Steel sheet with excellent surface quality, and manufacturing method therefor

By controlling the passage speed of hot-rolled coils through a pickling tank and maintaining specific steel compositions, the method addresses the non-uniformity of internal oxidation and decarburized layers, enhancing surface quality and productivity in steel plate manufacturing.

JP2024147778AInactive Publication Date: 2024-10-16CLEANSOLUTION CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024118600
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-02-18
Filing Date
2024-07-24
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for manufacturing steel plates fail to uniformly control the thickness of internal oxidation and decarburized layers in the longitudinal direction, leading to variations in surface quality and increased manufacturing costs due to inefficiencies in pickling processes.

Method used

Control the passage speed of hot-rolled coils through a pickling tank non-uniformly, adjusting speeds based on the regions of the coil to uniformly remove internal oxidation and decarburized layers, and maintain specific steel compositions to ensure uniform layer thickness and quality.

Benefits of technology

Achieves uniformly formed internal oxidation layers in the steel plate's length direction, improving pickling productivity and reducing costs without additional equipment, resulting in steel sheets with excellent surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147778000001
    Figure 2024147778000001
  • Figure 2024147778000002
    Figure 2024147778000002
  • Figure 2024147778000003
    Figure 2024147778000003
Patent Text Reader

Abstract

To provide s steel sheet with excellent surface quality, and a manufacturing method therefor.SOLUTION: The present invention provides an acid-cleaned steel sheet with excellent surface quality, comprising, by wt.%: carbon (C) in an amount greater than or equal to 0.05% and less than 0.4%; 0.5% or less (excluding 0%) of silicon (Si); 0.05% or less of phosphorus (P); 0.03% or less of sulfur (S); 0.01% or less of boron (B); 0.1-2.5% of one or more of manganese (Mn) and chromium (Cr); and the balance consisting of iron (Fe) and inevitable impurities, where the average thickness of an internal oxide layer and / or a decarburized layer, which are formed on a surface layer part of the steel sheet, is 1-10 μm, and where the standard deviation of the thickness of the internal oxide layer and / or the decarburized layer in the length direction of the steel sheet is 2 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel sheet having excellent surface quality and a manufacturing method thereof, and more particularly to a pickled steel sheet and a cold-rolled steel sheet having excellent surface quality with small thickness deviation of an internal oxidation layer and a decarburized layer in the longitudinal direction of the steel sheet, and a manufacturing method thereof. [Background technology]

[0002] In the case of carbon steel, the following patent documents are known which describe suppressing the formation of surface oxides and decarburized layers during the manufacturing stage in order to improve surface quality, and using heat treatment or special equipment to remove the surface oxides and decarburized layers that are formed.

[0003] Patent Document 1 proposes a technique of applying a decarburization inhibitor containing carbon to prevent decarburization that occurs during hot working of carbon steel. Although this can prevent decarburization during the heating stage, it is not preferable in terms of solving the problem of decarburization that occurs during coiling after hot rolling.

[0004] Patent Documents 2 and 3 propose a technique for improving the pickling treatment capacity by adding an additive mainly composed of sulfuric acid in order to remove scale formed on the surface of the steel material. However, this technique does not have the same effect as a technique for uniformly controlling the internal oxide layer along the length of the coil.

[0005] Patent Documents 4 and 5 present descaling technologies that use heat treatment in a decarburizing reducing atmosphere or induction heating to effectively remove scale formed on the surface of steel material. However, these technologies incur costs for the manufacture and use of additional equipment, and are also different from technologies that uniformly control the internal oxide layer along the length of the coil. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 1993-123739 [Patent Document 2] Japanese Patent Publication No. 1998-072686 [Patent Document 3] Japanese Patent Publication No. 2004-331994 [Patent Document 4] Japanese Patent Publication No. 1995-070635 [Patent Document 5] Korean Patent No. 10-1428311 Summary of the Invention [Problem to be solved by the invention]

[0007] According to one aspect of the present invention, there are provided a steel sheet having excellent surface quality and a manufacturing method thereof.

[0008] The object of the present invention is not limited to the above-mentioned contents, and a person skilled in the art will have no difficulty in understanding further object of the present invention from the general contents of this specification. [Means for solving the problem]

[0009] In one embodiment, the present invention relates to a pickled steel sheet having excellent surface quality, which contains, by weight, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, one or more of manganese (Mn) and chromium (Cr): 0.1 to 2.5%, the balance being iron (Fe) and unavoidable impurities, and which has an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the steel sheet of 1 to 10 μm and a standard deviation of the thickness of the internal oxidation layer and / or the decarburized layer in the longitudinal direction of the steel sheet of 2 μm or less.

[0010] In another embodiment of the present invention, the present invention relates to a cold-rolled steel sheet having excellent surface quality, which contains, by weight, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, 0.1 to 2.5% of one or more of manganese (Mn) and chromium (Cr), the balance being iron (Fe) and unavoidable impurities, and which has an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the steel sheet of 1 × [1 - cold rolling reduction rate (%)] μm to 10 × [1 - cold rolling reduction rate (%)] μm, and a standard deviation of the thickness of the internal oxidation layer and / or the decarburized layer in the longitudinal direction of the steel sheet of 2 μm or less.

[0011] Moreover, the pickled steel sheet and cold-rolled steel sheet of the present invention can satisfy the following relational expression 1.

[0012] [Equation 1] C(%)+Si(%) / 6+Mn(%) / 20+Cr(%) / 20+2×P(%)+4×S(%)<0.5

[0013] In still another embodiment, the present invention provides a method for producing a hot-rolled coil containing, by weight percent, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, one or more of manganese (Mn) and chromium (Cr) in an amount of 0.1 to 2.5%, and the balance being iron (Fe) and unavoidable impurities, by immersing and passing the hot-rolled coil through a pickling tank. and removing an internal oxidation layer and / or a decarburized layer in the surface layer portion, wherein when the hot-rolled coil is divided into a first region, a second region, a third region, a fourth region and a fifth region in the longitudinal direction, the speed at which the hot-rolled coil corresponding to the second region, the third region and the fourth region passes through the pickling tank is controlled to be slower than the speed at which the hot-rolled coil corresponding to the first region and the fifth region passes through the pickling tank.

[0014] In still another embodiment of the present invention, the present invention provides a method for manufacturing a steel sheet comprising the steps of preparing a hot-rolled coil containing, by weight, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, at least one of manganese (Mn) and chromium (Cr) in an amount of 0.1 to 2.5%, and the balance being iron (Fe) and unavoidable impurities; and immersing and passing the hot-rolled coil through a pickling tank to form an internal oxide layer and / or a decarburized layer in the surface layer. and cold rolling the hot-rolled steel sheet from which the internal oxidation layer and / or decarburized layer has been removed, wherein when the hot-rolled coil is divided into a first region, a second region, a third region, a fourth region and a fifth region in the longitudinal direction, the speed at which the hot-rolled coil corresponding to the second region, the third region and the fourth region passes through the pickling tank is controlled to be slower than the speed at which the hot-rolled coil corresponding to the first region and the fifth region passes through the pickling tank. Effect of the Invention

[0015] According to the present invention having the above-mentioned configuration, it is possible to provide a carbon steel sheet having excellent surface quality, in which an internal oxide layer, etc. is uniformly formed in the longitudinal direction of the steel sheet, and a manufacturing method thereof. In particular, there is an effect that the productivity of pickling is improved compared to the conventional art, and manufacturing costs are reduced, without incurring additional costs due to additional steps or devices, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will now be described.

[0017] Generally, as is well known, an internal defect layer such as an internal oxide layer and / or a decarburized layer exists in the surface layer of a hot rolled coil manufactured by normal reheating, finish rolling, cooling and coiling. The internal oxide layer may be generated in the process where components such as chromium (Cr), manganese (Mn), silicon (Si), zinc (Zn), magnesium (Mg) and aluminum (Al), which have a higher oxygen affinity than iron (Fe), cause oxidation in the base material. The decarburized layer may be generated in the process where carbon in the steel is combined with oxygen in the air and scale and then discharged into the air in the form of gas. The thickness of such an internal defect layer may vary depending on the components of the hot rolled steel sheet, the temperature when the hot rolled steel sheet is coiled into a hot rolled coil (HC), the cooling time after coiling, the width, thickness and length of the hot rolled steel sheet, etc., and may be within 50 μm.

[0018] On the other hand, such an internal defect layer also affects the subsequent pickling process and cold rolling process, and ultimately becomes a factor that deteriorates the surface properties of the finally manufactured steel sheet. Therefore, the present invention is characterized in that it provides pickled steel sheet and cold rolled steel sheet with excellent surface quality by providing optimal pickling conditions using a hot rolled coil showing thickness deviation of such an internal oxide layer.

[0019] The pickled steel sheet and cold-rolled steel sheet of the present invention will be described below.

[0020] First, the pickled steel sheet and cold-rolled steel sheet of the present invention use steel sheets containing, by weight percent, carbon (C): 0.05% or more but less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, at least one of manganese (Mn) and chromium (Cr) in an amount of 0.1 to 2.5%, and the balance being iron (Fe) and unavoidable impurities. The compositional components of these steels and the reasons for limiting the range of the components will be explained below. Here, "%" means "weight percent" unless otherwise specified.

[0021] Carbon (C): 0.05% or more but less than 0.4% Carbon (C) is an element that effectively contributes to improving the strength of steel, so in the present invention, carbon (C) can be contained at a certain level or more to ensure the strength of a high carbon steel plate. In addition, if the carbon content (C) is less than a certain level, the desired strength, hardness, and durability of the final part cannot be ensured, and the function of a high carbon steel plate cannot be achieved, so in the present invention, the lower limit of the carbon (C) content can be limited to 0.05%. On the other hand, if carbon (C) is added excessively, the strength is improved, but there is a possibility that cracks will occur during the manufacturing process due to the formation of excessive cementite, or cracks will occur on the surface, resulting in a problem of reduced surface quality, which causes a decrease in weldability, so in the present invention, the carbon (C) content can be limited to less than 0.4%. Therefore, the carbon (C) content of the present invention may be in the range of 0.05% to less than 0.4%.

[0022] Silicon (Si): 0.5% or less (excluding 0%) Silicon (Si) is an element with a strong affinity for oxygen, and therefore adding a large amount of it is undesirable because it may induce surface scratches that can be visually observed due to surface scale such as red scale. Therefore, in the present invention, the upper limit of the silicon (Si) content can be limited to 0.5%. However, since silicon (Si) is an element that not only acts as a deoxidizer but also contributes to improving the strength of steel, in the present invention, 0% can be excluded from the lower limit of the silicon (Si) content.

[0023] Phosphorus (P): 0.05% or less Phosphorus (P) is a major element that segregates at grain boundaries and induces a decrease in the toughness of steel. Therefore, it is preferable to control the phosphorus (P) content as low as possible. Therefore, it is theoretically most advantageous to limit the phosphorus (P) content to 0%. However, phosphorus (P) is an impurity that inevitably flows into steel during the steelmaking process, and controlling its content to 0% may induce excessive process load. Therefore, in the present invention, taking these points into consideration, the upper limit of the phosphorus (P) content can be limited to 0.05%.

[0024] ·Sulfur (S): 0.03% or less Sulfur (S) is a major element that forms MnS, increases the amount of precipitates, and embrittles steel. Therefore, it is preferable to control the sulfur (S) content as low as possible. Therefore, it is theoretically most advantageous to limit the sulfur (S) content to 0%. However, sulfur (S) is also an impurity that inevitably flows into steel during the steelmaking process, and controlling its content to 0% may induce excessive process load. Therefore, in the present invention, taking these points into consideration, the upper limit of the sulfur (S) content can be limited to 0.03%.

[0025] Boron (B): 0.01% or less Boron (B) is an element that slows down the transformation rate when austenite transforms into ferrite, pearlite, bainite, etc., and is an element that is easy to control the transformation by cooling. However, if boron (B) is added in excess, it segregates at grain boundaries, causing a decrease in strength, ductility, toughness, etc. Therefore, the boron (B) content of the present invention is preferably 0.01% or less.

[0026] One or more of manganese (Mn) and chromium (Cr): 0.1% or more but less than 2.5% Manganese (Mn) and chromium (Cr) are elements that contribute to the formation of hardenability of steel, so the present invention may contain manganese (Mn) and chromium (Cr) to achieve such an effect. However, excessive addition of expensive elements manganese (Mn) and chromium (Cr) is not preferable from an economical point of view, and excessive addition of manganese (Mn) and chromium (Cr) may reduce weldability, so the content of one or more of manganese (Mn) and chromium (Cr) in the present invention may be in the range of 0.1% or more and less than 2.5%.

[0027] [Equation 1] The pickled steel sheet and cold-rolled steel sheet of the present invention preferably contain C, Si, Mn, Cr, P and S so as to satisfy the following relational formula 1. In the present invention, the following relational formula 1 is specified because the elements in question cause deterioration of weldability. If the sum of the contents of the component elements defined by the following relational formula 1 is 0.5 or more, there is a problem that the weldability deteriorates and cracks occur around the welded part.

[0028] [Equation 1] C(%)+Si(%) / 6+Mn(%) / 20+Cr(%) / 20+2×P(%)+4×S(%)<0.5

[0029] In addition to the above-mentioned steel composition, the remainder of the present invention may contain Fe and inevitable impurities. Inevitable impurities are impurities that may be mixed unintentionally in a normal steel manufacturing process, and cannot be completely eliminated. Any engineer in the field of normal steel manufacturing can easily understand the meaning of this. In addition, the present invention does not completely eliminate the addition of compositions other than the above-mentioned steel composition.

[0030] In the pickled steel sheet of the present invention, the average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer of the steel sheet is required to be in the range of 1 to 10 μm. If the thickness is less than 1 μm, the internal oxidation layer and / or decarburized layer will be removed in large amounts, or will be completely removed to an uncontrollable level. This will not only reduce the productivity of pickling, but will also increase the amount of steel sheet consumed by pickling. On the other hand, if the thickness exceeds 10 μm, the internal oxidation layer and / or decarburized layer will remain thick on the surface, which will cause a problem of reducing surface quality such as durability.

[0031] In the present invention, the thickness of the internal oxidation layer and / or decarburized layer is measured by an optical microscope or an electron microscope (SEM) on the cross section of the steel sheet, and the average thickness is obtained by measuring five or more positions in the length direction of the steel sheet and averaging the measured values. That is, in the present invention, the thickness of the internal oxidation layer and / or decarburized layer is measured by an optical microscope or an electron microscope (SEM) on the cross section of the steel sheet, and the decarburized layer is divided into the base material layer and the decarburized layer by measuring the cross section corroded with a corrosive solution such as nital, and the internal oxidation layer is divided into the base material layer and the internal oxidation layer by directly observing the cross section without corroding. In this case, the average thickness of the internal oxidation layer and / or decarburized layer is measured by measuring five or more positions in the length direction of the steel sheet and averaging the measured values. The measurement positions in the length direction of the steel sheet are such that the coil is divided into five or more equal parts in the length direction, and one or more samples are taken from each of the sections and measured. The standard deviation is obtained by calculating the standard deviation value for the data of five or more positions in the length direction of the steel sheet measured as described above.

[0032] On the other hand, the cold-rolled steel sheet of the present invention has an average thickness of an internal oxide layer and / or a decarburized layer formed in the surface layer portion of the steel sheet that satisfies the range of 1×[1-cold rolling reduction (%)] μm to 10×[1-cold rolling reduction (%)] μm. That is, the thickness of the internal oxide layer and / or the decarburized layer formed in the surface layer portion of the steel sheet also decreases depending on the rolling reduction during cold rolling. Preferably, the average thickness of the internal oxide layer and / or the decarburized layer formed in the surface layer portion of the cold-rolled steel sheet is controlled in the range of 0.2 to 8 μm.

[0033] In addition, the pickled steel sheet and cold-rolled steel sheet of the present invention satisfy the standard deviation of the thickness of the internal oxide layer and / or decarburized layer in the longitudinal direction of the steel sheet of 2 μm or less. If the standard deviation of the thickness exceeds 2 μm, there will be a problem that the surface quality will vary depending on the position, and the amount of removal by pickling will vary, resulting in a large amount of steel sheet consumption removed by pickling or insufficient removal, degrading the surface quality. More preferably, the standard deviation of the thickness is limited to 1.6 μm or less.

[0034] Next, the method for producing the pickled steel sheet and cold-rolled steel sheet having excellent surface quality according to the present invention will be described.

[0035] First, in the present invention, a hot rolled coil is prepared.

[0036] The steel plate contains, by weight, carbon (C): 0.05% or more but less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, 0.1 to 2.5% of one or more of manganese (Mn) and chromium (Cr), and the remainder being iron (Fe) and unavoidable impurities.

[0037] In addition, the present invention is not limited to a specific manufacturing process for manufacturing the hot rolled coil, and a general manufacturing process can be used. Specifically, a general hot rolled coil manufacturing process can be used, including a step of reheating a slab having the above-mentioned steel composition, a step of hot rolling the reheated slab to provide a hot rolled steel sheet, a step of cooling the hot rolled hot rolled steel sheet, a step of coiling the cooled hot rolled steel sheet, and a step of cooling the coiled coil.

[0038] As an example, a hot rolled coil can be manufactured using the following manufacturing process.

[0039] Slab reheating and hot rolling Slabs produced by the normal slab production process may be reheated at a certain temperature range. The lower limit of the reheating temperature can be limited to 1050°C for sufficient homogenization, and the upper limit of the reheating temperature can be limited to 1350°C for economical and surface quality considerations.

[0040] The reheated slab is then rough rolled in a conventional manner, and the rough rolled steel slab may be rolled to a thickness of 1.5 mm to 10 mm by finish hot rolling. In the present invention, the hot rolling may be performed under conventional conditions, but the finish rolling temperature for controlling the rolling load and reducing surface scale may be in the range of 800 to 950°C.

[0041] Cooling and winding The hot-rolled steel sheet can be subjected to controlled cooling immediately after hot rolling. In the present invention, in order to strictly control the surface quality of the hot-rolled steel sheet, the cooling of the present invention is preferably started within 5 seconds. If the time from hot rolling to the start of cooling exceeds 5 seconds, an internal oxide layer and / or a decarburized layer, which is not intended by the present invention, may be formed in the surface layer of the steel sheet due to air cooling in the atmosphere. A more preferable time from hot rolling to the start of cooling may be within 3 seconds.

[0042] In addition, the hot-rolled steel sheet immediately after hot rolling may be cooled to a coiling temperature of 500°C or more and 750°C or less at a cooling rate of 10 to 1000°C / s. If the cooling rate is less than 10°C / s, an internal oxide layer and / or a decarburized layer may be formed in the surface layer of the steel sheet during cooling, which is a problem in that the surface quality targeted by the present invention cannot be ensured. In the present invention, the upper limit of the cooling rate is not particularly limited in order to ensure the targeted surface quality, but the upper limit of the cooling rate can be limited to 1000°C / s in consideration of the limitations of the equipment and economic efficiency. In addition, if the coiling temperature is less than 500°C, a low-temperature transformation structure such as bainite or martensite may be formed, which may cause cracking of the steel sheet. In addition, if the coiling temperature exceeds 750°C, an excessively large amount of an internal oxide layer and / or a decarburized layer may be formed in the surface layer of the steel sheet, which is a problem in that the surface quality targeted by the present invention cannot be ensured.

[0043] Cooling of wound coils The coiled coil is cooled in air, during which not only a scale layer is formed on the surface of the high carbon hot rolled steel sheet, but also an oxide and / or decarburized layer is formed immediately below the surface. The oxide and / or decarburized layer formed immediately below the surface is formed at different depths at the leading and tailing ends and the center in the length direction of the hot rolled steel sheet. This is because the temperatures of the leading and tailing ends and the center are different when the hot rolled coil is cooled in a coiled state. The oxide and decarburized layers immediately below the surface at the leading and tailing ends and the center may be 0 to 5 μm and 3 to 20 μm deep, respectively.

[0044] The hot-rolled steel sheet produced by the above-mentioned production method can have an internal oxide layer and / or decarburized layer formed in the surface layer portion with an average thickness of 2 to 20 μm.

[0045] In the present invention, the hot rolled coil is immersed in and passes through a pickling solution in a pickling tank, thereby removing the internal oxide layer and / or decarburized layer in the surface layer portion.

[0046] In this case, in the present invention, when the hot rolled coil is divided into a first region, a second region, a third region, a fourth region, and a fifth region in the length direction, the speed of passing through the pickling tank of the hot rolled coil corresponding to the second region, the third region, and the fourth region is controlled to be slower than the speed of passing through the pickling tank of the hot rolled coil corresponding to the first region and the fifth region. It is also preferable to control the speed of passing through the pickling tank of the hot rolled coil corresponding to the third region to be slower than the speed of passing through the pickling tank of the hot rolled coil corresponding to the second region and the fourth region. In this way, it is possible to obtain a pickled steel sheet in which the thickness deviation in the length direction is reduced by the pickling treatment, despite the thickness deviation according to the length of the internal oxide layer and / or the decarburized layer formed on the hot rolled coil. In the present invention, the thickness of the internal oxide layer and / or the decarburized layer in the third region is the thickest, and the division may be equal.

[0047] More preferably, the speed at which the hot-rolled coil passes through the pickling tank in the third region is controlled to be 5 mpm to 50 mpm, the average speed at which the hot-rolled coil passes through the pickling tank in the first and fifth regions is controlled to be 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third region] × 1 / 2 to 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third region] × 2, and the speed at which the hot-rolled coil passes through the pickling tank in the second and fourth regions is controlled to be 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third region / 2] × 1 / 2 to 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third region / 2] × 2.

[0048] The speed at which the hot-rolled coil passes through the pickling tank in the third region must be maintained at 50 mpm or less in order to effectively remove oxides and decarburized layers immediately below the surface. On the other hand, if the speed is too low, over-pickling occurs, resulting in a large amount of steel sheet being removed by pickling, and the pickling speed becomes slow, resulting in reduced productivity. Therefore, it is preferable to control the speed to 5 mpm or more.

[0049] The speed at which the hot-rolled coil passes through the pickling tank in the first and fifth zones can be controlled to be faster than that in the third zone, but the speed must be controlled based on the speed at which the hot-rolled coil passes through the pickling tank in the third zone to be 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third zone] × 1 / 2 to 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third zone] × 2. In this case, too, it is preferable to control the speed within a range that effectively removes oxides and decarburized layers just below the surface and does not reduce productivity.

[0050] The speed at which the hot-rolled coil passes through the pickling tank in the second and fourth zones can also be controlled to be faster than that in the third zone, but the speed must be controlled based on the speed at which the hot-rolled coil passes through the pickling tank in the third zone to be 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third zone / 2] × 1 / 2 to 5 × [speed at which the hot-rolled coil passes through the pickling tank in the third zone / 2] × 2. In this case, too, it is preferable to control the speed within a range that effectively removes oxides and decarburized layers immediately below the surface and does not reduce productivity.

[0051] In addition, in the present invention, when a hot-rolled coil is divided into n regions in the length direction, it is more preferable that the speed of passing through the pickling tank of the hot-rolled coil corresponding to the (n / 2)th region, which is the region having the thickest thickness of the internal oxidation layer and / or decarburized layer, is set to 5 mpm to 50 mpm, and when t≦(n / 2), the speed of passing through the pickling tank of the hot-rolled coil corresponding to each region is controlled according to the following relational expression 2, and when t>(n / 2), the speed of passing through the pickling tank of the hot-rolled coil corresponding to each region is controlled according to the following relational expression 3.

[0052] [Equation 2] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n × [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / t] × 1 / 2 ~ n × [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / t] × 2

[0053] [Equation 3] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n × [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / (n-t+1)] × 1 / 2~n × [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / (n-t+1)] × 2 [However, in the relational expression 2-3, n is a natural number, and the tth refers to an order given in sequence so as to correspond to each region divided in the length direction of the hot rolled coil.]

[0054] On the other hand, in the pickling process of the present invention, not only the above-mentioned pickling rate but also the acid concentration and temperature of the pickling solution in the pickling tank can be controlled to efficiently remove the internal oxide layer and / or decarburized layer formed on the surface layer.

[0055] Specifically, the concentration of hydrochloric acid in the pickling solution may be 5 to 25%. If the concentration of hydrochloric acid is less than 5%, there is a problem that the pickling ability decreases, whereas if it exceeds 25%, there is a problem that the concentration of hydrochloric acid is too high, resulting in over-pickling and increased costs.

[0056] The temperature of the pickling solution may be 70° C. to 90° C. If the temperature of the acid is less than 70° C., there is a problem that the pickling ability decreases, and if it is 90° C. or higher, there are problems that the pickling becomes excessive or the amount of consumption due to evaporation increases.

[0057] By the above-mentioned pickling treatment, it is possible to provide a high-carbon pickled steel sheet having excellent surface quality, in which the average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer portion is 1 to 10 μm and the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction is 2 μm or less, more preferably 1.6 μm or less.

[0058] In the present invention, the pickled steel sheet is then cold-rolled to produce a cold-rolled steel sheet.

[0059] The cold rolling reduction can be 10% to 80% depending on the strength and thickness requirements of the final product. When cold rolling is performed in this manner, the average thickness of the oxide layer and decarburized layer immediately below the surface of the pickled steel sheet is reduced in proportion to the reduction. That is, the thickness of the internal oxide layer and decarburized layer of the cold rolled steel sheet can be calculated as [thickness of the internal oxide layer and decarburized layer of the pickled steel sheet]×cold rolling reduction (%) / 100.

[0060] Therefore, the cold-rolled steel sheet of the present invention can have an average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer portion of the steel sheet satisfying 1×[1-cold rolling reduction (%)] μm to 10×[1-cold rolling reduction (%)] μm.

[0061] Preferably, the average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer portion of the cold rolled steel sheet satisfies the range of 0.2 to 8 μm.

[0062] On the other hand, the standard deviation of the thickness of the internal oxide layer and / or decarburized layer in the longitudinal direction of the cold-rolled steel sheet can be maintained at 2 μm or less, more preferably 1.6 μm or less, like the above-mentioned pickled steel sheet. EXAMPLES

[0063] The present invention will be described in detail below with reference to examples. It should be noted that the following examples are for the purpose of understanding the present invention, and are not intended to specify the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.

[0064] (Example) After producing a hot-rolled coil having the composition shown in Table 1 below, pickled steel sheets and cold-rolled steel sheets were produced using the conditions shown in Table 2 below. Each hot-rolled coil was produced using a conventional production method. That is, a steel slab having the composition shown in Table 1 below was reheated in a temperature range of 1050 to 1350°C, then rough-rolled, and the rough-rolled steel slab was finish-hot-rolled in a temperature range of 800 to 950°C. Thereafter, the finish-hot-rolled hot-rolled steel sheet was cooled to a temperature range of 500 to 750°C at a cooling rate of 10 to 1000°C / s, coiled, and then air-cooled to produce the hot-rolled steel sheet.

[0065] Then, each of the hot-rolled coils produced above was immersed in a pickling tank under the conditions shown in Table 2 below to pickle the internal oxide layer and / or decarburized layer formed on the surface, thereby producing pickled steel sheets. Specifically, each of the hot-rolled coils produced above was divided into five equal parts in the length direction, a first region, a second region, a third region, a fourth region, and a fifth region, and the speed at which the hot-rolled coil for each region passed through the pickling tank was controlled as shown in Table 2 below to produce pickled steel sheets.

[0066] Thereafter, the average thickness (μm) of the internal oxide layer and / or decarburized layer of the pickled steel sheet discharged from the pickling tank and having the internal oxide layer and / or decarburized layer removed from its surface was measured and compared with the average thickness (μm) of the internal oxide layer and / or decarburized layer of the hot-rolled coil before pickling, and the results are shown in Table 3 below. At this time, the standard deviation (μm) of the thickness of the internal oxide layer and / or decarburized layer in the length direction of the pickled steel sheet was also measured and is shown in Table 3 below.

[0067] Meanwhile, in the present invention, the above-prepared pickled steel sheets were cold-rolled under the conditions shown in Table 2 below to further produce cold-rolled steel sheets. The average thickness (μm) of the internal oxide layer and / or decarburized layer of each of the produced cold-rolled steel sheets was measured in comparison with the average thickness (μm) of the internal oxide layer and / or decarburized layer of the hot-rolled coil before pickling, and the results are shown in Table 3 below. At this time, the standard deviation (μm) of the thickness of the internal oxide layer and / or decarburized layer in the length direction of the above-prepared cold-rolled steel sheets was also measured and is shown in Table 3 below.

[0068] Here, the specific method for measuring the average thickness (μm) and standard deviation (μm) of the internal oxidation layer and / or decarburized layer is as follows. First, the thickness of the internal oxidation layer and / or decarburized layer is measured by measuring the cross section of the steel plate with an optical microscope or scanning electron microscope (SEM), and the decarburized layer is divided into the base material layer and the decarburized layer by measuring the cross section corroded with a corrosive solution such as nital, and the internal oxidation layer is divided into the base material layer and the internal oxidation layer by directly observing the cross section without corroding. In this case, the average thickness of the internal oxidation layer and / or decarburized layer is measured by measuring five or more positions in the length direction of the steel plate and calculating the average value. The measurement positions in the length direction of the steel plate are measured by dividing the coil into five or more equal parts in the length direction, and one or more samples are taken from each of the sections and measured. The standard deviation is measured by calculating the standard deviation value for the data of five or more positions in the length direction of the steel plate measured as described above.

[0069] [Table 1]

[0070] [Table 2]

[0071] [Table 3]

[0072] As shown in Table 1-3 above, in the case of Invention Examples 1 to 11, which satisfy all of the alloy compositions and manufacturing conditions of the present invention, it can be confirmed that the average thickness of the internal oxidation layer and / or decarburized layer of the hot-rolled steel sheet, the average thickness of the internal oxidation layer and / or decarburized layer of the pickled steel sheet, the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the pickled steel sheet, the average thickness of the internal oxidation layer and / or decarburized layer of the cold-rolled steel sheet, and the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the cold-rolled steel sheet all satisfy the required ranges.

[0073] In contrast, the average thickness of the internal oxidation layer and / or decarburized layer of the pickled steel sheet and cold-rolled steel sheet of Comparative Example 1-2, in which the speed of passage through the pickling tank was uniformly controlled, was evaluated to be at the desired level. However, it can be seen that the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the pickled steel sheet and cold-rolled steel sheet was too high, making it impossible to ensure uniform surface quality.

[0074] Moreover, in Comparative Example 3-4, the value of the weldability index defined by Relational Expression 1 is excessive, and it can be confirmed that the weldability is deteriorated.

[0075] On the other hand, the conventional example in which the speed of passage through the pickling tank is constantly controlled at an excessively low speed represents a case of over-pickling operation generally performed in pickling treatment, and it is understood that the internal oxidation / decarburization layer of the pickled steel sheet or cold-rolled steel sheet that has been slowly passed through the pickling tank is entirely removed. However, although this conventional method does not have the problem of surface defects of the product because the internal oxidation / decarburization layer of the pickled steel sheet or cold-rolled steel sheet is entirely removed, it has a problem that the time required for the pickling operation is very long, which is a fundamental problem of inefficiency and uneconomical.

[0076] Although the embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and it will be obvious to those having ordinary skill in the art that various modifications and variations are possible without departing from the technical idea of ​​the present invention described in the claims.

Claims

1. In weight percent, carbon (C): 0.05% or more but less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, one or more of manganese (Mn) and chromium (Cr): 0.1 to 2.5%, the balance being iron (Fe) and unavoidable impurities, The average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer portion of the steel sheet is 1 to 10 μm, and A pickled steel sheet having excellent surface quality, in which the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the steel sheet is 2 μm or less.

2. 2. The pickled steel sheet having excellent surface quality according to claim 1, which satisfies the following relational expression 1: [Relationship 1] C (%) + Si (%) / 6 + Mn (%) / 20 + Cr (%) / 20 + 2 × P (%) + 4 × S (%) < 0.5

3. 2. The high-carbon pickled steel sheet having excellent surface quality according to claim 1, wherein a standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the steel sheet is 1.6 μm or less.

4. In weight percent, carbon (C): 0.05% or more but less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, one or more of manganese (Mn) and chromium (Cr) 0.1 to 2.5%, and the balance iron (Fe) and unavoidable impurities. the average thickness of the internal oxidation layer and / or decarburized layer formed in the surface layer portion of the steel sheet is 1×[1−cold rolling reduction (%)] μm to 10×[1−cold rolling reduction (%)] μm, A cold-rolled steel sheet having excellent surface quality, in which the standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the steel sheet is 2 μm or less.

5. The cold rolled steel sheet having excellent surface quality according to claim 4, wherein an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the steel sheet is in a range of 0.2 to 8 μm.

6. The cold-rolled steel sheet having excellent surface quality according to claim 4, which satisfies the following relational expression 1. [Relationship 1] C (%) + Si (%) / 6 + Mn (%) / 20 + Cr (%) / 20 + 2 × P (%) + 4 × S (%) < 0.5

7. 5. The high carbon cold rolled steel sheet having excellent surface quality according to claim 4, wherein a standard deviation of the thickness of the internal oxidation layer and / or decarburized layer in the longitudinal direction of the steel sheet is 1.6 μm or less.

8. A method for producing a pickled steel sheet, comprising: preparing a hot-rolled coil containing, by weight, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, at least one of manganese (Mn) and chromium (Cr) in an amount of 0.1 to 2.5%, with the balance being iron (Fe) and unavoidable impurities; and immersing and passing the hot-rolled coil through a pickling tank to remove an internal oxide layer and / or a decarburized layer in a surface layer portion, A method for manufacturing a pickled steel sheet with excellent surface quality, in which, when the hot-rolled coil is divided into a first region, a second region, a third region, a fourth region, and a fifth region in the longitudinal direction, the speed at which the hot-rolled coil corresponding to the second region, the third region, and the fourth region passes through the pickling tank is controlled to be slower than the speed at which the hot-rolled coil corresponding to the first region and the fifth region passes through the pickling tank.

9. The method for producing a pickled steel sheet having excellent surface quality according to claim 8 , wherein the hot-rolled coil satisfies the following relational expression 1: [Relationship 1] C (%) + Si (%) / 6 + Mn (%) / 20 + Cr (%) / 20 + 2 × P (%) + 4 × S (%) < 0.5

10. The hot rolled coil is The steel slab is reheated in a temperature range of 1050 to 1350 ° C., then roughly rolled, and then the roughly rolled steel slab is finish hot rolled in a temperature range of 800 to 950 ° C.; cooling the finish hot-rolled hot-rolled steel sheet to a temperature range of 500 to 750° C. at a cooling rate of 10 to 1000° C. / s, and then coiling the steel sheet; and air-cooling the coiled hot-rolled coil.

11. 9. The method for producing a pickled steel sheet having excellent surface quality according to claim 8, wherein a speed at which the hot-rolled coil corresponding to the third region passes through the pickling tank is controlled to be slower than a speed at which the hot-rolled coil corresponding to the second region and the fourth region passes through the pickling tank.

12. The pickling tank passing speed of the hot-rolled coil in the third region is 5 mpm to 50 mpm, the average pickling tank passing speed of the first and fifth regions is 5 x [pickling tank passing speed of the hot-rolled coil in the third region] x 1 / 2 to 5 x [pickling tank passing speed of the hot-rolled coil in the third region] x 2, and the pickling tank passing speed of the hot-rolled coil in the second and fourth regions is 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2] x 1 / 2 to 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2] x 2. A method for producing a pickled steel sheet having excellent surface quality according to claim 8, wherein the pickling tank passing speed of the hot-rolled coil in the second and fourth regions is controlled to be 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2] x 1 / 2 to 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2] x 2.

13. 9. The method for producing a pickled steel sheet with excellent surface quality according to claim 8, wherein, when a hot-rolled coil is divided into n regions in the longitudinal direction, the pickling tank passing speed of the hot-rolled coil corresponding to the (n / 2)th region, which is the region having the thickest thickness of the internal oxidation layer and / or decarburized layer, is set to 5 mpm to 50 mpm, and when t≦(n / 2), the pickling tank passing speed of the hot-rolled coil corresponding to each region is controlled according to the following relational expression 2, and when t>(n / 2), the pickling tank passing speed of the hot-rolled coil corresponding to each region is controlled according to the following relational expression 3. [Relationship 2] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / t)] x 1 / 2 to n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / t] x 2 [Relationship 3] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / (n-t+1)] x 1 / 2 to n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / (n-t+1)] x 2 [However, in the relational expression 2-3, n is a natural number, and the t-th refers to an order given in sequence so as to correspond to each region divided in the length direction of the hot rolled coil.]

14. The method for producing a pickled steel sheet having excellent surface quality according to claim 8, wherein the concentration of hydrochloric acid in the pickling solution in the pickling tank is 5 to 25%.

15. The method for producing a pickled steel sheet having excellent surface quality according to claim 8, wherein the temperature of the pickling solution in the pickling tank is in the range of 70°C to 90°C.

16. 9. The method for producing a pickled steel sheet having excellent surface quality according to claim 8, wherein after the pickling, an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the steel sheet is 1 to 10 μm, and a standard deviation of the thickness of the internal oxidation layer and / or the decarburized layer in a longitudinal direction of the pickled steel sheet is 2 μm or less.

17. A method for producing a cold-rolled steel sheet, comprising the steps of: preparing a hot-rolled coil containing, by weight, carbon (C): 0.05% or more and less than 0.4%, silicon (Si): 0.5% or less (excluding 0%), phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, boron (B): 0.01% or less, at least one of manganese (Mn) and chromium (Cr) in an amount of 0.1 to 2.5%, with the balance being iron (Fe) and inevitable impurities; immersing and passing the hot-rolled coil through a pickling tank to remove an internal oxide layer and / or a decarburized layer in a surface layer portion; and cold-rolling the hot-rolled steel sheet from which the internal oxide layer and / or the decarburized layer has been removed, A method for manufacturing a cold-rolled steel sheet with excellent surface quality, in which, when the hot-rolled coil is divided into a first region, a second region, a third region, a fourth region, and a fifth region in the longitudinal direction, the speed at which the hot-rolled coil corresponding to the second region, the third region, and the fourth region passes through the pickling tank is controlled to be slower than the speed at which the hot-rolled coil corresponding to the first region and the fifth region passes through the pickling tank.

18. The method for producing a cold-rolled steel sheet having excellent surface quality according to claim 17, wherein the hot-rolled coil satisfies the following relational expression 1. [Relationship 1] C (%) + Si (%) / 6 + Mn (%) / 20 + Cr (%) / 20 + 2 × P (%) + 4 × S (%) < 0.5

19. The hot rolled coil is The steel slab is reheated in a temperature range of 1050 to 1350 ° C., then roughly rolled, and then the roughly rolled steel slab is finish hot rolled in a temperature range of 800 to 950 ° C.; cooling the finish hot-rolled hot-rolled steel sheet to a temperature range of 500 to 750° C. at a cooling rate of 10 to 1000° C. / s, and then coiling the steel sheet; and air-cooling the coiled hot rolled coil.

20. The method for producing a cold-rolled steel sheet having excellent surface quality according to claim 17, wherein a speed at which the hot-rolled coil corresponding to the third region passes through the pickling tank is controlled to be slower than a speed at which the hot-rolled coil corresponding to the second region and the fourth region passes through the pickling tank.

21. The pickling tank passing speed of the hot-rolled coil in the third region is 5 mpm to 50 mpm, the average pickling tank passing speed of the first region and the fifth region is 5 x [pickling tank passing speed of the hot-rolled coil in the third region] x 1 / 2 to 5 x [pickling tank passing speed of the hot-rolled coil in the third region] x 2, and the pickling tank passing speed of the hot-rolled coil in the second region and the fourth region is 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2] x 1 / 2 to 5 x [pickling tank passing speed of the hot-rolled coil in the third region / 2]. The method for producing a cold-rolled steel sheet having excellent surface quality according to claim 17, wherein the pickling tank passing speed is controlled to 2.

22. 18. The method for producing a cold-rolled steel sheet with excellent surface quality according to claim 17, wherein, when a hot-rolled coil is divided into n regions in the length direction, the pickling tank passing speed of the hot-rolled coil corresponding to the (n / 2)th region, which is the region having the thickest thickness of the internal oxidation layer and / or decarburized layer, is set to 5 mpm to 50 mpm, and when t≦(n / 2), the pickling tank passing speed of the hot-rolled coil corresponding to each region is controlled according to the following Relational Formula 2, and when t>(n / 2), the pickling tank passing speed of the hot-rolled coil corresponding to each region is controlled according to the following Relational Formula 3. [Relationship 2] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / t)] x 1 / 2 to n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / t] x 2 [Relationship 3] Pickling tank passing speed of hot-rolled coil corresponding to the tth region = n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region / (n-t+1)] x 1 / 2 to n x [(pickling tank passing speed of hot-rolled coil corresponding to the (n / 2)th region) / (n-t+1)] x 2 [However, in the relational expression 2-3, n is a natural number, and the t-th refers to an order given in sequence so as to correspond to each region divided in the length direction of the hot rolled coil.]

23. The method for producing a cold rolled steel sheet having excellent surface quality according to claim 17, wherein the cold rolling reduction is controlled in the range of 10 to 80% during the cold rolling.

24. The method for producing a cold-rolled steel sheet having excellent surface quality according to claim 17, wherein after the pickling, an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the hot-rolled steel sheet is 1 to 10 μm, and a standard deviation of the thickness of the internal oxidation layer and / or the decarburized layer is 2 μm or less.

25. 18. The method for producing a cold-rolled steel sheet with excellent surface quality according to claim 17, wherein after the cold rolling, an average thickness of an internal oxidation layer and / or a decarburized layer formed in a surface layer portion of the steel sheet is 1×[1−cold rolling reduction (%)] μm to 10×[1−cold rolling reduction (%)] μm, and a standard deviation of the thickness of the internal oxidation layer and / or the decarburized layer in the longitudinal direction of the cold-rolled steel sheet is 2 μm or less.

Citation Information

Patent Citations

  • Method for pickling hot rolled steel strip

    JP1999189885A

  • Hot-dip galvanized steel sheet and method of manufacturing the same

    JP2012012655A

  • Hot rolled steel strip, cold rolled steel strip, and production method of hot rolled steel strip

    JP2016130334A

  • High-strength plated steel sheet excellent in platability, workability and delayed fracture resistant characteristics, and method for producing the same

    JP2016130356A