Seamless steel pipe rolling plug, manufacturing method thereof, seamless steel pipe rolling plug mill and seamless steel pipe manufacturing method
The seamless steel pipe rolling plug with a roughened surface and oxide layer addresses the issues of surface abrasion and damage in conventional plugs, enhancing adhesion and wear resistance to extend plug life and reduce manufacturing costs.
Patent Information
- Application Number
- JP2024032952
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-03-05
AI Technical Summary
Conventional seamless steel pipe rolling plugs made of high Cr-based high alloy steel face issues with surface abrasion, local gouging, and plug damage due to high pressure and temperature, leading to reduced lifespan and poor dimensional accuracy, while existing solutions like multiple heat treatments are time-consuming and costly.
A seamless steel pipe rolling plug with a roughened outer surface and an oxide layer, featuring specific composition and roughness, enhances adhesion and wear resistance without requiring multiple heat treatments, ensuring prolonged plug life and improved deformation control.
The solution provides a plug with enhanced adhesion and wear resistance, extending its lifespan and reducing manufacturing costs by minimizing the need for frequent replacements, thus improving productivity and cost-efficiency.
Smart Images

Figure 2024147499000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a mandrel (hereinafter referred to as "plug") used in Mannesmann plug mill rolling of seamless steel pipes, and in particular to a plug for seamless steel pipe rolling having a hard oxide layer formed on its surface which has excellent adhesion to the base material and wear resistance and thereby improves the plug life, a manufacturing method thereof, a plug mill for seamless steel pipe rolling, and a manufacturing method of seamless steel pipes. [Background technology]
[0002] As the plug used in plug mill rolling in the conventional manufacturing method of seamless steel pipe, a high Cr-based high alloy steel containing, by mass%, 1.0-2.0% C, 12-20% Cr, 1.0-2.5% Ni, 1.0-2.5% Mo and / or W (Mo+W), with the balance being mainly Fe, is used. Such a plug made of a high Cr-based high alloy steel has excellent high-temperature strength and high-temperature oxidation resistance, and is therefore particularly suitable as a plug used under severe conditions such as plug mill rolling.
[0003] However, even plugs made of such materials have had the problem that they often become unusable due to damage to the plug caused by surface wear, local gouges, seizure, etc., at a stage when only a small number of plugs have been rolled due to high pressure and high temperature in actual operations. Since such damage causes inner surface defects and poor dimensional accuracy of the product, there is a demand for the development of plugs with excellent wear resistance in order to improve the life of the plug, etc.
[0004] Generally, in order to improve the wear resistance, it is necessary to increase the strength of the plug surface, and as a technology for solving this problem, for example, Patent Document 1 discloses a plug in which large amounts of Mo and W, which increase strength, are added to the plug so as to have a hardness of 900 HV or more.
[0005] Also, for example, Patent Document 2 discloses a method in which an oxide layer is formed on the surface of a plug material by heating in an oxidizing atmosphere, followed by a first heat treatment in which the plug material is cooled at a cooling rate equal to or faster than natural cooling in air over a temperature range of at least 350°C, and then a second heat treatment in which the plug material is heated again in an oxidizing atmosphere to form an oxide layer again on its surface. As a result, in the oxide layer formed by the first heat treatment, portions in which the generation of Ni-enriched base iron particles is insufficient and adhesion to the base iron is poor are peeled off during the cooling process at a cooling rate equal to or faster than natural cooling after the first heat treatment, and then, in the process in which a new oxide layer is formed by another heat treatment, Ni-enriched base iron particles increase in the portions with poor adhesion, and Ni is selectively oxidized to form an oxide layer like a nail at the interface between the oxide layer and the base iron (anchor effect). The anchor effect obtained by this second heat treatment improves adhesion between the oxide layer and the base iron, and the oxide layer protects the plug, enabling the plug life to be extended. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 57-198243 [Patent Document 2] Japanese Patent Publication No. 61-281819 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, there has been a trend toward higher alloying of rolled materials used in the manufacture of seamless steel pipes, which has resulted in increased rolling loads and a tendency to increase the rolling speed in order to improve productivity. There has been a problem that the high hardness caused by the addition of large amounts of high alloys to the rolled materials and the increase in rolling speed result in an increase in the unit cost of plugs. Patent Document 1 discloses a technology that contains a large amount of alloying elements for the purpose of increasing strength, but there is also a need to establish a technology that can improve wear resistance without containing a large amount of alloying elements.
[0008] Moreover, in manufacturing a plug, as in the technique described in Patent Document 2, performing heat treatment twice for the purpose of increasing adhesion between the oxide layer and the base steel takes time, which increases manufacturing costs.
[0009] Furthermore, as with the technology described in Patent Document 2, when the adhesion of the oxide layer is improved by heat treatment, if segregation occurs near the surface of the base material, the anchor effect may not be sufficient, and the oxide layer may partially peel off when it comes into contact with the rolled material, causing seizure and creating gouges. These gouges are then transferred to the rolled material, causing scratches on the inner surface of the rolled material. Because plug mill plugs have a rolled surface all around, they need to be replaced even if the oxide layer is only partially peeled off.
[0010] Furthermore, even if only the adhesion of the oxide layer is improved, it is difficult to also improve the wear resistance of the oxide layer. Under a severe rolling environment, the oxide layer wears away and becomes thinner, which can prevent seizure, but if the high-temperature strength of the plug body is low, it becomes difficult to suppress deformation of the plug. Conversely, even if the oxide layer has high high-temperature strength, if the adhesion of the oxide layer to the base metal is low, it is difficult to suppress seizure if the base metal component is mainly iron, and therefore early separation occurs, seizure occurs, and gouges occur. As described above, it has been difficult to obtain a plug which can be used under severe rolling conditions, has an oxide layer with good adhesion and wear resistance, and has a long life.
[0011] The present invention has been made in consideration of the above circumstances, and has an object to provide a plug for rolling seamless steel pipes which has improved adhesion and wear resistance and satisfactorily suppresses deformation without the need for multiple heat treatments, a manufacturing method thereof, a plug mill for rolling seamless steel pipes, and a manufacturing method of seamless steel pipes. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention provides a method for forming a highly adherent oxide layer that is not affected by the heat treatment method by subjecting the outer surface of the plug base metal to roughening. Therefore, even if the plug material is heat treated only once, a highly adherent oxide layer is formed, and therefore, even if the oxide layer wears away or peels off during the rolling process, a sufficient time can be secured until the base metal of the plug is exposed on the surface and the metal comes into contact with the rolled material.
[0013] The present invention has been completed based on the above findings, and provides the following [1] to [7]. [1] A seamless steel pipe rolling plug, characterized in that the arithmetic mean roughness Ra of an outer surface of a plug base metal is 0.04 μm or more, and the surface of the plug base metal has an oxide layer. [2] The plug for rolling seamless steel pipes according to [1], characterized in that an outer surface of the plug base metal has polished marks in a direction perpendicular to the rolling direction of the plug, and has an arithmetic mean roughness Ra of 0.04 μm or more in a test in which roughness measurement is performed in the rolling direction of the plug. [3] The seamless steel pipe rolling plug according to [1] or [2], characterized in that the plug base metal has a chemical composition containing, by mass%, 0.3-1.5% Si, 0.3-1.5% Mn, 0.01-5.0% Ni, 12-20% Cr, 0.1-3.0% in total of one or two of Mo and W, and the balance consisting of Fe and unavoidable impurities. [4] The seamless steel pipe rolling plug according to [3], characterized in that the chemical composition further contains, in mass%, C: 1.0 to 2.0%, Al: 0.01 to 0.1%, and V: 0.01 to 0.1%. [5] A method for producing a seamless steel pipe rolling plug according to any one of [1] to [4], 1. A method for producing a plug for rolling seamless steel pipes, comprising processing a plug base material by polishing, grinding or cutting. [6] A plug mill for rolling seamless steel pipes, comprising the plug for rolling seamless steel pipes according to any one of [1] to [4] above. [7] A method for producing a seamless steel pipe, comprising using a seamless steel pipe rolling plug according to any one of [1] to [4] above. Effect of the Invention
[0014] According to the present invention, there is provided a plug for rolling seamless steel pipes which has improved adhesion and wear resistance and which realizes suppression of deformation without the need for multiple heat treatments. This makes it possible to obtain a plug with a longer life than conventional plugs. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram showing an outline of plug mill rolling. [Diagram 2] FIG. 1 is a diagram showing an outline of a hot sliding test machine. [Diagram 3] FIG. 1 is a diagram showing a test piece after a typical hot sliding test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiments.
[0017] The seamless steel pipe rolling plug of the present invention has an outer surface of the plug base metal with an Ra of 0.04 μm or more, and has an oxide layer on the surface of the plug base metal.
[0018] Fig. 1 is a diagram showing an overview of plug mill rolling according to the present invention, and the plug for rolling seamless steel pipes will be described below. As shown in Fig. 1, the plug 1 of the present invention is installed in a rolling mill 101, and its rear end is supported by a bar 3. The plug 1 of the present invention is used for thinning rolling, which reduces the wall thickness of a hollow S fed between a pair of rolling arc-shaped (caliber) rolls 2a, 2b, to a predetermined wall thickness. After the subsequent steps, the plug becomes a seamless steel pipe.
[0019] The shapes of the plug 1 and the plug base metal of the present invention are not particularly limited; however, for example, as shown in FIG. 1, they may have a cylindrical shape or a generally conical shape whose cross-sectional shape gradually becomes smaller in the rolling direction.
[0020] The shape of the plug 1 of the present invention is not particularly limited, and in terms of size, if the outer diameter of the plug is less than φ40 mm, the dimensional accuracy of the mother tube is likely to be affected when the oxide scale wears away, and therefore, the outer diameter of the plug (the maximum outer diameter of the plug as viewed in a cross section perpendicular to the rolling direction) is preferably φ40 mm or more. There is no particular upper limit, but it is preferably φ500 mm or less.
[0021] <Outer surface roughness of plug base material> Next, the reason for limiting the arithmetic mean roughness Ra of the outer surface of the plug base metal of the present invention will be explained.
[0022] Ra:0.04μm or more In order to improve the adhesion between the plug base metal and the oxide layer formed on the plug base metal, the arithmetic mean roughness Ra of the outer surface of the plug base metal is set to 0.04 μm or more. In order to further suppress the peeling of the oxide, the outer surface roughness Ra of the plug base metal is preferably 0.50 μm or more. In consideration of ease of processing, it is more preferable that the outer surface roughness Ra is 1.00 μm or more, which is effective even when the base metal is as cut. Furthermore, it is more preferable that the outer surface roughness Ra is 5.00 μm or more. Although there is no particular upper limit, if the base material is too rough, irregularities along the roughness are formed on the surface of the test piece after heat treatment, which may cause transferred defects or partial seizure. Therefore, the outer surface roughness Ra of the plug base material is preferably less than 100.00 μm. The outer surface roughness Ra of the plug base material is more preferably less than 10.00 μm. The arithmetic mean roughness Ra is measured in accordance with the provisions of JIS B 0601:2013. The roughness measurement direction is not limited to a specific direction.
[0023] Furthermore, in particular, because the presence of polishing marks in a direction perpendicular to the rolling direction of the plug improves the adhesion of the oxide layer, the arithmetic mean roughness Ra of the outer surface of the plug base metal is preferably 0.04 μm or more in a test in which roughness measurement is performed in the rolling direction (axial direction) of the plug. In a test in which roughness measurement is performed in the rolling direction (axial direction) of the plug, the arithmetic mean roughness Ra is more preferably 0.50 μm or more, and even more preferably 1.00 μm or more. Most preferably 5.00 μm or more. In addition, although there is no particular upper limit, the arithmetic mean roughness Ra of the outer surface of the plug base metal is preferably less than 100.00 μm in a test in which roughness measurement is performed in the rolling direction (axial direction) of the plug. More preferably, the outer surface roughness Ra of the plug base metal is less than 10.00 μm. Note that measuring the roughness in the rolling direction (axial direction) of the plug means running the contact terminal of a roughness meter parallel to the rolling direction of the plug and measuring in accordance with the provisions of JIS B 0601:2013 mentioned above.
[0024] Although the detailed mechanism behind why polishing marks perpendicular to the rolling direction improve the adhesion of the oxide layer is unknown, the following can be cited. Because the roll shape of a plug mill is caliber-shaped, when the central plug comes into contact with the pipe, material flows in the circumferential direction. As a result, tensile stress acts in the circumferential direction of the plug. By providing roughness perpendicular to the rolling direction, metal flow becomes smoother and the load on the plug is reduced. On the other hand, when roughness is provided parallel to the rolling direction, unevenness occurs in the circumferential direction, making it difficult for material to flow, meaning that metal flow tends to stagnate. Therefore, it is thought that peeling of the oxide layer is less likely to occur when polishing marks are perpendicular to the rolling direction than when they are parallel to the rolling direction.
[0025] It should be noted that the "polishing marks" refer to linear patterns that are produced on the surface of the plug when grinding, polishing, or the like is performed while the plug is rotated. In other words, the linear patterns that are formed on the plug surface in a direction perpendicular to the rolling direction of the plug are polishing marks.
[0026] In addition, since the presence of polishing marks in a direction perpendicular to the rolling direction improves the adhesion of the oxide layer, it is preferable that the outer surface of the plug base metal has polishing marks in a direction perpendicular to the rolling direction (axial direction) of the plug.
[0027] Although there is no particular limitation on the inner surface roughness of the plug base metal, the inner diameter of the plug changes (increases) when the oxide layer on the inner diameter of the plug peels off, causing the fit between the bar and the plug to become loose and making it easier for rattle to occur, so the inner surface roughness Ra of the plug base metal is preferably 0.05 μm or more. The inner surface roughness Ra of the plug base metal is preferably less than 10.00 μm.
[0028] <Oxide layer> In the present invention, it is necessary to have an oxide layer on the surface of the plug base metal. Details will be explained below. If there is no oxide layer on the plug base metal, the adhesion and wear resistance of the plug base metal will decrease, so it is necessary to have an oxide layer on the surface of the plug base metal. In order to obtain heat insulating properties that contribute greatly to adhesion, wear resistance, and deformation suppression, the thickness of the oxide layer is preferably 0.10 mm or more. More preferably, it is 0.40 mm or more. On the other hand, if the oxide layer is too thick, the oxide layer may peel off all at once, so the thickness of the oxide layer is preferably 3.00 mm or less. More preferably, it is 2.00 mm or less. Furthermore, it is considered that the oxide layer of iron has a spinel type that is superior in high-temperature ductility to the corundum type, so that the oxide layer preferably has a spinel type structure, for example, a layer containing Cr and composed of Fe and O. The spinel type is a crystal structure that shows a face-centered cubic arrangement. In addition, the spinel type structure shown here includes both normal spinel type and inverse spinel type. In addition, oxide layers formed on the surface of normal hot work tool steels such as hematite, magnetite, and wustite are also included. In order to obtain the above oxide, it is preferable to control the oxygen concentration and water vapor amount in the furnace, as well as the heating temperature and holding time.
[0029] <Component composition of plug base material> If the amount of alloying elements added is small and the high-temperature strength is low, the plug becomes hot during rolling and is prone to deformation. However, if a large amount of alloying elements is added in order to increase the high-temperature strength, the oxide layer becomes thin or the adhesion becomes poor, and the plug may become prone to becoming hot. Taking these points into consideration, the preferable content ranges of the alloy components of the plug base metal of the present invention and the reasons therefor will be explained below. In the following, % indicating the alloy components is mass %.
[0030] The alloy of the plug base metal of the present invention preferably has a composition containing, by mass%, 0.3-1.5% Si, 0.3-1.5% Mn, 0.01-5.0% Ni, 12-20% Cr, 0.1-3.0% in total of one or both of Mo and W, and the balance being Fe and unavoidable impurities.
[0031] Silicon: 0.3 to 1.5% Si is contained to improve the deoxidation and flow of the molten metal. In addition, when Si is contained, the amount of wustite in the oxide layer is reduced, and the amount of magnetite, which is a high spinel type oxide that is said to be hard and highly wear-resistant, is increased. If the Si content is less than 0.3%, the effect cannot be obtained. Therefore, the Si content is set to 0.3% or more. It is preferably 0.4% or more. It is more preferably 0.5% or more. It is even more preferably 0.6% or more. On the other hand, if the Si content exceeds 1.5%, it will lead to a decrease in toughness. In addition, if Si is contained excessively, a SiO2 layer will be formed at the interface between the oxide and the base steel, and the impact resistance will decrease. Therefore, the Si content is set to 1.5% or less. In addition, the Si content is preferably 1.4% or less. In addition, the Si content is more preferably 1.2% or less. In addition, the Si content is even more preferably 1.0% or less. In addition, the Si content is most preferably 0.7% or less.
[0032] Mn: 0.3 to 1.5% Mn is added together with Si for deoxidation. If the Mn content is less than 0.3%, sufficient deoxidation effect cannot be obtained. Therefore, the Mn content is set to 0.3% or more. Preferably, it is 0.4% or more. More preferably, it is 0.5% or more. Even more preferably, it is 0.6% or more. On the other hand, if the Mn content is more than 1.5%, the toughness decreases. Therefore, the Mn content is set to 1.5% or less. Furthermore, taking into consideration the range in which the spinel-type oxide layer increases, the Mn content is preferably 1.4% or less. The Mn content is more preferably 1.3% or less, and even more preferably 1.2% or less.
[0033] Ni: 0.01 to 5.0% Ni improves the hardenability of the matrix, and there is no effect of adding it if the Ni content is less than 0.01%. Therefore, the Ni content is set to 0.01% or more. It is preferably set to 0.6% or more. It is more preferably set to 1.0% or more, and even more preferably set to 1.2% or more. On the other hand, such an effect of improving hardenability is saturated if Ni is contained in excess of 5.0%. Furthermore, Ni contributes to improving the adhesion of the oxide layer through the mixing of Ni-enriched base iron particles in the oxide layer, but if excessive Ni is added, it causes a decrease in machinability due to insufficient softening and a deterioration in heat treatability due to the generation of retained austenite. Therefore, the Ni content is set to 5.0% or less. Moreover, the Ni content is preferably set to 4.5% or less. The Ni content is more preferably set to 3.5% or less. It is even more preferably set to 3.0% or less.
[0034] Cr: 12~20% Cr provides high-temperature strength to plugs for plug mill rolling used under high temperature and high pressure, and also provides corrosion resistance to plugs that are often used in corrosive environments contained in lubricants. In order to obtain these effects, it is necessary to make the Cr content 12% or more. Therefore, the Cr content is 12% or more. It is preferably 13% or more. It is more preferably 14% or more, and further preferably 15% or more. On the other hand, if the Cr content exceeds 20%, it becomes difficult to make the oxide layer sufficiently thick when heat treatment is performed, and a ferrite phase is generated, impairing heat treatability. Therefore, the Cr content is 20% or less. Furthermore, in order to reduce the corundum-type oxide layer and to contain more spinel-type oxide, the Cr content is preferably 19% or less. It is more preferably 18% or less.
[0035] Sum of Mo and W (Mo+W): 0.1-3.0% Mo and W are dissolved in the matrix to improve high-temperature properties such as high-temperature softening resistance, and also bond with C during tempering to form fine composite carbides, improving wear resistance. Furthermore, Mo and W are more noble in bonding with O than Fe, so selective oxidation occurs when forming an oxide layer, and the interface between the oxide layer and the base steel becomes shaped like a nail, resulting in high adhesion due to the anchor effect. These effects can be obtained by making the total content of one or both of Mo and W (Mo+W) 0.1% or more. For this reason, the total content of one or both of Mo and W (Mo+W) is set to 0.1% or more. It is preferably set to 0.2% or more, more preferably 0.3% or more, and even more preferably 0.4% or more. On the other hand, since Mo and W are ferrite forming elements, increasing their contents narrows the composition range in which austenite is generated. Even if the amount of C or Ni is increased to compensate for this narrow composition range, the content of each element is limited as described above. Therefore, the total content of Mo and W (Mo+W) is 3.0% or less. It is preferably 2.8% or less, more preferably 2.6% or less, and further preferably 2.4% or less. For the above reasons and from the viewpoint of economy, one or both of Mo and W are contained, and the total content of Mo and W (Mo+W) is 0.1 to 3.0%.
[0036] In the present invention, the above-mentioned components are the basic composition. In the present invention, the following components may be further added as optional elements, if necessary.
[0037] C: 1.0-2.0% C combines with Cr, Mo, V, W, etc. to form a composite carbide with high hardness and improve wear resistance. It also partially dissolves in the austenite of the base, and contributes to the effect of high strength due to the martensite formed by the quenching operation. In this way, C has the effect of improving wear resistance and hardness and strength from room temperature to high temperature. If the C content is less than 1.0%, the amount of carbide crystallization is small, and therefore high wear resistance cannot be obtained. For this reason, when C is contained, the C content is 1.0% or more. In addition, from the viewpoint of improving the balance between the amount of carbide crystallization and thermal shock resistance, it is preferably 1.2% or more. More preferably, it is 1.3% or more. On the other hand, if the C content exceeds 2.0%, the amount of carbide crystallization becomes excessive, making the material extremely sensitive to thermal shock and causing early cracking. Therefore, when C is contained, the C content is 2.0% or less. In addition, it is preferably 1.8% or less. In terms of the balance between the amount of carbide crystallization and thermal shock resistance, it is more preferably 1.5% or less.
[0038] Al: 0.01 to 0.1% Al is added together with Si and Mn for deoxidation. If the Al content is less than 0.01%, a sufficient deoxidation effect cannot be obtained. Therefore, when Al is contained, the Al content is set to 0.01% or more. Preferably, it is set to 0.03% or more. On the other hand, if the Al content is more than 0.1%, the toughness decreases. Therefore, when Al is contained, the Al content is set to 0.1% or less. Preferably, it is set to 0.09% or less. More preferably, it is set to 0.08% or less.
[0039] V: 0.01 to 0.1% Addition of a small amount of V turns into carbides or nitrides, which contributes to the refinement of crystal grains and improves toughness. This effect can be obtained by making the V content 0.01% or more. Therefore, when V is contained, the V content is 0.01% or more. It is preferably 0.03% or more. On the other hand, when the V content exceeds 0.1%, the above effect is saturated and a hard phase is formed, which reduces toughness. Therefore, when V is contained, the V content is 0.1% or less. It is preferably 0.08% or less. It is more preferably 0.05% or less.
[0040] The balance other than the above consists of Fe and inevitable impurities.
[0041] <Plug manufacturing method> Next, the method for producing a seamless steel pipe rolling plug of the present invention will be described.
[0042] A plug may be manufactured by a general known manufacturing method. For example, it is manufactured by casting in which molten steel is poured into a frame made by a wooden mold or a lost wax method. In the case of as-cast (cast surface), the roughness of the base metal surface exceeds 100.00 μm. Furthermore, when observing the surface of the base metal, the cast surface is formed in a shape that is convex with respect to the reference surface. When the oxide layer wears away, the convex part of the cast surface becomes exposed, and this part may form seizure, gouge the plug surface, and promote deformation. Therefore, from the viewpoint of suppressing seizure, it is not preferable that the surface of the plug base metal has a convex roughness. In order to suppress seizure, it is important to prevent contact between the metal surface of the plug and the material to be rolled as much as possible, so it is preferable that the surface of the plug base metal has a concave roughness due to processing.
[0043] In order to achieve the outer surface roughness of the plug base material of the present invention, the plug base material is processed by polishing and grinding or cutting. Polishing and grinding is preferably performed using a coated abrasive having a grit size of 1000 or less. The smaller the grit size number of the polishing and grinding, the coarser the surface becomes. For polishing and grinding using a coated abrasive, emery paper, grinding wheel polishing, lapping polishing, polishing polishing (buff polishing), barrel polishing, and electrolytic polishing can be used. The grit size number of the abrasive cloth represents the grain size measured by the method specified in JIS R 6011 or JIS R 6012, as compared to the grain size specified in JIS R 6010. In the JIS standard, it is represented by P, but in this application, it is represented by the commonly called number (# or number).
[0044] The reason for setting the grit size number for polishing and grinding to 1000 or less is to obtain a specified outer surface roughness of 0.04 μm or more, Ra. Preferably, it is 240 or less. On the other hand, as for the lower limit, the lower the number, the easier it is to cut the base material, so if the force is not evenly applied, the corners, which have a smaller area, are cut too much and so-called sagging is likely to occur. If this sagging occurs, it is necessary to cut the entire surface to correct it, and there is a possibility that it will deviate from the specified dimensions. It is preferable to set it to 80 or more because it is difficult to achieve parallelism.
[0045] Polishing and grinding using abrasive cloth and paper, polishing and grinding using electrolytic polishing, and cutting are preferable because they can uniformly control the roughness. Furthermore, cutting in which the pitch and depth of the roughness can be controlled by a program, such as NC lathe processing, is more preferable. For example, the cutting speed is preferably 5 to 500 mm / sec, and the cutting amount per cut is preferably 0 to 30 μm, and more preferably the cutting speed is 100 to 300 mm / sec, and the cutting amount per cut is preferably 0 to 10 μm.
[0046] Another method of roughening the outer surface is shot blasting, but shot blasting is a method in which metal chips or sand are pushed out with air or other means and struck against the base material, and as the surface is processed by impact, there is a possibility that the base material surface will become convex. Also, the shape of the shot material changes the more shot blasting is used, so it is thought to be difficult to process uniformly. Since the adhesion changes in areas with different roughness, some of the oxide layer may peel off and cause gouges due to seizure. For this reason, processing by shot blasting is not recommended.
[0047] As explained above, in the present invention, by subjecting the surface of the plug base metal to a predetermined roughness treatment and, in some cases, manufacturing the plug with a predetermined composition, even with a single heat treatment (without repeating heat treatment multiple times), an oxide layer with excellent adhesion and excellent wear resistance is formed, and even after a severe rolling process, the base steel is unlikely to be exposed on the surface. This makes it possible to improve the life of the plug. In addition, since the desired effects can be obtained even if the content of alloy elements, which have a high unit price and are intended to increase strength, is reduced, the original unit price of the plug can be reduced. Furthermore, by improving the plug life, the amount of pipe that can be rolled per plug increases, which reduces the tool cost as a percentage of the product manufacturing cost, thereby also reducing manufacturing costs.
[0048] The present invention also provides a plug mill for rolling seamless steel pipes equipped with the above-mentioned plug for rolling seamless steel pipes, and further provides a method for manufacturing seamless steel pipes using the above-mentioned plug for rolling seamless steel pipes.
[0049] Furthermore, the present invention can also be applied to equipment other than a plug mill, such as plugs used in a piercer or elongator. EXAMPLES
[0050] The present invention will be further described below with reference to examples.
[0051] Example 1 In order to evaluate the adhesion of the oxide layer, a simulation experiment of plug mill rolling was carried out using a hot roll abrasion / thermal shock combined testing device, and the relationship between the remaining thickness of the oxide layer of a test piece simulating a plug and the state of peeling and seizure of the oxide layer, which serve as indicators of adhesion, was evaluated.
[0052] Figure 2 is a schematic diagram of the above simulation test (hot sliding test machine). Specifically, a rotating body called the counterpart R and a test piece 4, a sample with an oxide layer, were used. The counterpart R could be heated by installing a coil 5 around it, and was set to maintain a constant temperature throughout the test. The dimensions of the test piece 4 were length 30 mm x width 5 mm x height 15 mm, and the dimensions of the counterpart R were φ190 mm x 5L mm. The counterpart R, which had reached the specified temperature under a load of 150 kg for 1 minute, was brought into contact with the test piece 4 at 350 rpm.
[0053] The test pieces for adhesion evaluation were processed on the surface of the base material having the composition shown in Table 1 above, so as to have the roughness shown in Table 2. The processing was carried out by the method shown in Table 2, and the cutting processes of levels 1 to 4 were performed by surface processing by milling and surface grinding by surface grinding. In addition, for levels 5 and 6, polishing and grinding were carried out by a method of grinding with abrasive paper of No. 1000 and No. 3000. Each test piece was held at 1185°C for 2 hours in an air furnace to form an oxide layer on the surface of the test piece. The evaluation criteria are as follows, and the evaluation results are shown in Table 2. (judgment criteria) A (pass, better): There is no peeling of the oxide layer, and no gouges due to seizure are observed. B (pass, excellent): There is no deformation (gouges) due to seizure, and although some peeling of the oxide layer is observed, it accounts for less than 1.0% of the total, and the adhesion is judged to be excellent. C (Pass): There is localized seizure, transferred scratches are found on the mating piece, and some areas of the oxide layer have peeled off, but this is less than 1.0% of the total, and the adhesion is judged to be good. D (Fail): Peeling of the oxide layer was observed throughout the entire surface, and the adhesion was determined to be poor.
[0054] Figure 3 shows a front view (upper side) and a side view (lower side) of the test piece 4 after a typical hot sliding test. For the side view, the test piece 4 after the test was cut in half and processed so that the center of contact with the bottom R part of the mating piece R could be seen, and the mating piece contact area 13 was observed from the side with a digital microscope (Keyence VHX-5000) at a magnification of 30 times.
[0055] Figure 3(a) shows the results for level 4 in Table 2, and Figure 3(b) shows the results for level 6. As shown in Figure 3(a), in level 4 (Ra 0.640 μm) in Table 2, the oxide layer 11 remained in the mating piece contact area 13 (contact area with the mating piece R) even after the test, and no gouges 20 occurred, but as shown in Figure 3(b) in level 6 (Ra 0.025 μm), no oxide layer 11 remained on the base material 10 in the mating piece contact area 13 (contact area with the mating piece R), gouges 20 occurred, and the adhesion was poor. In level 5, some peeling of the oxide layer 11 was observed on the base material 10, but the peeled areas were less than 1.0% of the total, and no gouges 20 due to seizure occurred.
[0056] In the case of the unprocessed cast surface, level 1, some peeling of the oxide layer 11 was observed on the base metal 10, but the peeled area was less than 1.0% of the total area, and no gouges 20 were observed on the plug. However, localized seizure occurred, and transferred defects were observed on the mating piece. Level 1 (Ra121.290μm) had the same oxide layer thickness before the test as level 3 (Ra1.180μm), but the cast surface was left as it was, resulting in a convex shape. Furthermore, by increasing the roughness of the base metal, the oxide layer was present on the outer surface side of the base metal, and when the oxide layer wore away, the metal part of the base metal was exposed more quickly, causing the oxide layer to seize at that location. In addition, defects were observed on the mating piece R. This is thought to be due to transferred defects or partial seizure caused by the base metal being too rough, which resulted in unevenness along the roughness being formed on the surface of the test piece after heat treatment. In levels 2 to 4, no peeling of the oxide layer was observed over the entire test piece, and no deformation (gouges) due to seizure was observed. Based on the above results, the ranking of the evaluation results is (excellent) A>B>C>D, with levels of A, B, and C being judged to indicate good adhesion, and levels of A, B, and C, where the remaining oxide layer thickness after the test was 0.10 mm or more, were obtained and the adhesion was judged to have reached an acceptable level.
[0057] Example 2 Table 3 shows the composition of the plug base metal of the plug used in this example. Plug base metals having the chemical compositions of Steels No. A to W were subjected to a heat treatment in which they were held at 1,185°C for 2 hours in air (using an air atmosphere furnace) to form an oxide layer on the surface of the plug base metal, thereby obtaining plugs Nos. 1 to 35 listed in Table 4. For plugs No. 1 to 21, the base metal surface was processed by milling, and the target value of the arithmetic mean roughness Ra of the base metal was set to 10.00 μm. For plugs No. 22 to 23, the base metal was not processed, and the as-cast cast surface (Ra of 100.00 μm or more) was left. For plugs No. 24 to 27 using steel No. B, the target value of the arithmetic mean roughness Ra of the base metal was changed from 100.00 to 0.01 μm. For plugs Nos. 28 to 31 using steels Nos. H, K, V and W, the target value of the arithmetic mean roughness Ra of the base metal was set to 1.00 μm. The actual Ra values of the above plugs are shown in Table 4.
[0058] [evaluation] Using each of the above plugs, hot plug mill rolling was performed on the same rolled material, and the plug was rolled until the plug life. The rolled material used had an outer diameter of φ223 mm, a wall thickness of 16.99 mm, and a length of 8 m, and the material specifications were 0.2 mass% C-13 mass% Cr. The above rolling was performed under rolling conditions where the reduction amount was a thickness reduction rate of 30%. The temperature of the rolled material was 950 to 1000°C, as measured by a radiation thermometer. The plug was water-cooled once after rolling, and after the outer surface temperature of the plug became 50°C or less, the water cooling was continued for 10 minutes, and the plug was used again.
[0059] The plug life was evaluated based on the following criteria in order to evaluate whether good wear resistance and deformation suppression were achieved.
[0060] (Adhesion and abrasion resistance evaluation) After rolling, the plug surface was visually observed to see if any seizure had occurred, and in those cases in which no seizure had occurred, if the thickness of the oxide layer measured in a measurement area of 30 mm × 30 mm with a non-contact thickness gauge utilizing an ultrasonic sensor (37DL PLUS, made by Nippon Panametrics Co., Ltd.) was less than 0.10 mm, it was judged, based on the above results, that the oxide layer of the plug had peeled off and wear had occurred, whereas if the thickness of the oxide layer over the entire plug surface was 0.10 mm or more, it was judged that the oxide layer remained on the plug and no wear had occurred. Note that, when the oxide layer thickness was observed over the entire plug surface even after 10 or more rollings were performed, it was judged as ◎; when the oxide layer thickness was observed over the entire plug surface even after 5 to less than 10 rollings were performed, it was judged as ◯; when the oxide layer thickness was observed over most locations on the plug surface but some (10% or less of the measurement range) of the oxide layer thickness was less than 0.10 mm even after 5 to less than 10 rollings were performed, it was judged as △; and when the oxide layer thickness was less than 0.10 mm in more than 10% of the measurement range after less than 5 rollings, it was judged as ×. The results are shown in Table 4.
[0061] (Deformation evaluation) After rolling, dimensional measurements were performed using a 3D scanner. If a volume change of 10% or more was confirmed, it was deemed that the plug had been deformed, and if the volume change was less than 10%, it was deemed that the plug had not been deformed. In this evaluation, a contact thermometer was used to confirm that the surface temperature of the plug had reached room temperature (25°C or less), and then the presence or absence of deformation was judged. A plug that had a volume change of less than 10% over the entire plug even after 10 or more rolls was evaluated as ◎, a plug that had a volume change of less than 10% over the entire plug even after 5 to less than 10 rolls was evaluated as 〇, a plug that had a volume change of less than 10% over the entire plug even after 5 to less than 10 rolls was evaluated as △, and a plug that had a volume change of 10% or more over the entire plug after less than 5 rolls was evaluated as ×. The results are shown in Table 4.
[0062] (Overall evaluation criteria) ◎ (Pass (superior)): It was determined that even after 10 or more rolling processes, no wear or deformation occurred in the plug (adhesion and wear resistance evaluation: ◎ and deformation characteristics: ◎). ○ (Pass): Even after 5 or more but less than 10 rolling cycles, it was determined that no wear was generated in the plug and no deformation was generated in the plug (adhesion / wear resistance evaluation: ◯ and deformation characteristics: ◯, or adhesion / wear resistance evaluation: ◎ and deformation characteristics: ◯, or adhesion / wear resistance evaluation: ◯ and deformation characteristics: ◎). △ (Pass): Even if rolling was performed 5 to 10 times, it was determined that the adhesion and abrasion resistance were evaluated as △ and the deformation characteristics were △, or the adhesion and abrasion resistance were evaluated as △ and the deformation characteristics were OK, or the adhesion and abrasion resistance were evaluated as △ and the deformation characteristics were ◎, or the adhesion and abrasion resistance were evaluated as 〇 and the deformation characteristics were △, or the adhesion and abrasion resistance were evaluated as ◎ and the deformation characteristics were △. × (Fail): After less than five rolling passes, it was determined that at least one of wear and deformation had occurred in the plug (including either × in the evaluation of adhesion / wear resistance or × in deformation characteristics).
[0063] The results are shown in Table 4.
[0064] In the examples of the present invention, Ra was 0.04 μm or more, and the plugs of the examples of the present invention were excellent in adhesion and wear resistance of the oxide layer, and sufficient deformation suppression was achieved. This revealed that the plugs had good cost performance and a long life. Among the examples of the present invention, plugs Nos. 1, 2, 5, and 25 to 26, which are considered to have roughness in the suitable range and to have a thick spinel-type oxide layer with high wear resistance, in particular, obtained better results. In addition, plugs Nos. 28 to 29 also had high wear resistance because they were considered to have a thick spinel-type oxide layer formed to begin with, and furthermore, by setting Ra to around 1.00 μm, the adhesion of the oxide layer was improved, and even more excellent results were obtained. Also, plugs No. 30 to 31 obtained excellent results by reducing the Ra to 0.81 to 0.97 μm by surface grinding from the cast surface. Nos. 22 and 23 had the as-cast surface and had an Ra of more than 100.00 μm, and even after rolling 5 to less than 10 times, the oxide layer had a thickness of less than 0.10 mm on a part of the plug surface (10% or less of the measurement range), there was localized seizure, and transferred defects were observed on the mating piece.
[0065] On the other hand, the comparative examples falling outside the range of the present invention did not ensure an Ra of 0.04 μm or more, or did not have an oxide layer. Therefore, the plugs of the comparative examples did not obtain the desired effects of at least one of high adhesion, wear resistance, and deformation suppression of the oxide layer.
[0066] Example 3 In order to evaluate the effect of the direction of the polishing marks on the adhesion of the oxide layer, samples were prepared under the condition of level 3 in Table 2, in which the direction of the polishing marks of the base material was parallel to the rotation direction of the mating piece (corresponding to the outer surface of the plug base material having polishing marks in a direction parallel to the rolling direction of the plug) and perpendicular to the rotation direction of the mating piece (corresponding to the outer surface of the plug base material having polishing marks in a direction perpendicular to the rolling direction of the plug). The hot sliding test (FIG. 2) used in Example 1 was carried out using the samples with different polishing marks. The time until peeling of the oxide layer was observed over the entire surface was measured to evaluate the adhesion of the oxide layer. Specifically, after the test for 1 minute, the adhesion including the peeling state of the oxide layer was evaluated in the same manner as in Example 1, and if the judgment was A to C, the same sample was used and the same test as above was carried out again for 1 minute. This was repeated until the judgment was D. The evaluation results are as follows. The result for the grinding marks on the base material being parallel to the direction of rotation of the opposing piece was 3 minutes (a rating of D on the third test). The result was 5 minutes (a rating of D on the fifth test) when the grinding marks on the base material were aligned perpendicular to the direction of rotation of the opposing piece. From the above, by making the direction of the polishing marks (roughness) of the base material perpendicular to the rotation direction of the mating piece, it took longer to reach a D rating, which means that the oxide layer was more tightly adhered.
[0067] [Table 1]
[0068] [Table 2]
[0069] [Table 3]
[0070] [Table 4] [Explanation of symbols]
[0071] 1 Plug 2a Rolling arc type (caliber) roll 2b Rolling arc type (caliber) roll 3. Bar S Hollow 4. Test specimens 5 Coil 6. Rolling Direction 7 Rotation Direction R Counterpart 10 Base material 11 Oxide layer 13 Contact range of the other side 20 Egle 101 Rolling Mill 201 Hot roll wear and thermal shock combined test equipment
Claims
1. 1. A seamless steel pipe rolling plug, comprising: a plug base metal having an outer surface with an arithmetic mean roughness Ra of 0.04 μm or more; and an oxide layer on the surface of said plug base metal.
2. 2. The plug for rolling a seamless steel pipe according to claim 1, characterized in that an outer surface of the plug base metal has polished marks in a direction perpendicular to the rolling direction of the plug, and has an arithmetic mean roughness Ra of 0.04 μm or more in a test in which roughness measurement is performed in the rolling direction of the plug.
3. 2. The seamless steel pipe rolling plug according to claim 1, characterized in that the plug base metal has a component composition containing, by mass%, Si: 0.3 to 1.5%, Mn: 0.3 to 1.5%, Ni: 0.01 to 5.0%, Cr: 12 to 20%, and a total of one or two of Mo and W: 0.1 to 3.0%, with the balance being Fe and unavoidable impurities.
4. 3. The seamless steel pipe rolling plug according to claim 2, characterized in that the plug base metal has a component composition containing, by mass%, Si: 0.3 to 1.5%, Mn: 0.3 to 1.5%, Ni: 0.01 to 5.0%, Cr: 12 to 20%, and a total of one or two of Mo and W: 0.1 to 3.0%, with the balance being Fe and unavoidable impurities.
5. The seamless steel pipe rolling plug according to claim 3, characterized in that the component composition further contains, in mass%, C: 1.0 to 2.0%, Al: 0.01 to 0.1%, and V: 0.01 to 0.1%.
6. The seamless steel pipe rolling plug according to claim 4, characterized in that the component composition further contains, in mass%, C: 1.0 to 2.0%, Al: 0.01 to 0.1%, and V: 0.01 to 0.1%.
7. A method for producing a seamless steel pipe rolling plug according to any one of claims 1 to 6, 1. A method for producing a plug for rolling seamless steel pipes, comprising processing a plug base metal by polishing, grinding or cutting.
8. A plug mill for rolling seamless steel pipes, comprising the plug for rolling seamless steel pipes according to any one of claims 1 to 6.
9. A method for producing a seamless steel pipe, comprising using a seamless steel pipe rolling plug according to any one of claims 1 to 6.
Citation Information
Patent Citations
Manufacture of boring mandrel
JP1982050233A
Surface treatment of mandrel bar for rolling seamless steel tube
JP1992284905A
Mandrel bar for hot rolled seamless pipe
JP1996071618A
Mandrel bar for hot rolling of seamless pipe
JP2004344923A
Method for manufacturing seamless steel pipe
JP2016047546A