Rubber composition for undertreads
The rubber composition for undertreads balances handling stability, high-speed durability, and low heat generation by using isoprene and modified butadiene/styrene-butadiene rubbers with large particle size silica and carbon black, addressing the limitations of existing undertread compositions.
Patent Information
- Application Number
- JP2023057959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing rubber compositions for undertreads in tires face challenges in achieving a balance between handling stability, high-speed durability, and low heat generation, with methods like increasing the vulcanizing agent or reducing filler content compromising elongation at break and durability.
A rubber composition for undertreads comprising 40% to 90% isoprene rubber and 10% to 40% modified butadiene rubber or modified styrene-butadiene rubber, with silica having a CTAB adsorption specific surface area of 60 m²/g to 100 m²/g and carbon black in specific amounts, along with a silane coupling agent, to enhance low heat generation and durability.
The composition improves handling stability and high-speed durability while maintaining low heat generation, with balanced performance achieved through the use of isoprene-based rubbers and large particle size silica, and appropriate blending of carbon black and silica.
Smart Images

Figure 2024148179000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a rubber composition for undertreads intended primarily for use in the undertread layer of tires. [Background technology]
[0002] In pneumatic tires, there is a demand for improving fuel economy performance during driving in order to reduce environmental impact. To this end, efforts have been made to suppress heat generation in rubber compositions constituting various parts of pneumatic tires. In recent years, in order to further improve fuel economy performance, for example, studies have been made on suppressing heat generation in rubber compositions constituting the undertread rubber layer of pneumatic tires (rubber compositions for undertread).
[0003] Tan δ at 60°C (hereinafter referred to as "tan δ(60°C)") measured by dynamic viscoelasticity measurement is generally used as an index of heat buildup of a rubber composition, and the smaller the tan δ(60°C) of a rubber composition, the smaller the heat buildup. Methods for reducing the tan δ(60°C) of a rubber composition include, for example, increasing the amount of vulcanizing agent blended or reducing the amount of filler such as carbon black blended (see, for example, Patent Document 1). However, these methods do not sufficiently ensure the elongation at break required for a rubber composition for an undertread, and there is a risk that sufficient steering stability and high-speed durability of the tire may not be obtained. Therefore, there is a demand for further measures to improve steering stability and high-speed durability while ensuring good low heat buildup (tan δ(60°C)) in a rubber composition for an undertread. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-177113 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a rubber composition for an undertread which improves steering stability and high-speed durability while ensuring good low heat buildup, thereby achieving a high degree of compatibility between these performances in a well-balanced manner. [Means for solving the problem]
[0006] The rubber composition for undertread of the present invention, which achieves the above object, comprises a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene, and a CTAB adsorption specific surface area of 60 m 2 / g~100m 2 The composition is characterized in that 3 to 60 parts by mass of silica is blended, with the content being 1 / g. [Effects of the Invention]
[0007] The rubber composition for undertread of the present invention, which is made up of the above-mentioned blending, can improve steering stability and high-speed durability while ensuring good low heat buildup. Specifically, by using an isoprene-based rubber and a modified butadiene rubber and / or a modified styrene butadiene rubber in the above-mentioned blending ratio as the rubber component, it is possible to improve low heat buildup and high-speed durability in a well-balanced manner. In addition, by adding large particle size silica (CTAB adsorption specific surface area of 60 m) to this rubber component, 2 / g~100m 2 / g), which improves low heat buildup. These properties work together to ensure good low heat buildup while improving handling stability and high-speed durability, achieving a good balance of these performance characteristics.
[0008] In the present invention, the CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2It is preferable that 20 to 70 parts by mass of carbon black having a particle size of 1 / g is blended. In addition to the large particle size silica described above, by blending an appropriate amount of carbon black having a specific particle size as a filler, it is possible to improve processability (rubber cohesion, adhesion to other components, etc.).
[0009] In the present invention, the glass transition temperature of the modified butadiene rubber is preferably −85° C. or lower. Furthermore, the cis-1,4 bond content of the modified butadiene rubber is preferably 95% or higher. By using a modified butadiene rubber that satisfies these specific conditions, the effects of improving the low heat buildup and high-speed durability described above can be enhanced, which is advantageous for improving handling stability and high-speed durability while maintaining good low heat buildup.
[0010] In the present invention, a silane coupling agent can be blended, and in this case, the ratio of the blended amount of the silane coupling agent to the blended amount of silica is preferably 3.0% by mass to 10.0% by mass, which can improve the dispersion of silica and is advantageous for improving low heat buildup and high-speed durability.
[0011] The rubber composition for an undertread of the present invention can be suitably used in the undertread layer of a tire. Specifically, a tire using the rubber composition for an undertread of the present invention includes a tread portion extending in the tire circumferential direction to form an annular shape, a pair of sidewall portions disposed on both sides of the tread portion, and a pair of bead portions disposed radially inward of the sidewall portions. The tire also includes at least one carcass layer mounted between the pair of bead portions and multiple belt layers disposed on the outer circumferential side of the carcass layer in the tread portion. The tread portion is preferably constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer disposed on its inner circumferential side. In such a tire, the undertread layer is preferably constructed from the rubber composition for an undertread of the present invention. In this way, a tire having an undertread layer made from the rubber composition for an undertread of the present invention can improve handling stability and high-speed durability while ensuring good low heat buildup due to the excellent physical properties of the rubber composition for an undertread of the present invention.
[0012] At this time, the tensile stress M100 of the undertread rubber that constitutes the undertread layer at 23°C when elongated to 100% UT [Unit: MPa] and the tensile stress M100 of the coating rubber that covers the belt cord in the belt layer at 100% elongation at 23°C B [Unit: MPa] Ratio to M100 UT / M100 B It is preferable that M100 is 0.4 to 1.0. By optimizing the relationship of the tensile stress (M100) between the undertread layer (undertread rubber) using the rubber composition for an undertread of the present invention and the belt layer (belt coat rubber) disposed on the inner circumferential side thereof in this way, it is advantageous to improve low heat build-up properties and high-speed durability.
[0013] In the present invention, the "CTAB adsorption specific surface area" is measured in accordance with ISO 5794. The "glass transition temperature" can be measured as the midpoint temperature of the transition region from a thermogram obtained by differential scanning calorimetry (DSC) at a heating rate of 20°C / min. The "cis-1,4 bond content" is the proportion of cis-1,4 bonds among the cis-1,4-bonds, trans-1,4-bonds, and 1,2-vinyl bonds that are the bonding modes of butadiene, and is measured by infrared spectroscopy (Hampton method). The "tensile stress at 100% elongation at 23°C" is a value measured in accordance with JIS K6251 using a No. 3 dumbbell test piece at a tensile speed of 500 mm / min and a temperature of 23°C. [Brief explanation of the drawings]
[0014] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for an undertread of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0015] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.
[0016] As shown in FIG. 1, a pneumatic tire in which the rubber composition for an undertread of the present invention is used includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged radially inward of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross-section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction and form an annular shape, thereby constituting the basic toroidal structure of a pneumatic tire. The following explanation using FIG. 1 will be basically based on the meridian cross-section shape shown, but each tire constituent member also extends in the tire circumferential direction and forms an annular shape.
[0017] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the inner side to the outer side in the tire width direction around a bead core 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of the bead core 5, and this bead filler 6 is wrapped by the main portion and the folded back portion of the carcass layer 4. Meanwhile, a plurality of belt layers 7 (two layers in FIG. 1 ) are embedded on the outer periphery of the carcass layer 4 in the tread portion 1. Each belt layer 7 is configured by a plurality of reinforcing cords (belt cords) coated with a belt coat rubber. The plurality of reinforcing cords are arranged inclined with respect to the tire circumferential direction in each layer, and are arranged so that the reinforcing cords cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords (belt cords) with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers: a full cover 8a that covers the entire width of the belt layer 7 and an edge cover 8b that locally covers the end portions of the belt layer 7) can be provided on the outer peripheral side of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are angled at, for example, 0° to 5° with respect to the tire circumferential direction.
[0018] A tread rubber layer 10 is disposed on the outer peripheral side of the carcass layer 4 in the tread portion 1, a side rubber layer 20 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the sidewall portion 2, and a rim cushion rubber layer 30 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the bead portion 3. The tread rubber layer 11 has a structure in which two types of rubber layers with different physical properties (a cap tread 11 that forms the tread surface of the tread portion 1 and an undertread 12 disposed on its inner peripheral side) are laminated in the tire radial direction.
[0019] The tire in which the rubber composition for undertread of the present invention is used is preferably a pneumatic tire (a tire filled with air, an inert gas such as nitrogen, or other gases) as described above, but may also be a non-pneumatic tire. In the case of a non-pneumatic tire, the rubber composition for undertread of the present invention can be used in a rubber layer (a portion corresponding to the undertread layer 12 in a pneumatic tire) arranged on the inner circumferential side of the portion that comes into contact with the road surface (a portion corresponding to the cap tread layer 11 in a pneumatic tire). As long as the tread portion 1 (tread rubber layer 10) of the tire to which the present invention is applied is composed of the cap tread 11 and the undertread 12, the basic structure of the other portions is not limited to the above-mentioned structure.
[0020] In the rubber composition for undertread of the present invention, the rubber component is a diene rubber, and necessarily contains an isoprene rubber and a modified butadiene rubber and / or a modified styrene-butadiene rubber. The combined use of these rubbers is advantageous in improving low heat buildup while maintaining good elongation at break.
[0021] Examples of isoprene-based rubbers include various natural rubbers, epoxidized natural rubbers, and various synthetic polyisoprene rubbers. Among these isoprene-based rubbers, natural rubber is particularly suitable. The content of the isoprene-based rubber is 40% to 90% by mass, preferably 50% to 90% by mass, and more preferably 60% to 90% by mass, based on 100% by mass of the rubber component. By including such an amount of isoprene-based rubber (particularly natural rubber), it is possible to improve the elongation at break and low heat buildup in a balanced manner. If the amount of isoprene-based rubber is less than 40% by mass, the elongation at break decreases. If the amount of isoprene-based rubber is more than 90% by mass, the low heat buildup deteriorates.
[0022] In the rubber composition for undertread of the present invention, the rubber component contains the above-mentioned isoprene-based rubber as well as a modified butadiene rubber and / or a modified styrene-butadiene rubber, which will be described later. That is, the rubber composition for undertread of the present invention contains two rubber components, an isoprene-based rubber and a modified butadiene rubber, two rubber components, an isoprene-based rubber and a modified styrene-butadiene rubber, or three rubber components, an isoprene-based rubber, a modified butadiene rubber, and a modified styrene-butadiene rubber. It is particularly preferable to use a combination of an isoprene-based rubber (natural rubber) and a modified butadiene rubber. In this case, the content (total) of the modified butadiene rubber and / or the modified styrene-butadiene rubber is 10% by mass to 40% by mass, preferably 15% by mass to 35% by mass, and more preferably 20% by mass to 35% by mass, based on 100% by mass of the rubber component. By including such amounts of the modified butadiene rubber and / or the modified styrene-butadiene rubber, it is possible to improve hardness and low heat buildup in a balanced manner. In other words, by suppressing the heat buildup of the rubber composition for undertread while maintaining high hardness, it is possible to suppress belt lift-up during high-speed running in tires, which is particularly advantageous for improving durability against belt separation. If the compounding amount of modified butadiene rubber and / or modified styrene butadiene rubber is less than 10% by mass, the low heat buildup properties deteriorate. If the compounding amount of modified butadiene rubber and / or modified styrene butadiene rubber exceeds 90% by mass, the elongation at break decreases. When modified butadiene rubber and modified styrene butadiene rubber are contained, there are no particular restrictions on the individual contents, but it is preferable that the modified butadiene rubber be contained in an amount of 10% by mass to 35% by mass and the modified styrene butadiene rubber be contained in an amount of 100% by mass of the rubber component.
[0023] Modified butadiene rubber is a butadiene rubber in which one or both molecular ends have been modified with a functional group containing a heteroatom and reactive with the silanol groups on the silica surface. Examples of heteroatoms include oxygen, nitrogen, silicon, and sulfur, with nitrogen and silicon being preferred. Examples of such functional groups include at least one selected from polyorganosiloxane groups, hydroxyl group-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, aldehyde groups, carboxyl groups, amino groups, imino groups, epoxy groups, amide groups, thiol groups, and ether groups. Among these, polyorganosiloxane groups, hydroxyl group-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, and amino groups are preferred. A combination of multiple of these functional groups (e.g., two types of amino groups and alkoxysilyl groups) may also be used. The use of such modified butadiene rubber improves affinity with the large-particle silica described below, which is advantageous for achieving a balanced improvement in elongation at break and low heat buildup.
[0024] The modified butadiene rubber that can be suitably used preferably has a glass transition temperature Tg of -85°C or lower, more preferably -110°C to -90°C. Having such a glass transition temperature, it is possible to improve the strength at break and elongation at break. If the glass transition temperature Tg of the modified butadiene rubber exceeds -85°C, the effects of improving the elongation at break and low heat buildup cannot be expected to be sufficient.
[0025] The modified butadiene rubber preferably has a cis-1,4 bond content of 95% or more, more preferably 96% to 99%. A high cis-1,4 bond content is advantageous for improving the strength at break and elongation at break. If the cis-1,4 bond content is less than 95%, the strength at break and elongation at break decrease. The cis-1,4 bond content of the butadiene rubber can be increased or decreased by a conventional method such as using a catalyst.
[0026] The molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the modified butadiene rubber is preferably 1.5 to 3.5, more preferably 2.0 to 3.3. By optimizing the molecular weight distribution of the modified butadiene rubber in this way, the rubber's physical properties are improved, and the handling stability and high-speed durability of the resulting tire can be effectively improved while maintaining good low heat buildup. If the molecular weight distribution (Mw / Mn) of the modified butadiene rubber is less than 1.5, the extrusion processability deteriorates. If the molecular weight distribution (Mw / Mn) of the modified butadiene rubber is more than 3.5, the low heat buildup property deteriorates. The "weight average molecular weight Mw" and "number average molecular weight Mn" are measured by gel permeation chromatography (GPC) using standard polystyrene equivalents.
[0027] The modified butadiene rubber is preferably butadiene rubber (Nd-BR) synthesized using a neodymium catalyst modified with the above-mentioned functional groups. Although the desired effects can be achieved by using butadiene rubber polymerized using other catalysts (e.g., nickel, cobalt, titanium, etc.), Nd-BR is preferred from the perspective of achieving both low heat buildup, breaking strength, and breaking elongation. Neodymium-catalyzed butadiene rubber (Nd-BR) is a well-known material and is butadiene rubber polymerized using a neodymium-based catalyst, such as neodymium itself, compounds of neodymium with other metals, or organic neodymium compounds. These neodymium-catalyzed butadiene rubbers have the characteristics of high molecular weight and a narrow molecular weight distribution. Commercially available Nd-BR can be used.
[0028] The modified styrene-butadiene rubber is a styrene-butadiene rubber in which one or both molecular ends have been modified with a functional group containing a heteroatom and reactive with the silanol groups on the silica surface. Examples of heteroatoms include oxygen, nitrogen, silicon, and sulfur, with nitrogen and silicon being preferred. Examples of such functional groups include at least one selected from the group consisting of polyorganosiloxane groups, hydroxyl-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, aldehyde groups, carboxyl groups, amino groups, imino groups, epoxy groups, amide groups, thiol groups, and ether groups. Among these, polyorganosiloxane groups, hydroxyl-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, and amino groups are preferred. A combination of multiple of these functional groups (e.g., two types of amino groups and alkoxysilyl groups) may also be used. The use of such modified butadiene rubber improves affinity with the large-particle silica described below, which is advantageous for achieving a balanced improvement in elongation at break and low heat buildup.
[0029] The modified styrene butadiene rubber that can be suitably used is one having a glass transition temperature Tg of preferably -75°C to -45°C, more preferably -75°C to -55°C. When the modified styrene butadiene rubber has such a glass transition temperature, it is possible to improve the low heat buildup properties. If the glass transition temperature Tg of the modified styrene butadiene rubber is less than -75°C, the effect of improving the breaking strength cannot be expected to be sufficient. If the glass transition temperature Tg of the modified styrene butadiene rubber is more than -45°C, the effect of further improving the low heat buildup properties cannot be expected to be sufficient.
[0030] The styrene content of the modified styrene butadiene rubber used in the present invention is preferably 5% to 25% by mass, more preferably 5% to 20% by mass. The vinyl content of the modified styrene butadiene rubber is preferably 15% to 50% by mass, more preferably 20% to 45% by mass. By keeping the styrene content and vinyl content within these appropriate ranges, the reaction rate between silica and silane is improved, thereby improving low heat buildup. If the styrene content of the modified styrene butadiene rubber is less than 5% by mass, the effect of improving breaking strength cannot be fully expected. If the styrene content of the modified styrene butadiene rubber is more than 25% by mass, the effect of improving low heat buildup cannot be fully expected. If the vinyl content of the modified styrene butadiene rubber is less than 15% by mass, the effect of improving low heat buildup cannot be fully expected. If the vinyl content of the modified styrene butadiene rubber is more than 50% by mass, the effect of improving elongation at break cannot be fully expected. The styrene content and vinyl content of the modified styrene butadiene rubber are measured by infrared spectroscopy (Hampton method). The styrene content and vinyl content in the styrene-butadiene rubber can be appropriately adjusted by a conventional method such as using a catalyst.
[0031] The rubber component constituting the rubber composition for undertread of the present invention includes at least the above-mentioned isoprene-based rubber (particularly natural rubber), modified butadiene rubber, and modified styrene-butadiene rubber, but may optionally contain other diene-based rubbers. Examples of other diene-based rubbers that can be used include rubbers that are generally usable in rubber compositions for tires. Examples include unmodified butadiene rubber and unmodified styrene-butadiene rubber. Furthermore, when natural rubber is used as the isoprene-based rubber, isoprene rubber can also be used in combination as the other diene-based rubber. These other diene-based rubbers can be used alone or in any blend.
[0032] In the present invention, silica is always blended as a filler into the rubber component. The silica used in the present invention may be, for example, a silica typically used in rubber compositions for tires, such as wet-process silica, dry-process silica, or surface-treated silica. However, the CTAB adsorption specific surface area of the silica must be 60 m. 2 / g~100m 2 / g, preferably 70m 2 / g~90m 2 / g, more preferably 75m 2 / g~85m 2 / g. By using silica with such a large particle size, it is possible to improve low heat generation and wear resistance. When the CTAB adsorption specific surface area of silica is 60 m 2 If the CTAB adsorption specific surface area of silica is less than 100m / g, the low heat generation property will be deteriorated. 2 If the silica satisfies the above conditions, it may be selected from commercially available silicas, or silica obtained by a conventional manufacturing method may be used.
[0033] The amount of silica blended is 3 to 60 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 50 parts by mass, per 100 parts by mass of the rubber component. By blending an appropriate amount of silica in this way, it is possible to improve the low heat buildup properties, steering stability, and high-speed durability of a tire in a well-balanced manner. If the amount of silica blended is less than 3 parts by mass, the elongation at break decreases. If the amount of silica blended exceeds 60 parts by mass, the low heat buildup properties deteriorate.
[0034] In the present invention, in addition to the above-mentioned silica, carbon black can also be compounded as a filler. The carbon black used in the present invention is preferably a carbon black having a CTAB adsorption specific surface area of 40 m among the carbon blacks normally used in rubber compositions for tires. 2 / g~120m 2 / g, more preferably 70m 2 / g~100m 2 / g. Using such carbon black is advantageous for achieving a good balance between low heat buildup, steering stability, and high-speed durability when made into a tire. The CTAB adsorption specific surface area of the carbon black is 40m 2 If the CTAB adsorption specific surface area of the carbon black is less than 120 m / g, the abrasion resistance will decrease. 2 If it exceeds 1 / g, the low heat buildup property deteriorates.
[0035] When carbon black is used in addition to silica as described above, the total amount of silica and carbon black is preferably 40 to 95 parts by mass, more preferably 45 to 90 parts by mass, per 100 parts by mass of the rubber component. Blending appropriate amounts of silica and carbon black in this way is advantageous for achieving a balanced improvement in the low heat buildup, handling stability, and high-speed durability of the resulting tire. If the total amount of silica and carbon black is less than 40 parts by mass, the breaking strength decreases and high-speed durability deteriorates. If the total amount of silica and carbon black exceeds 95 parts by mass, fuel economy deteriorates and elongation at break decreases.
[0036] Furthermore, when silica and carbon black are used in combination, the ratio Ms / Mc (the amount of silica mixed to the amount of carbon black mixed) is preferably 0.05 to 0.7, more preferably 0.1 to 0.6. By blending silica and carbon black in an appropriate balance, and particularly by keeping the amount of silica in the filler low, it is possible to suppress the deterioration of tan δ (60°C) caused by blending large-particle silica, and to achieve a balanced improvement in elongation at break and low heat buildup. If the ratio Ms / Mc (the amount of silica mixed to the amount of carbon black mixed) exceeds 0.7, processability (e.g., rubber cohesion, adhesion to other components) deteriorates.
[0037] The rubber composition of the present invention may contain fillers other than silica and carbon black, such as clay, talc, calcium carbonate, mica, aluminum hydroxide, and other materials commonly used in rubber compositions for tires.
[0038] In the rubber composition for undertread of the present invention, a silane coupling agent may be compounded when compounding the silica. Compounding a silane coupling agent can improve the dispersibility of silica in the rubber component (diene rubber). Examples of silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazoletetrasulfide, γ-mercaptopropyltriethoxysilane, and 3-octanoylthiopropyltriethoxysilane. Among these, those having a tetrasulfide bond in the molecule are particularly suitable. The compounding amount of the silane coupling agent is preferably 3.0 to 10.0% by mass, more preferably 4.0 to 9.0% by mass, relative to the compounding amount of silica. If the compounding amount of the silane coupling agent is less than 3.0% by mass of the compounding amount of silica, the compounding amount is so small that the effect of compounding the silane coupling agent cannot be fully expected. If the amount of the silane coupling agent exceeds 10% by mass of the amount of silica, the silane coupling agents will condense with each other, making it difficult to obtain the desired hardness and strength in the rubber composition.
[0039] Other compounding agents than those described above can be added to the rubber composition for undertread of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antioxidants, and liquid polymers. The compounding amounts of these compounding agents can be conventional amounts as long as they do not contradict the object of the present invention. Furthermore, as the kneading machine, a conventional rubber kneading machine, such as a Banbury mixer, kneader, or roll, can be used.
[0040] As described above, the rubber composition for an undertread of the present invention can be suitably used in the undertread layer of a tire, and a tire having an undertread layer made of the rubber composition for an undertread of the present invention can improve steering stability and high-speed durability while ensuring good low heat buildup due to the excellent physical properties of the rubber composition for an undertread of the present invention. When the rubber composition for an undertread of the present invention is used in a tire, the tensile stress M100 at 100% elongation at 23°C of the undertread rubber constituting the undertread layer (i.e., the vulcanizate of the rubber composition for an undertread of the present invention) is UT [unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer 7 B [Unit: MPa] Ratio to M100 UT / M100 B is preferably 0.4 to 1.0, and more preferably 0.5 to 0.9. By optimizing the relationship of the tensile stress (M100) between the undertread layer using the rubber composition for undertread of the present invention and the belt layer 7 (coat rubber) disposed on the inner peripheral side thereof in this way, it is advantageous to improve the driving stability and high-speed durability while ensuring low heat buildup. The ratio M100 UT / M100 B If the ratio is less than 0.4, the effects of improving low heat buildup, steering stability, and high-speed durability will be limited. UT / M100 B If the value exceeds 1.0, the effects of improving low heat buildup, handling stability, and high-speed durability will be limited.
[0041] The present invention will be further explained below with reference to examples, but the scope of the present invention is not limited to these examples. [Example]
[0042] The tire size is 245 / 45R18, and has the basic structure shown in Figure 1. The compounding of the rubber composition for the undertread and the tensile stress (M100) at 100% elongation at 23°C of the undertread rubber and the belt coat rubber areUT , M100 B ) and its ratio M100 UT / M100 B Tires (test tires) of Standard Example 1, Comparative Examples 1 to 7, and Examples 1 to 10 were manufactured with the values set as shown in Tables 1 and 2.
[0043] Regarding the formulation of the rubber composition for undertread, the formulation common to all examples is summarized in Table 3. Tables 1 and 2 also list the type of belt coat rubber used in each example. The type of belt coat rubber is indicated by the number of coat rubbers A to B listed in Table 4, and the formulation of these coat rubbers A to B is as shown in Table 4.
[0044] The tensile stress (M100 UT , M100 B ) is the value (unit: MPa) measured using undertread rubber and coat rubber, using a No. 3 dumbbell test piece prepared in accordance with JIS K6251, at a tensile speed of 500 mm / min and a temperature of 23°C.
[0045] Using each test tire, the steering stability, low rolling resistance, and high-speed durability were evaluated by the methods described below.
[0046] Steering stability Each test tire was mounted on a wheel with a rim size of 18x7J, the air pressure was set to 240kPa, and the tire was mounted on a test vehicle with an engine displacement of 2000cc. A test driver then conducted a sensory evaluation of the handling stability on a test course consisting of a paved road. The evaluation results were rated on a 5-point scale, with the result of Standard Example 1 being given 3 points (standard). The higher the score, the better the handling stability.
[0047] Low rolling resistance Each test tire was mounted on a wheel with a rim size of 18x7J, and rolling resistance was measured using an indoor drum testing machine (drum diameter: 1707.6mm) in accordance with ISO28580 under conditions of an air pressure of 210kPa, a load of 4.82kN, and a speed of 80km / h. The evaluation results were expressed as an index using the reciprocal of the measured value, with standard example 1 being 100. The higher the index value, the lower the rolling resistance, indicating excellent low rolling resistance.
[0048] Belt separator durability Each test tire was mounted on a wheel with a rim size of 18x7J and stored for 7 days at 70°C with an internal pressure of 350 kPa and oxygen sealed in. The pretreated test tire was inflated to 230 kPa and mounted on an indoor drum testing machine (drum diameter: 1707.6 mm). A running test was conducted in which the tire was loaded with 88% of the JATMA maximum load capacity and driven for 12 hours over a distance of 30 km at a speed of 100 km / h. After running, the tire was cut open and the widthwise separation length at the belt widthwise edge was measured. The evaluation results were expressed as an index using the reciprocal of the measured value, with the value for Reference Example 1 being 100. A higher index value indicates a shorter separation length and better durability against belt edge separation.
[0049] [Table 1]
[0050] [Table 2]
[0051] [Table 3]
[0052] The types of raw materials used in Tables 1 to 3 are shown below. NR: Natural rubber, TSR20 BR1: Nipol 1220 manufactured by Zeon Corporation (unmodified butadiene rubber synthesized using a cobalt catalyst, glass transition temperature Tg = -105°C, cis-1,4 bond content: 98 mol%) BR2: Nipol 1250H manufactured by Nippon Zeon Co., Ltd. (modified butadiene rubber synthesized using a lithium catalyst, modifying group: N-methylpyrrolidone, glass transition temperature Tg = -93°C, cis-1,4 bond content: 35 mol%) BR3: ENEOS BR511 manufactured by JSR Corporation (modified butadiene rubber synthesized using a neodymium catalyst, glass transition temperature Tg = -78°C, cis-1,4 bond content: 25 mol%) BR4: ENEOS BR54 manufactured by JSR Corporation (modified butadiene rubber synthesized using a neodymium catalyst, glass transition temperature Tg = -107°C, modifying group: hydrocarbyloxysilane compound, cis-1,4 bond content: 96 mol%) SBR: JSR ENEOS HPR940 CB1: Carbon black (grade: ISAF), manufactured by Tokai Carbon Co., Ltd., SEA ST 6 (CTAB adsorption specific surface area: 109 m 2 / g) CB2: Carbon black (grade: HAF), manufactured by Tokai Carbon Co., Ltd., SEAT 3 (CTAB adsorption specific surface area: 82 m 2 / g) CB3: Carbon black (grade: FEF), manufactured by Tokai Carbon Co., Ltd., SEA ST F (CTAB adsorption specific surface area: 47 m 2 / g) ·Silica 1: Evonik ULTRASIL VN3GR (CTAB adsorption specific surface area: 175m 2 / g) Silica 2: Solvay ZEOSIL 115GR (CTAB adsorption specific surface area: 115 m 2 / g) Silica 3: Solvay Zeosil 1185GR (CTAB adsorption specific surface area: 80 m 2 / g) Silane coupling agent: Si69 manufactured by Evonik Industries AG Tackifier: Hitachi Chemical's Hitanol 1502Z Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Anti-aging agent: PILFLEX 13 manufactured by NOCIL LIMITED Stearic acid: Stearic acid 50S manufactured by Nisshin Rika Co., Ltd. Sulfur: Shikoku Chemical Industry Co., Ltd. Myucron OT-20 Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.
[0053] [Table 4]
[0054] The types of raw materials used in Table 4 are shown below. NR: Natural rubber, natural rubber, RSS#3 CB: Carbon black (grade: HAF), manufactured by Tokai Carbon Co., Ltd., Seast 300 Tackifier: Hitachi Chemical's Hitanol 1502Z Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Anti-aging agent: PILFLEX 13 manufactured by NOCIL LIMITED Cobalt stearate: Cobalt stearate manufactured by Airec Sulfur: Shikoku Chemical Industry Co., Ltd. Myucron OT-20 Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.
[0055] As is clear from Tables 1 and 2, Examples 1 to 10 improved steering stability, low rolling resistance, and belt separator durability compared to Reference Example 1, achieving a good balance of these performances. On the other hand, in Comparative Example 1, the CTAB specific surface area of the silica was large, resulting in poor steering stability and belt separator durability. In Comparative Example 2, the CTAB specific surface area of the silica was large, resulting in poor steering stability and belt separator durability. In Comparative Example 3, unmodified butadiene rubber was used, resulting in poor belt separator durability. In Comparative Example 4, the amount of silica blended was low, resulting in poor belt separator durability. In Comparative Example 5, the amount of silica blended was high, resulting in poor steering stability and belt separator durability. In Comparative Example 6, the amount of isoprene-based rubber (natural rubber) blended was high and the amount of unmodified butadiene rubber blended was low, resulting in poor belt separator durability. In Comparative Example 7, the amount of isoprene-based rubber (natural rubber) blended was low and the amount of unmodified butadiene rubber blended was high, resulting in poor steering stability and belt separator durability.
[0056] The present disclosure includes the following inventions. Invention [1] A rubber composition having a CTAB adsorption specific surface area of 60 m for 100 parts by mass of a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene. 2 / g~100m 2 1. A rubber composition for undertread, comprising 3 to 60 parts by mass of silica having a molecular weight of 1 / g. Invention [2] A CTAB adsorption specific surface area of 40 m for 100 parts by mass of the rubber component 2 / g~120m 2 The rubber composition for undertread according to invention [1], characterized in that 20 to 70 parts by mass of carbon black having a molecular weight of 1 / g is compounded. Invention [3] The rubber composition for undertread according to invention [1] or [2], characterized in that the glass transition temperature of the modified butadiene rubber is −85° C. or lower. Invention [4] The rubber composition for undertread according to any one of inventions [1] to [3], wherein the modified butadiene rubber has a cis-1,4 bond content of 95% or more. Invention [5] A rubber composition for undertread according to any one of inventions [1] to [4], characterized in that a silane coupling agent is blended therein, and the ratio of the blending amount of the silane coupling agent to the blending amount of the silica is 3.0% by mass to 10.0% by mass. Invention [6] A tire comprising a tread portion extending in the circumferential direction of the tire to form an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged on the radially inner side of these sidewall portions, and having at least one carcass layer mounted between the pair of bead portions and a plurality of belt layers arranged on the outer peripheral side of the carcass layer in the tread portion, the tread portion being constructed by laminating a cap tread layer that constitutes the tire tread surface and an undertread layer arranged on its inner peripheral side, wherein the undertread layer is constructed from the rubber composition for an undertread according to any one of Inventions [1] to [5]. Invention [7] The tensile stress M100 of the undertread rubber constituting the undertread layer at 23°C when elongated to 100% UT [unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer B [Unit: MPa] Ratio to M100 UT / M100 B The tire according to the invention [6], characterized in that is 0.4 to 1.0. [Explanation of symbols]
[0057] 1 Tread section 2 Sidewall 3 Bead section 4 carcass layers 5 bead core 6 Bead filler 7 Belt Layer 8 Belt cover layer 10 Tread rubber layer 11 Cap tread layer 12 Undertread layer 20 Side rubber layer 30 Rim cushion rubber layer CL Tire Equator
Claims
1. A rubber component having a CTAB adsorption specific surface area of 60 m for 100 parts by mass of a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene. 2 / g to 100m 2 / g of silica is blended in an amount of 3 to 60 parts by mass.
2. A CTAB adsorption specific surface area of 40 m per 100 parts by mass of the rubber component. 2 / g ~ 120m 2 2. The rubber composition for undertread according to claim 1, characterized in that 20 to 70 parts by mass of carbon black having a viscosity of 1 / g is blended.
3. The rubber composition for undertread according to claim 1 or 2, characterized in that the glass transition temperature of the modified butadiene rubber is −85° C. or lower.
4. 3. The rubber composition for undertread according to claim 1, wherein the modified butadiene rubber has a cis-1,4 bond content of 95% or more.
5. 3. The rubber composition for undertread according to claim 1, further comprising a silane coupling agent, the ratio of the amount of the silane coupling agent to the amount of the silica being 3.0% by mass to 10.0% by mass.
6. 3. A tire comprising a tread portion extending in a circumferential direction of the tire to form an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged on the radially inner side of the sidewall portions, the tire having at least one carcass layer mounted between the pair of bead portions, and a plurality of belt layers arranged on the outer peripheral side of the carcass layer in the tread portion, the tread portion being constructed by laminating a cap tread layer constituting a tire tread surface and an undertread layer arranged on its inner peripheral side, the undertread layer being constructed from the rubber composition for undertreads according to claim 1 or 2.
7. The tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer B Ratio to M100 [unit: MPa] UT / M100 B 7. The tire according to claim 6, wherein the tread width is 0.4 to 1.0.
Citation Information
Patent Citations
Rubber composition for tire, and pneumatic tire
JP2012219224A
Pneumatic tire
JP2013177113A
Rubber composition for tire
JP2019026757A
Rubber composition for tread, and tire
JP2019151738A
Rubber composition and tire made therefrom
JP2023069115A