium oxide, titanium oxide, titanium nitride, alumina (aluminum oxide), aluminum nitride, mica, zeolite, and glass. These inorganic fine particles are insulating fine particles. The fine particles may be used alone or in combination of two or more kinds.

[0077] Among the above-mentioned fine particles, fine particles made of an inorganic substance are preferred, and fine particles made of an inorganic oxide such as silica, calcium oxide, magnesium oxide, titanium oxide, alumina, mica, zeolite, aluminum hydroxide, or boehmite are more preferred, and fine particles of at least one type selected from the group consisting of silica, magnesium oxide, titanium oxide, aluminum hydroxide, boehmite, and alumina are even more preferred, with alumina being particularly preferred.

[0078] The content of the fine particles in the porous layer is preferably 1 to 99% by volume of the porous layer, and more preferably 5 to 95% by volume. By setting the content of the fine particles in the above range, the voids formed by the contact between the fine particles are less likely to be blocked by resin or the like. Therefore, sufficient ion permeability can be obtained, and the basis weight per unit area can be set to an appropriate value.

[0079] The fine particles may be used in combination of two or more types having different particle diameters or specific surface areas.

[0080] The thickness of the porous layer is preferably 0.5 to 15 μm per layer, more preferably 2 to 10 μm. If the thickness of the porous layer is 0.5 μm or more per layer, internal short circuit due to damage to the nonaqueous electrolyte secondary battery can be sufficiently suppressed, and the amount of electrolyte held in the porous layer is sufficient. On the other hand, if the thickness of the porous layer is 15 μm or less per layer, deterioration of rate characteristics or cycle characteristics can be suppressed.

[0081] The weight per unit area of ​​the porous layer, i.e., the basis weight per layer, is 1 to 20 g / m 2 It is preferable that the thickness is 4 to 10 g / m 2 It is more preferable that:

[0082] The volume of the porous layer constituents contained in one square meter of the porous layer is 0.5 to 20 cm per layer. 3 It is preferable that the thickness is 1 to 10 cm. 3 More preferably, it is 2 to 7 cm. 3 It is even more preferable that:

[0083] The porosity of the porous layer is preferably 20 to 90% by volume, more preferably 30 to 80% by volume, so that sufficient ion permeability can be obtained. Also, the pore size of the pores in the porous layer is preferably 3 μm or less, more preferably 1 μm or less, so that sufficient ion permeability can be obtained in the laminated separator.

[0084] <Laminated separator> The separator according to one embodiment of the present invention may be a laminated separator.

[0085] The thickness of the laminated separator is preferably 5.5 μm to 45 μm, and more preferably 6 μm to 25 μm.

[0086] The laminated separator preferably has an air permeability of 100 to 350 sec / 100 mL in Gurley value, and more preferably 100 to 300 sec / 100 mL.

[0087] The separator according to an embodiment of the present invention may include another porous layer other than the porous film and the porous layer, if necessary, within a range that does not impair the object of the present invention. Examples of the other porous layer include known porous layers such as a heat-resistant layer, an adhesive layer, and a protective layer.

[0088] The other porous layer may be provided on one or both sides of the laminate separator. When the laminate separator has an insulating porous layer on both sides of a porous film, the other porous layer may be provided on the insulating porous layer on both sides, or on the insulating porous layer on one side. When the laminate separator has an insulating porous layer on only one side of a porous film, the other porous layer may be provided on the insulating porous layer, or on the side of the porous film where the insulating porous layer is not provided. It can also be said that the other porous layer may be provided on the outermost layer of the laminate separator.

[0089] For example, the laminated separator further includes an adhesive layer in addition to the insulating porous layer. In this specification, the adhesive layer means a porous layer having adhesive properties. The adhesive layer may be provided on the surface of the laminated separator that contacts the electrode. Examples of components that contribute to adhesive properties contained in the adhesive layer include acrylic resin, PVDF, etc.

[0090] <Method of manufacturing porous layer and laminated separator> An example of a method for producing the insulating porous layer in one embodiment of the present invention and the laminated separator in one embodiment of the present invention is a method in which a coating liquid containing the resin contained in the porous layer is applied to one or both sides of the porous film and dried to precipitate the porous layer.

[0091] In addition, when a porous layer is deposited on both sides of the porous film, (a) the porous layer may be deposited simultaneously on both sides of the porous film, or (b) the coating liquid may be applied to one side of the porous film and dried to deposit a porous layer on one side of the porous film, and then the coating liquid may be applied to the other side of the porous film and dried to deposit a porous layer on the other side of the porous film.

[0092] Furthermore, before the coating liquid is applied to one or both sides of the porous film, the one or both sides of the porous film to be coated with the coating liquid may be subjected to a hydrophilization treatment, if necessary.

[0093] The coating liquid contains the resin contained in the porous layer. The coating liquid may also contain the fine particles described below that may be contained in the porous layer. The coating liquid may usually be prepared by dissolving the resin that may be contained in the porous layer in a solvent and dispersing the fine particles in the solvent. Here, the solvent that dissolves the resin also serves as a dispersion medium that disperses the fine particles. The resin may also be made into an emulsion by the solvent.

[0094] The solvent is not particularly limited as long as it does not adversely affect the porous film, dissolves the resin uniformly and stably, and disperses the fine particles uniformly and stably.Specific examples of the solvent include water and organic solvents.The solvent may be used alone or in combination of two or more.

[0095] The coating liquid may be formed by any method as long as it satisfies the conditions such as the resin solid content (resin concentration) and the amount of fine particles required to obtain a desired porous layer. Specific examples of the method for forming the coating liquid include mechanical stirring, ultrasonic dispersion, high pressure dispersion, and media dispersion. The coating liquid may also contain additives such as dispersants, plasticizers, surfactants, and pH adjusters as components other than the resin and fine particles, as long as the object of the present invention is not impaired. The amount of additives added may be within a range that does not impair the object of the present invention.

[0096] The method of applying the coating liquid to the porous film, that is, the method of forming a porous layer on the surface of the porous film, is not particularly limited.The method of forming the porous layer can be, for example, the method of applying the coating liquid directly to the surface of the porous film, and then removing the solvent; the method of applying the coating liquid to a suitable support, removing the solvent to form a porous layer, and then pressing the porous layer and the porous film, and then peeling off the support; the method of applying the coating liquid to a suitable support, pressing the porous film on the coating surface, and then peeling off the support, and then removing the solvent.

[0097] The coating liquid can be applied by a conventionally known method, and specific examples thereof include a gravure coater method, a dip coater method, a bar coater method, and a die coater method.

[0098] The solvent is generally removed by drying, or the solvent contained in the coating liquid may be replaced with another solvent before drying.

[0099] [Embodiment 2: Nonaqueous electrolyte secondary battery member, Embodiment 3: Nonaqueous electrolyte secondary battery] The member for a nonaqueous electrolyte secondary battery according to the second embodiment of the present invention comprises a positive electrode, the separator for a nonaqueous electrolyte secondary battery according to the first embodiment of the present invention, and a negative electrode arranged in this order.

[0100] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention includes the separator for nonaqueous electrolyte secondary batteries according to the first embodiment of the present invention.

[0101] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention is, for example, a nonaqueous secondary battery that obtains electromotive force by doping and dedoping lithium, and may include a nonaqueous electrolyte secondary battery member in which a positive electrode, the separator according to the first embodiment of the present invention, and a negative electrode are laminated in this order. Note that the components of the nonaqueous electrolyte secondary battery other than the separator are not limited to the components described below.

[0102] The nonaqueous electrolyte secondary battery according to the third embodiment of the present invention usually has a structure in which a battery element in which a negative electrode and a positive electrode are opposed to each other through the separator according to the first embodiment of the present invention and an electrolyte is impregnated in the structure is sealed in an exterior material. The nonaqueous electrolyte secondary battery is preferably a lithium ion secondary battery. Note that the term "doping" refers to occlusion, support, adsorption, or insertion, and refers to a phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.

[0103] A nonaqueous electrolyte secondary battery member according to embodiment 2 of the present invention includes the separator according to embodiment 1 of the present invention. Thus, the nonaqueous electrolyte secondary battery member has an effect of suppressing deterioration of battery performance caused by internal pressure during repeated charging and discharging in a nonaqueous electrolyte secondary battery. A nonaqueous electrolyte secondary battery according to embodiment 3 of the present invention includes the separator according to embodiment 1 of the present invention. Thus, the nonaqueous electrolyte secondary battery has an effect of suppressing deterioration of battery performance caused by internal pressure during repeated charging and discharging.

[0104] <Positive electrode> The positive electrode in the nonaqueous electrolyte secondary battery member and the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is generally used as a positive electrode in a nonaqueous electrolyte secondary battery, and for example, a positive electrode sheet having a structure in which an active material layer containing a positive electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.

[0105] The positive electrode active material may be, for example, a material capable of doping and dedoping lithium ions, specifically, a lithium composite oxide containing at least one transition metal such as V, Mn, Fe, Co, or Ni.

[0106] Examples of the conductive agent include carbonaceous materials such as natural graphite, artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, and organic polymer compound sintered bodies. The conductive agent may be used alone or in combination of two or more kinds.

[0107] Examples of the binder include fluorine-based resins such as polyvinylidene fluoride, acrylic resins, and styrene-butadiene rubber. The binder also functions as a thickener.

[0108] Examples of the positive electrode current collector include conductors such as Al, Ni, stainless steel, etc. Among these, Al is more preferable because it is easy to process into a thin film and is inexpensive.

[0109] Examples of methods for producing a sheet-shaped positive electrode include a method of pressurizing and molding a positive electrode active material, a conductive agent, and a binder on a positive electrode current collector; a method of forming a paste of a positive electrode active material, a conductive agent, and a binder using an appropriate organic solvent, applying the paste to a positive electrode current collector, drying the paste, and then pressing the paste to adhere it to the positive electrode current collector; and the like.

[0110] <Negative electrode> The negative electrode in the nonaqueous electrolyte secondary battery member and the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is generally used as a negative electrode in a nonaqueous electrolyte secondary battery, and for example, a negative electrode sheet having a structure in which an active material layer containing a negative electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.

[0111] Examples of the negative electrode active material include materials capable of doping and dedoping lithium ions, lithium metal, lithium alloys, etc. Examples of the material include carbonaceous materials, etc. Examples of the carbonaceous materials include natural graphite, artificial graphite, cokes, carbon black, and pyrolytic carbons, etc.

[0112] Examples of the negative electrode current collector include Cu, Ni, stainless steel, etc. Among them, Cu is more preferable because it is difficult to form an alloy with lithium in a lithium ion secondary battery and it is easy to process into a thin film.

[0113] Examples of methods for producing a sheet-shaped negative electrode include a method of pressurizing a negative electrode active material on a negative electrode current collector, a method of forming a paste of a negative electrode active material using an appropriate organic solvent, applying the paste to a negative electrode current collector, drying, and then pressing to fix the paste to the negative electrode current collector, etc. The paste preferably contains the conductive agent and the binder.

[0114] <Nonaqueous electrolyte> The nonaqueous electrolyte in the nonaqueous electrolyte secondary battery according to one embodiment of the present invention is not particularly limited as long as it is a nonaqueous electrolyte generally used in nonaqueous electrolyte secondary batteries, and for example, a nonaqueous electrolyte obtained by dissolving a lithium salt in an organic solvent can be used. Examples of the lithium salt include LiClO4, LiPF6, LiAsF6, LiSbF6, LiBF4, LiCF3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, Li2B 10 Cl 10 , lithium salts of lower aliphatic carboxylates, LiAlCl4, etc. The lithium salts may be used alone or in combination of two or more.

[0115] Examples of the organic solvent constituting the nonaqueous electrolyte include carbonates, ethers, esters, nitriles, amides, carbamates, sulfur-containing compounds, and fluorine-containing organic solvents obtained by introducing a fluorine group into these organic solvents. The organic solvent may be used alone or in combination of two or more kinds.

[0116] [summary] One embodiment of the present invention may include the following inventions [1] to [7]. [1] A separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, the separator comprising: a two-dimensional image of 960 pixels in the film thickness direction and 1280 pixels in the MD direction, obtained from a cross section of the polyolefin porous film using a scanning electron microscope under conditions of a magnification of 5000 times and 1 pixel of 19.8 μm × 19.8 μm; the image is binarized into a void region and a resin region to obtain a binarized image; and the binarized image is then subjected to a process of gradually expanding the void region. When the process requires 20 or fewer steps until the resin region is completely filled with the expanded void region, the stepwise expansion process is a process of repeatedly expanding each target pixel constituting the void region by one pixel in the pixel directions adjacent to the four sides of each target pixel per step; A separator for a non-aqueous electrolyte secondary battery, characterized in that a process for expanding the void region in stages is carried out and the required number of stages is calculated using any of the following methods (1) to (9). (1) An analysis region of 100 pixels in the thickness direction × 1280 pixels in the MD direction is extracted from the two-dimensional image. (2) An adaptive histogram equalization process of the luminance values ​​is performed on the analysis region extracted in (1). (3) The analysis region, whose brightness values ​​have been subjected to adaptive histogram equalization processing in (2), is subjected to brightness value inversion processing. (4) All pixels constituting the analysis area whose brightness values ​​have been inverted in (3) are divided into pixels whose brightness values ​​are equal to or less than a threshold value of 180 within the brightness range of 0 to 255 and pixels whose brightness values ​​exceed the threshold value of 180, and binarized. (5) In the analysis region binarized in (4), a region consisting of pixels whose brightness value exceeds a threshold value of 180 is identified as a void region. (6) For each of the void regions identified in (5) in the analysis region, an operation is performed to expand four neighboring pixels constituting the boundary of each void region outward by one pixel. (7) The area other than the void area after the expansion operation in (6) is regarded as a resin area, and the resin area is subjected to blob processing to count the number of pixels constituting the resin area. The number of pixels thus counted is regarded as the number of resin areas. Then, it is confirmed whether the number of resin areas thus counted is 0. (8) If the number of resin part areas measured in (7) is 0, the process of calculating the required number of stages is terminated. If the number of resin part areas is not 0, the processes described in (6) and (7) are repeated until the number of resin part areas becomes 0, and the process of calculating the required number of stages is terminated at the point when the number of resin part areas becomes 0. (9) In (8), the number of times the processes described in (6) and (7) are repeated until the process of calculating the required number of stages is completed is calculated, and the calculated number is set as the required number of stages. [2] The separator for a nonaqueous electrolyte secondary battery according to [1], further comprising an insulating porous layer containing a resin. [3] The separator for a non-aqueous electrolyte secondary battery according to [2], wherein the resin is at least one selected from the group consisting of polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins, and water-soluble polymers. [4] The separator for a nonaqueous electrolyte secondary battery according to [2] or [3], wherein the resin is an aramid resin. [5] The separator for a nonaqueous electrolyte secondary battery according to any one of [2] to [4], further comprising an adhesive layer in addition to the insulating porous layer. [6] A member for a non-aqueous electrolyte secondary battery, comprising a positive electrode, the separator for a non-aqueous electrolyte secondary battery according to any one of [1] to [5], and a negative electrode, arranged in this order.[7] [7] A non-aqueous electrolyte secondary battery comprising the separator for a non-aqueous electrolyte secondary battery according to any one of [1] to [5].

[0117] The scope of the nonaqueous electrolyte secondary battery separator, nonaqueous electrolyte secondary battery member, and nonaqueous electrolyte secondary battery according to one embodiment of the present invention may include any combination of the features described in the above-mentioned configurations within the scope of the claims. EXAMPLES

[0118] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0119] [Measurement method] The physical properties of the separators produced in Examples 1 to 4 and Comparative Examples 1 and 2 were measured by the following methods.

[0120] (Film thickness) The thickness of the separator was measured using a high-precision digital length measuring instrument (VL-50) manufactured by Mitutoyo Corporation.

[0121] (porosity) (a) Film thickness measurement The thickness of the separator was measured by the method described above in the section (Thickness). (b) Measurement of basis weight A square sample with a side length of 8 cm was cut from the separator, and the weight W (g) of the sample was measured. Then, the weight per unit area of ​​the separator was calculated according to the following formula (1).

[0122] Weight per unit area (g / m 2 )=W / (0.08×0.08) (1) (c) Measurement of true density The separator was cut into 4 mm to 6 mm squares and vacuum dried at 30° C. or less for 17 hours, after which the true density of the separator was measured by a helium gas substitution method using a dry automatic densitometer (AccuPyeII 1340 manufactured by Micromeritics). (d) Calculation of void ratio The thickness [μm] and weight [g / m2] of the separator calculated and measured in the above steps (a) to (c) 2 ] and true density [g / m 3 ], the porosity [%] of the separator was calculated based on the following formula (2).

[0123] (Porosity) = [1-(weight per unit area) / {(film thickness) x 10 -6 ×1[m 2 ]×(true density)}]×100 (2) (number average branch number) The number average branch number of polyethylene, which is a polyolefin resin used in the examples and comparative examples, was calculated by the method shown in steps 1 to 4 below. Step 1: A standard sample was prepared, which was made of the same type of polyolefin constituting the polyolefin resin as above, and which was made of a linear polyolefin with no branching. Step 2: For the standard samples prepared in step 1, conformation plots based on GPC-MALS were generated using DAWN HELEOS II. Step 3: Using the same method as in step 2, a conformation plot was created based on GPC-MALS for the polyolefin resin. Step 4: From the conformation plots prepared in steps 2 and 3, the number average branch number of the polyolefin resin was calculated according to the following formula.

[0124]

number

[0125] (In the formula, R gL is the radius of gyration of the linear polyolefin resin, and Rgb is the radius of gyration of the branched polyolefin resin, and g is the radius of gyration of the branched polyolefin resin at the same molecular weight (R gL / R gb ) 2 is the value of B n is the number of branches in a single chain.) (AC resistance) The separator obtained in the example or comparative example was cut to obtain 23 disk-shaped separator pieces with a diameter of 17 mm. Five of the separator pieces were stacked to prepare a separator A for coin cells. Eight of the separator pieces were stacked to prepare a separator B for coin cells. Ten of the separator pieces were stacked to prepare a separator C for coin cells. Each of the separators A to C for coin cells was sandwiched between two stainless steel (SUS) plate electrodes with a thickness of 0.5 mm and a diameter of 15.5 mm, and an electrolyte was poured to prepare coin cells (CR2032 type) A to C. As the electrolyte, a solution was used in which LiPF6 was dissolved in a mixed solvent of ethylene carbonate / ethyl methyl carbonate / diethyl carbonate = 3 / 5 / 2 (volume ratio) so that the concentration of the LiPF6 was 0.1 mol / L. Next, for each of the coin cells A to C, an AC impedance measurement was performed using an AC impedance device (FRA11255B) manufactured by Solartron under conditions of a frequency of 1 MHz to 0.1 Hz and an amplitude of 10 mV, to obtain three types of Nyquist plots. From the values ​​of the X-intercepts of the three types of Nyquist plots, the liquid resistance of each of the laminates in which 5, 8, and 10 separator pieces were stacked, i.e., coin cell separators A to C, was calculated. The liquid resistance (Ω / piece) per separator piece was calculated from the slope when the liquid resistance value of the coin cell separator was plotted against the number of separator pieces constituting the coin cell separator. The liquid resistance per separator piece was calculated based on the electrode area (1.89 cm 2 ) to obtain the AC resistance (Ω cm 2 ) was calculated.

[0126] (Number of stages required) <Acquisition of cross-sectional SEM images> The cross section of the separator was observed using an SEM according to the procedures (i) to (iii) below. (i) The separator was subjected to ion milling using a cross-sectional specimen preparation device IB-19520 manufactured by JEOL Ltd. to cut the separator to form a cross section. This cross section was obtained by cutting the separator along a straight line passing through the center of the separator and parallel to the MD in a direction perpendicular to the surface. (ii) Osmium was evaporated onto the cross section formed in (i) to form an evaporated film on the cross section. (iii) A scanning electron microscope (S-4800, Hitachi High-Tech Corporation) was used to observe the cross section on which the deposition film was formed in (ii) at a magnification of 5000 times to obtain a backscattered electron image of the cross section (film thickness direction: 960 pixels × MD direction: 1280 pixels). The observation conditions were an acceleration voltage of 0.8 kV and a working distance of 3.0 mm. In the SEM image, 1 pixel was equivalent to 19.8 μm × 19.8 μm.

[0127] <Calculating the number of stages required> According to the procedures 1. to 9. below, image analysis of the SEM image of the cross section was performed to calculate the number of steps required. 1. Using Python, the image data file (JPEG file) of the SEM image of the cross section was read. An analysis area of ​​100 pixels in the thickness direction × 1280 pixels in the MD direction was extracted from the image data read in 2.1. At this time, the analysis area was extracted so that the entire cross-sectional area of ​​the separator (porous film) was included in the analysis area. 3. Adaptive histogram equalization of brightness values ​​was performed on the analysis area extracted in 2. 4. In order to accurately identify voids during binarization, the analysis area in which the adaptive histogram equalization of brightness values ​​was performed in step 3 was subjected to an inversion process of brightness values. The analysis region in which the brightness values ​​were inverted in 5.4 was binarized using a threshold condition of 180. That is, all pixels constituting the analysis region were divided into pixels whose brightness values ​​were equal to or less than the threshold value of 180 within the brightness value range of 0 to 255, and pixels whose brightness values ​​were greater than the threshold value of 180. In the analysis region binarized in 6.5, a region consisting of pixels whose brightness value exceeds a threshold value of 180 was identified as a void region. For each of the identified void regions, an operation was performed in which the four neighboring pixels constituting the outer boundary of each void region were expanded outward by one pixel, in other words, an operation was performed in which each target pixel constituting the void region was expanded by one pixel in the direction of the pixels adjacent to the four sides of each target pixel. 7. The area other than the void area was determined as the resin area. Then, the resin area was subjected to blob processing, and the number of pixels constituting the resin area was counted. The number of pixels measured was determined as the number of resin areas. Then, it was confirmed whether the number of measured resin areas was 0 or not. 8. If the number of resin areas measured in 7. was 0, the image analysis of the SEM image was terminated. If the number of resin areas was not 0, the processes described in 6. and 7. were repeated until the number of resin areas became 0, and the image analysis was terminated when the number of resin areas became 0. In 9.8., the number of times the processes described in 6. and 7. were repeated until the image analysis was completed was calculated and defined as the number of required steps.

[0128] In addition, the adaptive histogram processing of the luminance values ​​described in 3 was specifically carried out according to the following procedure. (i) Divide the image data into partial regions of 8 pixels vertically by 8 pixels horizontally (corresponding to "adaptive"). (ii) For each partial region obtained in (i), the image histogram is expanded to the entire range (0 to 255, since 1 pixel is 8 bits) using the open source OpenCV: cv::CLAHE Class Reference (this is equivalent to "histogram equalization").

[0129] In addition, since the histogram equalization process described in (ii) is automatically performed by the open source, the required number of steps can be calculated uniquely by the above procedure.

[0130] (Difference in air permeability / film thickness before and after compression at 20 MPa) The difference in air permeability / film thickness of the separator before and after compression at 20 MPa was measured by the methods shown in steps 1 to 5 below. Step 1: A 6 cm x 6 cm square sample was cut from the separator. Step 2: The air permeability of the sample cut out in step 1 was measured in accordance with JIS P8117. The measured air permeability was taken as the air permeability of the separator when uncompressed: AP1 (unit: sec / 100 mL). In addition, the membrane thickness of the separator was measured using a high-precision digital length measuring machine (VL-50) manufactured by Mitutoyo Corporation. The measured membrane thickness was taken as the membrane thickness of the separator when uncompressed: t1 (unit: μm). Step 3: The sample cut out in step 1 was sandwiched between aluminum plates and pressed using a hydraulic compression molding machine (AH-1T, low-load heat press, manufactured by AS ONE Corporation). The pressing conditions were 20 MPa, 35°C, and 5 minutes. Step 4: For the sample pressed in step 3, the air permeability and film thickness were measured in the same manner as in step 2. The measured air permeability and film thickness were defined as the air permeability AP2 (unit: sec / 100 mL) and film thickness t2 (unit: μm) of the separator after compression, respectively. Step 5: Using AP1, AP2, t1, and t2 obtained in steps 2 and 4, the difference in air permeability / film thickness of the separator before and after compression at 20 MPa was calculated according to the following formula (3).

[0131] (Difference in air permeability / film thickness before and after compression at 20 MPa) (unit: sec / 100 mL / μm) = {(AP2) / (t2)}-{(AP1) / (t1)} (3) [Example 1] 27.4 parts by weight of ultra-high molecular weight polyethylene powder (intrinsic viscosity: 21 dL / g, viscosity average molecular weight: 3 million, number average branch number: 0.1, manufactured by Tosoh Corporation), 6.9 parts by weight of polyethylene wax (Excelex 40800, manufactured by Mitsui Chemicals, Inc.) having a weight average molecular weight of 4000, and 3.0 parts by weight of alumina (product name AEROXIDE Alu65, manufactured by Nippon Aerosil Co., Ltd.) were prepared. The total of the ultra-high molecular weight polyethylene, polyethylene wax, and alumina was 100 parts by weight, and 0.3 parts by weight of antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of antioxidant (IRGAFOS 168, manufactured by BASF), 0.4 parts by weight of sodium stearate, and 0.6 parts by weight of dispersing aid (BYK-MAX P4102, manufactured by BYK) were added. Further, calcium carbonate (manufactured by Maruo Calcium Co., Ltd.) having an average particle size of 0.07 μm was added so that the amount was 38 volume % relative to the total volume of the obtained mixture. These were mixed in powder form in a Henschel mixer, and then melt-kneaded in a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded in a single-screw extruder to obtain a resin sheet. The resin sheet was rolled by a pair of heated rolls to obtain a sheet-shaped polyolefin resin composition. The obtained sheet-shaped polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (4 mol / L hydrochloric acid, 0.5 wt % nonionic surfactant) to remove the calcium carbonate, thereby obtaining a primary sheet. Then, both ends of the obtained primary sheet in the TD direction were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretching speed of 10 m / min and a stretching ratio of 7.05 times. Then, the stretched primary sheet was heat-treated at a temperature of 129° C. for 21 seconds to be heat-set, thereby producing a porous film 1. The produced porous film 1 was used as a separator 1.

[0132] [Example 2] 70 parts by weight of ultra-high molecular weight polyethylene powder (GUR4032, number average branch number: 0.5, manufactured by Ticona) and 30 parts by weight of polyethylene wax (FNP-0115, manufactured by Nippon Seiro) having a weight average molecular weight of 1000 were prepared. The total of the ultra-high molecular weight polyethylene and the polyethylene wax was 100 parts by weight, and 0.4 parts by weight of an antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of an antioxidant (IRGAFOS 168, manufactured by BASF), and 1.3 parts by weight of sodium stearate were added. Furthermore, calcium carbonate having an average particle size of 0.1 μm (manufactured by Maruo Calcium Co., Ltd.) was added so that it was 38% by volume with respect to the total volume of the obtained mixture. These were mixed in powder form using a Henschel mixer, and then melt-kneaded using a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded using a single-screw extruder to form a resin sheet. The resin sheet was rolled by a pair of heated rolls to obtain a sheet-like polyolefin resin composition. The obtained sheet-like polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (4 mol / L hydrochloric acid, 0.5% by weight of a nonionic surfactant) to remove the calcium carbonate, and a primary sheet was obtained. Then, both ends of the obtained primary sheet in the TD direction were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretching speed of 10 m / min and a stretching ratio of 7.05 times. Then, the stretched primary sheet was heat-treated at a temperature of 120° C. for 21 seconds to be heat-set, thereby producing a porous film 2. The produced porous film 2 was used as a separator 2.

[0133] [Example 3] The same operation as in Example 2 was carried out except that the heat treatment temperature in the heat setting was changed from 120°C to 110°C, and the stretch ratio in the TD direction was changed from 7.05 times to 5.00 times, to produce a porous film 3. The produced porous film 3 was used as a separator 3.

[0134] [Example 4] 26.9 parts by weight of ultra-high molecular weight polyethylene powder (intrinsic viscosity: 21 dL / g, viscosity average molecular weight: 1.5 million, number average branch number: 0.1, manufactured by Tosoh Corporation) and 10.7 parts by weight of polyethylene wax (Excelex 40800, manufactured by Mitsui Chemicals, Inc.) having a weight average molecular weight of 4000 were prepared. The total of the ultra-high molecular weight polyethylene and the polyethylene wax was 100 parts by weight, and 0.3 parts by weight of an antioxidant (IRGANOX 1010, manufactured by BASF), 0.1 parts by weight of an antioxidant (IRGAFOS 168, manufactured by BASF), and 0.4 parts by weight of sodium stearate were added. Furthermore, calcium carbonate having an average particle size of 0.07 μm (manufactured by Maruo Calcium Co., Ltd.) was added so that the amount was 37% by volume with respect to the total volume of the obtained mixture. These were mixed in powder form using a Henschel mixer, and then melt-kneaded using a twin-screw kneader to obtain a polyolefin resin composition. The polyolefin resin composition was extruded using a single-screw extruder to form a resin sheet. The resin sheet was rolled by a pair of heated rolls to obtain a sheet-like polyolefin resin composition. The obtained sheet-like polyolefin resin composition was immersed in an aqueous hydrochloric acid solution (4 mol / L hydrochloric acid, 0.5 wt % nonionic surfactant) to remove the calcium carbonate, and a primary sheet was obtained. Then, both ends of the obtained primary sheet in the TD direction were held by a plurality of holding members adjacent in the MD direction. Then, the primary sheet was stretched in the TD direction at a stretching speed of 10 m / min and a stretching ratio of 7.05 times. Then, the stretched primary sheet was heat-treated at a temperature of 132° C. for 21 seconds to be heat-set, thereby producing a porous film 4. The produced porous film 4 was used as a separator 4.

[0135] [Comparative Example 1] The same operation as in Example 2 was carried out except that the heat treatment temperature in the heat setting was changed from 120°C to 125°C, the stretching speed in the TD direction was changed to 15m / min, and the heat treatment time in the heat setting was changed from 21 seconds to 13 seconds, to prepare a porous film C1. The prepared porous film C1 was used as a separator C1.

[0136] [Comparative Example 2] The same operation as in Example 2 was carried out except that the heat treatment temperature in the heat setting was changed from 120°C to 128°C, the stretching speed in the TD direction was changed to 16m / min, and the heat treatment time in the heat setting was changed from 21 seconds to 14 seconds, to prepare a porous film C2. The prepared porous film C2 was used as a separator C2.

[0137] [result] The heat treatment times for heat setting in Examples 1 to 4 and Comparative Examples 1 and 2, and the physical properties of Separators 1 to 4 and Separators C1 and C2 obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were measured by the above-mentioned methods, and the results are shown in Table 1 below.

[0138] [Table 1]

[0139] As shown in Table 1, separators 1 to 4 in Examples 1 to 4 include a porous film in which the required number of stages is 20 or less, and therefore correspond to a separator according to one embodiment of the present invention. On the other hand, separators C1 and C2 in Comparative Examples 1 and 2 include a porous film in which the required number of stages is more than 20, and therefore do not correspond to a separator according to one embodiment of the present invention. In addition, separators 1 to 4 have a smaller difference in air permeability / film thickness before and after compression at 20 MPa than separators C1 and C2, and the increase in air permeability, i.e., the degree of decrease in ion permeability, before and after compression is smaller. Therefore, it was found that the separator according to one embodiment of the present invention can maintain good ion permeability even when compressed.

[0140] In Examples 1 to 4, no relaxation operation in the MD direction was performed in the stretching step before heat setting. In addition, as shown in Table 1, the separators 1 to 4 described in Examples 1 to 4 have a small number of required stages and an AC resistance value of 3.5 Ω cm 2It is controlled within the following preferred range. Therefore, in one embodiment of the present invention, it is considered that the necessary number of stages can be suitably reduced and the value of AC resistance can also be suitably reduced by not performing the relaxation operation. In other words, it is considered that the necessary number of stages is likely to be increased and exceed 20 stages when the relaxation operation is performed. [Industrial Applicability]

[0141] The separator according to one embodiment of the present invention can maintain good ion permeability even when compressed, and therefore can be used as a separator for a high-capacity non-aqueous electrolyte secondary battery having a high internal pressure. [Explanation of symbols]

[0142] 1 Cavity area

Claims

1. A separator for a non-aqueous electrolyte secondary battery comprising a polyolefin porous film, a two-dimensional image of 960 pixels in the film thickness direction and 1280 pixels in the MD direction obtained from a cross section of the polyolefin porous film using a scanning electron microscope under conditions of a magnification of 5000 times and 1 pixel being 19.8 μm × 19.8 μm, the image being binarized into void regions and resin regions to obtain a binarized image, and then the binarized image is subjected to a process for gradually expanding the void regions, the number of stages required until the resin regions are completely filled with the expanded void regions is 20 or less, The stepwise expansion process is a process of repeating an operation of expanding each of the target pixels constituting the void region by one pixel in a direction of pixels adjacent to the four sides of each of the target pixels in each step, A separator for a nonaqueous electrolyte secondary battery, comprising: a process for expanding the void region in a stepwise manner; and a method for calculating the required number of steps, the method being any of the following methods (1) to (9). (1) An analysis region of 100 pixels in the thickness direction × 1280 pixels in the MD direction is extracted from the two-dimensional image. (2) Adaptive histogram equalization of luminance values ​​is performed on the analysis region extracted in (1). (3) The analysis region in which the adaptive histogram equalization process of the luminance values ​​has been performed in (2) is subjected to an inversion process of the luminance values. (4) All pixels constituting the analysis area whose brightness values ​​have been inverted in (3) are divided into pixels whose brightness values ​​are equal to or less than a threshold value of 180 in the brightness value range of 0 to 255 and pixels whose brightness values ​​exceed the threshold value of 180, and binarized. (5) In the analysis region binarized in (4), a region consisting of pixels whose brightness value exceeds a threshold value of 180 is identified as a void region. (6) For each of the gap regions identified in (5) in the analysis region, an operation is performed to expand four neighboring pixels constituting the boundary of each gap region outward by one pixel. (7) After the expansion operation in (6), the area other than the void area is determined as a resin area, and blob processing is performed on the resin area to count the number of pixels that make up the resin area. The number of measured pixels is regarded as the number of resin part regions. Then, it is confirmed whether the measured number of resin part regions is 0 or not. (8) If the number of resin part regions measured in (7) is 0, the process of calculating the required number of stages is terminated. If the number of resin part regions is not 0, the processes described in (6) and (7) are repeated until the number of resin part regions becomes 0, and the process of calculating the required number of stages is terminated at the point when the number of resin part regions becomes 0. (9) In (8), the number of times the processes described in (6) and (7) are repeated until the process of calculating the required number of stages is completed is calculated, and the calculated number is set as the required number of stages.

2. The separator for a non-aqueous electrolyte secondary battery according to claim 1 , further comprising an insulating porous layer containing a resin.

3. 3. The separator for a non-aqueous electrolyte secondary battery according to claim 2, wherein the resin is at least one selected from the group consisting of polyolefins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyester resins, and water-soluble polymers.

4. 3. The separator for a non-aqueous electrolyte secondary battery according to claim 2, wherein the resin is an aramid resin.

5. The separator for a non-aqueous electrolyte secondary battery according to claim 2 , further comprising an adhesive layer in addition to the insulating porous layer.

6. A member for a non-aqueous electrolyte secondary battery, comprising a positive electrode, the separator for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5, and a negative electrode, arranged in this order.

7. A non-aqueous electrolyte secondary battery comprising the separator for non-aqueous electrolyte secondary batteries according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for producing separator for nonaqueous electrolyte secondary battery

    JP2019175856A

  • Non-aqueous electrolyte secondary battery separator, non-aqueous electrolyte secondary battery member, and non-aqueous electrolyte secondary battery

    JP2022155051A

  • Finely porous polyethylene membrane

    JP1999130900A