Coating method using coating roller

A paint composition with specific properties and a specialized roller design addresses the uneven finishes of existing water-based paints, achieving a uniform and smooth coating film on walls.

JP2024147904APending Publication Date: 2024-10-17KIKUSUI CHEM IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023060639
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing water-based paint compositions using mica and calcium carbonate at specific concentrations result in uneven finishes and shine, limiting their application with paint rollers.

Method used

A paint composition with a Ti value of 2 to 10, solid content of 10.0 to 80.0% by weight, and a coating roller with a lining of crossed warp and weft threads and thread-like pile, applied with bristles of 5 to 32 mm, to achieve a uniform and smooth finish.

Benefits of technology

The method forms a flat paint film with uniform thickness, matching the wall surface shape, reducing paint scattering and waste, and ensuring a smooth, clean finish.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147904000001
    Figure 2024147904000001
Patent Text Reader

Abstract

To provide a coating method using a coating roller capable of obtaining a beautiful coated wall surface by coating utilizing the characteristics of the coating roller.SOLUTION: In the case of applying a coating material having a coating material Ti value within a range of 2-10 and a coating material solid portion within a range of 10.0-80.0 weight% to a coating object with a coating roller, a coating part of the coating roller is formed by knitting a thread-like pile into a backing fabric, whose warp and weft threads are crossed at right angles. The coating roller has a coating material content amount of 0.5-3.0 g / cm3. Since coating is performed by using the coating roller whose bristle length is within a range of 5-32 mm and utilizing the characteristics of the coating roller, it is possible to obtain a beautiful coated wall surface with the finished coated film also suitable for a surface shape such as a wall surface.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a coating method for the wall surfaces of architectural structures and the like using a coating composition such as a paint or coating material, and in particular to a coating method using a coating roller. [Background technology]

[0002] When painting the walls of buildings and structures, spray painting is often done using a spray gun, which makes it possible to obtain a beautiful painted wall surface that matches the surface shape of the wall, etc. For example, on smooth surfaces, a flat coating of uniform thickness can be formed. Spray painting is a method of painting that uses air pressure to spray paint, which makes the painting process quick and produces a good finish. However, because paint tends to scatter, this can have an adverse effect on the working environment and the surrounding area.

[0003] In addition, paint may be wasted. Furthermore, the finish may vary depending on the skill of the painter. Therefore, in recent years, painting with a paint roller has become more common instead of spray painting. This has significantly reduced paint splashing during the painting process and has greatly reduced paint waste. However, the finished product may be inferior to that of spray painting.

[0004] There are many different types of painting rollers available, and they can be selected based on the amount of paint to be applied and the finish of the coating film formed. For this reason, an aqueous paint composition such as that described in Patent Document 1, JP 2019-135282 A, has been proposed.

[0005] Prior Art 1 describes an aqueous coating composition which contains (a) a synthetic resin emulsion, (b) mica having an average particle size of 0.3 to 3 mm, and (c) calcium carbonate having an average particle size of 0.1 to 0.5 mm, in which the content of component (b) is 3 to 30 parts by mass and the content of component (c) is 20 to 100 parts by mass per 100 parts by mass of the solid content in component (a), and which has a viscosity of 1,000 to 100,000 mPa s measured using a B-type viscometer at a rotation speed of 20 rpm and a coating temperature of 25°C, and a Ti value (viscosity at a rotation speed of 2 rpm and a coating temperature of 25°C / viscosity at a rotation speed of 20 rpm and a coating temperature of 25°C) of 2 to 8.

[0006] As a result, by containing a synthetic resin emulsion, mica having a specified average particle size, and calcium carbonate in specified concentrations, it is possible to form a uniform coating film with excellent workability when roller-applied using a medium-pile roller, etc. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-135282 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the aqueous coating composition in Patent Document 1 contains mica having a specific average particle size and calcium carbonate at specific concentrations, which imposes limitations on the finished design. This is because the inclusion of mica in the aqueous coating composition makes the coating film shiny in parts, and the content of calcium carbonate affects the gloss of the coating film.

[0009] The present disclosure provides a paint that takes advantage of the characteristics of a painting roller, the finished coating film can be selected as desired, a flat coating film of uniform thickness can be formed on a smooth surface, and a beautifully painted wall surface that matches the surface shape of a wall or the like can be obtained, and an easy painting method using a painting roller is provided. [Means for solving the problem]

[0010] In the case where a paint having a Ti value of 2 to 10 and a paint solid content of 10.0 to 80.0% by weight is applied to an object to be coated by using a coating roller, the coating part of the coating roller is made of a backing in which warp and weft threads are crossed at right angles and thread-like pile is woven into the backing, and the coating amount of the coating roller is 0.5 to 3.0 g / cm 3 The coating is carried out using a coating roller having a bristle length in the range of 5 to 32 mm.

[0011] This allows the paint to take advantage of the characteristics of painting rollers, and the finished coating can be selected as desired. On smooth surfaces, a flat coating of uniform thickness can be formed, resulting in a beautifully painted wall surface that matches the surface shape of the wall, etc. The specific gravity of the paint is in the range of 0.8 to 2.5, the content of fillers contained in the paint is in the range of 10.0 to 70.0 weight %, and the particle size is in the range of 1.0 to 800.0 μm, so that the finish becomes more uniform and smooth.

[0012] By having the coating film formed by painting be in the range of 30 to 1000 μm, a more uniform and smooth coating film can be obtained, resulting in a good finish. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present disclosure will be described. The present disclosure relates to a method for coating a substrate with a coating material having a Ti value of 2 to 10 and a coating material solid content of 10.0 to 80.0% by weight using a coating roller, the coating portion of the coating roller being made of a backing having warp and weft threads crossed at right angles and having thread-like pile woven into it, and the coating material load of the coating roller being 0.5 to 3.0 g / cm 3 The coating is performed using a coating roller having a bristle length in the range of 5 to 32 mm.

[0014] First, the paint used in the present disclosure is a paint generally used in painting operations, and is mainly composed of a binder component such as an organic binder, such as synthetic resin, or an inorganic binder, such as cement. The types of paint include clear paint, enamel paint, matte paint, etc., as well as primers, sealers, and base conditioners, and further include coating materials for applying patterns such as undercoats. The type of paint to be used can be selected appropriately depending on the application.

[0015] Many of these binder components are made of synthetic resins, and paints that contain them as their main component are applied to the substrate or other object to be coated, and then cured and dried to form a coating film that covers the object. The synthetic resins include acrylic resin, silicone resin, acrylic silicone resin, fluororesin, polyurethane resin, styrene resin, epoxy resin, melamine resin, alkyd resin, vinyl chloride resin, vinyl acetate resin, polyester resin, polyether resin, phenolic resin, ketone resin, and other resins.

[0016] In many cases, synthetic resin emulsions are used, in which these synthetic resins are dispersed in water. Paints using these synthetic resin emulsions are water-based paints that use water as a solvent, and are preferred in terms of ease of handling and workability. These synthetic resins may be used alone or in combination of two or more kinds. The monomers constituting these resins are generally used alone or in copolymer form.

[0017] Among the synthetic resin emulsions using these synthetic resins, acrylic synthetic resin emulsions, acrylic styrene synthetic resin emulsions, acrylic silicone synthetic resin emulsions, and urethane synthetic resin emulsions, which have good water resistance, are preferably used. These synthetic resin emulsions are also suitable for use in terms of their suitability for coating materials, the physical properties of the coating film, and ease of availability, in addition to their water resistance.

[0018] Clear paints are often made using this synthetic resin and, if necessary, regular paint additives. These additives include surfactants used as defoamers, dispersants, and wetting agents, high-boiling point solvents used as film-forming aids and antifreeze agents, thickeners for adjusting viscosity, leveling agents, preservatives, anti-algae agents, anti-fungal agents, antibacterial agents, pH adjusters, crosslinking agents, and silane coupling agents.

[0019] Enamel paints, matte paints, etc. can be obtained by adding coloring components. These pigment components include white pigments such as titanium oxide and zinc oxide, inorganic pigments such as iron oxide, and organic pigments. Other fillers include extender pigments such as calcium carbonate, kaolin, talc, clay, aluminum hydroxide, bentonite, white carbon, and precipitated barium sulfate. It is also possible to add aggregates such as silica sand and kansui sand, as well as lightweight aggregates such as zeolite and perlite.

[0020] It is also possible to further add fibers, etc. In addition to inorganic aggregates, organic aggregates can also be used. These may be used alone or in combination of two or more kinds. It is preferable to add these fillers, and the content is preferably in the range of 10.0 to 70.0% by weight. This applies to paints such as enamel paints and matte paints that are used for the purpose of painting for decoration such as coloring, and are often used in combination with coloring components.

[0021] If the content of these fillers is within the range, the paint will shrink less when it dries, the finish will be more uniform and smooth, an appropriate film thickness can be ensured, and the physical properties of the paint film, such as weather resistance, will be good, making it easy to apply. A more preferable range is 10.0 to 50.0% by weight, and within this range, a more uniform and smooth finish can be achieved, an appropriate film thickness can be ensured, and a good coating film can be obtained.

[0022] In addition, the particle size is preferably in the range of 1.0 to 800.0 μm. If it is smaller than 1.0 μm, the specific surface area of ​​the fillers becomes large, making it difficult to apply the fillers with a painting roller as described below, and it may be difficult to form a flat painted surface. If the particle size is larger than 800.0 μm, it may be difficult to obtain a flat coating film due to the influence of the filler, and coating may be difficult because the coating roller described below may become clogged or the coating roller may not be able to hold the coating.

[0023] The thickness is preferably in the range of 1.0 to 100.0 μm. If a coating material within this range is used, a flat coating film of uniform thickness with few cracks can be formed, and a beautiful coated wall surface can be obtained. The paint is composed of the constituent materials as described above, and the Ti value of the paint must be in the range of 2 to 10, and the paint solids content must be in the range of 10.0 to 80.0.

[0024] The Ti value of this paint indicates the thixotropy, which is the viscosity of the paint, and is calculated by using a B-type viscometer to determine the ratio of apparent viscosities at two rotational speeds. The formula for calculating the Ti value is shown below. Ti value = viscosity at low rotation speed / viscosity at 10 times higher rotation speed. The measurement conditions are 23°C and the measured value after 60 seconds of rotation.

[0025] When the Ti value is 1, the paint is a Newtonian fluid, and the degree of thixotropy increases as the Ti value increases above 1. With the Ti value within this range, there is little dripping of the paint when applied, the evenness of the coating film is not impaired, and the storage stability of the paint is good. By keeping the solids content of the coating material within this range, shrinkage of the coating material during drying is small, and the flatness of the coating film is not impaired.

[0026] It is preferable that this Ti value is in the range of 2 to 7. If it is lower than 2, when applied to a vertical surface, the paint may drip before drying, which may prevent the formation of a uniform coating film, and the coating film may become too thin in some places. If it is higher than 7, it may be difficult to apply the paint and a smooth coating may not be obtained.

[0027] More preferably, the Ti value is in the range of 2 to 5. If the Ti value is within this range, the coating material is easy to apply and can give a flat coating film. The viscosity of the coating material is preferably in the range of 0.5 to 10.0 Pa·s. This viscosity is measured using a B-type viscometer in the same manner as in determining the Ti value, and the measurement conditions are 23° C., No. 3 rotor, 20 rpm, and 60 seconds.

[0028] If the viscosity is lower than 0.5 Pa·s, the paint is easy to apply, but when applied to a vertical surface, it is prone to dripping and may not produce a consistent finish, such as a flat coating. If the viscosity is higher than 10.0 Pa·s, the paint is difficult to apply with a paint roller, the thickness of the coating may be uneven, and the finish may not be consistent. More preferably, the viscosity of the coating material is in the range of 0.5 to 7.0 Pa·s. Within this range, coating workability with a coating roller is good, and a smooth, clean coating film can be obtained.

[0029] The paint solids content is in the range of 10.0 to 80.0% by weight, and being within this range makes it possible to obtain a beautifully painted wall surface that matches the surface shape of the object to be painted, etc. More preferably, the paint solids content is in the range of 20.0 to 70.0% by weight. If the paint solids content is lower than 20.0% by weight, the coating film may become thin and it may not be possible to obtain a coating film of uniform thickness, depending on the type of object to be coated.

[0030] If it is more than 70.0% by weight, coating may be difficult and a coating film of uniform thickness may not be obtained. Furthermore, when the paint is a clear paint, the range is preferably 20.0 to 40.0% by weight, and when it is an enamel paint or a matte paint, the range is preferably 30.0 to 55.0% by weight.

[0031] This is because enamel paints and matte paints contain pigment components, which means that the paint solids content is higher than that of clear paints. Since the coating material is in these ranges, shrinkage during drying is minimal, the flatness of the coating film is not impaired, and a beautifully painted wall surface can be obtained, making painting easy.

[0032] The specific gravity of the paint is preferably in the range of 0.8 to 2.5. When the specific gravity is within this range, the finish becomes more uniform and smooth, an appropriate film thickness can be ensured, and painting becomes easier. If it is lower than 0.8, it will take time to ensure an appropriate film thickness, and if it is higher than 2.5, the paint will be heavy and painting work may become difficult.

[0033] More preferably, it is in the range of 1.0 to 2.0, and within this range, a good coating film can be obtained. The specific gravity of the paint is preferably in the range of 0.8 to 1.8 when the paint is a clear paint, and in the range of 1.0 to 2.0 when the paint is an enamel paint or a matte paint.

[0034] This is because enamel paint and matte paint contain pigment components, which makes the specific gravity of the paint higher than that of clear paint. Furthermore, because the range is as described above, the finish is more uniform and smooth without impairing the flatness of the coating film, an appropriate film thickness can be ensured, and coating can be easily performed.

[0035] The coating part of the coating roller for coating the above-mentioned paint is made of a backing in which warp and weft threads cross at right angles, with thread-like pile woven into it, and the coating amount of the coating roller is 0.5 to 3.0 g / cm 3 The coating is performed using a coating roller having a bristle length in the range of 5 to 32 mm. The painting roller used in the present disclosure paints with a painting part made of woven thread-like pile, which is an aggregate of fibers. Because the pile has a high density, air bubbles are less likely to become caught in the paint, resulting in excellent finish and paint scattering properties.

[0036] In addition, because the fiber aggregate is firmly fixed to the lining, in which the warp and weft threads cross at right angles, there is little loss of pile in the painted area, allowing for the formation of a beautiful painted surface. The fibers used in this coating are not particularly limited, but synthetic fibers are mainly used, such as acrylic fibers, polyester fibers, and nylon fibers.

[0037] Paint rollers made of acrylic fibers are light and flexible, making them easy to paint with and easy to absorb paint. They are also relatively resistant to acids and alkalis, making them suitable for use with many types of paint. Polyester fiber is often used in high viscosity paints because it is relatively strong, resistant to abrasion, durable, and has excellent elasticity.

[0038] Nylon fiber is strong, has good paint release properties, and is highly elastic. This painting roller has a bristle length in the range of 5 to 32 mm, and the amount of paint contained in the bristle length is 0.5 to 3.0 g / cm 3 The range is to use one that is within this range.

[0039] This painting roller is composed of a roller portion having a painting part and a handle for supporting the roller portion. The roller has a different inner diameter depending on the type, and the inner diameter is in the range of about 10.0 to 40.0 mm in diameter, and the coating portion is formed from the outer periphery of the inner diameter.

[0040] Typical examples of this inner diameter include a 38 mm one for painting relatively large areas, a 27 mm one that is easy to use, and a 17 mm one that is suitable for painting small details. The paint load is expressed by the weight of paint that can be contained in the volume of the painting roller determined by the length, circumference, and bristles, and this load is 0.5 to 3.0 g / cm. 3 If the amount is less than this range, the area that can be painted at one time becomes small, resulting in poor workability.

[0041] If the amount is greater than this range, a larger amount of paint can be applied at one time, but it takes time to spread the amount of paint evenly, and in some cases the paint may dry out during the process, making it impossible to form a uniform coating. In addition, the amount of paint absorbed is affected by the bristle length of the painting roller, so it is selected within the range of 5 to 32 mm depending on the type and shape of the surface to be painted and the type of paint, etc., with a bristle length in the range of 5 to 20 mm being preferable.

[0042] If the bristle length is in the range of 5 to 6 mm, a smoother finish can be achieved, but since the amount of paint absorbed is small, there will be many patchwork areas on the painted surface. In addition, brushes with a bristle length of 7 to 8 mm can hold a sufficient amount of paint and expel the contained paint well, providing a good balance between the flatness of the painted surface and ease of use.

[0043] Those in the 10 to 14 mm range have a relatively high paint content and the paint is discharged well, providing a good balance between the flatness of the painted surface and workability. Those in the 15 to 20 mm range can hold a large amount of paint, have good discharge, and are easy to work with. They can also be used to paint slightly uneven surfaces.

[0044] Painting is performed using the paint and painting roller described above. This painting is often performed mainly on pillars, beams, floors, walls, etc. that constitute buildings, and these buildings may have a large paint area and complex shapes in the details, and in such cases, the effects of the present disclosure are fully exhibited. Examples of surfaces that can be painted include mortar, concrete, ALC boards, extruded boards, siding boards, calcium silicate boards, gypsum boards, calcium carbonate foam boards, non-flammable volcanic vitreous laminate boards, fiber-reinforced cement boards, and lightweight cement boards, all of which contain inorganic components such as cement.

[0045] Other examples include iron products such as steel materials, iron sheets, metal siding, etc. Other examples include tiles, glass, stone, wood, and plastic products. It is preferable that the coating film formed by coating is in the range of 30 to 1000 μm. If it is in this range, a more uniform and smooth coating film can be obtained, and a good finish can be obtained.

[0046] A more preferable range is 80 to 200 μm, and within this range, the film thickness is sufficient, the surface to be coated can be protected, and the coating operation can be carried out efficiently. Such a coating film is smooth, and this smoothness means that there is no unevenness in color or gloss, and when the coated surface is touched with the hand, there are no agglomerates of the paint components or unnatural unevenness, and it has a consistent feel to the touch.

[0047] This condition means that the variation in thickness on the cross section of the coating film is within an error range of ±15.0% from the center value of the coating film. Within this range, painting can be carried out efficiently, a flat coating film of uniform thickness can be formed, and a clean, smooth painted wall surface that matches the surface shape of the wall, etc. can be obtained.

[0048] If the error is outside this range, the unevenness of the gloss of the coating film can be confirmed. More preferably, the error is within the range of ±10.0%, and if it is within this range, a coating film with a more uniform thickness and flatness can be formed, and a smooth painted wall surface can be obtained. The above embodiment will now be described in more detail.

[0049] Various paints were applied to slate boards using a paint roller to check the workability and finish. The specifications and results are shown in Table 1.

[0050] [Table 1]

[0051] The fillers contained in various paints are mainly calcium carbonate, and the particle size is the D50 value calculated from the volume-based particle size distribution measured by laser diffraction method. The viscosity of the paint was measured using a Brookfield viscometer at 20 rpm and 23°C.

[0052] The painting rollers used were a roller generally called a woven roller, which has a coating part made of thread-like pile woven into a woven backing in which warp and weft threads cross at right angles, and a roller generally called a high pile roller, which has a coating part made of cotton-like pile woven together with the backing. The amount of paint absorbed is calculated by first weighing the roller, then submerging it in a container of paint, then weighing it again after removing it, and dividing the difference by the volume of the roller.

[0053] To evaluate workability, the ease of spreading various paints using the paint rollers listed in Table 1 and the paint scattering properties were confirmed. Regarding the finish, workability was confirmed, and the formed coating film was visually inspected for flatness, bubbles in the coating film, and the presence or absence of bristles on the coating roller. The coating thickness was measured at three random points on the dried coating formed by painting with various specifications.

[0054] In the case of the specifications of Comparative Example 1, the paint was difficult to spread and there was a lot of rebound, probably due to the high solid content in the paint. In addition, the formed paint film was uneven. In the case of the specification of Comparative Example 2, the solid content of the paint was low, and the amount of paint absorbed by the painting roller was high, so there was a lot of paint splashing during painting. Also, there were many bubbles in the formed paint film.

[0055] The specifications for Comparative Example 3 were the same paint as in Example 1 and a high-pile painting roller. Compared to the woven painting roller used in Example 1, the high-pile painting roller was slightly more difficult to spread the paint. The coating formed also contained bubbles and some areas had loose hairs from the painting roller.

[0056] The specifications for Comparative Example 4 were the same paint as in Example 1, and a woven painting roller with shorter bristles was used than the painting roller used in Example 1. Because the bristles were short, the amount of paint absorbed was small, making it difficult to spread the paint.

Claims

1. In the case where a paint having a Ti value in the range of 2 to 10 and a paint solid content in the range of 10.0 to 80.0% by weight is applied to an object to be coated with a coating roller, The coating part of the coating roller is made of a backing in which warp and weft threads are crossed at right angles, and thread-like pile is woven into the backing, The paint load of the painting roller is 0.5 to 3.0 g / cm 3 It is a painting roller, This coating method uses a coating roller having a bristle length in the range of 5 to 32 mm to coat the paint.

2. 2. The coating method using a coating roller according to claim 1, wherein the specific gravity of the coating material is in the range of 0.8 to 2.5, the content of the fillers contained in the coating material is in the range of 10.0 to 70.0% by weight, and the particle size is in the range of 1.0 to 800.0 μm.

3. 3. A coating method using a coating roller according to claim 1 or 2, wherein the coating film formed by the coating is in the range of 30 to 1000 μm.