Method for producing cured geopolymer, and cured geopolymer

The method enhances geopolymer strength by kneading specific inorganic powders and curing techniques, effectively utilizing non-JIS fly ash to produce high-strength geopolymer bodies suitable for construction and environmental applications.

JP2024148042APending Publication Date: 2024-10-17CENTRAL RESEARCH INSTITUTE OF ELECTRIC POWER INDUSTRY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023060923
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing methods for producing geopolymer concrete do not effectively utilize non-JIS fly ash and struggle to enhance the strength of cured geopolymer bodies, leading to environmental waste and limited application in high-strength structures.

Method used

A method involving the kneading of inorganic powders such as fly ash, blast furnace slag powder, calcium aluminate powder, and silica powder, followed by room temperature and steam curing, to produce a cured geopolymer with enhanced strength, utilizing hydroxides like sodium hydroxide to extend pot life and incorporating aggregates for improved properties.

Benefits of technology

The method results in high-strength geopolymer bodies, capable of using non-JIS fly ash, reducing environmental impact, and enabling applications in high-strength construction materials and environmental purification due to improved compressive and bending strengths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148042000001_ABST
    Figure 2024148042000001_ABST
Patent Text Reader

Abstract

To enhance the strength of a cured geopolymer.SOLUTION: A method for producing a cured geopolymer includes: a kneading step for kneading raw materials containing inorganic powder, hydroxide, water and aggregate to obtain the kneaded mixture; and a curing step for curing the kneaded mixture. The inorganic powder includes fly ash, blast furnace slag fine powder, calcium aluminate-based powder, and silica-based powder.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a hardened geopolymer body, and a hardened geopolymer body. [Background technology]

[0002] Geopolymer hardened materials, such as geopolymer concrete, which uses fly ash as a main raw material, are known.

[0003] For example, Patent Document 1 proposes a method for accelerating the hardening of a geopolymer composition, in which a hardening accelerator containing calcium aluminates as an active ingredient is added to a geopolymer composition containing fly ash, an alkaline solution, and aggregate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-33104 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, because geopolymer hardened bodies are used in structures, there is a demand for technology to increase the strength of these bodies.

[0006] The present invention has been made in consideration of the above, and provides a technology for increasing the strength of a geopolymer hardened body. [Means for solving the problem]

[0007] In order to solve the above problems and achieve the object, the method for producing a geopolymer hardened body of the present invention includes a kneading step of kneading raw materials including inorganic powder, hydroxide, water, and aggregate to obtain a kneaded mixture, and a curing step of curing the kneaded mixture. The inorganic powder includes fly ash, ground granulated blast furnace slag, calcium aluminate-based powder, and silica-based powder. Effect of the Invention

[0008] According to the method for producing a hardened geopolymer body of the present invention, the hardened geopolymer body can be strengthened. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram showing an example of a flow of a method for producing a geopolymer hardened body according to an embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of a blending ratio during the production of a geopolymer hardened body according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing an example of the change in strength of the geopolymer hardened body according to Example 1 depending on the curing time. [Figure 4] FIG. 4 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 2. [Diagram 5] FIG. 5 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 3. [Figure 6] FIG. 6 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 3. [Figure 7] FIG. 7 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 4. [Figure 8] FIG. 8 is a diagram showing an example of the change in strength of a geopolymer hardened body depending on the specific surface area of ​​fly ash in Example 5. [Figure 9] FIG. 9 is a diagram showing an example of the blending ratio during the production of the geopolymer hardened body according to Example 6. [Figure 10] FIG. 10 is a diagram showing an example of the change in strength of the hardened geopolymer body according to Example 6. [Figure 11] FIG. 11 is a diagram showing an example of the blending ratio during the production of the geopolymer hardened body according to Example 7. [Figure 12] FIG. 12 is a diagram showing an example of the flow value of the hardened geopolymer body according to Example 7. [Figure 13] FIG. 13 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following describes in detail the embodiment of the method for producing a geopolymer hardened body according to the present invention and the geopolymer hardened body based on the drawings. Note that the present invention is not limited to this embodiment. The embodiments can be appropriately combined within the scope of the processing content.

[0011] FIG. 1 is a diagram showing an example of a flow of a method for producing a geopolymer hardened body according to an embodiment.

[0012] The method for producing a hardened geopolymer body according to the embodiment includes a kneading step (S1) and a curing step (S2).

[0013] In the kneading step (S1), inorganic powder, hydroxide, water and aggregate are kneaded as raw materials to obtain a kneaded product. The inorganic powder includes fly ash, ground granulated blast furnace slag, calcium aluminate-based powder, and silica-based powder. By producing a geopolymer hardened body using four types of inorganic powder, namely fly ash, ground granulated blast furnace slag, calcium aluminate-based powder, and silica-based powder, the strength (compressive strength and bending strength) of the geopolymer hardened body can be increased, and the strength of the geopolymer hardened body can be increased.

[0014] In the curing step (S2), the kneaded material is subjected to room temperature curing, steam curing, or room temperature curing followed by steam curing. In particular, in the curing step (S2), by performing room temperature curing followed by steam curing, the strength of the geopolymer hardened body can be further increased, and the strength of the geopolymer hardened body can be increased.

[0015] As the fly ash, fly ash type I to type IV for concrete specified in JIS A 6201 can be used. As the fly ash, fly ash raw powder (i.e., non-JIS product) can also be used. As the fly ash, two or more types of JIS-I to IV products and non-JIS products can also be used in combination. Fly ash raw powder has a wide particle size distribution of constituent particles and also contains coarse particles because no classification process is performed on fly ash generated from coal-fired power plants. For this reason, fly ash raw powder tends to be less reactive than JIS-I to IV products, and most of it is currently only used as a cement raw material. Most of the fly ash that is not used as a cement raw material is disposed of in landfills. Here, only about 2% of the fly ash generated is JIS product, and the remaining 98% is non-JIS product. The amount of non-JIS fly ash raw powder generated is expected to increase further in the future. However, it is expected that the amount of fly ash raw powder used as a cement raw material will reach a plateau. Therefore, there is an urgent need to establish a new method for effectively utilizing fly ash raw powder, which is a non-JIS product. The manufacturing method for hardened geopolymer according to the embodiment can use fly ash raw powder as a raw material, so it can contribute to the manufacture of environmentally friendly building materials, etc., without using cement, even though it uses non-JIS fly ash raw powder.

[0016] As for the ground granulated blast furnace slag, either JIS or non-JIS products may be used, or a combination of these may be used. Non-JIS ground granulated blast furnace slag products are hardly available on the market, and non-JIS products with too small a Blaine value may have a small strength-enhancing effect. For this reason, it is preferable to use JIS products, which are easily available, as the ground granulated blast furnace slag. Specifically, the ground granulated blast furnace slag may be JIS ground granulated blast furnace slag (Blaine value 3000 cm) as specified in JIS A 6206. 2 / g class, 4000cm 2 / g class, 6000cm 2 / g class, 8000cm 2 / g class) can be used, especially with a Blaine value of 4000 cm 2 In addition, two or more of these four JIS products can be used in combination as the ground granulated blast furnace slag.

[0017] Examples of calcium aluminate powders include calcium aluminates having mineral compositions represented as C3A, C2A, CA, CA2, etc., when CaO is represented as C, Al2O3 as A, Na2O as N, and Fe2O3 as F, calcium aluminoferrites represented as C2AF, C4AF, etc., calcium sodium aluminates represented as C3N2A5, etc., and alumina cement.

[0018] Silica-based powders are powders that mainly contain SiO2 as a chemical composition, and examples of such powders include silica fume, Portland cement, sewage sludge slag calcined powder, municipal waste molten slag powder, waste glass powder, silica fine powder, talc powder, metakaolin, volcanic ash, and silica gel. Portland cement is manufactured by calcining raw materials such as lime, and a large amount of CO2 is emitted during manufacturing. On the other hand, silica fume is an industrial by-product produced when ferrosilicon or silicon metal is manufactured in an arc-type electric furnace. For example, when silica fume is used as the silica-based powder, the CO2 intensity in the manufacture of the geopolymer hardened body can be reduced compared to when Portland cement is used, and this can contribute to the construction of a low-carbon society. In addition, the use of industrial by-products such as silica fume and fly ash as raw materials for the geopolymer hardened body can contribute to the construction of a recycling-based society.

[0019] Silica fume can be either JIS or non-JIS, or a combination of both. JIS products are defined as those that meet the requirements of JIS A 6207. It is a silica fume for concrete specified in.

[0020] The blending ratio of fly ash, ground granulated blast furnace slag, calcium aluminate powder, and silica powder in the inorganic powder is not particularly limited as long as the effect of the present invention is exhibited. For example, when the fly ash in the inorganic powder is 100 parts by mass, the inorganic powder preferably contains 30 to 140 parts by mass of ground granulated blast furnace slag, 4 to 25 parts by mass of calcium aluminate powder, and 4 to 25 parts by mass of silica powder. In addition, the inorganic powder preferably contains calcium aluminate powder and silica powder in total at 5% by mass or more, more preferably 5 to 20% by mass, and even more preferably 5 to 10% by mass, based on the total mass of the inorganic powder. As an example, the calcium aluminate powder is alumina cement, and the silica powder is silica fume. When the fly ash is 40% by mass based on the total mass of the inorganic powder, the alumina cement and silica fume are preferably in the range of 5 to 20% by mass in total based on the total mass of the inorganic powder. Furthermore, when the fly ash is 60 mass % based on the total mass of the inorganic powder, the alumina cement and silica fume are preferably in the range of 5 to 10 mass % in total based on the total mass of the inorganic powder.

[0021] As the hydroxide, a hydroxide other than sodium silicate can be used. For example, the hydroxide can be sodium hydroxide or potassium hydroxide. It is preferable that the sodium hydroxide is dissolved in water (mixing water) in advance to obtain an aqueous sodium hydroxide solution, and then the solution is subjected to the mixing step. As the water, it is preferable to use, for example, ion-exchanged water, but distilled water or tap water may also be used.

[0022] In the conventional method for producing a geopolymer hardened body, raw materials such as inorganic powder and a sodium silicate aqueous solution are mixed to produce a geopolymer hardened body. However, when using a sodium silicate aqueous solution, the time from starting to mix the raw materials to coagulation is very short, and the material may coagulate during mixing. Therefore, there is a problem that it is difficult to ensure the usable time.

[0023] On the other hand, the method for producing a geopolymer hardened body according to the embodiment uses hydroxides other than sodium silicate, such as sodium hydroxide or potassium hydroxide, to produce a geopolymer hardened body. In this case, as in the case of using an aqueous sodium silicate solution, the time from starting to knead the raw materials to coagulation is very short, and the problem of difficulty in securing the usable time does not occur.

[0024] As the aggregate, coarse aggregate (e.g., gravel, etc.) and fine aggregate (e.g., sand, coal gasification slag fine aggregate, etc.) generally used in concrete and mortar can be appropriately used. The mixing ratio of the aggregate to the raw materials other than the aggregate is not particularly limited, and the conditions generally used in concrete and mortar can be appropriately selected, for example.

[0025] The kneading step (S1) is carried out by feeding the raw materials into a stirring device such as a twin-shaft mixer and kneading them. Regarding the feeding of aggregate, when producing mortar (paste + fine aggregate), it is preferable to knead the raw materials and fine aggregate together. When producing concrete (paste + fine aggregate + coarse aggregate), it is preferable to knead the raw materials and fine aggregate together, prepare mortar, and then feed the coarse aggregate.

[0026] The kneaded material obtained in the kneading step (S1) is cast into a formwork and is subjected to the next step, the curing step (S2), in which the kneaded material is subjected to room temperature curing, steam curing, or room temperature curing followed by steam curing.

[0027] Room temperature curing is performed at room temperature (10°C to 30°C). Steam curing is performed by holding the kneaded material in steam. There are no particular limitations on the conditions for steam curing, and general conditions employed in the manufacturing method of geopolymer hardened bodies may be adopted. For example, the steam curing conditions may be in the temperature range of 60°C to 90°C, but are not limited thereto.

[0028] The curing time in the curing step (S2) is not particularly limited as long as it is within a range generally adopted for concrete or mortar. The curing time may be, for example, 6 hours or more, preferably 12 hours or more, more preferably 24 hours or more, and even more preferably 48 hours or more. If the curing time is too short, the strength enhancing effect may not be fully achieved. It is preferable to carry out the curing while preventing the escape of moisture from the kneaded material. For example, the curing can be carried out while preventing the escape of moisture from the kneaded material by covering the casting surface with a sheet or the like. EXAMPLES

[0029] Examples of the hardened geopolymer body produced by the manufacturing method according to the embodiment will be described below. Note that the manufacturing method of the hardened geopolymer body of the present invention is not limited to these examples.

[0030] In the following explanation and drawings, the blending conditions of the inorganic powder may be abbreviated as follows: F: Fly ash G: Ground granulated blast furnace slag A: Alumina cement S: Silica fume CGS: Coal gasification slag fine aggregate

[0031] [Example 1] In Example 1, the strength of the geopolymer hardened body was compared in the following cases: when the inorganic powder was three types (fly ash, ground granulated blast furnace slag, and alumina cement); when the inorganic powder was three types (fly ash, ground granulated blast furnace slag, and silica fume); and when the inorganic powder was four types (fly ash, ground granulated blast furnace slag, alumina cement, and silica fume).

[0032] Fig. 2 is a diagram showing an example of the mixing ratio during the production of the geopolymer hardened body according to the embodiment. Note that Fig. 2 shows the mixing ratio in a paste obtained by mixing inorganic powder, which is a raw material other than aggregate, and an aqueous sodium hydroxide solution.

[0033] The mix notation uses the name of each hardened geopolymer body produced and the mixing ratio of inorganic powder. F60-G-A10 is a mix with three types of inorganic powder: fly ash, ground granulated blast furnace slag, and alumina cement. F60-G-A10 has 60 mass% fly ash (F), 40 mass% ground granulated blast furnace slag (G), and 10 mass% alumina cement (A). F60-G-S10 is a mix with three types of inorganic powder: fly ash, ground granulated blast furnace slag, and silica fume. F60-G-S10 has 60 mass% fly ash (F), 40 mass% ground granulated blast furnace slag (G), and 10 mass% silica fume (S). F60-G-AS10 is a case where the inorganic powder is four types: fly ash, ground granulated blast furnace slag, alumina cement, and silica fume. The composition ratio of the inorganic powder in F60-G-AS10 is 60 mass% fly ash (F), 40 mass% ground granulated blast furnace slag (G), 5 mass% alumina cement (A), 5 mass% silica fume (S), and 10 mass% alumina cement and silica fume.

[0034] In addition, in all of the blending ratios shown in FIG. 2, the concentration of the sodium hydroxide aqueous solution was 7 mol / kg, and the moisture / powder ratio was 36 mass %.

[0035] Fig. 3 is a diagram showing an example of the change in strength depending on the curing time of the geopolymer hardened body according to Example 1. Fig. 3 shows the change in compressive strength for each age (days) of F60-G-A10, F60-G-S10, and F60-G-AS10 when cured at room temperature at 20°C after casting. As shown in Fig. 3, F60-G-AS10 shows a significant increase in strength over the age of 3 to 7 days compared to F60-G-A10 and F60-G-S10, and the compressive strength at the age of 28 days is about 1.8 times higher.

[0036] In this way, the manufacturing method of the geopolymer hardened body according to the embodiment uses four types of inorganic powders, namely, fly ash, ground granulated blast furnace slag, alumina cement, and silica fume, and thus can increase the strength (compressive strength and bending strength) of the geopolymer hardened body, compared to a case where the inorganic powders are three types, namely, fly ash, ground granulated blast furnace slag, and alumina cement, or a case where the inorganic powders are three types, namely, fly ash, ground granulated blast furnace slag, and silica fume. Thus, the strength of the geopolymer hardened body can be increased, compared to a case where the inorganic powders are three types, namely, fly ash, ground granulated blast furnace slag, and silica fume.

[0037] [Example 2] In Example 2, the strength of the geopolymer hardened body was compared when the curing step (S2) was steam curing.

[0038] Figure 4 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 2. Figure 4 shows the compressive strength of F60-G-A10, F60-G-S10, and F60-G-AS10 when steam curing was performed at 85°C for one day after casting. As shown in Figure 4, F60-G-AS10 has increased strength and has a higher compressive strength than F60-G-A10 and F60-G-S10.

[0039] In this way, the manufacturing method of the geopolymer hardened body according to the embodiment can increase the strength of the geopolymer hardened body even when the curing process (S2) is steam curing.

[0040] [Example 3] In Example 3, the curing process (S2) was performed by performing room temperature curing followed by steam curing, and the strength of the geopolymer hardened body was compared when the room temperature curing and steam curing times were changed.

[0041] Fig. 5 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 3. Fig. 5 shows the compressive strength at 3 days for F60-G-A10, F60-G-S10, and F60-G-AS10, which were cast, cured at room temperature for 24 hours at 20 ° C, steam cured for 24 hours at 85 ° C, and then cured at room temperature at 20 ° C. As shown in Fig. 5, F60-G-AS10 has increased strength and has a higher compressive strength than F60-G-A10 and F60-G-S10.

[0042] Figure 6 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 3. Figure 6 shows the compressive strength at 3 days for F60-G-A10, F60-G-S10, and F60-G-AS10, which were cast, cured at room temperature for 6 hours at 20°C, steam cured for 8 hours at 85°C, and then cured at room temperature at 20°C.

[0043] In both Figures 5 and 6, room temperature curing is followed by steam curing in the curing step (S2). In both Figures 5 and 6, F60-G-AS10 has increased strength and a higher compressive strength compared to F60-G-A10 and F60-G-S10. In Figure 6, the room temperature curing and steam curing times are shorter than in Figure 5, but F60-G-AS10 has increased strength and a higher compressive strength compared to F60-G-A10 and F60-G-S10.

[0044] In this way, the manufacturing method of the geopolymer hardened body according to the embodiment can increase the strength of the geopolymer hardened body even when steam curing is performed after room temperature curing in the curing process (S2).

[0045] [Example 4] In Example 4, the strength of the geopolymer hardened body was compared when the curing step (S2) was performed at room temperature and when the curing step was performed at room temperature followed by steam curing.

[0046] Fig. 7 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 4. Fig. 7 shows the compressive strength at 3 days for F60-G-A10 when it is cast, cured at room temperature for 3 days at 20 ° C, and when it is cast, cured at room temperature for 24 hours at 20 ° C, steam cured at 85 ° C for 24 hours, and then cured at room temperature at 20 ° C. As shown in Fig. 7, F60-G-AS10 has a higher compressive strength when it is cured at room temperature and then steam cured.

[0047] In this way, the manufacturing method of the geopolymer hardened body according to the embodiment can increase the strength of the geopolymer hardened body by performing steam curing after room temperature curing in the curing process (S2).

[0048] [Example 5] In Example 5, the change in strength of the hardened geopolymer body depending on the specific surface area of ​​fly ash was examined.

[0049] FIG. 8 is a diagram showing an example of the change in strength of the geopolymer hardened body depending on the specific surface area of ​​the fly ash according to Example 5. FIG. 8 shows the change in compressive strength of the geopolymer hardened body when the specific surface area of ​​the fly ash used is changed for F60-G-A10, F60-G-S10, and F60-G-AS10. FIG. 8 shows the compressive strength at 3 days after casting, curing at room temperature for 24 hours at 20°C, steam curing for 24 hours at 85°C, and then curing at room temperature at 20°C. Fly ash with a small specific surface area has a coarse grain size and is of low quality. As shown in FIG. 8, F60-G-A10 and F60-G-S10 tend to have a lower compressive strength when low-quality fly ash with a small specific surface area is used. On the other hand, F60-G-AS10 has a small strength variation due to the specific surface area of ​​the fly ash, and sufficient compressive strength is obtained even with low-quality fly ash.

[0050] For this reason, the manufacturing method of the geopolymer hardened body according to the embodiment can produce sufficient compressive strength even with low-quality fly ash. For example, fly ash is specified in JIS A 6201 as types I to IV. Type I is a type with a specific surface area of ​​5000 cm 2 / g or more, and types II and III have a specific surface area of ​​2500 cm 2 / g or more, and Class IV is specified as a specific surface area of ​​1500 cm 2 / g or more. The manufacturing method of the geopolymer hardened body according to the embodiment can generate sufficient compressive strength even when using fly ash type I to IV products or non-JIS fly ash raw powder.

[0051] In this way, the method for producing a hardened geopolymer body according to the embodiment can increase the strength of the hardened geopolymer body regardless of the quality of the fly ash. For example, the method for producing a hardened geopolymer body according to the embodiment can increase the strength of the hardened geopolymer body even when fly ash raw powder is used.

[0052] [Example 6] In Example 6, the strength of the hardened geopolymer body was compared when the mixing ratio of fly ash, ground granulated blast furnace slag, calcium aluminate powder, and silica powder mixed with the inorganic powder was changed.

[0053] Fig. 9 is a diagram showing an example of the mixing ratio during the production of a geopolymer hardened body according to Example 6. Fig. 9 shows the mixing ratio in a paste obtained by mixing inorganic powder, which is a raw material other than aggregate, and an aqueous sodium hydroxide solution.

[0054] The blend notation lists the name of each manufactured geopolymer hardened body using the blend ratio of inorganic powder. F60-G and F40-G are cases where the inorganic powder is two types, fly ash and ground granulated blast furnace slag. F60-G has a composition ratio of 60 mass% fly ash (F) and 40 mass% ground granulated blast furnace slag (G). F40-G has a composition ratio of 40 mass% fly ash (F) and 60 mass% ground granulated blast furnace slag (G).

[0055] F60-G-AS5, F60-G-AS10, F60-G-AS20, F40-G-AS5, F40-G-AS10, and F40-G-AS20 are cases where the inorganic powder is four types: fly ash, ground granulated blast furnace slag, alumina cement, and silica fume. F60-G-AS5 has a composition ratio of inorganic powder of 60 mass% fly ash (F), 35 mass% ground granulated blast furnace slag (G), 2.5 mass% alumina cement (A), 2.5 mass% silica fume (S), and 5 mass% alumina cement and silica fume. F60-G-AS10 has a composition ratio of inorganic powder of 60% by mass of fly ash (F), 30% by mass of ground granulated blast furnace slag (G), 5% by mass of alumina cement (A), 5% by mass of silica fume (S), and 10% by mass of alumina cement and silica fume. F60-G-AS20 has a composition ratio of inorganic powder of 60% by mass of fly ash (F), 20% by mass of ground granulated blast furnace slag (G), 10% by mass of alumina cement (A), 10% by mass of silica fume (S), and 20% by mass of alumina cement and silica fume. F40-G-AS5 has a composition ratio of inorganic powder of 40% by mass of fly ash (F), 55% by mass of ground granulated blast furnace slag (G), 2.5% by mass of alumina cement (A), 2.5% by mass of silica fume (S), and 5% by mass of alumina cement and silica fume. F40-G-AS10 has a composition ratio of inorganic powder of 40% by mass of fly ash (F), 50% by mass of ground granulated blast furnace slag (G), 5% by mass of alumina cement (A), 5% by mass of silica fume (S), and 10% by mass of alumina cement and silica fume. The inorganic powder composition of F40-G-AS20 is 40% by mass of fly ash (F), 40% by mass of ground granulated blast furnace slag (G), 10% by mass of alumina cement (A) and 10% by mass of silica fume (S), for a total of 20% by mass of alumina cement and silica fume.

[0056] In addition, in all of the blending ratios shown in FIG. 9, the concentration of the sodium hydroxide aqueous solution was 7 mol / kg, and the moisture / powder ratio was 36 mass %.

[0057] FIG. 10 is a diagram showing an example of the change in strength of the geopolymer hardened body according to Example 6. In FIG. 10, the change in compressive strength of the geopolymer hardened body is shown as "F60%" for F60-G, F60-G-AS5, F60-G-AS10, and F60-G-AS20, which have 60% fly ash (F), in correspondence with the mass% (A+S) of alumina cement and silica fume. In addition, in FIG. 10, the change in compressive strength of the geopolymer hardened body is shown as "F40%" for F40-G, F40-G-AS5, F40-G-AS10, and F40-G-AS20, which have 40% fly ash (F), in correspondence with the mass% (A+S) of alumina cement and silica fume. Figure 10 shows the compressive strength at 3 days after pouring, when the concrete was cured at room temperature for 6 hours at 20°C, then steam cured at 85°C for 8 hours, and then cured at room temperature at 20°C.

[0058] As shown in Fig. 10, in F60, which contains 60% fly ash by mass, the strength increases with an increase in the ratio of alumina cement and silica fume (A+S), and even at 5% by mass of alumina cement and silica fume, there is a significant increase in strength. Therefore, when fly ash is 60% by mass relative to the total mass of the inorganic powder, the alumina cement and silica fume are preferably in the range of 5 to 20% by mass in total relative to the total mass of the inorganic powder.

[0059] In addition, in F40, which contains 40% fly ash by mass, the strength increases as the ratio of alumina cement and silica fume (A+S) increases, but the strength decreases when the ratio of alumina cement and silica fume (A+S) reaches 20% by mass. Therefore, when the fly ash is 40% by mass relative to the total mass of the inorganic powder, the alumina cement and silica fume are preferably in the range of 5 to 10% by mass in total relative to the total mass of the inorganic powder.

[0060] [Example 7] In Example 7, we investigated the change in strength of the hardened geopolymer body depending on the aggregate mixing ratio.

[0061] Fig. 11 is a diagram showing an example of a blending ratio when manufacturing a geopolymer hardened body according to Example 7. Fig. 11 shows a case where crushed sand and coal gasification slag fine aggregate (CGS) are blended as aggregates.

[0062] The mix proportions are indicated by the name of each hardened geopolymer body produced, using the mix proportion of aggregate. For "crushed sand," the aggregate composition is 100% crushed sand, the inorganic powder composition is 60% fly ash (F), 30% ground granulated blast furnace slag (G), 5% alumina cement (A), and 5% silica fume (S). For "crushed sand + GCS," the aggregate composition is 50% crushed sand, 50% fine coal gasification slag aggregate (CGS), and the inorganic powder composition is 60% fly ash (F), 30% ground granulated blast furnace slag (G), 5% alumina cement (A), and 5% silica fume (S).

[0063] In addition, in all of the blending ratios shown in FIG. 11, the concentration of the sodium hydroxide aqueous solution was 7 mol / kg, and the moisture / powder ratio was 36 mass %.

[0064] FIG. 12 is a diagram showing an example of the flow value of the geopolymer hardened body according to Example 7. FIG. 12 shows the flow value of the mixture of "crushed sand" and "crushed sand + GCS" shown in FIG. 11. FIG. 13 is a diagram showing an example of the strength of the geopolymer hardened body according to Example 7. FIG. 13 shows the compressive strength at 3 days after casting for "crushed sand" and "crushed sand + GCS" shown in FIG. 11, after room temperature curing at 20°C for 6 hours, steam curing at 85°C for 8 hours, and then room temperature curing at 20°C.

[0065] As shown in Figure 12, "crushed sand + GCS" has a higher flow value and is more fluid than "crushed sand." Also, as shown in Figure 13, "crushed sand + GCS" has a compressive strength close to that of "crushed sand." Therefore, when coal gasification slag fine aggregate (CGS) is mixed with ordinary crushed sand, it is possible to improve fluidity while ensuring a strength level sufficient for practical use.

[0066] In this way, the manufacturing method of the geopolymer hardened body according to the embodiment can ensure the strength of the geopolymer hardened body while improving the fluidity of the kneaded material by mixing crushed sand and coal gasification slag fine aggregate as aggregate. [Industrial Applicability]

[0067] The geopolymer hardened body obtained by the method for producing a geopolymer hardened body of the present invention can be produced in the same steam curing equipment and facilities as existing general precast concrete products such as various blocks such as pedestrian and roadway separation blocks, utility poles, and culverts, and has potential for use in general precast concrete products. In addition, since it has excellent acid resistance, it can be used as a sewerage material where deterioration due to sulfuric acid caused by microbial activity is a problem, and as a construction material (U-shaped gutters, revetment blocks, etc.) in hot spring areas where acid deterioration due to acidic hot spring water is a problem. Furthermore, since it has excellent cation exchange ability, it can be used as an environmental purification material that adsorbs ammonium ions, which are one of the causes of bad odors in water environments.

Claims

1. A kneading step of kneading raw materials including inorganic powder, hydroxide, water, and aggregate to obtain a kneaded material; a curing step of curing the kneaded mixture; Including, The inorganic powder includes fly ash, ground granulated blast furnace slag, calcium aluminate-based powder, and silica-based powder. A method for producing a geopolymer hardened body, comprising:

2. The calcium aluminate powder is an alumina cement. The method for producing the hardened geopolymer body according to claim 1.

3. The hydroxide is a hydroxide other than sodium silicate. The method for producing the hardened geopolymer body according to claim 1.

4. The hydroxide is sodium hydroxide or potassium hydroxide. The method for producing the hardened geopolymer body according to claim 1.

5. In the curing step, the kneaded material is cured at room temperature, steam cured, or cured at room temperature and then steam cured. The method for producing the hardened geopolymer body according to claim 1.

6. The fly ash is fly ash raw powder. The method for producing the hardened geopolymer body according to claim 1.

7. The silica-based powder is silica fume The method for producing the hardened geopolymer body according to claim 1.

8. The aggregate is crushed sand, gravel, coal gasification slag fine aggregate, or a mixture thereof. The method for producing the hardened geopolymer body according to claim 1.

9. The inorganic powder contains 30 to 140 parts by mass of ground granulated blast furnace slag, 4 to 25 parts by mass of calcium aluminate-based powder, and 4 to 25 parts by mass of silica-based powder, relative to 100 parts by mass of fly ash. The method for producing the hardened geopolymer body according to claim 1.

10. The aggregate includes crushed sand and coal gasification slag fine aggregate. The method for producing the hardened geopolymer body according to claim 1.

11. A geopolymer hardened body produced by the method for producing a geopolymer hardened body according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Curing acceleration method and production method of geopolymer composition

    JP2016033104A