Curable composition

The curable composition addresses the issues of insufficient antibacterial properties and color changes in sealing materials by using a specific polymer, amine compound, and antibacterial agent, ensuring effective detergents resistance and maintaining matte and uneven textures, thus enhancing the durability and appearance of building walls.

JP2024146911AActive Publication Date: 2024-10-15SEKISUI FULLER CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024057130
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing curable compositions for sealing materials in building walls lack sufficient antibacterial properties, are prone to color changes due to detergents, and do not maintain matte and uneven textures effectively.

Method used

A curable composition comprising a curable polymer, an amine compound with a melting point of 25 to 80°C, particles with a size of 5 to 1000 μm, and an antibacterial agent, which together enhance antibacterial properties, detergents resistance, and maintain matte and uneven textures by forming a thin film on the cured product surface.

Benefits of technology

The composition produces a cured product with excellent antibacterial properties, detergent resistance, and reduced color tone changes, maintaining design integrity and cleanliness without impairing the aesthetic appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146911000001
    Figure 2024146911000001
Patent Text Reader

Abstract

To provide a curable composition which can produce a cured object which has excellent antibacterial ability, detergent resistance in washing, and excellent matting property and uneven feeling, the curable composition being reduced in a hue change before and after curing.SOLUTION: There is provided a curable composition comprising; a curable polymer; 2 pts.mass or less of an amine compound whose melting point is 25 to 80°C; particles whose diameters are 5 to 1000 μm; and an antibacterial agent, therefore from the curable composition, a cured object which has excellent antibacterial ability, detergent resistance in washing, excellent matting property and uneven feeling, can be produced, and before and after curing, a change of a hue is reduced. The curable composition does not damage design property and antibacterial property of other members which are used with the curable composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition. [Background technology]

[0002] In recent years, there has been an increasing demand for high design quality in buildings, and wall designs, particularly for exterior walls which occupy a large area, have become more diverse due to improvements in printing technology and surface treatment processing technology for resin wall components.

[0003] Furthermore, due to the current social situation, there is a growing demand for clean building materials, and in addition to the above-mentioned design features, walls are also required to have antibacterial properties and resistance to detergents when cleaning.

[0004] On the other hand, the wall is constructed by arranging wall members having a predetermined width vertically and horizontally, and the joints formed between the wall members are filled with a sealant. In order not to impair the design required for the wall members, the sealant is also required to have a matte finish and a textured feel. Furthermore, the sealant is also required to have the antibacterial properties and detergent resistance required for cleaning, which are required for the wall.

[0005] Patent Document 1 discloses a curable composition having an uneven appearance, which contains a reactive polymer and spherical particles, and in which the content of (P1) spherical particles having a particle size of 850 to 1300 μm is 0.5 to 10 volume % of the composition, the content of (P2) spherical particles having a particle size of 250 to 600 μm is 0.5 to 10 volume % of the composition, and the content of (P3) spherical particles having a particle size of 600 to 850 μm is 45 volume % or less of the total of particles (P1) and particles (P2).

[0006] Patent Document 2 discloses a sealant composition containing (A) a modified polymer having a crosslinkable silyl group at its terminal, (B) an alkylamine having an alkyl group having 20 or more carbon atoms and having a melting point or freezing point of 50°C or higher, (C) an amine-based silane coupling agent having a triethoxysilyl group, (D) calcium carbonate having an average particle size of 300 to 450 μm, (E) black silica having an average particle size of 150 to 250 μm, (F) a filler, (G) a plasticizer, and (H) a curing catalyst.

[0007] Patent Document 3 discloses an antibacterial and antifungal organopolysiloxane composition that is less prone to discoloration, which comprises an organopolysiloxane (A), a hydrolyzable silane compound and / or a partial hydrolyzate thereof (B), a triazolyl group-containing compound (C), and an inorganic antibacterial agent (D). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2019-151687 A [Patent Document 2] JP 2019-151676 A [Patent Document 3] Japanese Patent Application Publication No. 11-199777 Summary of the Invention [Problem to be solved by the invention]

[0009] However, even if the curable composition of Patent Document 1 contains an antibacterial agent as in Patent Document 3, there is a problem that the cured product of the curable composition cannot exhibit sufficient antibacterial properties. In addition, there is also a problem that the cured product of the curable composition may be discolored by detergent components depending on the type of particles.

[0010] In addition, even if the sealant composition of Patent Document 2 contains an antibacterial agent as in Patent Document 3, it is not possible to impart sufficient antibacterial properties to the cured product of the sealant composition. Furthermore, there is a problem in that the color tone of the sealant composition changes before and after curing, which may impair the color tone of the wall.

[0011] The present invention provides a curable composition which produces a cured product having excellent antibacterial properties, detergent resistance during cleaning, and excellent matte finish and textured feel, and which exhibits reduced change in color tone before and after curing. [Means for solving the problem]

[0012] The curable composition of the present invention contains 100 parts by mass of a curable polymer, 2 parts by mass or less of an amine compound having a melting point of 25 to 80° C., particles having a particle size of 5 to 1000 μm, and an antibacterial agent.

[0013] [Curable polymer] The curable composition contains a curable polymer (A). The curable polymer (A) is preferably cured at 0 to 100° C. for ease of use.

[0014] The curable polymer may be a polymer having a known crosslinking reactive group in the molecule. The crosslinking reactive group is not particularly limited, and may be, for example, a hydrolyzable silyl group, an isocyanate group, an epoxy group, an amino group, a hydroxyl group, etc., and is preferably a hydrolyzable silyl group because it can produce a cured product with high reaction safety and strength. The crosslinking reactive group may be used alone or in combination of two or more kinds.

[0015] The polymer constituting the curable polymer is not particularly limited, and examples thereof include polyether-based polymers, silicone-based polymers, polyurethane-based polymers, polysulfide-based polymers, acrylic-based polymers, polyisobutylene-based polymers, and rubber-based polymers. Since the antibacterial properties of the cured product of the curable composition are improved, polyether-based polymers and acrylic-based polymers are preferred, and polyether-based polymers are more preferred.

[0016] As the polymer constituting the curable polymer, a polymer having a polyoxyalkylene structure is more preferable, and specifically, a polyoxyalkylene-based polymer whose main chain structure contains a repeating unit represented by general formula (1) is preferable. -(R 1 -O)n- (1) (In the formula, R 1 represents an alkylene group having 1 to 14 carbon atoms, and n is the number of repeating units and is a positive integer.

[0017] An alkylene group is a divalent atomic group resulting from the removal of two hydrogen atoms bonded to two different carbon atoms in an aliphatic saturated hydrocarbon, and includes both linear and branched atomic groups. Note that branched includes the case where one carbon (methyl group) is bonded as a side chain.

[0018] Examples of the alkylene group include an ethylene group, a propylene group [-CH(CH3)-CH2-], a trimethylene group [-CH2-CH2-CH2-], a butylene group, an amylene group [-(CH2)5-], and a hexylene group.

[0019] The main chain of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0020] Examples of the main chain skeleton of the polyoxyalkylene polymer include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer, with polyoxypropylene being preferred.

[0021] The content of the repeating unit represented by general formula (1) in the main chain skeleton of the polyoxyalkylene polymer is preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 99% by mass or more, and more preferably 100% by mass.

[0022] The hydrolyzable silyl group refers to a group that undergoes a condensation reaction in the presence of moisture or a crosslinking agent, and if necessary, using a catalyst, such as a silicon-containing group or a silanol group having a hydrolyzable group bonded to a silicon atom. Note that a silanol group refers to a functional group (≡Si-OH) in which a hydroxyl group (-OH) is directly bonded to a silicon atom.

[0023] The hydrolyzable group of the hydrolyzable silyl group is not particularly limited, and examples thereof include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group.

[0024] Examples of the hydrolyzable silyl group include monoalkoxysilyl groups such as a methoxysilyl group, an ethoxysilyl group, a dimethylmethoxysilyl group, and a dimethylethoxysilyl group; dialkoxysilyl groups such as a dimethoxysilyl group, a methyldimethoxysilyl group, and a methyldiethoxysilyl group; trialkoxysilyl groups such as a trimethoxysilyl group and a triethoxysilyl group; and halogenated silyl groups to which a halogen is bonded, such as a trichlorosilyl group. Of these, an alkoxysilyl group is preferred, a dialkoxysilyl group is preferred, and a dimethoxysilyl group is preferred.

[0025] The polyoxyalkylene polymer having a hydrolyzable silyl group can be produced, for example, by reacting a polyoxyalkylene polymer having a functional group such as a hydroxyl group at its terminal with an organic compound having an active group and an unsaturated group that are reactive with the functional group, and then allowing a hydrosilane having a hydrolyzable group to act on the resulting reaction product to carry out hydrosilylation.

[0026] The number average molecular weight of the curable polymer (A) is preferably 8000 or more, more preferably 9000 or more, more preferably 10000 or more, and more preferably 11000 or more. The number average molecular weight of the curable composition (A) is preferably 50000 or less, more preferably 40000 or less, more preferably 38000 or less, more preferably 35000 or less, more preferably 32000 or less, and more preferably 31000 or less.

[0027] The molecular weight distribution of the curable polymer (A) is preferably 1.6 or less, more preferably 1.5 or less, and more preferably 1.45 or less. When the molecular weight distribution of the curable polymer (A) is 1.6 or less, the viscosity of the curable polymer (A) decreases, and the workability of the curable composition is improved.

[0028] In the present invention, the number average molecular weight and weight average molecular weight of the curable polymer are values ​​measured by GPC (gel permeation chromatography). Specifically, 6 to 7 mg of the curable polymer is collected, the collected curable polymer is fed to a test tube, and tetrahydrofuran (THF) is added to the test tube to dilute the curable polymer to a concentration of 1 mg / mL, to obtain a measurement sample. The number average molecular weight and weight average molecular weight of the curable polymer can be measured by GPC using this measurement sample.

[0029] The number average molecular weight and weight average molecular weight of the curable polymer can be measured, for example, using the following measuring device and measuring conditions. Measuring Equipment Waters 2690 Measurement conditions Column: Shodex LF-804 (8.0 x 300 mm) x 2 Column temperature: 40℃ Mobile phase: THF Flow rate: 1mg / mL Injection volume: 50μL Detector: UV260nm

[0030] [Amine compounds] The curable composition contains an amine compound (B) having a melting point of 25 to 80°C [hereinafter, sometimes simply referred to as "amine compound (B)"]. By containing the amine compound (B) in the curable composition, in the cured product of the curable composition (hereinafter, sometimes simply referred to as "cured product"), the film of the amine compound (B) formed on the surface of the cured product can be thinned by a synergistic effect with the particles (C) described later, and a small amount of the amine compound (B) can impart excellent matte properties to the cured product, and the change in color tone before and after curing of the curable composition by the amine compound (B) can be reduced, a cured product with excellent color tone is produced, and the color tone of the curable composition with the exterior wall material can be improved. When the curable composition has a dark color such as black or navy blue, the color tone of the curable composition is likely to change before and after curing, but even in such a case, the change in color tone of the curable composition before and after curing is reduced, and the change in color tone is generally prevented. Furthermore, since the film of the amine compound (B) is thin, the antibacterial agent can smoothly permeate the film of the amine compound (B), and the cured product exhibits excellent antibacterial properties. Also, since the surface of the cured product is covered with an extremely thin film of the amine compound (B), the cured product of the curable polymer (A) and the particles (C) can be protected from detergents, and changes in color tone such as discoloration caused by detergents can be substantially prevented.

[0031] The amine compound (B) preferably contains a monoamine compound having one amino group (-NH2) in one molecule, or a diamine compound having two amino groups (-NH2) in one molecule, and more preferably contains a monoamine compound having one amino group (-NH2) in one molecule. In the amine compound (B), the hydrogen atom of the amino group may be substituted with an organic group such as an alkyl group or an aryl group. In addition, it is preferable that the amine compound (B) does not contain a silicon atom. The amine compound (B) may be used alone or in combination of two or more kinds.

[0032] Preferred examples of the amine compound (B) include monoamine compounds represented by the following formula (2). R 2 -NH2(2) (In formula (2), R 2 is a linear or branched alkyl group, or a monovalent saturated alicyclic hydrocarbon group.

[0033] R 2 Examples of the linear or branched alkyl group in the above formula include a decyl group, an isodecyl group, an undecyl group, a lauryl group, an isododecyl group, a tridecyl group, a myristyl group, a pentadecyl group, a palmityl group, a heptadecyl group, a n-hexadecyl group, an isohexadecyl group, a stearyl group, an isooctadecyl group, a nonadecyl group, an eicosyl group, and a behenyl group. Of these, a lauryl group, an isododecyl group, a tridecyl group, a myristyl group, a pentadecyl group, a palmityl group, a heptadecyl group, a n-hexadecyl group, an isohexadecyl group, a stearyl group, an isooctadecyl group, a nonadecyl group, an eicosyl group, and a behenyl group are preferred.

[0034] In the amine compound (B) represented by formula (2), R 2 In the amine compound (B) represented by formula (2), R 2 The number of carbon atoms in R is preferably 40 or less, more preferably 30 or less, and still more preferably 25 or less. 2 By using the amine compound (B) having a carbon number within the above range, a synergistic effect with the particles (C) can be achieved, which reduces the change in color tone before and after curing of the curable composition and improves the matte properties.

[0035] As the amine compound (B), laurylamine (C 12 H 25 -NH2, melting point: 28℃), stearylamine (C 18 H 37 -NH2, melting point: 50°C), myristylamine (melting point: 38°C), cetylamine (n-hexadecylamine, C 16 H 33 -NH2, melting point: 47°C), and behenylamine (melting point: 63°C) are preferred.

[0036] The melting point of the amine compound (B) is preferably 25°C or higher, more preferably 26°C or higher, more preferably 27°C or higher, more preferably 35°C or higher, more preferably 40°C or higher, and more preferably 45°C or higher. When the melting point of the amine compound (B) is 25°C or higher, the stickiness on the surface of the cured product of the curable composition is reduced, and the change in color tone of the cured product due to the adhesion of foreign matter to the surface of the cured product can be reduced. The melting point of the amine compound (B) is preferably 80°C or lower, more preferably 70°C or lower, more preferably 60°C or lower, more preferably 55°C or lower, and more preferably 50°C or lower. When the melting point of the amine compound (B) is 80°C or lower, the amine compound (B) formed on the surface of the cured product can be mixed evenly throughout the curable composition to reduce the film thickness of the amine compound (B), and a film of the amine compound (B) having an even film thickness can be formed on the surface of the cured product. Therefore, while imparting excellent matte properties to the cured product, it is possible to further reduce the change in color tone of the curable composition before and after curing due to the amine compound (B), produce a cured product with excellent color tone, and further improve the color tone harmony with the exterior wall material. Furthermore, since the film of the amine compound (B) is thin, the antibacterial agent smoothly permeates the film of the amine compound (B), and the cured product exhibits excellent antibacterial properties.

[0037] In the present invention, the melting point of the amine compound (B) refers to a temperature measured by differential scanning calorimetry (DSC) in accordance with JIS K7121 (1987). Specifically, the amine compound (B) is heated from 10°C to 150°C at a heating rate of 5°C / min using a differential scanning calorimeter (e.g., Shimadzu Corporation's DSC-60), and the melting peak temperature of the DSC curve during this heating process is taken as the melting point of the amine compound (B). In addition, when there are multiple melting peaks, the temperature at the apex of the melting peak with the greatest heat absorption is taken as the melting point.

[0038] The content of the amine compound (B) in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the curable polymer (A). The content of the amine compound (B) in the curable composition is preferably 2 parts by mass or less, more preferably 1.5 parts by mass or less, more preferably 1.3 parts by mass or less, more preferably 1.1 parts by mass or less, and more preferably 1.0 parts by mass or less, relative to 100 parts by mass of the curable polymer (A). When the content of the amine compound (B) is 0.1 parts by mass or more, a thin film of the amine compound (B) is formed on the surface of the cured product of the curable composition, and the cured product of the curable polymer (A) and the particles (C) can be protected from detergent, and changes in color tone such as discoloration caused by detergent can be substantially prevented. When the content of the amine compound (B) is 2 parts by mass or less, the change in color tone before and after curing of the curable composition can be reduced, and it is possible to achieve harmony with the exterior wall material.

[0039] [Particles with a diameter of 5 to 1000 μm (C)] The curable composition contains particles (C) having a particle diameter of 5 to 1000 μm (hereinafter, sometimes simply referred to as "particles (C)"). By containing particles (C) in the curable composition, it is possible to impart a suitable unevenness to the cured product of the curable composition and improve the matte property of the cured product. Furthermore, by making the particle diameter of the particles (C) 5 to 1000 μm, unevenness is formed in the cured product to give a suitable surface area, and by bleeding out the amine compound (B) on the uneven surface having the suitable surface area, a thin film of the amine compound (B) can be formed on the surface of the cured product. By forming the amine compound (B) in a thin film, it is possible to generally prevent the unevenness formed by the particles (C) from being reduced by the thin film of the amine compound (B), and the matte effect due to the unevenness is effectively exerted, and further, the matte effect due to the amine compound (B) also acts, and the cured product exhibits an excellent matte effect. A thin film of the amine compound (B) can be easily formed by the presence of the particles (C), and the content of the amine compound (B) can be reduced. As a result, the change in color tone caused by the amine compound (B) before and after the curing of the curable composition can be reduced, improving the color tone harmony with the exterior wall material, and the antibacterial agent can easily permeate the film of the amine compound (B), allowing the cured product to exhibit excellent antibacterial properties.

[0040] The particles (C) are not particularly limited as long as they are solid particles at -40 to 100°C and have a particle diameter of 5 to 1000 μm, and examples thereof include inorganic particles containing inorganic materials such as minerals, shirasu, ceramics, and glass, organic particles containing synthetic resins such as silicone resins, epoxy resins, polystyrene, acrylic resins, and phenolic resins, and composite particles obtained by combining inorganic materials and synthetic resins. The particles (C) may be used alone or in combination of two or more kinds.

[0041] The particle diameter of the particles (C) is 5 μm or more, preferably 10 μm or more, more preferably 20 μm or more, more preferably 30 μm or more, more preferably 35 μm or more, more preferably 40 μm or more, and more preferably 45 μm or more. The particle diameter of the particles (C) is 1000 μm or less, preferably 900 μm or less, more preferably 800 μm or less, more preferably 700 μm or less, more preferably 650 μm or less, and more preferably 600 μm or less. When the particle diameter of the particles (C) is 5 μm or more, the surface of the cured product of the curable composition is formed with appropriate unevenness, and the matte property and unevenness of the cured product can be improved, and the antibacterial property of the cured product can be improved. When the particle diameter of the particles (C) is 1000 μm or less, the unevenness of the cured product can be made to be of appropriate size, and the antibacterial agent that has penetrated the surface of the cured product can be well exposed to the outside, and excellent antibacterial property can be imparted to the cured product. The particle size of the particles (C) refers to the equivalent sphere diameter (the diameter when converted into a sphere of the same volume) measured by a laser diffraction method.

[0042] The particles (C) contain first particles having a particle diameter in a predetermined range and second particles having a particle diameter larger than the upper limit of the particle diameter range of the first particles, so that fine irregularities can be formed on the cured surface of the curable composition, and the matte property and unevenness of the cured surface can be further improved. Specifically, the particles (C) preferably contain first particles having a particle diameter of 5 μm or more and 45 μm or less and second particles having a particle diameter of more than 45 μm and 1000 μm or less, more preferably contain first particles having a particle diameter of 5 μm or more and 45 μm or less and second particles having a particle diameter of 46 μm or more and 700 μm or less, and more preferably contain first particles having a particle diameter of 5 μm or more and 45 μm or less and second particles having a particle diameter of 46 μm or more and 650 μm or less.

[0043] In the particles (C), the content ratio of the first particles to the second particles (mass of the first particles / mass of the second particles) is preferably 0.5 or more, more preferably 0.6 or more, more preferably 0.7 or more, and more preferably 0.8 or more. In the particles (C), the content ratio of the first particles to the second particles (mass of the first particles / mass of the second particles) is preferably 1.5 or less, more preferably 1.4 or less, more preferably 1.3 or less, and more preferably 1.2 or less.

[0044] In the curable composition, the volume concentration of the particles (C) is preferably 1% by volume or more, more preferably 2% by volume or more, and more preferably 3% by volume or more. In the curable composition, the volume concentration of the particles (C) is preferably 10% by volume or less, more preferably 9.8% by volume or less, and more preferably 9.5% by volume or less. When the volume concentration of the particles (C) is 1% by volume or more, appropriate unevenness is formed on the surface of the cured product of the curable composition, and the matte property and unevenness of the cured product can be improved, and the antibacterial property of the cured product can be improved. When the volume concentration of the particles (C) is 10% by volume or less, the unevenness of the cured product can be made appropriate in size, and the antibacterial agent that has penetrated the surface of the cured product can be well exposed to the outside, and excellent antibacterial property can be imparted to the cured product.

[0045] The volume concentration of the particles (C) refers to the percentage of the total volume of the particles (C) in the volume of the curable composition, and is represented by the following formula. Volume concentration (volume%) of particles (C) = 100 × total volume of particles (C) / total volume of curable composition

[0046] The particles (C) may be either solid with no internal voids or hollow with internal voids. When the curable composition is applied, the particles (C) having a small specific gravity tend to come out to the surface of the curable composition, forming unevenness on the surface of the cured product of the curable composition, thereby improving the matte properties of the cured product.

[0047] When the particles (C) are hollow particles, the porosity of the particles (C) is preferably 20% or more, more preferably 25% or more, and more preferably 30% or more. The porosity of the particles (C) is preferably 80% or less, more preferably 75% or less, and more preferably 70% or less. When the porosity of the particles (C) is within the above range, the particles (C) are easily exposed to the surface of the curable composition, forming unevenness on the surface of the cured product of the curable composition, and improving the matte property of the cured product.

[0048] The porosity of the particles (C) is a value calculated based on the following. Porosity (%) of particle (C) = 100 × bulk density (g / cm 3 ) / true density(g / cm 3 )

[0049] The bulk density refers to the packed bulk density defined in JIS R1628. The true density refers to the density of the volume of only the particles themselves measured by the Gay-Lussac type pycnometer method defined in JIS Z8807.

[0050] The content of the particles (C) in the curable composition is preferably 3 parts by mass or more, more preferably 4 parts by mass or more, and more preferably 5 parts by mass or more, based on 100 parts by mass of the curable polymer. The content of the particles (C) in the curable composition is preferably 30 parts by mass or less, more preferably 28 parts by mass or less, and more preferably 25 parts by mass or less, based on 100 parts by mass of the curable polymer. When the content of the particles (C) is 3 parts by mass or more, appropriate unevenness is formed on the surface of the cured product of the curable composition, and the matte property and unevenness of the cured product can be improved, and the antibacterial property of the cured product can be improved. When the content of the particles (C) is 30 parts by mass or less, the unevenness of the cured product can be made appropriate in size, and the antibacterial agent that has penetrated the surface of the cured product can be well exposed to the outside, thereby imparting excellent antibacterial property to the cured product.

[0051] The most preferred combination of amine compound (B) and particles (C) having a particle diameter of 30 μm or more is that the amine compound (B) contains 1.2 parts by weight or less of an amine compound having a melting point of about 50 ° C., and the particles (C) contains particles having a particle diameter of 100 to 300 μm. When the amine compound having a melting point of about 50 ° C. is 1.2 parts by weight or less and particles having a particle diameter of 100 to 300 μm are included, the surface of the cured product expands due to the unevenness of the particles, and the film thickness of the amine compound covering the surface of the cured product can be thinned, and the antibacterial property can be exhibited without suppressing the penetration of the antibacterial agent component to the surface of the cured product. Furthermore, the amount of the amine compound added as a matting agent can be reduced due to the matting effect caused by the diffuse reflection of light due to the unevenness of the particles, and the effect of the amine compound on the color tone can be suppressed.

[0052] [Antibacterial agents] The curable composition contains an antibacterial agent (D). By containing the antibacterial agent (D), it is possible to impart antibacterial properties to a cured product of the curable composition.

[0053] As the antibacterial agent (D), a known antibacterial agent can be used, and both inorganic and organic antibacterial agents can be used. Inorganic antibacterial agents are preferred, and metal antibacterial agents are more preferred, since they can be easily mixed into the curable polymer and can reduce runoff when the surface of the cured product of the curable composition is washed with a detergent.

[0054] Examples of inorganic antibacterial agents include metal-based antibacterial agents in which metal atoms (e.g., silver, copper, zinc, etc.) are contained in inorganic compounds (e.g., minerals, etc.), and photocatalyst-based antibacterial agents such as titanium oxide.

[0055] The method for making an inorganic compound contain a predetermined metal atom is not particularly limited, and examples thereof include a method of making an inorganic compound support a metal atom by physical adsorption or chemical adsorption, a method of replacing a cation contained in an inorganic compound with a metal ion by an ion exchange reaction to make the inorganic compound contain the metal atom, a method of making an inorganic compound support the metal atom as metallic gold, metallic silver, metallic copper, silver oxide or copper oxide, a method of making an inorganic compound support the metal atom as a metal complex (e.g., a silver thiosulfato complex, etc.), a method of making an inorganic compound contain a metal atom as a glass component (e.g., a method of making a soluble glass such as SiO2-B2O3-Na2O glass contain a metal atom as a glass component), a method of making an inorganic compound support a compound containing a metal atom by using a binder, a method of making an inorganic compound support the metal atom by implanting a silver compound or a copper compound into the inorganic compound, and a method of making an inorganic compound support the metal atom by forming a thin layer of a compound containing a metal atom on the surface of the inorganic compound by a thin film formation method such as vapor deposition, dissolution deposition reaction, or sputtering.

[0056] In the metal-based antibacterial agent, the content of the metal atom is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, more preferably 0.4% by mass or more, and more preferably 0.5% by mass or more. The content of the metal atom is preferably 10% by mass or less, more preferably 9% by mass or less, more preferably 8% by mass or less, and more preferably 7% by mass or less. When the content of the metal atom is 0.1% by mass or more, the cured product of the curable composition can be given excellent antibacterial properties. When the content of the metal atom is 10% by mass or less, coloring of the curable composition can be suppressed.

[0057] When an inorganic antibacterial agent (D) is used, zeolite is preferred because of the ease of supporting metal ions.

[0058] The crystal structure of the zeolite is not particularly limited, and examples thereof include A-type, ferrierite-type, MCM-22-type, ZSM-5-type, mordenite-type, L-type, Y-type, X-type, and beta-type. From the viewpoint of stable support of metal atoms, A-type, Y-type, and X-type are preferred, and A-type is more preferred.

[0059] Examples of organic antibacterial agents include surfactant-based antibacterial agents such as benzalkonium chloride, alkyldi(aminoethyl)glycine hydrochloride, and fatty acid monoglycerides; antibacterial agents derived from natural products such as chitosan-based antibacterial agents and hinokitiol-based antibacterial agents; biguanide-based antibacterial agents such as chlorhexidine gluconate; alcohol-based antibacterial agents, phenol-based antibacterial agents, anilide-based antibacterial agents, iodine-based antibacterial agents, imidazole-based antibacterial agents, thiazole-based antibacterial agents, isothiazolone-based antibacterial agents, triazine-based antibacterial agents, nitrile-based antibacterial agents, fluorine-based antibacterial agents, and organometallic antibacterial agents.

[0060] The average particle size of the antibacterial agent (D) is preferably 0.1 μm or more, more preferably 0.2 μm or more, more preferably 0.3 μm or more, and more preferably 0.5 μm or more. The average particle size of the antibacterial agent (D) is preferably 11 μm or less, more preferably 10 μm or less, and more preferably 5 μm or less. When the average particle size of the antibacterial agent (D) is 0.1 μm or more, the antibacterial agent (D) can be uniformly dispersed in the curable polymer without agglomeration, and the antibacterial agent can be uniformly permeated to the surface of the cured product, thereby allowing all of the cured products to exhibit excellent antibacterial properties. When the average particle size of the antibacterial agent (D) is 11 μm or less, the antibacterial component on the surface of the cured product is increased by increasing the surface area of ​​the antibacterial agent (D), and the antibacterial properties of the cured product are improved.

[0061] The average particle diameter of the antibacterial agent (D) refers to a value measured by image analysis using a transmission electron microscope (TEM). A transmission electron microscope (accelerating voltage 200 kV, observation magnification 30,000 times) is used for the TEM, and the antibacterial agent lightly crushed in a mortar is ultrasonically dispersed in acetone, dropped onto a plastic support film, and naturally dried to prepare a specimen for microscopic examination, which is then photographed. For each primary particle in the photograph, the arithmetic mean value of the longest diameter R1 and the diameter R2 in the perpendicular direction at its midpoint is calculated, and this arithmetic mean value is taken as the particle diameter of the primary particle. The particle diameters of a total of 300 primary particles are measured, and the arithmetic mean value of the particle diameters of the primary particles is taken as the average particle diameter of the antibacterial agent. For the TEM, for example, a transmission electron microscope commercially available from JEOL Ltd. under the product name "JEM-2100" can be used.

[0062] The content of the antibacterial agent (D) in the curable composition is preferably 0.0001 parts by mass or more, more preferably 0.0003 parts by mass or more, relative to 100 parts by mass of the curable polymer (A). The content of the antibacterial agent (D) in the curable composition is preferably 10 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the curable polymer (A). When the content of the antibacterial agent (D) is 0.0001 parts by mass or more, the antibacterial property of the curable composition is improved. When the content of the antibacterial agent (D) is 10 parts by mass or less, the change in color tone before and after the effect of the curable composition can be suppressed.

[0063] [Filling material] The curable composition may contain particles having a particle size of less than 5 μm or particles having a particle size of more than 1000 μm, in addition to the particles (C), within the range that does not impair the physical properties of the composition.

[0064] The hardenable composition may contain calcium carbonate having a particle size of less than 5 μm as a filler. Examples of calcium carbonate include ground calcium carbonate, precipitated calcium carbonate, calcium chloride carbonate, and light calcium carbonate.

[0065] Ground calcium carbonate can be obtained, for example, by grinding natural calcium carbonate such as natural chalk, marble, limestone, etc. into a fine powder.

[0066] Precipitated calcium carbonate can be produced, for example, by using limestone as a raw material and subjecting it to a chemical reaction.

[0067] The calcium carbonate may or may not be surface-treated. When the calcium carbonate is surface-treated, it is preferably treated with a fatty acid, a fatty acid ester, or a fatty acid metal salt, and more preferably treated with a fatty acid.

[0068] Examples of fatty acids include caproic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, alaic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, obscylic acid, caroleic acid, undecylenic acid, Linderic acid, tsuzuic acid, physeteric acid, moristoleic acid, palmitoleic acid, petroselinic acid, oleic acid, elaidic acid, asclevic acid, vaccenic acid, gadoleic acid, gondoic acid, cetoleic acid, erucic acid, brassidic acid, selacholeic acid, xymenic acid, lumecic acid, sorbic acid, and linoleic acid. Of these, lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid are preferred.

[0069] Examples of fatty acid esters include stearyl stearate, lauryl stearate, stearyl palmitate, and lauryl palmitate.

[0070] Examples of the fatty acid metal salts include the sodium and potassium salts of the above-mentioned fatty acids, and preferred are the sodium salt of lauric acid, the sodium salt of myristic acid, the sodium salt of palmitic acid, the sodium salt of stearic acid, and the sodium salt of oleic acid.

[0071] The particle size of the filler is preferably 0.001 μm or more, more preferably 0.008 μm or more, more preferably 0.01 μm or more, more preferably 0.02 μm or more, and more preferably 0.03 μm or more. The particle size of the filler is preferably 0.2 μm or less, more preferably 0.008 μm or less, more preferably 0.01 μm or less, more preferably 0.02 μm or less, and more preferably 0.03 μm or less.

[0072] The particle size of the filler refers to a value calculated based on the following formula using the specific surface area value per 1 g of the filler. For example, a powder specific surface area measuring device commercially available from Shimadzu Corporation under the product name "SS-100 Model" can be used. Average particle diameter (μm) = 6 x 10000 / (specific gravity x specific surface area)

[0073] In the curable composition, the content of the filler is preferably 100 parts by mass or more relative to 100 parts by mass of the curable polymer (A). In the curable composition, the content of the filler is preferably 300 parts by mass or less, more preferably 250 parts by mass or less, relative to 100 parts by mass of the curable polymer (A).

[0074] [Silanol condensation catalyst] The curable composition preferably contains a silanol condensation catalyst. The silanol condensation catalyst is a catalyst for promoting a dehydration condensation reaction between silanol groups formed by hydrolysis of a hydrolyzable silyl group, when the curable polymer contains a hydrolyzable silyl group.

[0075] The silanol condensation catalyst is not particularly limited, and examples thereof include organotin compounds such as dibutyltin diacetylacetonate, dibutyltin oxylaurate, dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin lauric acid) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), dioctyltin bis(triethoxysilicate), dioctyltin dilaurate, bis(dibutyltin bistriethoxysilicate) oxide, and dibutyltin oxybisethoxysilicate. ; organic titanium compounds such as tetra-n-butoxy titanate and tetraisopropoxy titanate; cycloamidine compounds such as 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 6-dibutylamino-1,8-diazabicyclo[5.4.0]undec-7-ene, and 1,5-diazabicyclo[4.3.0]non-5-ene; dibutylamine-2-ethylhexoate, etc., can improve the curability of the curable composition and can improve the storage stability of the curable composition, so organic tin compounds are preferred. In addition, other acidic catalysts and basic catalysts can also be used as silanol condensation catalysts. The silanol condensation catalysts may be used alone or in combination of two or more.

[0076] The content of the silanol condensation catalyst in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the curable polymer (A). The content of the silanol condensation catalyst in the curable composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, based on 100 parts by mass of the curable polymer (A).

[0077] [Silane coupling agents] The curable composition may further contain a silane coupling agent.

[0078] The silane coupling agent improves the adhesion of the cured product of the curable composition, so it is preferable that the composition contains an amino group-containing silane coupling agent or an epoxy group-containing silane coupling agent, and it is more preferable that the composition contains an amino group-containing silane coupling agent.

[0079] The amino group-containing silane coupling agent means a compound containing, in one molecule, a silicon atom to which an alkoxy group is bonded and a functional group containing a nitrogen atom. The amino group-containing silane coupling agent is not particularly limited, and examples thereof include 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N'-bis-[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(triethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(methyldimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(trimethoxysilyl)propyl]hexamethylenediamine, and N,N'-bis-[3-(triethoxysilyl)propyl]hexamethylenediamine, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is preferred.

[0080] The epoxy group-containing silane coupling agent means a compound that contains a silicon atom with an alkoxy group bonded to it in one molecule and a functional group that contains an epoxy group.The epoxy group-containing silane coupling agent is not particularly limited, and can be, for example, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and is preferably 3-glycidoxypropyltriethoxysilane.

[0081] The content of the silane coupling agent in the curable composition is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, based on 100 parts by mass of the curable polymer (A). The content of the silane coupling agent in the curable composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the curable polymer (A).

[0082] [Plasticizer] The curable composition may contain a plasticizer. The plasticizer is not particularly limited, and examples thereof include phthalates such as dibutyl phthalate, di(2-ethylhexyl)phthalate, diisononyl phthalate, diisodecyl phthalate, and butyl benzyl phthalate; non-aromatic dibasic acid esters such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, and isodecyl succinate; aliphatic esters such as butyl oleate and methyl acetyl ricinoleate; esters of polyalkylene glycols such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; phosphates such as tricresyl phosphate and tributyl phosphate; trimellitic acid esters; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, and the like. Examples of suitable plasticizers include: chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; polyether polyols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and polyether polyols such as derivatives in which the hydroxyl groups of polyether polyols are converted to ester groups, ether groups, and the like; epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate; polyester plasticizers obtained from dibasic acids such as sebacic acid, adipic acid, azelaic acid, and phthalic acid and dihydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; and vinyl polymers obtained by polymerizing vinyl monomers such as acrylic plasticizers by various methods. The plasticizers may be used alone or in combination of two or more.

[0083] [Other additives] The curable composition may contain other additives such as a dehydrating agent, an antioxidant, an ultraviolet absorber, a light resistance stabilizer, a pigment, a dye, an anti-settling agent, an anti-fungal agent, etc. Among these, an antioxidant is preferred.

[0084] Examples of the antioxidant include hindered phenol-based antioxidants, monophenol-based antioxidants, bisphenol-based antioxidants, and polyphenol-based antioxidants, and hindered phenol-based antioxidants are preferred. The content of the antioxidant in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, per 100 parts by mass of the curable polymer (A). The content of the antioxidant in the curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of the curable polymer (A).

[0085] The curable composition may be colored by including a pigment or a dye. The pigment and dye can be used without any particular limitation. Pigments are preferred. The pigment may be either an inorganic pigment or an organic pigment. Specific examples of the inorganic pigment include black pigments such as carbon black, titanium black, and graphite; and metal oxides, nitrides, and oxynitrides. Examples of the metal include at least one of iron, cobalt, aluminum, cadmium, lead, copper, titanium, magnesium, chromium, zinc, and antimony. The content of the pigment in the curable composition is not particularly limited, and is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the curable polymer (A). The content of the pigment in the curable composition is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, relative to 100 parts by mass of the curable polymer (A).

[0086] In general, when the color tone of a curable composition changes before and after curing, a problem may occur in which the expected color tone cannot be obtained after curing. Such a problem is likely to occur when the curable composition is colored using a pigment or dye (especially a black pigment). However, in the curable composition of the present invention, even when a pigment or dye is used, the change in color tone before and after curing can be reduced, and the expected color tone can be obtained after curing. Therefore, since the effect of the present invention is particularly easily obtained, it is preferable that the curable composition contains at least one of a pigment and a dye, and it is more preferable that the curable composition contains a black pigment.

[0087] [Curable composition] The curable composition can be produced by mixing the curable polymer (A), the amine compound (B), the particles (C), the antibacterial agent (D), and other additives as required. The mixing is preferably carried out under reduced pressure.

[0088] The curable composition cures by moisture (water) in the air or moisture (water) contained in a member such as a wall member to produce a cured product. The curable composition can be used as a sealant for a joint structure to form a joint structure.

[0089] The cured product produced by curing the curable composition has a matte surface and a textured surface, and has a reduced gloss. The gloss of the cured product of the curable composition is preferably 15 or less, more preferably 13 or less, more preferably 10 or less, and more preferably 8 or less.

[0090] The gloss of the cured product can be measured using a 60-degree specular gloss meter, such as that commercially available from Tasco Japan under the product name "TMS-724."

[0091] The cured product produced by curing the curable composition preferably has an uneven surface with a maximum height Pz of 100 μm or more, which allows the uneven surface of the cured product to have an appropriate size, and allows the antibacterial agent that has permeated the cured product surface to be satisfactorily exposed to the outside, thereby imparting excellent antibacterial properties to the cured product.

[0092] The maximum height Pz of the uneven shape on the cured product surface of the curable composition is preferably 100 μm or more, more preferably 120 μm or more, more preferably 145 μm or more, more preferably 500 μm or more, and more preferably 1000 μm or more. The maximum height Pz of the uneven shape on the cured product surface of the curable composition is preferably 3000 μm or less, more preferably 2800 μm or less, and more preferably 2500 μm or less. By making the maximum height Pz of the uneven shape 3000 μm or less, the antibacterial agent that has permeated the cured product surface can be well exposed to the outside, and the antibacterial properties of the cured product can be maintained.

[0093] The maximum height Pz of the uneven shape on the surface of the cured product of the curable composition is the "maximum height Pz of the cross-sectional curve" in accordance with JIS B0601:2013.

[0094] The maximum height Pz of the uneven shape can be measured using an electron microscope (e.g., Keyence Corporation's product name "Microscope VHX Series"). For example, when using a Keyence Corporation's product name "Microscope VHX Series" as the electron microscope, the surface of the cured product of the curable composition is observed with an electron microscope (magnification 20 times) to obtain three-dimensional image data, and then the three-dimensional image data is analyzed using a DFD (Depth from Defocus) analysis application installed in the "Microscope VHX Series", whereby the maximum height Pz of the uneven shape on the cured product surface of the curable composition can be measured.

[0095] The average thickness of the cured product produced by curing the curable composition is not particularly limited and may be determined according to the application of the curable composition. The average thickness of the cured product of the curable composition is preferably 100 μm or more, more preferably 500 μm or more. The average thickness of the cured product of the curable composition is preferably 20000 μm or less, more preferably 10000 μm or less. The average thickness of the cured product of the curable composition can be determined by measuring the thickness of the cured product at any 20 points and calculating the arithmetic average value of the measured values.

[0096] As a method for applying the curable composition to the joints to obtain a joint structure, a method is used in which the curable composition is filled into the joints and then cured to harden them. The obtained joint structure has wall members constituting the walls of the architectural structure and a hardened product of the curable composition filled into the joints formed between the adjacent wall members. Examples of the walls of the architectural structure include exterior walls, interior walls, and ceilings.

[0097] An example of a joint in a wall of an architectural structure is a joint formed at a joint. The wall member does not necessarily have to be a plate-like member as long as it constitutes the wall of the architectural structure, and may be a member having an opening that can be opened or closed, such as a sash (window frame), and includes a member that constitutes one side of the architectural structure. Examples of wall members include wood-based materials such as mortar boards, concrete boards, ceramic siding boards, metal siding boards, ALC boards, metal boards, sashes, plywood, and medium density fiberboard (MDF), tiles, polyvinyl chloride, melamine resin, epoxy resin, and stone materials.

[0098] The cured product of the above-mentioned curable composition has excellent matte properties and a textured feel, and the change in color tone before and after curing is reduced, so that the design of the wall member is not impaired, and together with the wall member, a wall section having excellent design can be formed.

[0099] Furthermore, the cured product of the curable composition has excellent antibacterial properties, and can fully meet recent demands for cleanliness. Even when the wall is washed with a detergent, the color will not change due to the detergent, and the excellent design of the wall can be maintained for a long period of time. Effect of the Invention

[0100] The curable composition of the present invention produces a cured product having excellent antibacterial properties, detergent resistance during cleaning, and excellent matte finish and textured feel, and the change in color tone before and after curing is reduced, so that the design and antibacterial properties of other components used together with the curable composition are not impaired. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES

[0102] The following compounds were used in the preparation of the curable compositions of the Examples and Comparative Examples.

[0103] [Curable polymer (A)] Polyoxyalkylene polymer (A1) having a hydrolyzable silyl group (Polyoxyalkylene polymer (A1), number average molecular weight: 18,000, molecular weight distribution: 1.40, main chain: -[CH(CH3)-CH2-O]n-, product name "Exestar 3430" manufactured by Asahi Glass Co., Ltd.) Polyoxyalkylene polymer (A2) having a hydrolyzable silyl group (Polyoxyalkylene polymer (A2), number average molecular weight: 30,000, molecular weight distribution: 1.60, main chain: -[CH(CH3)-CH2-O]n-, manufactured by Wacker Asahi Kasei Silicone Co., Ltd., product name "GENIOSIL STP-E35)

[0104] [Amine compound (B)] Monoamine compound (B1) (stearylamine, melting point: 50°C, Kao Corporation, product name "Fa Min 80S Monoamine compound (B2) (laurylamine, melting point: 28°C, NOF Corp., product name "Nissan Amine BB") Monoamine compound (B3) (behenylamine, melting point: 63°C, NOF Corp., product name "Nissanamine VB-S")

[0105] [Particle (C)] Particles (C1) (glass balloons, Showa Chemical Industry Co., Ltd., product name "Hard Light B04", particle size: 46 to 600 μm, porosity: 30%) Particles (C2) (glass balloons, Potters Ballotini product name "Q Cell 7040", particle size: 5-45 μm, porosity: 70%)

[0106] [Antibacterial agents (D)] Metal-based antibacterial agent (metal-containing inorganic compound, metal atom content: 0.1-10% by mass, zeolite crystal structure: A-type, average particle size: 2.5 μm, manufactured by Sinanen Zeomic Co., Ltd., product name "Zeomic Ztype")

[0107] [Silane coupling agents] Aminosilane coupling agent [N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, product name "KBM-603" manufactured by Shin-Etsu Chemical Co., Ltd.]

[0108] [Pigment] Black pigment (Nippon Pigment Co., Ltd., carbon black)

[0109] [Silanol condensation catalyst] Dibutyltin oxylaurate (manufactured by Nitto Kasei Co., Ltd., product name "Neostan U-130")

[0110] (Examples 1 to 8, Comparative Examples 1 to 5) The curable polymer (A), amine compound (B), particles (C), metal-based antibacterial agent (D), aminosilane coupling agent, black pigment, and dibutyltinoxylaurate shown in Table 1 in predetermined amounts were uniformly mixed under reduced pressure to prepare a curable composition.

[0111] For the obtained curable composition, the volume concentration of particles (C) having a particle size of 5 to 1000 μm is shown in Table 1.

[0112] The obtained curable composition was cured for one week in an environment with an atmospheric temperature of 23° C. and a relative humidity of 50%, to obtain a cured product.

[0113] The gloss of the resulting cured product was measured as described above, and the results are shown in Table 1.

[0114] The maximum height Pz (μm) of the irregularities formed on the surface of the obtained cured product was measured in the manner described above, and the measurement results are shown in Table 1. The average thickness of the obtained cured product was 3000 μm.

[0115] The resulting cured product was measured for unevenness, color tone, antibacterial properties and detergent resistance in the manner described below. The results are shown in Table 1.

[0116] (Uneven feeling) The irregularities formed on the surface of the cured product of the curable composition were visually observed and evaluated according to the following criteria. A: Large irregularities were observed. B Fine irregularities were observed. C: No irregularities were observed.

[0117] (color tone) The color tone of the surface before curing the curable composition and the color tone of the surface of the cured product obtained by curing the curable composition were measured using a spectrophotometer (manufactured by Konica Minolta, product name "CM-5", measurement method: SCE method, field of view: 10 degrees, light source: D65). Then, the color difference (ΔL: difference in light and dark) of the cured product surface after curing was calculated based on the color tone of the surface of the curable composition before curing. Note that the larger the value of ΔL, the whitish the surface of the cured product is compared to the reference color, and the smaller the value of ΔL, the darker the surface of the cured product is compared to the reference color. The value of ΔL is preferably -2.0 or more and +2.0 or less.

[0118] (Antibacterial) The cured product of the curable composition was observed for antibacterial properties in accordance with JIS Z 2801, the antibacterial property test method for antibacterial processed products, and evaluated based on the following criteria. A: The logarithm of the viable cell count was -0.2 or less. B: The logarithm of the viable cell count was greater than -0.2 and less than 0.5. C: The absolute value of the viable cell count was 0.5 or more.

[0119] (detergent resistance) 0.2 mL of chlorine bleach was dropped onto the cured product of the curable composition, covered with glass and left to stand for 24 hours, after which the chlorine bleach was thoroughly washed off with running water. Thereafter, the surface of the cured product was observed with an optical microscope and with the naked eye, and evaluated based on the following criteria. A: No color change on the surface of the cured material was observed either visually or under an optical microscope. B: No color change was observed on the surface of the cured product with the naked eye, but was observed using an optical microscope. C: Color changes on the surface of the cured material were observed both visually and with an optical microscope.

[0120] When no color change on the surface of the cured product is observed both visually and with an optical microscope (criterion A above), the surface of the cured product can still be maintained free of color change even after a long period of time, such as several months or more, has passed since the chlorine bleach was washed away, and the product can be evaluated as having particularly excellent detergent resistance.

[0121] [Table 1]

Claims

1. A curable composition comprising 100 parts by mass of a curable polymer, 2 parts by mass or less of an amine compound having a melting point of 25 to 80°C, particles having a particle size of 5 to 1000 μm, and an antibacterial agent.

2. 2. The curable composition according to claim 1, wherein the gloss of the cured product is 15 or less.

3. 3. The curable composition according to claim 1, wherein the curable polymer has a hydrolyzable silyl group in the molecule.

4. 3. The curable composition according to claim 1, wherein the curable polymer has a polyoxyalkylene structure.

5. 3. The curable composition according to claim 1, wherein the volume concentration of the particles having a particle diameter of 5 to 1000 μm is 10% by volume or less.

6. 3. The curable composition according to claim 1, wherein the particles having a particle diameter of 5 to 1000 μm have a porosity of 20 to 80%.

7. 3. The curable composition according to claim 1, wherein the surface of the cured product has an uneven shape with a maximum height Pz of 100 μm or more.

Citation Information

Patent Citations

  • Room temperature-curable composition

    JP1997100408A

  • Sealing material composition

    JP1999035923A

  • Antimicrobial mildewproof organopolysiloxane composition

    JP1999199777A

  • Sealing material composition and exterior wall

    JP2019151676A

  • Curable composition

    JP2019151687A