Crystal piece of single crystal silicon
By employing a fused silica crucible with a specific promoter concentration and optimized gas flow, the production of high-quality semiconductor wafers with minimal pinholes and impurities is achieved, addressing the defects in existing methods and improving yield and quality.
Patent Information
- Application Number
- JP2024104133
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-07-14
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Existing methods for producing semiconductor wafers suffer from high defect rates, particularly pinholes and impurities like carbon and iron, leading to economic losses due to incorrect classification and increased costs from additional measurement techniques.
The use of a fused silica crucible with an inner layer of fused silica and a specific concentration of crystallization promoters like barium, combined with optimized crucible material handling and gas flow during crystal pulling, significantly reduces pinhole density and impurity levels, allowing for higher-quality semiconductor wafers.
This approach results in semiconductor wafers with a pinhole-free rate of over 99.8% and reduced impurity levels, enhancing production yield and quality, while minimizing additional measurement-induced contamination and costs.
Smart Images

Figure 2024147585000002 
Figure 2024147585000003 
Figure 2024147585000004
Abstract
Description
[Technical field]
[0001] The present invention relates to silicon single crystals that are particularly suitable for producing semiconductor wafers from silicon. [Background technology]
[0002] Monocrystalline semiconductor wafers are the basis of modern electronics. During the production of components on said semiconductor wafers, they are currently subjected to thermal operations using highly complex coating steps.
[0003] Semiconductor wafers, particularly silicon semiconductor wafers, are typically first grown into single crystals by the float zone (FZ) or Czochralski (CZ) process. The rods thus produced are then separated into crystal pieces by a saw suitable for that purpose, such as a wire saw, an ID saw or a band saw, and these pieces are then processed into semiconductor wafers, typically by a wire saw or an ID saw.
[0004] After further mechanical, chemical-mechanical and / or chemical steps, a layer may optionally be applied by CVD.
[0005] These semiconductor wafers thus produced are then available for further component processing.
[0006] A proper quality assurance defines the intensive deployment of analytical methods that determine the success or failure of the performed production steps. Different measurement methods are therefore typically used, possibly after individual processing steps, on the one hand to monitor the production process and on the other hand to reject semiconductor wafers that are considered unusable. Semiconductor wafers here are typically evaluated using only a single measurement method or the results of one measurement parameter at any one time.
[0007] When single crystals are pulled according to the Czochralski method (CZ method) from a melt held in a quartz crucible, the crucible material forms a source of interstitial oxygen which is incorporated into the single crystal and into the semiconductor wafers obtained therefrom. The concentration of incorporated interstitial oxygen can be controlled very precisely, for example by adjusting the pressure or the flow of argon through the pulling apparatus, or by coordinating the crucible rotation with the seed crystal rotation during pulling of the single crystal, or by the application of a magnetic field imposed on the melt, or by a combination of these measures. Generally speaking, the interstitial oxygen concentration measured in crystals produced by the CZ method is in the range of 5×10 16 at / cm 3 That's all (new ASTM).
[0008] Interstitial oxygen plays an important role in the generation of BMD (Bulk Micro Defects), which are oxygen precipitates formed by the growth of BMD species during heat treatment. They act as internal getters, in other words as an energy sink for impurities, and are therefore in principle an advantage. One exception is their presence at locations where electronic components are intended to be located. To avoid BMD formation at such locations, it is possible to deposit epitaxial layers on the semiconductor wafer and provide electronic components to be located on the epitaxial layers.
[0009] The crucible is usually constructed of a silicon dioxide-containing material, such as quartz. It is generally filled with chunks and / or granules of polycrystalline silicon, which are melted by side heaters positioned around the crucible and a base heater positioned below the crucible. After a stage of thermal stabilization of the melt, a single crystal seed is immersed in the melt and lifted. During this procedure, silicon crystallizes at the end of the seed wetted by the melt. The crystallization rate is substantially influenced by the speed at which the seed is lifted (crystal lift rate) and by the temperature of the interface where the molten silicon undergoes crystallization. Through proper control of these parameters, first a section called the "neck" is lifted to eliminate dislocations, followed by a single crystal conical section and finally a single crystal cylindrical section from which the semiconductor wafers are later cut.
[0010] As described, for example, in US Pat. No. 5,954,873 A, the corresponding operating parameters during the crystal pulling process are adjusted in such a way as to achieve a radially uniform defect distribution in the crystal.
[0011] WO 98 / 45508 A1 is one of many publications that describe how the time profile of the pull rate v can be experimentally ascertained to control the pull rate v in such a way that the ratio v / G during the growth of the single crystal remains substantially unchanged and the single crystal can grow in the intended area. v Area and P i Detection methods are described for characterization and differentiation of the regions.
[0012] Liberated gaseous inclusions in the crucible material, gas surrounding lumps and / or granules, silicon oxides formed in the melt, and gas diffusing into the melt are all considered possible causes that can lead to the formation of cavities in the single crystal, called "pinhole" defects (not to be confused with COPs). They arise when gas bubbles reach the interface between the growing single crystal and the melt, and the single crystal crystallizes around these bubbles. If the parting plane intersects the cavities when the semiconductor wafer is cut, the resulting semiconductor wafer has a circular depression or hole whose diameter can typically be from a few micrometers to a few millimeters. Semiconductor wafers containing such cavities cannot be used as substrate wafers for the production of electronic components.
[0013] The density of pinholes formed in an ingot piece can be measured, for example, by a scanning ultrasound method, which is described, for example, in DE 102 006032431 A1. The method detects pinholes from a diameter of about 50 μm. Using this method, determining the exact size of the pinholes in each case is hindered by relatively large measurement errors.
[0014] US-9665931 A1 describes a corresponding method for determining the density and respective size of pinholes in a semiconductor wafer, which method allows the size of the pinholes to be indicated with high accuracy.
[0015] In order to be able to accurately measure the size of the pinholes in the ingot piece, the measuring ingot piece is subjected to a measurement in accordance with the prior art as per DE 102 006 032431 A1 and the coordinates of the pinholes found are stored.
[0016] The corresponding pinhole-containing zones are then cut into semiconductor wafers and analyzed by the method described in US-9665931 A1. The size of the correspondingly found pinholes can thus be determined with a measurement error of a few percent.
[0017] The justification for rejecting semiconductor wafers is that if their unsuitable or defective nature is detected only while they are undergoing processing in component fabrication, there will be costs involved. Conversely, if material is misclassified as unsuitable for use, there will inevitably be economic damage to the manufacturer of the semiconductor wafers.
[0018] There are different defects that can affect semiconductor wafers. Depending on the part processing, both the defect type and its appearance (location and shape of the appearance) determine whether the defect is classified as harmful or of lesser importance as far as the part processing is concerned.
[0019] For example, a pinhole in the interior of a semiconductor wafer (i.e., away from the surface) can exist without observable consequence to part processing, whereas if the pinhole is located on or near the surface, it can actually cause adverse effects in part processing.
[0020] US 2008 / 0032429 A1 takes up this problem and describes a technique for a measurement method that prepares additional images of the defect zone on a semiconductor wafer when a defect occurs and uses them to identify the defect type in this area. For this reason, a defect once recognized by the system is re-measured with further measurement data on the same measurement tool and the decision is either proven true or proven false accordingly. This requires an increase in the analysis effort and therefore in the costs.
[0021] In US 2008 / 0163140 A1, after the defects are recognized, the coordinates of the defects on the semiconductor wafer are stored and the defects are subjected to a second measurement method in a targeted manner. The purpose of this measurement step is to unambiguously identify the defect type. Again, increased costs arise through the application of the further measurement method. Summary of the Invention [Problem to be solved by the invention]
[0022] Both methods described in the prior art allow for the defect, once discovered, to be either proven true or disproved, which is called defect review. Both approaches aim at unambiguous identification of the defect once detected, which can then be used in a targeted manner to perform additional measurements.
[0023] The background to this additional measurement is that the measurement techniques currently used in standards provide suitable classifications but only with limitations.
[0024] Each additional measurement technique firstly incurs costs and secondly may introduce changes (e.g. contamination) to the semiconductor wafer. These changes in turn prevent the semiconductor wafer thus analyzed from being used in component processing. Therefore, these techniques cannot be deployed in mass production of semiconductor wafers.
[0025] A series of proposals have also already been published on how pinhole formation during crystal pulling can be suppressed, with most of these proposals focusing on improving the properties of the crucible material.
[0026] There are also proposals (eg EP 247 1980 A1) to optimise the feeding of the crucible in order to prevent damage to the crucible and thus the formation of bubbles in the melt and pinholes in the single crystal.
[0027] Other proposals focus on suppressing or eliminating pinholes during the melting of the lumps and / or granules: for example, US 2011 / 304081 A1 recommends a gentle approach to managing the crucible in such a way as to reduce the density of pinholes produced in the crystal by a suitable timed power distribution of the heaters used.
[0028] To achieve the desired (defect) properties of the pulled crystal, the distribution of the heating power should be adjusted accordingly. This contradicts, for example, the method proposed in DE 10 339 792 A1, in which it is then possible to achieve both objectives (low pinhole density and desired defect properties).
[0029] JP-5009097 A2 describes a method for producing monocrystalline silicon, in which during melting of the polysilicon the pressure in the crystal pulling unit is reduced to a pressure of 5-60 mbar, and during pulling of the crystal the pressure is above 100 mbar.
[0030] US 2011 / 214603 A1 describes a technique for producing monocrystalline silicon in which the heater power during melting is set higher than the power during subsequent crystal pulling, and in addition the pressure during melting is set below 30 mbar, which is lower than the pressure during subsequent crystal pulling.
[0031] The inventors have recognized that ostensibly defect-free semiconductor material contains a relatively high density of pinholes. While the techniques described in the prior art can solve part of this problem, it has been found that semiconductor wafers produced according to the prior art are still highly susceptible to defects during component production.
[0032] The inventors have also recognised that the techniques described in the prior art suffer from further drawbacks: in particular, it has been noted that the pulled single crystals have increased levels of carbon and iron impurities.
[0033] The inventors have additionally recognized that the methods proposed in the prior art do not allow for the production of single crystals by the Czochralski process that have a very low density of large pinholes as well as very low levels of iron and carbon contamination, while at the same time possessing the desired defect characteristics (defect free).
[0034] The object of the present invention is to provide silicon crystals, and semiconductor wafers produced therefrom, which do not have the above-mentioned drawbacks. [Means for solving the problem]
[0035] This object is achieved by a piece of monocrystalline silicon intended for the production of semiconductor wafers, the piece having a length between 8 cm and 50 cm and a diameter between 280 mm and 320 mm, the proportion of semiconductor wafers produced therefrom which are free of pinholes having a size of 30 μm or less is greater than 95%.
[0036] This object is further achieved by the methods and products as set forth in the dependent claims. The features reported above for the embodiments of the method of the invention may be rewritten to correspond to the products of the invention. Conversely, the features reported above for the embodiments of the product of the invention may be rewritten to correspond to the methods of the invention. These and other features of the embodiments of the invention are elucidated in the drawings and in the description of the claims. The individual features may be realized separately or in combination as embodiments of the invention. In addition, they may describe advantageous configurations which can be protected independently.
[0037] Definition of Terms MWS (multi wire saw) refers to the simultaneous slicing of semiconductor wafers from a crystal piece by means of sawing wires. A general description of this method is given in WO18149631 A1.
[0038] ENG (edge notch grinding) is generally referred to as DE1020132 Refers to the method for edge rounding reproduced in 12850 A1.
[0039] CMP (chemical mechanical polishing) is a process that uses non-bonded abrasives and suitable It refers to polishing in which ablative polishing occurs on one side of a semiconductor wafer using chemicals. Further details are given, for example, in DE 10 2008 045 534 B4.
[0040] Double-sided polishing (DSP) is a method from the group of chemical mechanical processing steps (CMP). DSP processing of semiconductor wafers is described, for example, in US 2003 / 054650 A1, and an apparatus suitable for this purpose is described in DE 100 07 390 A1. DSP comprises chemical etching using alkali and mechanical erosion using a non-bonded abrasive, which is dispersed in an aqueous medium and brought into contact with the semiconductor wafer by an abrasive cloth that does not contain hard substances in contact with the semiconductor wafer. Thus, material is ablated from the semiconductor wafer under pressure and reciprocal motion.
[0041] CVD (chemical vapor deposition) stands for chemical vapor deposition, and is generally defined as WO190 It is described in 20387 A1.
[0042] DDG (double-sided grinding) is a method of grinding with a support, e.g. a grinding disk. This method is described by way of example in DE 10 2017 215 705 A1.
[0043] Etching refers to the chemically or alkaline-induced ablation of a semiconductor, a method which is exemplarily described in US7829467 B2.
[0044] Edge rounding refers to the mechanical rounding of the edges of a semiconductor wafer. Edge polishing refers to polishing the edge of a semiconductor wafer.
[0045] Resistivity measurement (resistance) refers to the measurement of the electrical resistance of single crystal silicon. Preferred for this purpose is the measurement technique known as four-point measurement, although other techniques can be used.
[0046] Light scattering is understood to refer to measurement techniques such as, for example, MO6, MO4, LLS, IR-LST (localized light scattering), in which the object under analysis, i.e. the silicon wafer, is scanned with a light beam and the light scattered and / or reflected by irregularities on the surface or in the volume is recorded using a detector. In the case of scattered light, the term used is dark field inspection, while the detection of reflected light is called bright field measurement (see also SEMI standard M52).
[0047] Infrared depolarization (SIRD) is used to is scanned using an infrared beam, where non-uniformities in the polarization of the reflected or transmitted laser light are recorded with spatial resolution in order to determine possible local stresses in the material.
[0048] In ultrasonic measurements (ultrasound), the sample is penetrated by ultrasonic waves. When the sound waves hit an asperity, a reflection occurs and is detected. The sample here is also scanned. Together with measuring the transit time for the wave, it is possible to precisely determine the local position of the asperity.
[0049] Minority charge carrier lifetime measurements (lifetime): Recombination lifetime of generated free charge carriers to states below the Fermi energy in response to pulses on crystal defects and impurities (Reference: SEMI standard MF1535).
[0050] Measurement of the free path length of the minority charge carriers (free path length): It is calculated from the lifetime and the free diffusion constant (physical constant, ref. SEMI Standard MF391).
[0051] Measurement of local shape (local shape): for this technique, local variations in the flatness and / or thickness of a sample are determined by volumetric measurements, by interferometry or by triangulation (see also SEMI Standard M49).
[0052] Microscopy (electron microscopy, optical microscopy in the visible light wavelength range): Microscopes are used for the constant monitoring of specific zones of silicon wafers after the corresponding manufacturing steps. These zones include in particular the edge zone, the notch zone, the zone of laser marking and the contact points with the wafer handling and positioning system.
[0053] Mass spectrometry and x-ray fluorescence are routinely used to identify foreign atoms in silicon (sometimes with local resolution) and to determine the concentrations of such atoms.
[0054] FTIR can be used to ascertain the thickness of layers (eg, epitaxial or oxide layers) and also to ascertain the concentration of foreign atoms such as O, C, H, N (via spectral analysis).
[0055] LLS (localized light scattering) identifies light scattering points identified on the wafer surface by light scattering. [Brief description of the drawings]
[0056] [Figure 1] 1 shows the relationship of the inert gas flow rate f [l / h] as a function of the plant pressure p [mbar]. [Diagram 2] 4 shows a typical time profile of the brightness measured by the camera during heating of silicon s, for each brightness value b in relative units in each case. [Diagram 3] The percentage of semiconductor wafers formed from crystalline pieces that are pinhole-free is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0057] 1 shows the relationship of the inert gas flow rate f [l / h] as a function of the plant pressure p [mbar]. The area identified by (102) represents a preferred range and the area identified by (101) represents a particularly preferred range for the pressure to flow rate ratio for the molten silicon s.
[0058] Those skilled in the art will understand that the unit l / h (liters per hour) refers to standard liters per hour, in other words the volume per unit time that a gas would have under standard pressure.
[0059] 2 shows a typical time profile of the brightness measured by the camera during the heating of silicon s, with respect to the brightness value b in relative units in each case. The designation (201) denotes a zone where the silicon is still solid, the designation (203) denotes a zone where the silicon is already completely liquid, and the designation (202) denotes a zone where the silicon is still solid and already partially liquid.
[0060] The ordinate in FIG. 3 indicates the percentage of pinhole-free semiconductor wafers formed from the crystal fragments. The names A to E here represent different experimental conditions, which are This will be explained later.
[0061] Detailed Description of the Invention A number of crystals in each case were pulled from a crucible by the Czochralski pulling technique. Measurements of both the mean free path length of the minority charge carriers (SPV) and the length of the dislocation-free crystal were made. The length of the dislocation-free portion of the crystal was expressed relative to the total theoretically achievable length.
[0062] During crystal pulling, measures known from the prior art were used to produce defect-free crystals. In principle, this can be achieved using cusp, horizontal or moving magnetic fields. Furthermore, the crystal rotation and crucible rotation are set accordingly for this purpose.
[0063] The characteristic mean free path length of the minority charge carriers was expressed relative to the maximum free path length measured. This statistic is used below as a quality criterion for possible impurities present in the crystals and which may interfere with components subsequently made on the silicon. In theory, it would also be possible to use other statistics for the quality of the crystals. Examples of these are lifetime measurements by μPCD and, alternatively, chemical analysis of the resulting silicon by ICP-MS. Many suitable methods are now available to the skilled person.
[0064] The inventors have identified the measurement techniques mentioned above as suitable techniques, particularly as being readily accessible.
[0065] The concentration of carbon in the silicon was determined by gas fusion analysis, as described, for example, in DE 1020 14217514 A1. Alternatively, it is also possible to use FTIR.
[0066] The iron concentration was measured using inductively coupled plasma-mass spectrometry (ICPMS). It can also be measured by neutron activation analysis (NAA) performed with appropriate calibration. .
[0067] Each pulled single crystal ingot was accordingly split into ingot pieces using a band saw and then cut into wafers, which were inspected for pinholes, defect characteristics and impurities (carbon, iron).
[0068] The inventors recognized that the use of crucibles manufactured in accordance with the prior art had distinct disadvantages when the crucibles were used to successively pull multiple crystals by the Czochralski method: crystal pulling also appeared to become more difficult with increasing duration of the pulling process.
[0069] It has been found that when crystals are pulled using a crucible made from naturally occurring SiO2 and coated internally with a barium-containing component, as described in the prior art, a significant decrease in the mean free path length is evident, although the length of the dislocation-free portion of the crystal remains large. Thus, the mean free path length decreases to, on average, 70% of its initial value. It is therefore not true that crystals of consistent quality can be produced using the crucible.
[0070] When crystals are pulled using crucibles made from synthetically obtained SiO2 and internally coated with a barium-containing component, as described in the prior art, a significantly increased scattering in the measured free path length is found.
[0071] Even under optimal conditions, for example, the crystals exhibit a mean free path length that is on average 10% smaller. Crystals of this quality are not sufficient for the semiconductor industry. The dislocation-free lengths of the crystals thus obtained also exhibit unacceptable scattering that can result in corresponding economic losses.
[0072] The inventors first identified the crucible material as the source of the measured defects and undertook extensive experimentation to eliminate said defects.
[0073] It is known from the prior art that β-cristobalite has a higher melting temperature than quartz, and it is also known that there are certain crystallization promoters that can favor the formation of β-cristobalite.
[0074] Another known fact is that quartz crucibles made from synthetically derived SiO2 have different properties than quartz crucibles made from naturally derived SiO2.
[0075] The inventors have surprisingly discovered that a fused silica crucible having an interior with an internal layer of fused silica forming a surface, the internal layer being provided with a crystallization promoter, exhibits positive properties with regard to the multiple pulling of crystals from the crucible, in particular when the concentration C of synthetically obtained SiO2 located at a certain distance from the surface is greater than the concentration of synthetically obtained SiO2 located at a further distance from the surface.
[0076] Substances which have a particularly favorable effect here as crystallization promoters include barium and strontium, with barium being particularly preferred.
[0077] The inventors have also realised that it is advantageous if the concentration C of synthetically obtained SiO2 is greater than 90% at a distance from the surface of less than 0.4 mm.
[0078] Further experiments have shown that the relationship that fits the concentration of synthetically obtained SiO2 as a function of distance d is: C[%]≦100-(d[mm]-0.25)×30, and C[%]≧100-(d[mm]+0.25)×80 It has been unexpectedly found that when
[0079] Through further experimentation, the inventors have been able to narrow the range somewhat, and have determined that the relationship that applies to the concentration of synthetically obtained SiO2 as a function of distance d is: C[%]≦100-(d[mm]+0.1)×80, and C[%]≧100-(d[mm]-0.05)×36 It has been found that when t is 0.05, advantages arise in terms of both crystal quality (SPV) and dislocation free length fraction.
[0080] Particularly preferably here, the concentration of the crystallization promoter is less than 1 ppba and more than 0.05 ppba, based on silicon.
[0081] The single crystals produced using the crucible materials described above were then processed into semiconductor wafers.
[0082] The inventors have now discovered that the processing of crystal pieces into semiconductor wafers must be modified to provide better detection of deleterious pinholes and to enable more effective and rapid optimization of corresponding comprehensive measures.
[0083] After the corresponding manufacturing step, measurements are typically performed so that the semiconductor wafer is either rejected or approved for the next processing step.
[0084] This approach was modified by performing measurements after the individual manufacturing steps for the production of a semiconductor wafer, using a measurement method that appears to be suitable for these measurements, and storing the results in a database. Here, independent of the measurement results, an individual semiconductor wafer is always approved for its next intended fabrication step. A measurement result in this context is considered as the nature of a possible anomaly or defect, the local coordinates of this anomaly or defect, the measurement method used (including details), and the nature of the fabrication step.
[0085] The inventors have realised that the overall measurement results after all of the manufacturing steps performed and their associated measurements result in a significantly improved assessment of the material.
[0086] This approach has proven to be very advantageous with regard to the assessment of the data of the individual measurement results after each production step. By combining the measurement data after different process steps, it becomes possible to determine with greater precision the cause of the defect, and therefore its nature and its location on or within the semiconductor wafer. The quality of the identification of the defects and the associated assessment of the semiconductor wafer with regard to its suitability for component processing can be optimized accordingly.
[0087] The resulting crystal pieces were analyzed using ultrasonic measurements and the results (coordinates of possible irregularities in the crystal) were stored. The crystal pieces were then cut into semiconductor wafers by the MWS, regardless of the results already obtained. IR measurements were then performed on the resulting semiconductor wafers and the results of these measurements were stored again with spatial resolution.
[0088] An additional control measure, as proposed in the prior art as a second measurement, performed at locations where the IR measurement indicated an anomaly, was a defect review using a further IR measurement at a higher resolution. These data were used to obtain an assessment of the anomaly, as proposed in the prior art. However, in contrast to the prior art, semiconductor wafers exhibiting possibly harmful defects were not discarded, but instead subjected to the next fabrication step. For the subsequent steps, the same principle was adopted. Finally, the additional data thus obtained was used as the data basis for the subsequent validation of the method of the present invention.
[0089] After double-sided polishing (DSP), the resulting semiconductor wafers were subjected to IR measurements and the data was restored with spatial resolution.
[0090] After further processing of the semiconductor wafer by CMP, the semiconductor wafer was subjected to SIRD measurements and data therefrom was stored with spatial resolution. Additionally, after CMP, the semiconductor wafer was subjected to front and back surface light scattering measurements and the resulting data was stored with spatial resolution.
[0091] Some of the semiconductor wafers thus obtained were further processed by CVD processing and then analyzed by light scattering measurements on the front and back surfaces, and all of the data were again stored with spatial resolution.
[0092] A summary of the fabrication steps used is given in Table 1, along with the measurements performed on these steps.
[0093] [Table 1]
[0094] Finally, all of the measurements were analyzed with a global rating. Surprisingly, the inventors have now ascertained that the minimum size of the pinholes found accordingly is about 7 μm, and that the maximum size of the pinholes found is 30 μm.
[0095] Alternatively, although somewhat more time consuming and therefore less preferred, the resulting semiconductor wafer can also be analyzed for the occurrence of pinholes by infrared microscopy (e.g., using a transmission SIRD). The minimum pinhole size measured is again 7 μm.
[0096] Looking at the overall results, the inventors determined that even though an optimized crucible material was employed, a significant degree of pinholes still meant that the percentage of semiconductor wafers with crystal fragments unsuitable for component processing was about 3.8%. Figure 3 shows in column A the measured percentage of semiconductor wafers without pinholes (about 96.2%). The measured iron contamination was 1.0 x 10 10 at / cm 3 The carbon pollution found is less than 7×10 14 at / cm 3 Depending on the pulling method used, the 17 ~7×10 17 at / cm 3 It was possible to establish the oxygen concentration (new ASTM). The resistance was set from 1mohmcm to 1ohmcm.
[0097] Using the modified crucible material, the delivery and melting of polysilicon in the crucible was then modified.
[0098] 2cm 2 It has been found to be advantageous to use silicon with an average mass-based specific surface area smaller than 100 nm / g.
[0099] Very particularly preferably, the crucible has a diameter of 1 cm 2 The polysilicon having a mass specific surface area of less than 1 cm / g is oriented at a distance of less than 5 cm and more than 2 cm from the crucible wall. The remainder of the crucible volume is oriented at a distance of less than 1 cm 2 / g or larger than 5cm 2 The final result is shown in FIG. 3 by column E. Approximately 98% are pinhole free, so this measure also increases yield.
[0100] Once the polysilicon is melted, a pressure, preferably less than 10 mbar, is established in the crystal pulling plant. At the same time, the overall flow rate f of the purge gas through the pulling plant is preferably set such that it is greater than the flow rate f[l / h]×160.
[0101] FIG. 1 now shows a preferred zone consisting of a pressure p and a flow rate f. Particularly preferably, the overall flow rate of the purge gas through the pulling plant is set so that it is greater than the flow rate f[l / h]×400, very preferably greater than the flow rate f[l / h]×720. The pressure set in this case is preferably less than or equal to 10 mbar.
[0102] Generally speaking, it is advantageous to keep the flow rate f as high as possible while at the same time providing the lowest possible pressure. The maximum flow rate for a given pressure depends only on the pump power.
[0103] The purge gas used during melting includes gases from the following list: argon, helium, nitrogen, or combinations thereof. It is preferred to use argon having a purity of greater than 99.99 vol%.
[0104] Column C of Figure 3 shows the result of this procedure: over 99% of the wafers are pinhole free. In yet another embodiment, the pressure (and thus the flow rate of the purge gas) was increased as soon as the first polysilicon became liquid, in this case the pressure increase being 4 mbar, preferably 8 mbar, very preferably 12 mbar.
[0105] The melting action here was monitored using a camera using suitable techniques of digital image processing to determine when the first silicon became liquid.
[0106] The inventors have realised that the time at which a significant increase in brightness of the analysed image data can be ascertained can be very effectively correlated with the timing of the onset of the solid to liquid phase transition.
[0107] 2, for example, plots brightness as a function of time. It has been found that, preferably in the time between zones (201) and (202), the pressure should be increased to achieve a further positive effect on pinhole density and carbon and iron concentrations.
[0108] Column D of Figure 3 shows the results achieved for a crystal using the inventive procedure as described above, where over 99.8% of the wafer is pinhole free.
[0109] In an additional embodiment, polysilicon having a chlorine content of greater than 1 ppba was used for delivery.
[0110] The inventors have now surprisingly realised that, despite the assumption made by those skilled in the art that at high temperatures chlorine would inevitably release iron from the plant and contaminate the silicon, the use of polysilicon with a chlorine content above 1 ppba has the additional positive consequence of iron contamination. The Fe contamination thus achieved is 5.0×10 9 at / cm 3 It was determined to be less than
Claims
1. A piece of single crystal silicon for producing a semiconductor wafer, comprising: A length of 8 cm or more and 50 cm or less; A diameter of 280 mm or more and 320 mm or less, A crystal piece, after the crystal piece is cut by a wire saw into semiconductor wafers suitable for the semiconductor industry, wherein the percentage of the produced semiconductor wafers that are free of pinholes having a size greater than 7 μm and less than or equal to 30 μm as measured by transmission infrared depolarization measurement (SIRD) is greater than 98%.
2. A piece of single crystal silicon for producing a semiconductor wafer, comprising: A length of 8 cm or more and 50 cm or less; A diameter of 280 mm or more and 320 mm or less, A crystal piece, wherein the percentage of the semiconductor wafers produced from the crystal piece that are free of pinholes having a size of 30 μm or less is greater than 96.2%.
3. The crystal pieces are 1×10 17 at / cm 3 More than 3×10 17 at / cm 3 Above, and 7 x 10 17 at / cm 3 Less than 6×10 17 at / cm 3 2. The crystal piece of claim 1, comprising the following interstitial oxygen: (new ASTM)
4. All of the semiconductor wafers from the proportion of the produced semiconductor wafers have a region P in which silicon interstitials are predominant. i and the region P where silicon vacancies are dominant v 2. The crystal piece of claim 1, wherein the crystal piece comprises:
5. The area P v and the area P i The crystal piece according to claim 4, wherein the sum of the areas of the first and second crystals is greater than 95%, preferably greater than 99%, of the area of the semiconductor wafer.
6. The area P v 6. The crystal piece according to claim 5, wherein said area is less than 10% of said area of said semiconductor wafer.
7. Carbon (C) impurity is 7 x 10 14 at / cm 3 Less than 5.5×10 14 at / cm 3 At the same time, the iron (Fe) impurity is less than 1.0×10 10 at / cm 3 Less than 5.0×10 9 at / cm 3 2. The crystal piece of any one of the preceding claims, wherein said crystal piece is less than 1 mm in diameter.
8. 2. The crystal piece of claim 1, wherein the resistivity measured on all of the semiconductor wafers is greater than or equal to 1 mohmcm and less than or equal to 1 ohmcm.
9. The crystal piece according to any one of claims 1 to 8 is used, The wire saw cuts it into semiconductor wafers, A method for producing a semiconductor wafer which is polished and optionally subjected to epitaxy.
Citation Information
Patent Citations
Apparatus and method for producing single crystal
JP2003221296A
METHOD FOR MANUFACTURING Si SINGLE CRYSTAL INGOT BY CZ METHOD
JP2007261935A
Silicon single crystal
JP2016044109A
Single crystal silicon semiconductor wafer and method of manufacturing the semiconductor wafer
JP2020529958A
Silica vessel for pulling monocrystalline silicon and method for producing same
WO2013105165A1