Light-shielding film
The light-shielding film with a binder resin, black pigment, and acrylic resin particles addresses brittleness issues, ensuring low gloss and reflectivity, facilitating thinner and lighter optical equipment.
Patent Information
- Application Number
- JP2023061266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing light-shielding films using plastic materials face issues with brittleness due to amorphous silica particles, leading to burrs and cracks during punching, which impair the low reflectivity and light-shielding properties of the end face.
A light-shielding film with a light-shielding layer containing a binder resin, black pigment, and resin particles with a recovery rate of 10% to 95%, where the resin particles are acrylic resin, maintaining low gloss and excellent processability.
The film achieves low gloss and excellent low reflectivity, enabling thinner and lighter optical equipment with improved workability and reduced end-face reflection.
Smart Images

Figure 2024148269000004 
Figure 2024148269000005 
Figure 2024148269000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-shielding film. [Background technology]
[0002] The light-shielding film is a member having a light-shielding layer for shielding light of a desired wavelength by scattering and / or absorbing the light, for example, in various applications such as optical members such as lens units, as well as optical device members, display device members, machine parts, electric and electronic parts, etc. For example, in optical applications such as high-performance single-lens reflex cameras, compact cameras, video cameras, digital cameras, and camera modules for mobile phone cameras, the light-shielding members of optical devices that have been made of metal materials are being replaced by plastic materials due to demands for smaller, thinner, and lighter devices.
[0003] In addition, as a light-shielding layer using such a plastic material, there is also a method of forming a light-shielding layer by directly applying a coating liquid for forming a light-shielding layer to an optical member. However, with this method, it is difficult to form the surface shape of the light-shielding layer and the shape of the light-transmitting end face of the light-shielding layer into a shape suitable for the optical member. Therefore, instead of directly applying a coating liquid for forming a light-shielding layer to an optical member, the use of a light-shielding film in the form of a film prepared separately has been considered. For example, Patent Document 1 discloses a light-shielding film containing a black pigment and amorphous silica as essential resin components. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-194514 A Summary of the Invention [Problem to be solved by the invention]
[0005] The light-shielding film described in Patent Document 1 is expected to have low reflectivity and light-shielding properties on the surface and punched end faces. However, the amorphous silica particles themselves are hard, making the light-shielding layer brittle, and burrs and cracks are generated when the light-shielding layer is punched. There is a problem in that the burrs and cracks generated during punching impair the low reflectivity and light-shielding properties of the end faces of the punched parts in particular. The present invention has been made in consideration of the above-mentioned background, and aims to provide a light-shielding film having a light-shielding layer with a low surface gloss and excellent low reflectivity, excellent processability, and excellent low reflectivity at the end face of the punched-out portion. [Means for solving the problem]
[0006] As a result of intensive research aimed at solving the above problems, the present inventors have found that the problems of the present invention can be solved in the following aspects, and have thus completed the present invention. That is, the present invention relates to a light-shielding film having a light-shielding layer containing a binder resin, a black pigment, and resin particles, characterized in that the resin particles have a restoration rate of 10% or more and 95% or less.
[0007] The present invention also relates to the above light-shielding film, wherein the resin particles are acrylic resin particles.
[0008] The present invention also relates to the above light-shielding film, in which the 60° gloss of one surface of the light-shielding layer is 5 or less, as measured by a specular gloss measurement method in accordance with JIS Z8741.
[0009] The present invention also relates to the above light-shielding film consisting of only the above light-shielding layer.
[0010] The present invention also relates to the above light-shielding film for use as an optical member. Effect of the Invention
[0011] According to the present invention, it is possible to provide a light-shielding film having a light-shielding layer with a low surface gloss and excellent low reflectivity, excellent processability, and excellent low reflectivity at the end face of the punched portion. The light-shielding film of the present invention makes it possible to reduce the thickness and weight of optical devices. [Brief description of the drawings]
[0012] [Figure 1] 1 shows the state of a punched end surface of a light-shielding film in Example 1 of the present application. [Diagram 2] 1 shows the state of a punched end surface of a light-shielding film in Comparative Example 1 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An example of an embodiment to which the present invention is applied will be described below. Needless to say, other embodiments are also included in the scope of the present invention as long as they are consistent with the gist of the present invention. The numerical values specified in this specification are values obtained by the methods disclosed in the embodiments or examples. Furthermore, the numerical values "A to B" specified in this specification refer to a range that includes numerical value A and numerical value B, and is greater than numerical value A and smaller than numerical value B and numerical value B. Furthermore, the term "film" in this specification includes not only "film" as defined by JIS, but also "sheet".
[0014] 《Light blocking layer》 The light-shielding film of the present embodiment has a light-shielding layer containing a binder resin, a black pigment, and resin particles, and can provide a light-shielding film with excellent processability by suppressing the surface glossiness of the light-shielding layer.
[0015] <Binder resin> Examples of the binder resin include thermoplastic resins or thermosetting resins such as poly(meth)acrylic acid resins, polyester resins, polyvinyl acetate resins, polyvinyl chloride resins, polyvinyl butyral resins, cellulose resins, polystyrene / polybutadiene resins, polyurethane resins, alkyd resins, acrylic resins, unsaturated polyester resins, epoxy ester resins, epoxy resins, epoxy acrylate resins, urethane acrylate resins, polyester acrylate resins, polyether acrylate resins, phenol resins, melamine resins, urea resins, and diallyl phthalate resins, but are not limited thereto. Thermoplastic elastomers, thermosetting elastomers, ultraviolet curable resins, and electron beam curable resins can also be used. These can be used alone or in combination of two or more. The binder resin is preferably a cellulose-based resin in terms of dispersibility of the black pigment and resin particles, and heat resistance and strength of the light-shielding layer.
[0016] The cellulose-based resin includes cellulose and cellulose derivatives, etc. Examples of the cellulose derivatives include cellulose ester, cellulose carbamate, cellulose ether, etc. Among these, from the viewpoints of dispersibility of the black pigment and resin particles and handling during production, solvent-soluble cellulose resins are preferred, and cellulose esters are particularly preferred.
[0017] Examples of cellulose esters include cellulose acetates such as cellulose diacetate and cellulose triacetate; cellulose C3-5 acylates such as cellulose propionate and cellulose butyrate; and cellulose acylates such as cellulose acetate propionate and cellulose acetate butyrate. Moreover, an example of the cellulose carbamate is cellulose phenyl carbamate. Examples of cellulose ethers include alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose, carboxyalkyl cellulose, alkyl-carboxyalkyl cellulose, and derivatives thereof (eg, sodium carboxymethyl cellulose, etc.).
[0018] The number average molecular weight of the binder resin is preferably 10,000 or more and 150,000 or less, more preferably 20,000 or more and 100,000 or less, in terms of polystyrene. By having a number average molecular weight of 10,000 or more, more sufficient coating strength can be obtained. By having a number average molecular weight of 150,000 or less, an increase in viscosity can be suppressed when the resin composition for forming a light-shielding layer is prepared.
[0019] The binder resin preferably has a glass transition temperature measured in accordance with JIS K7121 of 0° C. or higher, more preferably 50° C. or higher, and even more preferably 100° C. or higher. When the glass transition temperature is within this range, the heat resistance of the light-shielding layer can be maintained.
[0020] The binder resin preferably has a functional group capable of reacting with an isocyanate curing agent. By reacting with the isocyanate curing agent, the heat resistance and chemical resistance of the light-shielding layer can be improved. Examples of the functional group capable of reacting with the isocyanate curing agent include a hydroxyl group, an amino group, a carboxyl group, an epoxy group, an N-methylol group, and an N-alkoxymethyl group.
[0021] <Isocyanate hardener> The isocyanate curing agent is an isocyanate compound having two or more isocyanate groups. Examples of the isocyanate curing agent include isocyanate compounds such as aromatic isocyanates, aliphatic isocyanates, and alicyclic isocyanates. These can be used alone or in combination of two or more.
[0022] In addition, so-called modified polyisocyanates (modified products of isocyanates) such as adduct modified products, biuret modified products, allophanate modified products, uretonimine modified products, uretdione modified products, carbodiimide modified products, etc. of the above-mentioned isocyanate compounds can also be used as the isocyanate curing agent.
[0023] The isocyanate curing agent is preferably an aliphatic isocyanate. By using an aliphatic isocyanate, cracking of the light-shielding layer can be suppressed. More preferably, it is a polyisocyanate modified to three or more functional groups, which is a trimer of an aliphatic isocyanate (also called a multifunctional modified polyisocyanate or modified body). By using a multifunctional modified polyisocyanate, cracking of the coating film can be suppressed and heat resistance can be improved. More preferably, it is a polyisocyanate modified from an aliphatic isocyanate to an isocyanurate (isocyanurate body) or a polyisocyanate modified from an aliphatic isocyanate to a biuret (biuret body). By using an isocyanurate body or a biuret body, heat resistance can be improved and cracking of the coating film can be suppressed.
[0024] The light-shielding layer in the light-shielding film preferably contains 5 to 50 parts by mass of an isocyanate curing agent relative to 100 parts by mass of the binder resin, and more preferably 10 to 40 parts by mass. By containing 5 parts by mass or more of an isocyanate curing agent, curling of the light-shielding layer can be easily suppressed, and by containing 50 parts by mass or less, a strong light-shielding layer that is less likely to crack can be easily formed.
[0025] <Black pigment> Examples of black pigments include known black pigments such as carbon black, titanium black, etc. These black pigments can be used alone or in any combination of two or more. As the black pigment, carbon black is preferably used from the viewpoints of pigment dispersibility, cost reduction, etc., and when an antistatic effect is to be imparted to the light-shielding layer, conductive carbon black such as furnace black, channel black, acetylene black, etc. Carbon black may be in the form of an aggregate, agglomerate, etc.
[0026] The content of the black pigment in the light-shielding layer is from 2 to 40 parts by mass, and preferably from 5 to 30 parts by mass, relative to 100 parts by mass of the binder resin, from the viewpoints of light-shielding property and depth of appearance. By being in this range, it becomes possible to maintain the tensile strength of the light-shielding layer while maintaining the light-shielding property of the light-shielding layer. In addition, when the resin particles described below contain a black pigment such as carbon black or black titanium oxide, the black pigment in the resin particles is not included in the content of the black pigment per 100 parts by mass of the binder resin.
[0027] The average primary particle size of the black pigment is preferably 100 nm or less. This range makes it possible to improve the light-shielding properties and rigidity of the light-shielding layer and to prevent a decrease in tensile strength. Furthermore, the preferred range for the average primary particle size is 10 nm or more and 50 nm or less. The average primary particle size referred to here can be determined by a general method of directly measuring the size of primary particles from a magnified image (e.g., 1,000 to 10,000 times) of an electron microscope or optical microscope. Specifically, 50 to 100 particles are sampled, their minor axis diameter and major axis diameter are measured, and the average is taken as the particle size of the particles.
[0028] The BET specific surface area of black pigments (sometimes simply abbreviated as "specific surface area") is 30 m 2 / g or more, 1500m 2 / g or less. More preferably, it is 50m 2 / g or more, 500m 2 / g or less.
[0029] In addition, the DBP (dibutyl phthalate) oil absorption (sometimes simply abbreviated as "oil absorption") of the black pigment is preferably 100 ml / 100 g or more. By making the DBP (dibutyl phthalate) oil absorption 100 ml / 100 g or more, the affinity with the binder resin can be improved and the coating strength can be more effectively increased. More preferably, it is 500 ml / 100 g or less.
[0030] <Resin particles> Resin particles are defined as a substance in which organic resin is in particulate form. The resin particles are supported in a dispersed state in the binder resin and are not compatible with the binder resin. The resin particles have a restoration rate of 10% or more and 95% or less. When the restoration rate is in this range, a flexible coating film can be formed while maintaining the strength of the coating film of the light-shielding layer. Furthermore, by adding resin particles, cracks at the end of the processed part when the light-shielding film is punched can be suppressed, and reflections at the end surface of the processed part can be suppressed. The restoration rate of the resin particles is preferably 10% or more and 50% or less, and more preferably 10% or more and 30% or less. The recovery rate of the resin particles can be determined by a load-unload test using a micro-compression tester, which will be described later in the section on examples.
[0031] Examples of the resin particles include various synthetic resin particles, such as melamine resin particles, benzoguanamine resin particles, benzoguanamine / melamine / formaldehyde resin particles, acrylic resin particles, urethane resin particles, styrene resin particles, ethylene resin particles, fluororesin particles, and silicone resin particles. These resins can be used as particles of one type alone, or two or more types of resins can be combined and used as particles, or inorganic pigments can be compounded or encapsulated. More preferably, black pigments such as carbon black and black titanium oxide are encapsulated. By encapsulating a black pigment, the light-blocking properties of the light-blocking layer can be maintained. Among these, acrylic resin particles, which have excellent durability, are preferably used.
[0032] The average particle size of the resin particles is preferably 1 μm or more and 15 μm or less, more preferably 2 μm or more and 10 μm or less. By being in this range, the light-shielding properties of the light-shielding layer can be maintained and the glossiness of the coating film surface can be suppressed. The average particle size here refers to the 50% particle size (d50) in the cumulative particle size distribution based on the volume measured using a laser diffraction particle size distribution meter.
[0033] The content of the resin particles in the light-shielding layer is preferably from 10 to 150 parts by mass, more preferably from 20 to 100 parts by mass, relative to 100 parts by mass of the binder resin. When the content is within this range, the strength of the coating film of the light-shielding layer can be maintained, and the glossiness of the coating film surface can be suppressed.
[0034] The light-shielding layer may contain other additives such as inorganic pigments, other resin particles, plasticizers, stabilizers (antioxidants, ultraviolet absorbers, light-resistance stabilizers, heat stabilizers, etc.), flame retardants, flame retardant assistants, impact resistance improvers, fillers (or reinforcing agents), dispersants, antistatic agents, foaming agents, antibacterial agents, lubricants, etc. These additives may be used alone or in combination of two or more.
[0035] <Method for producing a light-shielding film having a light-shielding layer> Next, an example of a method for producing a light-shielding film having a light-shielding layer will be described, but the method for producing the light-shielding layer of the present invention is not limited to the following method.
[0036] The light-shielding layer can be formed from a resin composition for forming a light-shielding layer, which contains a binder resin, a black pigment, and resin particles. The resin composition for forming the light-shielding layer can be produced by adding other components and solvents, etc., as necessary, to the binder resin, black pigment, and resin particles, mixing them, and dispersing them using various dispersing means such as a kneader, a two-roll mill, a three-roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, or an attritor.
[0037] The light-shielding film in the present invention may be of a laminate type in which a light-shielding layer is provided on a non-peelable substrate, or of a type having only a light-shielding layer (hereinafter also referred to as a single-layer light-shielding layer or a single-layer type). The laminated type can be obtained by coating a resin composition for forming a light-shielding layer on a non-releasable substrate, volatilizing the solvent, and curing the binder resin as necessary to form a light-shielding layer, or by coating a resin composition for forming a light-shielding layer on a peelable substrate, volatilizing the solvent, transferring the light-shielding layer from the peelable substrate to a non-releasable substrate, and further curing the binder resin as necessary to form a light-shielding layer. In the case of only the light-shielding layer, the light-shielding layer can be obtained by coating a resin composition for forming a light-shielding layer onto a peelable substrate, volatilizing the solvent, curing the binder resin as necessary to form the light-shielding layer, and then peeling the peelable substrate from the light-shielding layer. From the viewpoint of minimizing or preventing light reflection on the end faces of the punched portions, a single light-shielding layer is preferred.
[0038] Examples of the non-releasable substrate include synthetic resin films such as polyester film, polyimide film, polystyrene film, and polycarbonate film, synthetic paper, paper, and metal plate. Among them, polyester film is preferably used, and polyester film that has been stretched, particularly biaxially stretched, is particularly preferred in terms of excellent mechanical strength and dimensional stability. Polyimide film is preferably used for applications requiring heat resistance. From the viewpoint of enhancing light-shielding properties in synergy with the light-shielding layer, the substrate may contain a colorant such as carbon black as necessary. The thickness of the non-peeling substrate varies depending on the application and configuration of the light-shielding film, but is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 50 μm or less, and particularly preferably 4 μm or more and 30 μm or less. By making it 1 μm or more, the productivity of the light-shielding film can be ensured. Also, by making it 100 μm or less, it is possible to make the film thinner and lighter.
[0039] The peelable substrate may be a substrate having a release layer on the surface of the non-peeling substrate. Examples of the treatment agent for providing the release layer include an alkyd-based resin compound, a fluorine-based compound, and a silicone-based compound.
[0040] In either case, the substrate that can be peeled off or the substrate that cannot be peeled off is preferably one that has a roughened surface in order to effectively reduce the glossiness of the surface of the light-shielding layer that is to be formed. By forming a light-shielding layer on the roughened surface of a peelable substrate and then peeling off the peelable substrate, the state of the rough surface of the peelable substrate can be transferred to the surface of the light-shielding layer, and as a result, the glossiness of the light-shielding layer can be effectively reduced. Examples of methods for roughening the surface of a peelable substrate include adding inorganic pigments, resin particles, etc. to a treatment agent for providing a peelable layer, and performing a peeling treatment at the same time as roughening, or performing a peeling treatment after physically and / or chemically roughening the surface of the substrate to be treated. Examples of physical and / or chemical roughening methods include sandblasting, which sprays fine sand at a high speed onto the substrate surface to be treated, embossing, which passes the substrate between a metal engraving roll and an elastic roll, and chemical etching, which treats the substrate surface with chemicals. It is preferable to use a peelable substrate that is roughened and peeled at the same time for the sake of simplicity in the treatment process.
[0041] The degree of roughening of the peelable substrate varies depending on the required gloss, but the arithmetic mean roughness Ra (JIS B0601:2001) is preferably 0.1 μm to 6 μm, more preferably 0.3 μm to 5 μm, and even more preferably 0.5 μm to 4 μm. By making Ra 0.1 μm or more, it is possible to easily suppress the gloss low, and by making it 6 μm or less, it is possible to easily peel the peelable substrate from the light-shielding layer. The thickness of the peelable substrate is not particularly limited, but is preferably about 25 to 250 μm in consideration of the workability during peeling.
[0042] There is no particular limitation on the method for roughening the surface of the non-releasable substrate used in the case of the laminated type. For example, the surface can be roughened by applying a coating liquid for forming a matte layer (without a function of imparting releasability) containing a matting agent onto the surface to be treated and drying it, or the surface can be roughened physically and / or chemically by sandblasting, embossing, chemical etching, etc., as in the above-mentioned case.
[0043] The method for coating the resin composition for forming a light-shielding layer on a non-releasable or releasable substrate may be a general coating method, such as a conventionally known coating method, including dip coating, roll coating, bar coating, die coating, blade coating, and air knife coating.
[0044] The thickness of the light-shielding layer in the laminated light-shielding film varies depending on the required optical density and composition, but in applications where the thickness is acceptable, the light-shielding layer should be sufficiently thick, which allows the content of the black pigment in the light-shielding layer to be significantly reduced, and a light-shielding layer with high coating strength can be realized. In such applications, the thickness of the light-shielding layer is preferably 10 μm or more and 100 μm or less, and more preferably 10 μm or more and 50 μm or less. On the other hand, in applications where a thin film is particularly required, the thickness of the light-shielding layer is preferably 1 μm or more and less than 10 μm, more preferably 3 μm or more and 9 μm or less, and even more preferably 5 μm or more and 8 μm or less. By being in such a range, a sufficient optical density can be obtained.
[0045] The thickness of the light-shielding layer in the case of a single layer type varies depending on the required optical density and the configuration of the light-shielding film, but in applications where thickness is acceptable, the light-shielding layer should be sufficiently thick, which allows the content of the black pigment in the light-shielding layer to be significantly reduced, thereby realizing a light-shielding layer with high coating strength. In such applications, the thickness of the light-shielding layer is preferably 50 μm or more and 100 μm or less. On the other hand, in applications where a thin film is particularly required, the thickness of the light-shielding layer is preferably 1 μm or more and less than 50 μm, more preferably 10 μm or more and 30 μm or less. By making the thickness 1 μm or more, it is possible to make it difficult for pinholes and the like to occur in the light-shielding layer, and it is easy to obtain sufficient light-shielding properties. In addition, by making the thickness 10 μm or more, it is possible to obtain a light-shielding layer with high coating strength.
[0046] In addition, when the light-shielding layer is formed using a peelable substrate, the thickness of the light-shielding layer is preferably greater than the arithmetic mean roughness Ra (JIS B0601:2001) of the roughened surface of the peelable substrate.
[0047] Whether the light-shielding film is a laminated type or a single-layer type, it is preferable that the glossiness of at least one surface is 5 or less. More preferably, the glossiness is 3 or less, and even more preferably, 1 or less. Furthermore, it is preferable that both surfaces have a low glossiness. The lower the glossiness of the light-shielding film, the more diffuse reflection of light can be suppressed. For example, when used as a lens unit, the risk of noise causing malfunction can be effectively prevented. The gloss level can be determined by measuring at a measurement angle (θ) of 60 degrees using a gloss meter VG-8000 manufactured by Nippon Denshoku Industries Co., Ltd. In addition, the surface of the light-shielding film preferably has an uneven shape, and the arithmetic mean roughness Ra (JIS B0601:2001) of the surface of the light-shielding film is preferably 0.1 μm or more and 6 μm or less. More preferably, it is 0.3 μm or more and 5 μm or less, and even more preferably, it is 0.5 μm or more and 4 μm or less. By being in this range, the glossiness of the surface can be efficiently suppressed. In order to effectively suppress the glossiness of the surface of the light-shielding film, it is effective to use a peelable substrate having a surface arithmetic mean roughness Ra (JIS B0601:2001) of 0.1 μm or more and 6 μm or less when forming the light-shielding layer.
[0048] The light-shielding film, whether it is a laminated type or a single-layer type, preferably has an optical density of 3 or more. More preferably, it is 4 or more, and even more preferably, it is 5 or more. When the optical density of the light-shielding film is in this range, the light-shielding properties can be effectively improved. The optical density can be measured using an optical densitometer (361T tabletop transmission densitometer: manufactured by X-RITE).
[0049] The surface resistance of the light-shielding film, whether it is a laminated type or a single-layer type, is 1×10 10 By setting the surface resistance in the above range, it is easy to prevent the light-shielding films from sticking to each other or to a processing machine during processing. More preferably, it is 1×10 8 It is less than Ω / □.
[0050] The light-shielding film of the present invention can be used in a state where it is further provided with a functional layer such as an adhesive layer, a pressure-sensitive adhesive layer, etc., within a range that does not impair the effects of the present invention. By providing these functional layers, even if the light-shielding film (particularly a single-layer type) is thin, it has excellent light-shielding properties, handleability, stability, and processability.
[0051] The adhesive layer is for adhering the light-shielding layer in the light-shielding film to optical components, display device components, mechanical components, electric / electronic components, etc. The adhesive layer can be formed from various adhesives such as pressure-sensitive adhesives such as acrylic adhesives, urethane adhesives, polyester adhesives, silicone adhesives, and heat-sensitive adhesives. EXAMPLES
[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0053] [Example 1] A mixture of the following composition was uniformly stirred and mixed using a shaker (Scandex SK450: manufactured by Fast & Fluid Management) to obtain a light-shielding layer-forming resin composition 1. Next, the obtained light-shielding layer-forming resin composition 1 was applied onto a release-treated surface of a peelable substrate, dried to form a light-shielding layer having a thickness of 20 μm after drying, and the substrate was peeled off to obtain a light-shielding film consisting of a single light-shielding layer. Here, the peelable substrate is a polyester film having a thickness of 100 μm that has been sandblasted to have a surface roughened to an arithmetic mean roughness Ra (JIS B0601 (2001)) of 0.8, and the roughened surface has been treated with a release agent (release agent name X: manufactured by Lintec Corporation) for release.
[0054] <Resin composition for forming light shielding layer 1> Binder resin: Cellulosic resin (CAP482-20: Eastman Kodak Company): 100 parts Hardener: Isocyanate hardener (Takenate D-170N: manufactured by Mitsui Chemicals): 20 parts Black pigment Carbon black (Vulcan XC72R: manufactured by CABOT): 15 parts Resin particles: Acrylic resin particles (ARX-806: Sekisui Chemical Industries) 100 parts Dilution solvent (mixture of methyl ethyl ketone / cyclohexanone = 1 / 1 (mass ratio)): 900 parts
[0055] [Examples 2 to 10, Comparative Examples 1 to 3] A resin composition for forming a light-shielding layer and a light-shielding film were produced in the same manner as in Example 1, except that the type of binder resin was changed to the binder resin shown in Table 1, the type of resin particles was changed to the resin particles shown in Table 2, and the blending amount of the resin particles was changed as shown in Table 3. In the table, unless otherwise specified, the numerical values indicate parts, and "none" indicates that no resin particles were blended. The amount of Resin-2 in Example 9 in Table 3 means the amount as solid content.
[0056] [Resin particle recovery rate] The recovery rate of the resin particles shown in Table 2 was determined by a load-unload test using a microcompression tester (MCT-211: manufactured by Shimadzu Corporation). First, the resin particles were placed on the lower pressure plate (SKS flat plate), and an independent resin particle was selected using the optical microscope (objective lens magnification: 50x) of the "MCTM-211". The diameter d of the selected resin particle was measured using the particle size measurement cursor of the "MCTM-211". The resin particles to be selected were determined according to the particle size to be measured. Next, the test indenter is applied to the apex of the selected resin particle at the following loading speed to measure the particle diameter A when the resin particle is loaded to the maximum test force of 20 mN, and then the particle diameter B when the load is removed to the minimum test force of 0.3 mN. The following formula for calculating the recovery rate is used from the displacement (recovery amount) L obtained from particle diameter A and particle diameter B, and the diameter d measured with the particle diameter measurement cursor. Restoration rate (%) = restoration amount L (μm) / diameter d (μm) × 100 The restoration rate of each resin particle is calculated by the above method. The restoration rates of three resin particles are measured, and the average value is taken as the restoration rate.
[0057] <Conditions for measuring restoration rate> Test temperature: Room temperature (20℃), relative humidity 65% Upper pressure indenter: Flat indenter with a diameter of 50 μm (material: diamond) Lower pressure plate: SKS flat plate Test type: Load-unload test Maximum test force: 20mN Minimum test force: 0.3mN Load speed: 4.5mN / sec Load holding time: 3sec Unloading holding time: 1min
[0058] [Average particle size of resin particles] The average particle size of the resin particles shown in Table 2 is the average particle size d50 measured using a laser diffraction particle size distribution analyzer.
[0059] [Evaluation of light-shielding film] The light-shielding films obtained in the examples and comparative examples were evaluated for optical density, processability, and glossiness. The results are shown in Table 3.
[0060] [Evaluation items] 1.Optical density The optical density of the obtained light-shielding film was measured. The optical density was measured using an optical densitometer (361T tabletop transmission densitometer: manufactured by X-RITE). An optical density of 6 or more was marked as "◎◎", an optical density of less than 6 and 4 or more was marked as "◎", and an optical density of less than 4 was marked as "◯".
[0061] 2. Processability The processability of the obtained light-shielding film was evaluated by folding the light-shielding film. The light-shielding film was folded in half so that the surface that was not in contact with the peelable substrate was concave, and the folded part was ironed back and forth once. If cracks were visible at the fold of the light-shielding film at this point, it was marked as "X". Next, the folded part was folded in half on the opposite side (i.e., folded in half so that the surface of the light-shielding film that was not in contact with the peelable substrate was convex), and the folded part was rubbed back and forth once. If cracks were visible at the fold of the light-shielding film at this point, it was rated as "△". The bending up to this point was counted as one set, and for those that showed no visible cracks in the folds of the light-blocking film in the first set, two more sets of bending were performed (total of three sets), and those in which cracks were visible in the folds of the light-blocking film were marked with an "O". After a total of five sets, those in which cracks were visible in the folds of the light-blocking film were marked with an "◎", and those in which there were no cracks in the folds of the light-blocking film after a total of five sets were marked with an "◎◎".
[0062] 4. Glossiness The glossiness of the surface of the obtained light-shielding film that was not in contact with the peelable substrate was measured. The glossiness was obtained by measuring at a measurement angle (θ) of 60 degrees using a glossmeter (VG-8000: manufactured by Nippon Denshoku Industries Co., Ltd.). A glossiness of 1 or less was evaluated as "◎", a glossiness of more than 1 and less than 3 was evaluated as "◯", a glossiness of more than 3 and less than 5 was evaluated as "△", and a glossiness of more than 5 was evaluated as "×".
[0063] 5.Reflection from processed end surface The obtained light-shielding film was punched out using a press die, and the degree of reflection at the end face after punching was observed. Using a digital microscope (VHX-7000: manufactured by Keyence), the processed end face was placed on an observation stage so that it was horizontal, and a coaxial incident light was applied from above the end face in a vertical direction with a brightness setting of 100, and a color image of the end face was taken at an observation magnification of 500 times. In order to make it easier to observe the whitish reflective parts observed in the color images (e.g., Fig. 1(a) and Fig. 2(a)), the obtained color images were binarized (black and white) using image processing software (specifically, GIMP-2.0, which is free software) (e.g., Fig. 1(b) and Fig. 2(b)), and the proportion of the area of the white parts was calculated. The white parts were the parts where light was strongly reflected, and the proportion of the white parts less than 5% was marked as "○", 5% to less than 10% was marked as "△", and 10% or more was marked as "×".
[0064] 6. Durability of light-shielding film The obtained light-shielding film was left to stand for 500 hours in an environment of 60°C and 90% relative humidity, and the presence or absence of deformation of the light-shielding film after the test was observed. Films that showed no deformation were rated "Good", those that showed slight deformation were rated "Good", and those that showed deformation were rated "Poor".
[0065] [Table 1]
[0066] [Table 2]
[0067] [Table 3]
[0068] As shown in Table 3, the light-shielding film of the present invention has a light-shielding layer containing a binder resin, a black pigment, and resin particles. By using resin particles with a restoration rate of 10% or more, it was confirmed that the glossiness of the light-shielding layer surface can be reduced while maintaining the processability of the light-shielding layer, and the reflection of the processed edge surface can be reduced, resulting in good results. [Industrial Applicability]
[0069] The light-shielding film of the present invention has excellent processability even when it is a single layer of a light-shielding layer, so it can be made small, thin and lightweight.In addition, even when the light-shielding film has a substrate, it can be evaluated in the same way as when it is a single layer of a light-shielding layer.From these results, the light-shielding film of the present invention can be suitably used for optical components such as shutters and aperture members of optical instruments such as high-performance single-lens reflex cameras, compact cameras, video cameras, mobile phones and projectors.
Claims
1. A light-shielding film having a light-shielding layer containing a binder resin, a black pigment, and resin particles, the resin particles having a restoration rate of 10% or more and 95% or less. Light-blocking film.
2. 2. The light-shielding film according to claim 1, wherein the resin particles are acrylic resin particles.
3. 3. The light-shielding film according to claim 1, wherein the 60° gloss of one of the surfaces of the light-shielding layer is 5 or less in a specular gloss measurement method according to JIS Z8741.
4. The light-shielding film according to claim 1 or 2, which consists of the light-shielding layer alone.
5. 3. The light-shielding film according to claim 1 or 2, which is for use as an optical member.
Citation Information
Patent Citations
Light shielding film, manufacturing method thereof, and application therefor
JP2012194514A
Cited By
Light-shielding film and lens unit
JP2026095134A