Foam particle and method for producing the same
A method for producing expanded particles with specific resin compositions and ethylene propylene rubber enhances moldability and compressive strength, addressing the limitations of using post-consumer polypropylene resin in foamed particles.
Patent Information
- Application Number
- JP2023061453
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
The moldability and compressive strength of foamed particles produced from polypropylene resin derived from post-consumer materials are inadequate for effective in-mold molding.
A method for producing expanded particles using a polypropylene resin composition with specific melting points, flexural moduli, and mass ratios, combined with ethylene propylene rubber, to enhance moldability and compressive strength.
The method enables the production of foamed particles with improved in-mold moldability and excellent compressive strength, effectively utilizing resin components from post-consumer materials.
Smart Images

Figure 2024148365000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an expanded bead and a method for producing the same. [Background technology]
[0002] Polypropylene resin expanded bead molded articles are lightweight and have excellent shock-absorbing properties and rigidity, and are therefore used in various applications such as packaging materials, containers, and cushioning materials. Polypropylene resin expanded bead molded articles are produced, for example, by a method called in-mold molding, in which polypropylene resin expanded beads are filled into a mold and heated with steam. In the in-mold molding method, when steam is supplied into the mold to heat the expanded beads, the expanded beads soften and undergo secondary expansion. As a result, the expanded beads in the mold are fused to each other, and a molded article having a desired shape corresponding to the shape of the cavity of the mold can be obtained.
[0003] In recent years, post-consumer materials have been attracting attention from the viewpoint of reducing the environmental load. Examples of post-consumer materials containing polypropylene resins include polypropylene resin parts recovered from used home appliances and automobiles, and automobile shredder residue (hereinafter referred to as "ASR") generated during the disposal of automobiles, as described in Patent Document 1. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-122299 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when polypropylene-based resins contained in post-consumer materials are used as raw materials for expanded beads, there is room for improvement in the moldability when the expanded beads are molded in a mold and in the compressive strength of the resulting expanded bead moldings.
[0006] The present invention has been made in view of the above background, and aims to provide expanded beads and a manufacturing method thereof that can effectively utilize resin components derived from post-consumer materials, have good in-mold moldability, and can give expanded bead moldings having excellent compressive strength. [Means for solving the problem]
[0007] One aspect of the present invention resides in the method for producing expanded beads according to the following items (1) to (7). [1] A method for producing expanded beads by expanding polypropylene-based resin beads to obtain expanded beads, comprising the steps of: The resin particles contain a polypropylene-based resin composition a derived from post-consumer materials and have a melting point Tm A is 160°C or more, and the flexural modulus M A A polypropylene resin composition A having a melting point Tm B is less than 160°C, and the flexural modulus M B and polypropylene-based resin B having a modulus of 900 MPa or more and 1400 MPa or less, The bending elastic modulus M A The bending modulus M B Ratio of M B / M A is 1 or more, The method for producing expanded beads, wherein a mass ratio of the polypropylene resin composition A to the polypropylene resin B in the resin beads is polypropylene resin composition A:polypropylene resin B=10:90 to 70:30.
[0008] [2] The resin particles have a melting point Tm r is 150°C or more and 162°C or less, and the flexural modulus M rThe method for producing expanded beads according to [1], wherein the expanded beads are composed of a polypropylene-based resin composition r having a modulus of elasticity of 900 MPa or more and 1300 MPa or less. [3] The melting point Tm of the polypropylene resin composition A A and the melting point Tm of the polypropylene resin B B Difference from Tm A -Tm B The method for producing expanded beads according to [1] or [2], wherein the temperature is 5°C or higher and 20°C or lower. [4] The method for producing expanded beads according to any one of [1] to [3], wherein the polypropylene resin composition A has a melt mass flow rate of 10 g / 10 min or more and 40 g / 10 min or less when measured at a temperature of 230° C. under a load of 2.16 kg.
[0009] [5] The method for producing expanded beads according to any one of [1] to [4], wherein the polypropylene-based resin composition A exhibits a morphology in which a polypropylene-based resin is a matrix and a rubber-like body containing an ethylene-propylene-based rubber is a domain. [6] The bulk density of the expanded particles is 10 kg / m 3 More than 200kg / m 3 The method for producing expanded beads according to any one of [1] to [5] below. [7] The method for producing expanded beads according to any one of [1] to [6], wherein the expanded beads have a closed cell rate of 90% or more.
[0010] Another aspect of the present invention is the expanded beads according to the following items [8] to
[10] .
[0011] [8] A polypropylene-based resin composition a derived from post-consumer materials, having a melting point Tm R is 150°C or more and 162°C or less, and the flexural modulus M R The expanded particles are composed of a polypropylene-based resin composition R having a compressive strength of 900 MPa or more and 1,300 MPa or less. [9] The bulk density of the expanded particles is 10 kg / m 3 More than 200kg / m 3 The expanded particles according to [8], which are as follows:
[10] The expanded beads according to [8] or [9], wherein the expanded beads have a closed cell rate of 90% or more. Effect of the Invention
[0012] According to the above-mentioned aspect, it is possible to provide expanded beads and a manufacturing method thereof that can effectively utilize resin components derived from post-consumer materials, have good moldability within a mold, and can give expanded bead moldings having excellent compressive strength. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is an explanatory diagram showing a method for calculating the heat of fusion of a high-temperature peak. [Diagram 2] FIG. 2 is an electron microscope photograph of a cross section of the polypropylene resin composition A1 in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (Method of manufacturing expanded beads) [Polypropylene-based resin particles] In the method for producing the expanded beads, first, polypropylene-based resin beads made of a polypropylene-based resin composition are prepared. The resin beads contain a polypropylene-based resin composition a derived from post-consumer materials and have a melting point Tm A is 160°C or more, and the flexural modulus M A A polypropylene resin composition A having a melting point Tm B is less than 160°C, and the flexural modulus M B The composition is a molten mixture of polypropylene resin B having a modulus of 900 MPa or more and 1,400 MPa or less.
[0015] Polypropylene resin composition A The polypropylene resin composition A used for the resin particles (hereinafter referred to as "resin composition A") has a melting point Tm of 160°C or higher. A The flexural modulus M of the resin composition A is Ais 800 MPa or more and 1200 MPa or less. In this specification, the polypropylene resin composition refers to a resin composition containing a polypropylene resin as a main component. The mass ratio of the polypropylene resin in the polypropylene resin composition is preferably 50 mass% or more, more preferably 60 mass% or more, and further preferably 70 mass% or more.
[0016] The melting point of the resin composition A is determined based on JIS K7121:1987. Specifically, first, a test piece made of the resin composition A is prepared, and the condition of the test piece is adjusted based on "(2) When the melting temperature is measured after a certain heat treatment" in "3. Conditioning of the test piece" in JIS K7121:1987. The heating rate and cooling rate in the condition adjustment are both 10°C / min. The condition-adjusted test piece is heated from 30°C to 230°C at a heating rate of 10°C / min to obtain a DSC curve, and the apex temperature of the melting peak that appears on the DSC curve is taken as the melting point. In addition, when multiple melting peaks appear on the DSC curve, the apex temperature of the melting peak with the highest height based on the baseline is taken as the melting point of the resin composition A.
[0017] From the viewpoint of further increasing the moldability of the expanded beads in a mold and widening the range of molding pressures in which a good expanded bead molded article (hereinafter referred to as a "molded article") can be obtained, it is preferable to set the melting point Tm A It is preferable that the heating temperature is 165° C. or less.
[0018] The flexural modulus M of the resin composition A A In order to more reliably improve the moldability of the foamed beads in the mold, the flexural modulus M of the resin composition A is preferably 800 MPa or more and 1200 MPa or less. A The flexural modulus M of the resin composition A is more preferably 900 MPa or more and 1100 MPa or less, and further preferably 950 MPa or more and 1050 MPa or less. A can be calculated based on JIS K7171:2008.
[0019] Resin composition A contains at least a polypropylene-based resin composition a derived from a post-consumer material. From the viewpoint of effective use of resources and material recycling, resin composition A preferably contains polypropylene-based resin composition a derived from a post-consumer material as a main component. More specifically, the mass ratio of polypropylene-based resin composition a derived from a post-consumer material in resin composition A is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0020] In this specification, the polypropylene-based resin refers to a homopolymer of a propylene monomer (i.e., a propylene homopolymer), a propylene-based copolymer containing 70% by mass or more of a structural unit derived from propylene, and a mixture of the propylene homopolymer and the propylene-based copolymer. The propylene-based copolymer may be a copolymer of propylene and ethylene and / or an α-olefin having 4 or more carbon atoms. In addition, the total content of the structural unit derived from ethylene and the structural unit derived from an α-olefin having 4 or more carbon atoms in the propylene-based copolymer is preferably 1 to 15% by mass, more preferably 2 to 12% by mass. In addition, the polypropylene-based resin and an elastomer such as an ethylene-propylene-based rubber are different substances, and in this respect, the polypropylene-based resin is distinguished from a polypropylene-based resin composition containing an ethylene-propylene-based rubber such as impact polypropylene. The presence of the ethylene-propylene-based rubber or the like can be confirmed, for example, by preparing an observation sample by electronically staining a section made from the polypropylene-based resin composition or the like, and observing the observation sample with a transmission electron microscope.
[0021] In this specification, post-consumer materials refer to "materials discarded from households, or materials generated as products that can no longer be used for their original purposes by commercial facilities, industrial facilities, and various facilities that are end users of products," as described in JIS Q14021:2000. Post-consumer materials also include materials returned from distribution channels.
[0022] More specifically, the post-consumer materials include, for example, post-consumer materials derived from automobile parts and post-consumer materials derived from home appliances. Examples of post-consumer materials derived from automobile parts include exterior materials such as bumpers and interior materials such as instrument panels removed from used automobiles, and ASR (i.e., automobile shredding residue) generated during the disposal of automobiles. The polypropylene-based resin composition a is recovered from such post-consumer materials. The main component of the polypropylene-based resin composition a is preferably impact polypropylene in which a rubber-like body containing an ethylene propylene-based rubber is dispersed in a polypropylene-based resin having a melting point of 160°C or higher.
[0023] From the viewpoint of effective resource utilization and material recycling, the main component of the polypropylene-based resin composition a is preferably derived from an automobile component. From the same viewpoint, the resin composition A preferably contains the polypropylene-based resin composition a1 recovered from ASR as the main component. More specifically, the mass ratio of the polypropylene-based resin composition a1 recovered from ASR in the resin composition A is preferably 50 mass% or more, more preferably 60 mass% or more.
[0024] The polypropylene resin composition a1 recovered from ASR contains, as a main component, a polypropylene resin that has been subjected to heat history due to molding processing for forming automobile parts. In addition, the polypropylene resin composition recovered from ASR usually contains polypropylene resins recovered from many automobile parts and many used automobiles. For these reasons, it has been considered difficult to use the polypropylene resin composition a1 recovered from ASR for producing expanded beads. In contrast, in the above-mentioned production method, by mixing the resin composition A and the resin B at the specific mass ratio, good expanded beads can be easily produced even when the polypropylene resin composition a1 recovered from ASR is used as a raw material.
[0025] In this specification, ASR refers to "automobile shredding residue" defined in Article 2-5 of the "Law on Recycling, etc. of End-of-Life Vehicles" (Law No. 87 of 2002). More specifically, ASR refers to the material remaining after dismantling an end-of-life vehicle after removing recyclable parts such as engines and batteries, separating metals and other useful materials from the shredded material, and recovering them. In addition to polypropylene-based resins derived from automobile parts, ASR usually contains other plastics and rubbers other than polypropylene-based resins such as polystyrene (PS) and acrylonitrile-butadiene-styrene resin (ABS), various metals, etc. The method of recovering the polypropylene-based resin composition a1 mainly composed of polypropylene-based resin from ASR is not particularly limited, and polypropylene-based resins can be recovered from ASR by appropriately combining known sorting methods.
[0026] An example of a method for obtaining ASR includes a dismantling process for removing reusable and non-reusable parts from used automobiles, an accessory separation process for removing automobile accessories from the dismantled automobiles that have been through the dismantling process, and a crushing and sorting process for crushing the dismantled automobiles and / or automobile accessories that have been through the separation process, separating metals from the resulting crushed material, and recovering ASR. More specifically, ASR can be obtained by the methods described in Patent Nos. 6609877, 6627142, 6762071, etc.
[0027] The method for recovering the polypropylene-based resin composition a1 from the ASR is not particularly limited, and the polypropylene-based resin composition a1 can be recovered from the ASR by appropriately combining known sorting methods. For example, the polypropylene-based resin composition a1 can be recovered by a method in which the following sorting steps (α) to (δ) are carried out alone or in combination of two or more. (α) A magnetic separation process in which metals and non-metals are separated by magnetic force. (β) Wind sorting process to separate light and heavy objects by wind force (γ) A wet gravity separation process in which light and heavy materials are separated using a solvent (δ) Electrostatic sorting process to sort resins based on their ease of charging
[0028] For example, in the wet specific gravity sorting step (γ), the polypropylene-based resin composition a1 contained in the ASR can be sorted by a method using water flow classification and sedimentation velocity as described in Japanese Patent No. 3711472, or a method using an apparatus having a pulsating bubbling tank and a sedimentation tank for intermittently discharging air bubbles and a floating matter separation tank for separating substances lighter than water and substances heavier than water as described in Japanese Patent Laid-Open No. 2004-58032. In addition, as described in Japanese Patent Laid-Open No. 2008-178846 and Japanese Patent No. 6762071, these sorting steps can be performed in combination. For example, the wind sorting step and the wet specific gravity sorting step can be combined to separate the light and heavy substances contained in the ASR by wind force, and then immersing each of them separately in a sorting liquid for specific gravity sorting to sort the polypropylene-based resin composition a1 contained in the ASR.
[0029] Melt mass flow rate (MFR) of resin composition A measured at a temperature of 230°C and a load of 2.16 kg A Preferably, the resin composition A has a viscosity of 10 g / 10 min or more and 40 g / 10 min or less, more preferably, the resin composition A has a viscosity of 14 g / 10 min or more and 35 g / 10 min or less, and further preferably, the resin composition A has a viscosity of 20 g / 10 min or more and 30 g / 10 min or less. In this case, while containing a resin component derived from a post-consumer material, the moldability of the expanded beads in the mold can be further improved, and the range of molding pressures under which a good expanded bead molding can be obtained can be wider.
[0030] The melt mass flow rate MFR of the above-mentioned resin composition A A is a value measured based on JIS K7210-1:2014 under conditions of a test temperature of 230°C and a load of 2.16 kg.
[0031] The ash content of the resin composition A is preferably 1% by mass or more and 25% by mass or less. In this case, the MFR of the resin composition A is AEven when the pressure is relatively high, the moldability of the expanded beads in a mold can be improved while maintaining the expandability of the resin beads, and the range of molding pressures within which a good expanded bead molded article can be obtained can be broadened.
[0032] The reason why the above-mentioned action and effect can be obtained by using the resin composition A having an ash content within the above-mentioned specific range is, for example, as follows. From the viewpoint of enhancing the expandability of the resin particles, it is preferable to use a polypropylene-based resin having a relatively high melt mass flow rate. However, the expanded particles obtained using the polypropylene-based resin having a high melt mass flow rate have a problem that the molded body is likely to shrink when molded in a mold at a high molding pressure, probably because the resin is likely to be excessively stretched during molding in the mold. In contrast, by using the resin composition A having an ash content within the above-mentioned specific range, the bubble diameter of the expanded beads can be made relatively small and the bubble film can be made thin. And, it is considered that such expanded beads are likely to be softened by heating, while the resin is unlikely to be excessively stretched. Therefore, it is considered that by using the resin composition A having an ash content within the above-mentioned specific range, the shrinkage of the molded body can be suppressed even when molding in a mold at a high molding pressure, and the moldable range can be widened while maintaining the expandability of the resin particles.
[0033] The ash content of the resin composition A is more preferably 2% by mass or more, and further preferably 3% by mass or more. In this case, a polypropylene-based resin composition having a relatively high ash content, such as the polypropylene-based resin composition a derived from post-consumer materials, can be more easily blended, and the resin component derived from the post-consumer material can be more easily utilized.
[0034] Furthermore, from the viewpoint of maintaining the expandability of the resin particles while further improving the in-mold moldability of the expanded particles, the ash content of resin composition A is more preferably 20 mass% or less, even more preferably 15 mass% or less, even more preferably 10 mass% or less, particularly preferably 8 mass% or less, and most preferably 6 mass% or less.
[0035] The above-mentioned upper limit and lower limit of the ash content can be combined arbitrarily to define a preferred range of the ash content of the resin composition A. For example, the preferred range of the ash content of the resin composition A may be 1% by mass or more and 20% by mass or less, 2% by mass or more and 15% by mass or less, 2% by mass or more and 10% by mass or less, 3% by mass or more and 8% by mass or less, or 3% by mass or more and 6% by mass or less.
[0036] The ash content of the resin composition A can be measured in accordance with the direct incineration method (method A) of JIS K7250-1:2006. More specifically, the ash content of the resin composition A can be calculated from the mass of the residue remaining after burning the resin composition A. The ash content contained in the combustion residue of the resin composition A is mainly composed of inorganic substances contained in the resin composition A, such as inorganic fillers.
[0037] The resin composition A preferably contains an ethylene propylene-based rubber, and more preferably contains an ethylene propylene-based rubber derived from a post-consumer material. In this case, it is more preferable that the resin composition A exhibits a morphology in which a polypropylene-based resin is a matrix (i.e., a continuous phase) and a rubber-like body containing an ethylene propylene-based rubber is a domain (i.e., a dispersed phase). In this case, even if the amount of the polypropylene-based resin composition a derived from a post-consumer material is relatively large, expanded beads having good moldability in a mold can be stably obtained. Furthermore, by performing molding in a mold using the expanded beads, a molded body having good mechanical properties such as compressive strength can be easily obtained. In this case, it is more preferable that the melting point of the polypropylene-based resin constituting the matrix is 160°C or higher. Furthermore, the domain of the rubber-like body in the resin composition A may contain a polyethylene-based resin in addition to the ethylene propylene-based rubber.
[0038] The ethylene propylene rubber is a rubber-like material composed of an ethylene propylene copolymer containing an ethylene component and a propylene component. That is, the ethylene propylene rubber may be a copolymer of ethylene and propylene (that is, EPM). The ethylene propylene rubber may also be an ethylene propylene copolymer (e.g., EPDM) containing a component derived from a monomer other than ethylene and propylene, such as a diene, within a range that does not impair the above-mentioned action and effect. In the ethylene propylene rubber, the mass ratio of the component derived from ethylene to the component derived from propylene (component derived from ethylene:component derived from propylene) is usually 30:70 to 80:20. Whether or not the resin composition A contains an ethylene propylene rubber can be confirmed by observing the morphology of the resin composition A.
[0039] The method for observing the morphology of the resin composition A is as follows. First, a sample for observation is cut out from the resin composition A. There is no particular limitation on the method for cutting out the sample for observation. For example, when the shape of the resin composition A is a cylindrical pellet, the pellet may be cut perpendicularly to the height direction of the pellet so as to pass through the center of the pellet. In this way, a sample for observation in which the cross section of the center of the pellet made of the resin composition A is exposed can be obtained. Next, the sample for observation is embedded in an epoxy resin, and after performing electronic staining with ruthenium tetroxide, a slice is prepared from the sample using an ultramicrotome or the like. The slice is placed on the grid of a transmission electron microscope (for example, "JEM-1040Flash" manufactured by JEOL Ltd.) and observed at a predetermined magnification (for example, 5000 times), and a cross-sectional photograph (i.e., a TEM photograph) of the resin composition A is taken. From the cross-sectional photograph, the morphology of the polypropylene resin phase and the rubber-like body phase containing the ethylene propylene rubber in the resin composition A is visually observed.
[0040] From the viewpoint of stably increasing the moldability of the foamed beads in the mold, the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber in the resin composition A is preferably 0.5 μm or more and 5 μm or less, more preferably 0.8 μm or more and 3 μm or less, and even more preferably 1 μm or more and 2 μm or less. The average diameter of the domains is calculated based on the TEM photograph. Specifically, the longest diameter and the shortest diameter of 50 or more domains randomly selected from the domains appearing in the TEM photograph are measured, and then the arithmetic mean of these is calculated. The arithmetic mean value of the longest diameter and the shortest diameter thus obtained is regarded as the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber.
[0041] From the viewpoint of stably increasing the moldability of the expanded beads in the mold, the area ratio of the domains in the morphology is preferably 20% or more and 40% or less, and more preferably 25% or more and 35% or less.
[0042] The area ratio of the domains is calculated based on the TEM photograph. More specifically, using image analysis software (for example, "WinROOF2013" manufactured by Mitani Shoji Co., Ltd.), monotone processing is performed to make the domain parts in the TEM photograph black and the parts other than the domains white, and the measurement object is taken. Then, the image analysis software is used to calculate the total area occupied by the domain parts in the measurement object, and the ratio of the total area occupied by the domain parts to the total area of the measurement object is calculated. The ratio of the total area occupied by the domain parts thus obtained is taken as the area ratio of the domains in the morphology of resin composition A. The parts other than the domains include inorganic substances such as matrix and talc.
[0043] When the resin composition A has the specific morphology, from the viewpoint of more reliably obtaining the above-mentioned action and effect, the amount of the component contained in the resin composition A that is soluble in decane at 23° C. and insoluble in acetone (hereinafter also referred to as "23° C. n-decane solubles"), that is, the amount of the acetone insolubles contained in the extract when the soluble components in the resin composition A are extracted in n-decane at 23° C., is more preferably 5% by mass to 30% by mass, even more preferably 6% by mass to 25% by mass, and particularly preferably 8% by mass to 20% by mass. The 23° C. n-decane solubles in the resin composition A are mainly components derived from ethylene propylene rubber.
[0044] The method for measuring the 23°C n-decane soluble content in the resin composition A is as follows. First, a sample made of the resin composition A is added to n-decane and heated to dissolve the soluble content in the resin composition A in the n-decane. After cooling the n-decane solution to 23°C, the insoluble content in the n-decane solution is removed to obtain a filtrate. The filtrate is added to acetone to precipitate the 23°C n-decane soluble content in the resin composition A. Based on the mass of the precipitate obtained as described above, the 23°C n-decane soluble content in the resin composition A can be calculated. A more detailed method for measuring the 23°C n-decane soluble content in the resin composition A will be described in detail in the Examples.
[0045] The resin composition A may contain resins other than polypropylene-based resins and elastomers other than ethylene propylene-based rubbers, etc., within the scope that does not impair the above-mentioned action and effect. Examples of resins that can be contained in the resin composition A include polystyrene-based resins, polyethylene-based resins, and acrylonitrile-butadiene-styrene resins, and examples of elastomers include ethylene butene rubber and ethylene octene rubber. These resins and elastomers may be derived from post-consumer materials.
[0046] The resin composition A may contain inorganic substances such as talc, silica, and glass fiber within a range that does not impair the above-mentioned action and effect. The main component of the inorganic substances contained in the resin composition A is preferably talc. In this case, even when a resin composition A having a relatively high melting point is used, the fusibility of the expanded beads can be further improved. As a result, the moldability of the expanded beads in the mold can be further improved. The reason for this is thought to be that the average cell diameter of the expanded beads tends to be small, etc.
[0047] The resin composition A may contain additives such as a cell regulator, a crystal nucleating agent, a flame retardant, a flame retardant assistant, a plasticizer, an antistatic agent, an antioxidant, an ultraviolet absorber, a light stabilizer, an antibacterial agent, and a colorant, within a range that does not impair the above-mentioned action and effect. In addition, the resin composition A preferably contains carbon black as a colorant. In this case, for example, the content of carbon black in the resin composition A may be 0.1% by mass or more and 2% by mass or less, or 0.2% by mass or more and 1% by mass or less. By setting the content of carbon black in the resin composition A within the above-mentioned specific range, it is possible to obtain an expanded bead molding having excellent design, which is provided with a mottled pattern of relatively light black (gray) and white.
[0048] Polypropylene resin B The polypropylene resin B used in the resin particles has a melting point Tm of less than 160°C. B The flexural modulus of resin B is M B In the above-mentioned manufacturing method, the melting point Tm A and bending modulus M A Resin composition A having a melting point Tm B and bending modulus M BThe resin particles are made of a molten mixture of resin composition A and resin B, in which the ratio of the flexural modulus of resin B to the flexural modulus of resin composition A satisfies a specific relationship, and the mass ratio of resin composition A to resin B is within the above-mentioned specific range, whereby expanded beads having excellent moldability in a mold can be easily obtained. From the viewpoint of more reliably obtaining such an effect, it is preferable that the melting point Tm of resin B is set to 100° C. B The temperature is preferably 140°C or higher and lower than 160°C, more preferably 142°C or higher and 158°C or lower, even more preferably 145°C or higher and 156°C or lower, and particularly preferably 148°C or higher and 155°C or lower.
[0049] Melting point Tm of resin B B If the flexural modulus M of resin B is too high, it may be difficult to obtain resin particles having good expandability or expanded particles having good moldability in a mold. B If the content is excessively outside the above-mentioned specific range, it may be difficult to obtain resin particles having good expandability or expanded beads having good moldability in a mold.
[0050] Melting point Tm of resin B B is determined based on JIS K7121:1987. Specifically, first, a test piece made of resin B is prepared. At this time, when two or more types of polypropylene resins are used as resin B in producing the resin particles, the multiple types of polypropylene resins are melt-mixed so that the mass ratio is the same as the mass ratio in the resin particles, and a test piece made of a molten mixture of these polypropylene resins is prepared.
[0051] Next, the test piece is conditioned based on "(2) Measurement of melting temperature after a certain heat treatment" in "3. Conditioning of test piece" in JIS K7121:1987. The heating rate and cooling rate in the conditioning are both 10°C / min. The conditioned test piece is heated from 23°C to 230°C at a heating rate of 10°C / min to obtain a DSC curve, and the apex temperature of the melting peak that appears on the DSC curve is the melting point Tm of resin B. BIn addition, when multiple melting peaks appear on the DSC curve, the melting point Tm is determined as the apex temperature of the melting peak with the highest melting peak height relative to the baseline. B Let us assume that.
[0052] From the viewpoint of making it easier to obtain foamed beads with excellent moldability in the mold, the flexural modulus M B The flexural modulus M of resin B is preferably 950 MPa or more and 1350 MPa or less, more preferably 1000 MPa or more and 1300 MPa or less, and even more preferably 1100 MPa or more and 1300 MPa or less. B can be calculated based on JIS K7171:2008.
[0053] Resin B may be a polypropylene-based resin that has not been subjected to a thermal history due to molding or the like for forming a molded product (i.e., a non-recycled polypropylene-based resin), or may be a polypropylene-based resin that has been subjected to a thermal history (i.e., a recycled polypropylene-based resin). From the viewpoint of being able to more easily obtain expanded beads with excellent moldability in a mold, it is preferable that resin B be a non-recycled polypropylene-based resin.
[0054] In addition, in the production of resin particles, one type of polypropylene resin may be used as resin B, or two or more types of polypropylene resins may be used. In addition, when two or more types of polypropylene resins are used as resin B, the melting point of a sample obtained by melt-mixing these polypropylene resins in the same mass ratio as that in the production of resin particles is defined as the melting point Tm of resin B. B The bending modulus of the sample is the bending modulus of resin B M B Let us assume that.
[0055] Resin B used in the production of resin particles is preferably a propylene-based copolymer containing 70% by mass or more of structural units derived from propylene, more preferably a propylene-based copolymer containing 80% by mass or more of structural units derived from propylene. Note that Resin B may contain two or more kinds of propylene-based copolymers.
[0056] From the viewpoint of further improving the moldability of the expanded beads in a mold and broadening the range of molding pressures at which a good expanded bead molding can be obtained, it is preferable that resin B is a copolymer of propylene with ethylene and / or an α-olefin having 4 or more carbon atoms. Moreover, it is more preferable that the copolymer is a random copolymer (i.e., a propylene-based random copolymer).
[0057] Examples of the α-olefin used in the propylene-based copolymer include 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-butene, etc. In the propylene-based copolymer, the total content of the structural units derived from ethylene and the structural units derived from the α-olefins having 4 or more carbon atoms (i.e., the content of the comonomer components) is preferably 1% by mass or more and 15% by mass or less, more preferably 2% by mass or more and 12% by mass or less.
[0058] When two or more polypropylene resins are used as resin B, the content of the comonomer component is defined as the ratio of the mass of the comonomer component to the total mass of these polypropylene resins (i.e., the total mass of resin B). In other words, when two or more polypropylene resins are used as resin B, the content of the comonomer component is the sum of the content of the ethylene-derived structural unit and the content of the structural unit derived from an α-olefin having 4 or more carbon atoms in a sample obtained by melt-mixing multiple polypropylene resins in the same mass ratio as that used in producing the resin particles.
[0059] The main component of the resin B is preferably a polypropylene-based resin b1 containing a structural unit derived from ethylene (i.e., an ethylene component) as a copolymerization component and / or a polypropylene-based resin b2 containing a structural unit derived from ethylene and 1-butene (i.e., an ethylene component and a butene component) as a copolymerization component. Examples of such polypropylene-based resin b1 include a propylene-ethylene random copolymer. Examples of the polypropylene-based resin b2 include a propylene-ethylene-butene random copolymer. The sum of the proportion of the polypropylene-based resin b1 and the proportion of the polypropylene-based resin b2 relative to the total mass of the resin B contained in the resin particles is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0060] When the resin B contains a polypropylene-based resin b1 as a main component, the content of the ethylene component in the polypropylene-based resin b1 is preferably 1% by mass or more, more preferably 2% by mass or more, in which case the moldability of the expanded beads in the mold can be further improved when the molding is performed in the mold at a low molding pressure.
[0061] The content of the ethylene component in the polypropylene resin b1 is preferably 6% by mass or less, more preferably 5% by mass or less, further preferably 4% by mass or less, and particularly preferably 3% by mass or less, in which case it is easier to obtain an expanded bead molding having good compressive strength, etc.
[0062] When the resin B contains a polypropylene resin b2 as a main component, the total content of the ethylene component and the butene component in the polypropylene resin b2 is preferably 2% by mass or more, more preferably 4% by mass or more, and even more preferably 6% by mass or more. In this case, the moldability of the expanded beads in the mold can be further improved when the molding is performed in the mold at a low molding pressure.
[0063] The total content of the ethylene component and the butene component in the polypropylene resin b2 is preferably 15% by mass or less, more preferably 12% by mass or less, which makes it easier to obtain an expanded bead molding having good compressive strength and the like.
[0064] In addition, from the viewpoint of enabling molding at a relatively low molding pressure and making it easier to obtain an expanded bead molding having good compressive strength, etc., the ratio of the butene component content to the ethylene component content in the polypropylene-based resin b2 is preferably 7 or more and 25 or less, more preferably 8 or more and 20 or less, and even more preferably 10 or more and 18 or less.
[0065] The contents of the ethylene-derived component and the butene-derived component in the resin B can be determined, for example, based on an IR spectrum. The method for measuring the contents of the ethylene-derived component and the butene-derived component in the resin B will be described in detail in the Examples.
[0066] In configuring a preferred range for the content of the comonomer component in Resin B, the above-mentioned upper limit value and lower limit value can be combined arbitrarily.
[0067] The ash content of resin B is preferably less than 1% by mass, and more preferably 0.5% by mass or less. In this case, the moldability of the expanded beads in the mold can be improved while maintaining the expandability of the resin beads, and the range of molding pressure at which a good expanded bead molding can be obtained can be broadened. When two or more types of polypropylene-based resins are used as resin B, the ratio of the total mass of the ash of the polypropylene-based resins to the total mass of these polypropylene-based resins (i.e., the total mass of resin B) is the ash content of resin B. In other words, the ash content of resin B is obtained by preparing a sample by melt-mixing multiple types of polypropylene-based resins contained in resin B in the same mass ratio as that when the resin beads are produced, and measuring the ash content of this sample as described below.
[0068] The ash content of the resin B can be measured in accordance with the direct incineration method (method A) of JIS K7250-1: 2006. More specifically, the ash content of the resin B can be calculated from the mass of the residue remaining after burning the resin B.
[0069] Melt mass flow rate (MFR) of resin B measured at 230°C and a load of 2.16 kg B The melt mass flow rate MFR of resin B is preferably 6 g / 10 min or more and 9 g / 10 min or less. In this case, expanded beads having good moldability in a mold can be obtained more easily. When two or more kinds of polypropylene resins are used as resin B, the melt mass flow rate MFR of resin B is determined by melt mixing these polypropylene resins in the same mass ratio as that in the production of resin beads. B Let us assume that.
[0070] Heat of fusion of resin B H B The heat of fusion H of the polypropylene resin B is preferably 70 J / g or more and 100 J / g or less. In this case, expanded beads having excellent moldability in a mold can be more stably obtained. From the same viewpoint, the heat of fusion H of the polypropylene resin B is preferably 70 J / g or more and 100 J / g or less. B It is more preferable that the heat of fusion is 75 J / g or more and 98 J / g or less, further preferably 80 J / g or more and 96 J / g or less, and particularly preferably 85 J / g or more and 95 J / g or less. When two or more kinds of polypropylene resins are used as resin B, the heat of fusion of a sample obtained by melt-mixing these polypropylene resins in the same mass ratio as that in the production of the resin particles is defined as the heat of fusion H of resin B. B Let us assume that.
[0071] The resin B may contain additives such as a bubble adjuster, a crystal nucleating agent, a flame retardant, a flame retardant assistant, a plasticizer, an antistatic agent, an antioxidant, an ultraviolet absorber, a light stabilizer, an antibacterial agent, and a colorant, as long as the above-mentioned action and effect are not impaired.
[0072] Flexural modulus M of resin composition A A Flexural modulus M of resin B B Ratio of M B / MA is 1 or more. The flexural modulus M of the resin B to be combined with the resin composition A B By setting the ratio of the flexural modulus M within the above-mentioned specific range, it is possible to improve the moldability of the expanded beads in a mold while containing a resin component derived from post-consumer materials, and it is also possible to obtain an expanded bead molding having good compressive strength. B / M A If the flexural modulus M of the resin composition A is too low, the moldability of the expanded beads in the mold may be deteriorated. A and the flexural modulus M of resin B B can be calculated based on JIS K7171:2008.
[0073] The reason why the above-mentioned effect is obtained is considered to be, for example, as follows. The resin composition A containing the polypropylene-based resin composition a derived from post-consumer materials used in the above-mentioned production method has a melting point Tm A Flexural modulus M A The ratio of flexural modulus tends to be relatively low. When such resin composition A is used to sufficiently fuse the expanded beads during molding in a mold, the molded body tends to shrink locally after heating, making it difficult to obtain a good molded body. On the other hand, by producing resin beads using resin composition A having such a relationship between melting point and flexural modulus and resin B having a lower melting point and a relatively higher flexural modulus than resin composition A, it is considered that expanded beads capable of molding a molded body having excellent in-mold moldability and excellent compressive strength over a wide range of molding pressures can be obtained, probably because the balance between the melting point and flexural modulus in the polypropylene resin composition constituting the expanded beads is improved. From the viewpoint of more reliably obtaining the above-mentioned action and effect, the ratio of flexural modulus M B / M A is preferably 1.1 or more and 1.6 or less, and more preferably 1.2 or more and 1.5 or less.
[0074] The mass ratio of resin composition A to polypropylene-based resin B (hereinafter referred to as "resin B") in the resin particles (where the sum of the mass of resin composition A and the mass of resin B is 100 mass%) is resin composition A:resin B=10:90 to 70:30. That is, the mass ratio of resin composition A to the sum of resin composition A and resin B in the resin particles is 10 mass% or more and 70 mass% or less.
[0075] By setting the mass ratio of the resin composition A to 10% by mass or more, the amount of the polypropylene-based resin composition a derived from post-consumer materials that can be blended in the resin particles can be increased, and the resin components derived from post-consumer materials can be more effectively utilized. If the mass ratio of the resin composition A is excessively low, the amount of the polypropylene-based resin composition a that can be blended in the resin particles decreases, which is undesirable from the viewpoint of effective use of resources.
[0076] From the viewpoint of increasing the amount of polypropylene-based resin composition a that can be blended into the resin particles and making more effective use of the resin components derived from post-consumer materials, the mass ratio of resin composition A to the total of resin composition A and resin B is preferably 15 mass% or more, more preferably 20 mass% or more, even more preferably 25 mass% or more, and particularly preferably 30 mass% or more.
[0077] Moreover, by setting the mass ratio of the resin composition A to 70 mass% or less, expanded beads having good moldability in a mold and compressive strength can be easily obtained. If the mass ratio of the resin composition A is excessively high, the moldability in a mold and compressive strength of the expanded beads may be reduced. From the viewpoint of more easily obtaining expanded beads having excellent moldability in a mold and compressive strength, the mass ratio of the resin composition A to the total of the resin composition A and the resin B is preferably 65 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less.
[0078] In determining the preferred range of the mass ratio of the resin composition A, it is possible to arbitrarily combine the upper limit value and the lower limit value of the mass ratio of the resin composition A. For example, the preferred range of the mass ratio of the resin composition A to the resin B may be resin composition A:resin B=15:85 to 65:35, 20:80 to 60:40, 25:75 to 50:50, or 30:70 to 50:50.
[0079] In addition, the melt mass flow rate MFR of resin composition A A and Melt Mass Flow Rate MFR of Resin B B Difference between MFR A -MFR B is preferably 5 g / 10 min to 35 g / 10 min, more preferably 8 g / 10 min to 30 g / 10 min, and even more preferably 12 g / 10 min to 25 g / 10 min. In this case, the variation in moldability of the expanded beads in the mold can be further reduced, and expanded beads having excellent moldability in the mold can be more easily obtained.
[0080] The melting point Tm of the resin composition A A and the melting point Tm of the resin B B Difference from Tm A -Tm B The temperature is preferably from 5° C. to 20° C., more preferably from 7° C. to 19° C., and even more preferably from 10° C. to 18° C. In this case, while containing a resin component derived from post-consumer materials, the moldability of the expanded beads in the mold can be further improved, and the range of molding pressure within which a good expanded bead molded article can be obtained can be broadened.
[0081] The heat of fusion H of the polypropylene resin composition A A is 60 J / g or more and 100 J / g or less, and the heat of fusion H of the polypropylene resin B is B is 70 J / g or more and 100 J / g or less, and the heat of fusion H A and the heat of fusion H B Tonowa H A +H BThe heat of fusion H of resin composition A is preferably 150 J / g or more and 175 J / g or less. Since resin composition A contains polypropylene-based resin composition a derived from post-consumer materials, the physical properties tend to vary greatly when compared between different lots. In contrast, the heat of fusion H of resin composition A is A and the heat of fusion of resin B, H B and are within the above-mentioned specific ranges, and further, the sum of the heats of fusion H A +H B By setting the heat of fusion H of the resin composition A within the above-mentioned specific range, even when the resin composition A having a large variation in physical properties is used, expanded beads having excellent moldability in the mold can be obtained more stably. A Heat of fusion of resin B against B The ratio of H B / H A is preferably 0.90 or more and 1.20 or less.
[0082] The heat of fusion of resin composition A and resin B can be determined based on a DSC curve obtained by performing differential scanning calorimetry (DSC) in accordance with JIS K 7122:1987. Specifically, first, resin composition A or resin B is used as a test piece, and the condition of the test piece is adjusted based on "(2) When the melting temperature is measured after a certain heat treatment" in "3. Conditioning of the test piece" in JIS K 7122:1987. The heating rate and cooling rate in the condition adjustment are both 10°C / min, and the temperature range is from 23°C to 230°C. Then, the condition-adjusted test piece is heated again from 23°C to 230°C at a rate of 10°C / min to obtain a DSC curve (DSC curve at the time of the second heating). In this DSC curve, a straight line is drawn connecting the point corresponding to 80°C and the high-temperature end point of the melting peak with the highest apex temperature. The heat of fusion H of resin composition A is calculated by the following formula: A and the heat of fusion of resin B, H B can be calculated based on the area of the region enclosed by the straight line thus determined and the melting peak of the DSC curve.
[0083] [Preparation of resin particles] In the manufacturing method, first, resin particles consisting of a molten mixture of the resin composition A and the resin B are prepared. The method of preparing the resin particles is not particularly limited. For example, when preparing the resin particles by the strand cut method, the resin composition A and the resin B are fed into an extruder, and the resin composition A and the resin B are heated and kneaded in the extruder to obtain a molten mixture. This molten mixture is extruded in a strand shape from a small hole in a die attached to the downstream side of the extruder. This strand-shaped extrudate is taken up and cut to a desired length to obtain resin particles consisting of a molten mixture (more specifically, a molten kneaded product) of the resin composition A and the resin B. The resin particles thus obtained contain a polypropylene-based resin composition a derived from post-consumer materials. In addition, the melting point Tm of the polypropylene-based resin composition r constituting the resin particles is 0.01 to 0.01 mm. r is 150°C or more and 162°C or less, and the flexural modulus M r is 900MPa or more and 1300MPa or less.
[0084] The operation of producing a molten mixture of the resin composition A and the resin B and the operation of producing resin particles from the molten mixture may be performed in the same extruder as described above. Alternatively, for example, the above-mentioned two operations may be performed using separate extruders.
[0085] The resin particles may contain resins other than polypropylene resins and elastomers other than ethylene propylene rubbers, etc., within the scope of not impairing the above-mentioned effects. Examples of resins that may be contained in the resin particles include polystyrene resins, polyethylene resins, and acrylonitrile-butadiene-styrene copolymers, and examples of elastomers include ethylene butene rubber and ethylene octene rubber. These resins and elastomers may be derived from post-consumer materials.
[0086] [Foaming] In the above-mentioned manufacturing method, the polypropylene-based resin particles are expanded. The method for expanding the resin particles is not particularly limited, but it is preferable to expand the resin particles by a method called "direct expansion method" in which polypropylene-based resin particles containing a blowing agent dispersed in an aqueous medium in a container are released together with the aqueous medium into an atmosphere with a pressure lower than that in the container. A preferred embodiment of the expansion method will be described below.
[0087] When expanding resin particles by the direct foaming method, first, the resin particles are placed in a container such as a pressure vessel and dispersed in an aqueous medium. At this time, a dispersant, a dispersion aid, a surfactant, or the like may be added as necessary to disperse the resin particles in the aqueous medium in the container.
[0088] As the dispersant, inorganic fine particles such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, and mica can be used. These inorganic fine particles may be used alone, or two or more kinds of inorganic fine particles may be used in combination. As the dispersion aid, for example, aluminum sulfate or the like can be used. As the surfactant, for example, anionic surfactants such as sodium alkylbenzenesulfonate, sodium dodecylbenzenesulfonate, and sodium alkanesulfonate can be used. These surfactants may be used alone, or two or more kinds of surfactants may be used in combination.
[0089] Next, a foaming agent is supplied into the container, and the pressure in the container is increased to impregnate the resin particles with the foaming agent. This allows resin particles containing the foaming agent to be obtained. At this time, the resin particles in the container are heated together with the aqueous medium to promote the impregnation of the foaming agent into the resin particles.
[0090] Examples of the foaming agent used in the foaming step include inorganic physical foaming agents such as carbon dioxide, air, nitrogen, helium, and argon, and organic physical foaming agents such as hydrocarbons such as propane, n-butane, isobutane, n-pentane, isopentane, and hexane, and halogenated hydrocarbons such as ethyl chloride, 2,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, and trans-1-chloro-3,3,3-trifluoropropene. From the viewpoint of environmental load and ease of handling, carbon dioxide is preferably used as the foaming agent. The amount of the foaming agent added is preferably 0.1 parts by mass or more and 30 parts by mass or less, and more preferably 0.5 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the resin particles.
[0091] The pressure in the container immediately before foaming is preferably 0.5 MPa (G) or more in terms of gauge pressure. On the other hand, the pressure in the container is preferably 4.0 MPa (G) or less in terms of gauge pressure. If it is within the above range, the expanded beads can be safely produced without risk of damage or explosion of the container.
[0092] After the resin particles are impregnated with the blowing agent, the contents of the container are released into an atmosphere with a lower pressure than the container, whereby the resin particles are expanded to form a cellular structure, and are cooled by the outside air (i.e., the atmosphere) to stabilize the cellular structure, thereby obtaining expanded particles.
[0093] In the above-mentioned production method, a step of adjusting the crystal structure of the resin component constituting the resin particles may be carried out between dispersing the resin particles in an aqueous medium and expanding the resin particles. By expanding the resin particles after adjusting the crystal structure of the resin component, it is possible to easily obtain expanded beads having excellent moldability in a mold and excellent mechanical strength.
[0094] The method for adjusting the crystal structure of the resin component is, for example, as follows. First, a holding step is performed in which the temperature of the resin particles is held within a temperature range of (melting point of the molten mixture constituting the resin particles -15°C) or more and (melting point of the molten mixture +15°C) or less for a sufficient period of time, preferably about 10 to 60 minutes. By foaming the resin particles that have been subjected to this holding step, expanded particles having a crystal structure that exhibits a specific melting peak, which will be described later, can be obtained. The temperature inside the container during foaming is preferably (melting point of the molten mixture -5°C) or more and (melting point of the molten mixture +10°C) or less.
[0095] In the method for producing expanded beads, the resin particles subjected to the holding step may be prepared in advance, and the resin particles may be expanded to obtain expanded beads. From the viewpoint of increasing productivity of expanded beads, it is preferable to carry out the holding step by heating the resin particles dispersed in the dispersion medium in a container in the presence of a foaming agent, and then release the contents of the sealed container from the container into an atmosphere with a pressure lower than the pressure in the container to expand the resin particles, thereby obtaining expanded beads having a crystal structure in which a specific melting peak appears, as described later.
[0096] The reason why the mechanical strength and moldability of the expanded beads can be improved by heating and expanding under the above-mentioned conditions is thought to be that secondary crystals of the polypropylene resin are formed in the resin components constituting the expanded beads. Whether or not secondary crystals of the polypropylene resin are formed can be determined by the presence or absence of a high-temperature peak in the DSC curve. The method for determining the presence or absence of a high-temperature peak will be described later.
[0097] In the method for producing the expanded beads, when the resin particles are expanded, the resin particles may be expanded in one stage as described above, or the resin particles may be expanded in two or more stages. When the resin particles are expanded in two stages, the resin particles are expanded by a direct expansion method in the first stage expansion step to obtain the first stage expanded particles. In the second stage expansion step, for example, the first stage expanded particles are pressurized with air or the like to increase the pressure (internal pressure) in the bubbles of the first stage expanded particles, and then the first stage expanded particles are heated with steam or the like to be further expanded. By expanding the resin particles in multiple stages in this way, expanded beads having a higher expansion ratio (i.e., a lower bulk density) can be easily obtained.
[0098] (foam particles) The expanded beads obtained by the above-mentioned production method contain a polypropylene-based resin composition a derived from post-consumer materials, and have a melting point Tm R is 150°C or more and 162°C or less, and the flexural modulus M R The polypropylene resin composition R has a compressive strength of 900 MPa or more and 1300 MPa or less.
[0099] The expanded beads made of the polypropylene-based resin composition R are preferably obtained by expanding resin beads made of a molten mixture of the polypropylene-based resin composition A and the polypropylene-based resin B. In this case, the mass ratio of the resin composition A and the resin B in the polypropylene-based resin composition R is approximately the same as the mass ratio of the resin composition A and the resin B used when preparing the resin beads. The detailed configurations of the resin composition A and the resin B are as described above. In addition, the melting point Tm of the polypropylene-based resin composition R constituting the expanded beads is R and bending modulus M R The physical properties are determined by the melting point Tm of the polypropylene resin composition r constituting the polypropylene resin particles. r and bending modulus M r Therefore, the melting point Tm of the polypropylene resin composition R is approximately the same as that of the polypropylene resin composition R. R , flexural modulus M RThe melting point Tm of the polypropylene resin composition r r , flexural modulus M r It can be regarded as the same.
[0100] From the viewpoint of improving the moldability of the foamed beads in the mold, the melting point Tm R The melting point Tm of the polypropylene resin composition R is preferably 152°C or more and 161°C or less, and more preferably 155°C or more and 160°C or less. R The measurement method is the same as that of the melting point Tm of the resin composition A described above, except that the expanded beads are used as samples. A The melting point (Tm) of the polypropylene resin composition R is measured according to JIS K7121:1987. R can be sought.
[0101] In addition, from the viewpoint of improving the moldability of the expanded beads in the mold, the flexural modulus M R The flexural modulus M of the polypropylene resin composition R is preferably 900 MPa or more and 1300 MPa or less, more preferably 950 MPa or more and 1250 MPa or less, and even more preferably 1000 MPa or more and 1200 MPa or less. R The measurement method of the flexural modulus M of the resin composition A described above was the same as that of the resin composition A except that a non-foamed sheet prepared by heat pressing the foamed beads was used as a test piece. A The flexural modulus M of the polypropylene resin composition R was measured based on JIS K7171:2008 in the same manner as in the measurement of the flexural modulus M of the polypropylene resin composition R based on JIS K7171:2008. R can be sought.
[0102] Melt mass flow rate (MFR) of polypropylene resin composition R measured at a temperature of 230°C and a load of 2.16 kg RThe melt mass-flow rate MFR of the polypropylene resin composition R is preferably 8 g / 10 min or more and 20 g / 10 min or less, and more preferably 10 g / 10 min or more and 15 g / 10 min or less. In this case, expanded beads capable of producing an expanded bead molding having good moldability in a mold and good compressive strength can be more reliably obtained. R The measurement method is the same as that of the melt mass flow rate MFR of the resin composition A described above, except that the expanded beads are used as samples. A More specifically, the melt mass-flow rate MFR of the polypropylene resin composition R is R is a value measured under conditions of a test temperature of 230° C. and a load of 2.16 kg based on JIS K7210-1:2014. Note that the expanded beads used as a sample may be previously subjected to a defoaming treatment.
[0103] The resin composition R preferably contains an ethylene propylene-based rubber, and more preferably contains an ethylene propylene-based rubber derived from a post-consumer material. In this case, it is more preferable that the resin composition R exhibits a morphology in which the polypropylene-based resin is the matrix (i.e., continuous phase) and the rubber-like body containing the ethylene propylene-based rubber is the domain (i.e., dispersed phase). In this case, even if the amount of the polypropylene-based resin composition a derived from a post-consumer material is relatively large, the foamed beads capable of molding a foamed bead molding having good in-mold moldability and good mechanical properties such as compressive strength can be stably obtained. The method for observing the morphology of the resin composition R is the same as the method for observing the morphology of the resin composition A described above, except that a sample for observation is obtained from the vicinity of the center of the foamed bead.
[0104] From the viewpoint of stably increasing the moldability of the foamed beads in the mold, the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber in the resin composition R is preferably 0.5 μm or more and 5 μm or less, more preferably 0.8 μm or more and 3 μm or less, and even more preferably 1 μm or more and 2 μm or less. The average diameter of the domains is calculated based on the TEM photograph. Specifically, the longest diameter and the shortest diameter of 50 or more domains randomly selected from the domains appearing in the TEM photograph are measured, and then the arithmetic mean of these is calculated. The arithmetic mean value of the longest diameter and the shortest diameter thus obtained is regarded as the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber.
[0105] From the viewpoint of stably increasing the in-mold moldability of the expanded beads, the 23°C n-decane soluble content in the expanded beads, i.e., the amount of components contained in the expanded beads that are soluble in decane at 23°C and insoluble in acetone, is preferably 2% by mass or more and 10% by mass or less, more preferably 3% by mass or more and 9% by mass or less, and even more preferably 4% by mass or more and 8% by mass or less. The method for measuring the 23°C n-decane soluble content in the expanded beads is the same as the method for measuring the 23°C n-decane soluble content in resin composition A described above, except that expanded beads are used as the sample.
[0106] From the viewpoint of more stably obtaining expanded beads having excellent moldability in a mold, the heat of fusion H R The heat of fusion H of the polypropylene resin composition R is preferably 70 J / g or more and 100 J / g or less, more preferably 80 J / g or more and 98 J / g or less, and even more preferably 85 J / g or more and 95 J / g or less. R The method for measuring the heat of fusion H of the polypropylene resin composition R is the same as the method for measuring the heat of fusion H of the resin composition A described above, except that expanded particles are used as a sample. The heat of fusion H of the polypropylene resin composition R is measured based on a DSC curve obtained by performing differential scanning calorimetry in accordance with JIS K 7122:1987. R can be sought.
[0107] The foamed beads may have a fusion layer on the surface thereof to enhance the fusion between the foamed beads during molding in a mold. The fusion layer may be present on the entire surface of the foamed beads, or may be present on a part of the surface. Examples of the resin constituting the fusion layer include a crystalline polyolefin resin having a melting point lower than the melting point of the molten mixture constituting the foamed beads, and an amorphous polyolefin resin having a softening point lower than the melting point of the molten mixture constituting the foamed beads.
[0108] The method for forming a fusion layer on the surface of the expanded beads is not particularly limited, and examples thereof include a method of foaming resin particles having a fusion layer on the surface, a method of obtaining expanded beads and then attaching a fusion layer to the surface of the expanded beads, etc. When foaming resin particles having a fusion layer on the surface to obtain expanded beads, it is preferable to adopt a method in which, when producing the resin beads, a molten mixture for forming the resin particle body and a resin melt for forming the fusion layer are co-extruded using an extrusion device capable of co-extrusion, thereby laminating a fusion layer on the surface of the resin beads.
[0109] [Bulk density of expanded particles] The bulk density of the foamed particles is 10 kg / m 3 More than 200kg / m 3 It is preferable that the thickness is less than 12 kg / m 3 More than 100kg / m 3 More preferably, it is 15 kg / m or less. 3 More than 80kg / m 3 More preferably, it is 20 kg / m or less. 3 More than 70kg / m 3 In this case, a molded article that is lightweight and has good mechanical strength can be easily obtained over a wide range of molding pressures.
[0110] The method for calculating the bulk density of expanded beads is as follows. First, the expanded beads are left to stand for 24 hours or more in an environment of 50% relative humidity, 23°C temperature, and 1 atm pressure to condition the expanded beads. The expanded beads thus obtained are filled into a measuring cylinder, and the bottom of the measuring cylinder is lightly tapped on the floor several times to stabilize the filling height of the expanded beads in the measuring cylinder. The bulk volume (unit: L) of the expanded beads is read from the graduations on the measuring cylinder. The mass (unit: g) of the expanded beads in the measuring cylinder is then divided by the aforementioned bulk volume to obtain the bulk density of the expanded beads (unit: kg / m2) by converting the value into units. 3 ) can be obtained.
[0111] [Average bubble diameter of expanded beads] The average cell diameter of the expanded beads is preferably 40 μm to 100 μm, more preferably 45 μm to 90 μm, and even more preferably 50 μm to 80 μm, in which case the moldability of the expanded beads in the mold can be further improved, and a good molded product can be easily obtained over a wide range of molding pressures.
[0112] The average bubble diameter of expanded beads is a value calculated by the following method. First, an expanded bead is cut into roughly two equal parts. Next, an enlarged photograph is taken so that the exposed cut surface is entirely within the field of view. On the enlarged photograph obtained, four line segments are drawn from the outermost surface of the expanded bead through the center to the outermost surface on the opposite side, with adjacent line segments forming equal angles (i.e., adjacent line segments forming an angle of 45°). The total length of the four line segments thus obtained is divided by the total number of bubbles intersecting the lines to determine the bubble diameter of each expanded bead.
[0113] The above procedure is carried out on 10 or more randomly selected expanded beads, and the arithmetic mean of the cell diameters obtained for each expanded bead is taken as the average cell diameter of the expanded beads.
[0114] [Closed cell ratio of expanded beads] The closed cell rate of the expanded beads is preferably 90% or more, which further enhances moldability in a mold and makes it possible to easily obtain good molded articles over a wide range of molding pressures.
[0115] The closed cell ratio of the expanded beads is a value measured using an air comparison type specific gravity meter based on ASTM-D2856-70 Procedure C. The specific method for measuring the closed cell ratio of the expanded beads is as follows. Bulk volume after conditioning: about 20 cm 3 The expanded particles are used as a measurement sample, and the apparent volume Va of the measurement sample is measured from the rise in the liquid level when the measurement sample is submerged in a graduated cylinder containing ethanol. After the measurement sample whose apparent volume Va has been measured is thoroughly dried, the true volume value Vx of the measurement sample is measured using an air comparison type specific gravity meter (Tokyo Science Co., Ltd.'s "Beckman Model 1000 Air Comparison Pycnometer") in accordance with procedure C described in ASTM-D2856-70. Then, using these volume values Va and Vx, the closed cell ratio (unit: %) of the measurement sample is calculated based on the following formula (1). The above operation is performed five times by changing the measurement sample, and the arithmetic average value (N=5) of the closed cell ratios of the five measurement samples is taken as the closed cell ratio (unit: %) of the expanded particles.
[0116] Closed cell ratio = (Vx-W / ρ)×100 / (Va-W / ρ) (1) In the above formula (1), the symbols have the following meanings: Vx: The true volume of the measurement sample measured by the above method, i.e., the sum of the volume of the resin constituting the foamed beads and the total volume of the air bubbles in the closed cell part in the foamed beads (unit: cm 3 ) Va: The apparent volume of the sample measured by the amount of rise in the liquid level when the sample is submerged in a graduated cylinder containing ethanol (unit: cm 3 ) W: Mass of the measurement sample (unit: g) ρ: Density of the resin that composes the foamed particles (unit: g / cm 3 )
[0117] [Ash content of expanded particles] The ash content of the expanded beads is preferably 0.1% by mass or more and 4% by mass or less, in which case the amount of components derived from post-consumer materials can be increased while ensuring good moldability of the expanded beads in a mold, making it easier to utilize post-consumer materials.
[0118] From the viewpoint of more effectively utilizing the polypropylene-based resin composition derived from post-consumer materials, the ash content of the expanded beads is more preferably 0.2% by mass or more, further preferably 0.5% by mass or more, and particularly preferably 1% by mass or more. On the other hand, from the viewpoint of more stably realizing good in-mold moldability of the expanded beads, the ash content of the expanded beads is more preferably 3% by mass or less, and further preferably 2% by mass or less.
[0119] In determining the preferred range of the ash content of the expanded beads, the above-mentioned upper and lower limits of the ash content of the expanded beads can be combined arbitrarily. For example, the preferred range of the ash content of the expanded beads may be 0.1% by mass or more and 3% by mass or less, 0.2% by mass or more and 3% by mass or less, or 0.4% by mass or more and 2% by mass or less.
[0120] The ash content of the expanded beads can be measured in accordance with the direct incineration method (Method A) of JIS K7250-1: 2006. More specifically, the ash content of the expanded beads can be calculated from the mass of the residue remaining after burning the expanded beads.
[0121] [High temperature peak] The expanded beads preferably have a crystal structure in which a melting peak due to melting inherent to the resin component constituting the expanded beads and one or more melting peaks located at a higher temperature than the melting peak appear in a DSC curve obtained when the expanded beads are heated from 23°C to 230°C at a heating rate of 10°C / min. Expanded beads having such a crystal structure have excellent moldability in a mold and also have excellent mechanical properties. In the following, the melting peak due to melting inherent to the resin component appearing in the DSC curve is referred to as a "resin-specific peak", and the melting peak appearing at a higher temperature than the resin-specific peak is referred to as a "high-temperature peak". The resin-specific peak appears due to melting of crystals that the resin component constituting the expanded beads usually has. On the other hand, the high-temperature peak is presumed to appear due to melting of secondary crystals formed in the resin component during the manufacturing process of the expanded beads. That is, when a high-temperature peak appears in a DSC curve, it is presumed that secondary crystals are formed in the resin component.
[0122] Whether or not the expanded beads have the above-mentioned crystal structure may be determined based on a DSC curve obtained by carrying out differential scanning calorimetry (DSC) under the above-mentioned conditions in accordance with JIS K7122: 1987. In addition, when carrying out DSC, 1 to 3 mg of the expanded beads may be used as a sample.
[0123] Specifically, in the DSC curve obtained when heating from 23°C to 230°C at a heating rate of 10°C / min (i.e., the first heating) as described above, both the resin peak specific to the resin component constituting the expanded beads and a high-temperature peak appear. In contrast, in the DSC curve obtained when the first heating is performed, the resin component is cooled from 230°C to 23°C at a cooling rate of 10°C / min, and then heated again from 23°C to 230°C at a heating rate of 10°C / min (i.e., the second heating), only the resin peak specific to the resin component constituting the expanded beads appears. Therefore, by comparing the DSC curve obtained during the first heating with the DSC curve obtained during the second heating, the resin peak specific to the resin component and the high-temperature peak can be distinguished.
[0124] From the viewpoint of further improving the moldability and mechanical properties of the expanded beads, the melting peak temperature of the high-temperature peak of the expanded beads is preferably from 168° C. to 175° C., and more preferably from 170° C. to 174° C. From the same viewpoint, the heat of fusion of the high-temperature peak is preferably from 10 J / g to 40 J / g, and more preferably from 13 J / g to 35 J / g, and even more preferably from 15 J / g to 30 J / g.
[0125] The heat of fusion of the high-temperature peak described above is a value that can be determined as follows. First, 1 to 3 mg of expanded beads are used as a sample, and a DSC curve is obtained by performing differential scanning calorimetry under conditions of heating from 23°C to 230°C at a heating rate of 10°C / min. An example of a DSC curve is shown in Figure 1. When the expanded beads have a high-temperature peak, as shown in Figure 1, the DSC curve will have a resin-specific peak ΔH1 and a high-temperature peak ΔH2 having a peak at a higher temperature side than the peak of the resin-specific peak ΔH1.
[0126] Next, a straight line L1 is drawn connecting point α corresponding to 80° C. on the DSC curve and point β corresponding to the melting end temperature T of the expanded beads. The melting end temperature T is the high temperature end point of the high temperature peak ΔH2, that is, the intersection point of the high temperature peak ΔH2 and the baseline on the higher temperature side of the high temperature peak ΔH2 on the DSC curve.
[0127] After drawing the line L1, a line L2 is drawn that passes through the maximum point γ between the resin intrinsic peak ΔH1 and the high-temperature peak ΔH2 and is parallel to the vertical axis of the graph. This line L2 divides the resin intrinsic peak ΔH1 and the high-temperature peak ΔH2. The heat of fusion of the high-temperature peak ΔH2 can be calculated based on the area of the part of the DSC curve that constitutes the high-temperature peak ΔH2 and the part surrounded by the lines L1 and L2.
[0128] (Foamed bead molding) After the foamed beads are filled into a mold, a heating medium such as steam is supplied into the mold to perform molding within the mold, thereby obtaining a foamed bead molded article. The density of the molded article is 10 kg / m 3More than 200kg / m 3 In this case, the molded body can have a good balance between light weight and mechanical strength.
[0129] From the viewpoint of further increasing the mechanical strength of the molded body, the density of the molded body is 12 kg / m 3 More preferably, it is 15 kg / m or more. 3 More preferably, it is 20 kg / m or more. 3 From the viewpoint of further increasing the lightness of the molded body, the density of the molded body is preferably 100 kg / m or more. 3 More preferably, it is 80 kg / m or less. 3 More preferably, it is 70 kg / m or less. 3 It is particularly preferable that the content is 60 kg / m or less. 3 The density of the molded body is calculated by dividing the mass (unit: g) of the molded body by the volume (unit: L) determined from the outer dimensions of the molded body, and converting the result into units. If it is not easy to determine the volume from the outer dimensions of the molded body, the volume of the molded body can be determined by a water immersion method.
[0130] From the viewpoint of further improving the mechanical properties of the molded article, the closed cell ratio of the molded article is preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more.
[0131] The closed cell ratio of the molded body is measured in accordance with ASTM2865-70 Procedure C. Specifically, a test specimen measuring 25 mm in length, 25 mm in width, and 30 mm in height is cut out from the center of the molded body, and the geometric volume Va (unit: cm 3), that is, the product of the length (unit: cm), width (unit: cm), and height (unit: cm). Next, in accordance with procedure C described in ASTM-D2856-70, the true volume Vx of the test specimen is measured using an air comparison pycnometer (specifically, a Beckman Model 1000 Air Comparison Pycnometer manufactured by Tokyo Science Co., Ltd.). The true volume Vx obtained using the air comparison pycnometer is the sum (unit: cm) of the volume of the resin that constitutes the measurement sample and the total volume of the air bubbles in the closed cell portion of the measurement sample. 3 ).
[0132] The closed cell ratio (unit: %) of the test specimen is calculated by multiplying the mass W (unit: g) of the test specimen by the density ρ (unit: g / cm 3 ) and the geometric volume Va of the test specimen obtained by the above-mentioned method and the true volume Vx of the test specimen are used to express the following equation (2). Closed cell ratio = (Vx-W / ρ)×100 / (Va-W / ρ) (2)
[0133] The above procedure is carried out for five test specimens, the closed cell ratio of each test specimen is calculated, and the arithmetic mean value of the closed cell ratios of these five test specimens is regarded as the closed cell ratio of the molded article. EXAMPLES
[0134] An example of the method for producing the expanded beads will now be described.
[0135] (Polypropylene Resin Composition A) Table 1 shows the properties of the polypropylene resin composition A used in the production of the expanded beads. The resin composition A1 used in this example is "PLC-A02" manufactured by Planic Co., Ltd., and the resin composition A2 is "ELVBP-10" manufactured by Haison Co., Ltd. Both the resin compositions A1 and A2 are polypropylene resin compositions a derived from post-consumer materials. The main component of the resin composition A1 is the polypropylene resin composition a1 recovered from ASR, and the resin composition A2 is the polypropylene resin composition a recovered from used automobile parts (more specifically, bumpers). The shape of the polypropylene resin composition A is a cylindrical pellet, the average length in the height direction of the pellets (average length in the extrusion direction during pellet production) is 3 mm, the diameter of the pellets is 3 mm, and the average mass of the pellets is 16 mg. The polypropylene resin composition A also contains an inorganic substance mainly composed of talc. When the morphology of the resin composition A used in this example was observed using the method described below, both resin compositions A1 and A2 exhibited a morphology in which a polypropylene resin was used as the matrix and a rubber-like body containing an ethylene propylene rubber was used as the domain.
[0136] [Table 1]
[0137] The physical properties of the resin composition A shown in Table 1 were measured as follows.
[0138] [23°C n-decane solubles in resin composition A] The amount of 23°C n-decane soluble matter in the resin composition A, that is, the amount of components dissolved in n-decane at 23°C and unnecessary for acetone, was determined by the following method. Specifically, first, about 5 g of the resin composition A was precisely weighed as a sample. The sample was added to 200 ml of n-decane, and heated and dissolved at 145°C for 30 minutes. Next, the obtained n-decane solution was cooled to 23°C over 2 hours, and left at 23°C for 30 minutes to precipitate components insoluble in n-decane. Thereafter, the n-decane solution was filtered to filter out components insoluble in n-decane at 23°C, and a filtrate containing 23°C n-decane soluble matter was obtained. This filtrate was added to about three times the amount of acetone relative to the filtrate, and left at 23°C for 18 hours to precipitate a precipitate containing 23°C n-decane soluble matter. The precipitate was then filtered and dried, and its mass was measured. The mass of the precipitate thus measured was divided by the mass of the sample and expressed as a percentage to calculate the content of n-decane soluble matter at 23° C. in resin composition A (unit: mass %).
[0139] [Morphology of Resin Composition A] The morphology of the resin composition A1 was observed by the following method. First, a cylindrical pellet made of the resin composition A1 was cut perpendicularly to the height direction of the pellet so as to pass through the center of the pellet, and an observation sample was prepared in which the cross section of the center of the pellet was exposed. Next, the observation sample was embedded in epoxy resin and subjected to electronic staining with ruthenium tetroxide, and then a slice including the center of the pellet was prepared from the sample using an ultramicrotome or the like. The slice was placed on the grid of a transmission electron microscope (for example, "JEM-1040Flash" manufactured by JEOL Ltd.) and observed at a magnification of 5000 times, and a cross-sectional photograph (i.e., a TEM photograph) of the resin composition A1 was taken.
[0140] The morphology of the polypropylene resin phase and the rubber-like body phase containing the ethylene propylene rubber in the resin composition A1 was visually observed from the cross-sectional photograph. A cross-sectional photograph of the resin composition A1 is shown in Figure 2. In Figure 2, the domain D of the rubber-like body containing the ethylene propylene rubber is shown in a relatively dark tone, and the matrix M of the polypropylene resin is shown in a lighter tone than the domain D.
[0141] The average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber was calculated based on the TEM photograph. More specifically, the longest diameter and the shortest diameter of 50 domains randomly selected from the domains appearing in the TEM photograph were measured. The arithmetic mean value of the longest diameter and the shortest diameter thus obtained was taken as the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber. As a result, the average diameter of the domains of the rubber-like body containing the ethylene propylene-based rubber in the resin composition A1 was 1.2 μm.
[0142] The area ratio of the domains in the morphology was calculated based on the TEM photograph. More specifically, an image analysis software ("WinROOF2013" manufactured by Mitani Shoji Co., Ltd.) was used to perform monotone processing to make the domains in the TEM photograph black and the non-domain parts white, and the measurement object was used. Then, the image analysis software was used to calculate the total area occupied by the domains in the measurement object, and the ratio of the total area occupied by the domains to the total area of the measurement object was calculated. As a result, the area ratio of the domains in the morphology of resin composition A1 was 28%. I did.
[0143] [Ash content] The ash content of the resin composition A was measured according to the direct ashing method (method A) of JIS K7250-1:2006. Specifically, about 5 g of the resin composition A was weighed out and then placed in a crucible. The resin composition A in the crucible was heated for 1 hour in an electric furnace with the atmospheric temperature set to 600°C, thereby burning the resin composition A. After the heating was completed, the mass of the residue remaining in the crucible was measured. The ratio of the mass of the residue to the mass of the resin composition A before heating, expressed as a percentage, was taken as the ash content (unit: mass%) of the resin composition A.
[0144] [Melting point Tm A and heat of fusion H A 〕 Melting point Tm of resin composition AA was determined based on JIS K7121:1987. Specifically, first, the condition of a test piece made of resin composition A was adjusted based on "(2) In the case of measuring the melting temperature after a certain heat treatment" in "3. Condition adjustment of test piece" described in JIS K7121:1987. The test piece after the condition adjustment was heated from 23°C to 230°C at a heating rate of 10°C / min to obtain a DSC curve. The apex temperature of the melting peak that appeared in the DSC curve was determined as the melting point Tm A The measurement device used was a heat flux differential scanning calorimeter (manufactured by SII NanoTechnology, Inc., model number: DSC7020).
[0145] In addition, from the DSC curve obtained by performing differential scanning calorimetry in accordance with JIS K 7122:1987, the heat of fusion H A Specifically, the melting point Tm A On the DSC curve obtained in the measurement, a straight line was drawn connecting the point corresponding to 80°C on the DSC curve and the high-temperature end point of the highest melting peak. The heat of fusion H of resin composition A was calculated based on the area surrounded by the straight line thus determined and the melting peak of the DSC curve. A was calculated.
[0146] [Melt mass flow rate MFR A 〕 According to JIS K7210-1:2014, the melt mass flow rate (MFR) of resin composition A was measured at a temperature of 230°C and a load of 2.16 kg. A was measured.
[0147] [Flexural modulus M A 〕 Resin composition A was heat pressed at 180°C to produce a sheet with a thickness of 4 mm, and a test piece with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm was cut out from this sheet. The flexural modulus M Awas determined in accordance with JIS K7171:2008. The radius R1 of the indenter and the radius R2 of the support table were both 5 mm, the distance between the supports was 64 mm, and the test speed was 2 mm / min.
[0148] (Polypropylene resin B) Table 2 shows the properties of the polypropylene resin B used in the production of the expanded beads. The resins B used in this example are all composed of non-recycled polypropylene resins. The resins B used in this example are either propylene-ethylene random copolymers (B1 to B3) or homopropylene (B4). In Table 2, the propylene random copolymers are indicated as "rPP" and the homopropylene as "hPP".
[0149] The methods for measuring the physical properties shown in Table 2 are the same as those for the above-mentioned resin composition A. The method for calculating the "ethylene component content" of resin B in Table 2 is as follows.
[0150] The content of the ethylene component in the resin B was determined by a known method determined by IR spectrum. Specifically, it was determined by the method described in Polymer Analysis Handbook (edited by the Polymer Analysis Research Forum of the Japan Analytical Chemistry Society, published in January 1995, published by Kinokuniya Shoten, page numbers and item names: 615-616 "II.2.3 2.3.4 Propylene / ethylene copolymer", 618-619 "II.2.3 2.3.5 Propylene / butene copolymer"), that is, by a method of quantitative determination based on the relationship between the value of the absorbance of ethylene and butene corrected by a predetermined coefficient and the thickness of a film-like test piece, etc.
[0151] More specifically, resin B was first heat-pressed in an environment of 180° C. to form a film, and a number of test pieces with different thicknesses of 0.1 to 0.3 mm were prepared. Next, the IR spectrum of each test piece was measured to confirm the presence of the 722 cm -1 and 733 cm -1 Absorbance at (A 722 , A 733) and 766 cm -1 Absorbance at (A 766 ) was read. Next, for each test piece, the ethylene component content (unit: mass%) in Resin B was calculated using the following formulas (3) to (5). The ethylene component contents obtained for each test piece were averaged to obtain the ethylene component content (unit: mass%) in Resin B.
[0152] (K 733 ) c =1 / 0.96{(K´ 733 ) a -0.268(K´ 722 ) a}···(3) (K 722 ) c =1 / 0.96{(K´ 722 ) a -0.150(K´ 733 ) a}···(4) Ethylene content = 0.575 {(K' 722 ) c +(K´ 733 ) c}···(5)
[0153] However, K' in formulas (3) to (5) a is the apparent absorption coefficient (K´) at each wave number. a =A / ρt) and K´ c is the corrected extinction coefficient, A is the absorbance, and ρ is the density of the resin (unit: g / cm 3 ) and t is the thickness of the film-like test piece (unit: cm).
[0154] [Table 2]
[0155] Next, the configuration and manufacturing method of the expanded beads of this embodiment will be described.
[0156] Example 1 Resin composition A, resin B, and a bubble control agent shown in Table 3 were charged into an extruder in the mass ratio shown in Table 3 to form a molten mixture containing resin composition A and resin B in the extruder. Zinc borate was used as the bubble control agent. The amount of zinc borate added was 500 ppm by mass relative to the total amount of resin composition A and resin B.
[0157] The molten mixture was then extruded in the form of a strand from a small hole in a die provided downstream of the extruder. The strand-shaped extrudate was taken off, cooled, and then cut to an appropriate length using a pelletizer to obtain resin particles.
[0158] The resin particles thus obtained were expanded by a direct expansion method. Specifically, 1 kg of resin particles was first put into a container with an internal volume of 5 L together with 3 L of water as an aqueous medium. Next, 0.3 parts by mass of a dispersant, 0.02 parts by mass of sodium alkylbenzene sulfonate as a dispersing agent, and 0.01 parts by mass of aluminum sulfate were added to the container relative to 100 parts by mass of the resin particles, and the resin particles were dispersed in the aqueous medium. Kaolin was used as the dispersant.
[0159] Then, carbon dioxide was supplied as a blowing agent into the sealed container while stirring the contents of the container, and the temperature inside the container was raised to 155.5°C. The pressure inside the container at this time was 2.1 MPa (G). The temperature inside the container was then adjusted to 156°C, and this temperature was maintained for 15 minutes, thereby impregnating the resin particles with the blowing agent. The container was then opened, and the contents were released into an atmospheric pressure atmosphere, thereby expanding the resin particles to obtain first-stage expanded particles. The first-stage expanded particles were then dried for 24 hours in an atmosphere at a temperature of 23°C and a relative humidity of 50%.
[0160] Next, the first-stage expanded particles were loaded into a pressure vessel, and air was injected into the pressure vessel to increase the pressure in the pressure vessel from atmospheric pressure to 0.6 MPa (G) over 24 hours. This pressure was maintained for 24 hours to allow the air to be impregnated into the bubbles. Thereafter, the first-stage expanded particles were removed from the pressure vessel and loaded into a second-stage expansion machine, and steam was supplied at a pressure of 0.15 MPa (G) to further expand the first-stage expanded particles. In this manner, the expanded particles of Example 1 were obtained.
[0161] Example 2 The manufacturing method of the expanded beads in Example 2 is generally the same as that of Example 1, except that the mass ratio of resin composition A and resin B was changed to resin composition A:resin B = 50:50, as shown in Table 3.
[0162] Example 3 The method for producing the expanded beads of Example 3 was generally the same as that for producing the expanded beads of Example 1, except that, as shown in Table 3, polypropylene-based resin B2 was used as resin B instead of polypropylene-based resin B1.
[0163] Example 4 The method for producing the expanded beads of Example 4 was generally the same as that for producing the expanded beads of Example 1, except that, as shown in Table 3, polypropylene-based resin composition A2 was used instead of polypropylene-based resin composition A1 as resin composition A.
[0164] Example 5 The expanded beads of Example 5 were obtained by a method similar to that of Example 1, and had a bulk density of 45 kg / m 3 The first-stage expanded particles were used.
[0165] Comparative Example 1 The expanded beads of Comparative Example 1 were composed only of resin composition A. The manufacturing method of the expanded beads of Comparative Example 1 was generally similar to that of Example 1, except that the resin particles were produced using only resin composition A1 without using resin B, as shown in Table 4.
[0166] (Comparative Examples 2 to 3) The methods for producing the expanded beads in Comparative Examples 2 and 3 were generally similar to the method for producing the expanded beads in Example 1, except that, instead of polypropylene-based resin B1, either polypropylene-based resin B3 or polypropylene-based resin B4 was used as resin B as shown in Table 4.
[0167] (Reference example) The expanded beads of the Reference Example are composed only of resin B. The manufacturing method of the expanded beads of the Reference Example is generally similar to the manufacturing method of the expanded beads of Example 1, except that the resin particles are produced using only resin B1 without using resin composition A, as shown in Table 4.
[0168] The properties of the resin particles, expanded particles, and molded articles obtained by molding the expanded particles in a mold are shown in Tables 3 and 4. The properties shown in Tables 3 and 4 were evaluated as follows.
[0169] [Ash content of resin particles and expanded particles] The method for measuring the ash content of the resin particles and the ash content of the expanded beads is the same as the method for measuring the ash content of the resin composition A described above, except that resin particles or expanded beads are used instead of resin composition A.
[0170] [Bulk density of expanded particles] The expanded particles were left to stand for 24 hours or more in an environment of 50% relative humidity, 23°C temperature, and 1 atm pressure to condition the expanded particles. The expanded particles thus obtained were filled into a measuring cylinder, and the bottom of the measuring cylinder was lightly tapped on the floor several times to stabilize the filling height of the expanded particles in the measuring cylinder. The bulk volume (unit: L) of the expanded particles was then read from the graduations on the measuring cylinder. The mass (unit: g) of the expanded particles in the measuring cylinder was then divided by the aforementioned bulk volume to convert the value into units to obtain the bulk density (unit: kg / m 3 ) was calculated.
[0171] [Average bubble diameter of expanded beads] The expanded beads were cut into roughly two equal parts. Next, an enlarged photograph was taken so that the exposed cut surface was entirely within the field of view. Four line segments were drawn on the enlarged photograph from the outermost surface of the expanded beads through the center to the outermost surface on the opposite side, with the adjacent line segments forming equal angles (i.e., the angle between adjacent line segments was 45°). The total length of the four line segments thus obtained was divided by the total number of bubbles intersecting the lines to determine the bubble diameter of each expanded bead.
[0172] The above procedure was carried out on 10 or more randomly selected expanded beads, and the arithmetic mean of the cell diameters obtained for each expanded bead was taken as the average cell diameter of the expanded beads.
[0173] [Closed cell ratio of expanded beads] The closed cell ratio of the foamed particles was measured using an air comparison type specific gravity meter according to ASTM-D2856-70 procedure C. Specifically, first, the bulk volume after conditioning was about 20 cm 3 The expanded particles were used as a measurement sample, and the measurement sample was submerged in a graduated cylinder containing ethanol. The apparent volume Va of the measurement sample was measured from the amount of rise in the liquid level at this time. After the measurement sample whose apparent volume Va was measured was thoroughly dried, the true volume value Vx of the measurement sample was measured using an air comparison type specific gravity meter (Tokyo Science Co., Ltd.'s "Beckman Model 1000 Air Comparison Pycnometer") in accordance with procedure C described in ASTM-D2856-70. Then, using these volume values Va and Vx, the closed cell ratio (unit: %) of the measurement sample was calculated based on the following formula (1). The above operation was performed five times by changing the measurement sample, and the arithmetic average value (N = 5) of the closed cell ratios of the five measurement samples was taken as the closed cell ratio (unit: %) of the expanded particles.
[0174] Closed cell ratio = (Vx-W / ρ)×100 / (Va-W / ρ) (1)
[0175] In the above formula (1), the symbols have the following meanings: Vx: The true volume of the measurement sample measured by the above method, i.e., the sum of the volume of the resin constituting the foamed beads and the total volume of the air bubbles in the closed cell part in the foamed beads (unit: cm 3 ) Va: The apparent volume of the sample measured by the amount of rise in the liquid level when the sample is submerged in a graduated cylinder containing ethanol (unit: cm 3 ) W: Mass of the measurement sample (unit: g) ρ: Density of the resin that composes the foamed particles (unit: g / cm 3 )
[0176] [Melting point Tm of polypropylene resin composition R R , flexural modulus M R , Melt mass flow rate MFR R and heat of fusion H R 〕 Melting point Tm of polypropylene resin composition R R , flexural modulus M R , Melt mass flow rate MFR R and heat of fusion H R The measurement method was the same as that of the melting point Tm of the resin composition A, except that foamed beads were used instead of the resin composition A. A , flexural modulus M A , Melt mass flow rate MFR A and heat of fusion H A The measurement method is the same as that of
[0177] The flexural modulus M of the polypropylene resin composition R R In the measurement of the flexural modulus M, the foamed particles were heat pressed at 180°C to produce a sheet with a thickness of 4 mm, and a test piece with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm was cut out from the sheet. R Measurements were carried out.
[0178] In addition, the melt mass flow rate MFR of the polypropylene resin composition R RIn the measurement of the melt mass flow rate (MFR), the foamed beads were first heat-pressed at 180°C for 3 minutes to defoam the foamed beads, and a resin sheet was prepared from the mixed resin that constitutes the foamed beads. The resin sheet was cut into pellets to obtain a sample, and the melt mass flow rate (MFR R Measurements were carried out.
[0179] [High temperature peak] The apex temperature and heat of fusion of the high-temperature peak were obtained from a DSC curve obtained by performing differential scanning calorimetry (DSC) in accordance with JIS K7122:1987. Specifically, first, about 3 mg of expanded particles was used as a sample, and the sample was heated from 23°C to 230°C at a heating rate of 10°C / min to perform differential scanning calorimetry to obtain a DSC curve. Next, a straight line L1 was drawn connecting a point α corresponding to 80°C on the DSC curve and a point β corresponding to the melting end temperature T of the expanded particles. Furthermore, a straight line L2 was drawn parallel to the vertical axis of the graph through a maximum point γ existing between the resin intrinsic peak ΔH1 and the high-temperature peak ΔH2, and the resin intrinsic peak ΔH1 and the high-temperature peak ΔH2 were divided by the straight line L2.
[0180] Then, the heat of fusion of the high-temperature peak ΔH2 was calculated based on the area of the portion of the DSC curve that is surrounded by the line L1 and the line L2 and the portion that constitutes the high-temperature peak ΔH2.
[0181] The above procedure was carried out three times using different samples, and the arithmetic mean value of the heat of fusion of the high-temperature peak ΔH2 obtained in each measurement was taken as the heat of fusion of the high-temperature peak ΔH2 of the expanded beads.
[0182] [Moldable range] In evaluating the moldable range, foamed bead moldings were produced by in-mold molding while changing the molding pressure during main heating from 0.32 MPa (G) to 0.44 MPa (G) in increments of 0.01 MPa, and the lower molding pressure limit and moldable range were determined based on the surface properties, fusion properties, and recovery properties of the obtained moldings.
[0183] The manufacturing method of the expanded bead molding is as follows. First, the expanded beads are placed in a pressure vessel, and the inside of the pressure vessel is pressurized with air to impregnate the expanded beads with air, and an internal pressure of 0.10 MPa (G) is applied to the expanded beads. Next, the expanded beads to which the internal pressure has been applied are filled into a mold by a cracking filling method. In this example, a mold having a cavity capable of molding a flat expanded bead molding having a length of 250 mm, a width of 200 mm, and a thickness of 50 mm was used. In the cracking filling, the expanded beads are filled into the mold with a cracking gap of 5 mm (i.e., a cracking amount of 10%) opened in the thickness direction of the molding, and then the mold is completely closed to mechanically compress the expanded beads in the mold.
[0184] Next, steam was supplied into the mold to perform in-mold molding. In the in-mold molding, first, steam was supplied into the mold for 5 seconds with the drain valve of the mold open to perform preheating. Next, the drain valve was closed, and steam was supplied from one side of the mold until a pressure 0.08 MPa (G) lower than the molding pressure during main heating was reached, to perform a first one-sided heating. Next, steam was supplied from the other side of the mold until a pressure 0.04 MPa (G) lower than the molding pressure during main heating was reached, to perform a second one-sided heating. After that, steam was supplied from both sides of the mold until the molding pressure during main heating was reached, to perform main heating. After main heating was completed, the pressure in the mold was released, and the molded body was cooled in the mold until the surface pressure due to the foaming force of the molded body became 0.04 MPa (G).
[0185] Thereafter, the expanded bead molding removed from the mold was left in an oven at 80°C for 12 hours to carry out a curing process. After the curing process, the expanded bead molding was left at rest for 24 hours under conditions of 50% relative humidity, 23°C, and 1 atm to condition the expanded bead molding. The surface properties, fusion properties, and recovery properties of the expanded bead molding after the condition control were evaluated, and the range of molding pressures that passed all items in the evaluation criteria described below (i.e., molding pressures at which a passing product could be obtained) was determined as the moldable range. The wider the moldable range, the better the moldability. In addition, the lower the moldable molding pressure, the less steam is required for in-mold molding, and the better the productivity.
[0186] The methods for evaluating the surface property, fusion property and recovery property in the evaluation of the moldable range are as follows.
[0187] ·Superficiality A 100 mm x 100 mm square was drawn in the center of one skin surface in the thickness direction of the expanded bead molding, and then a diagonal was drawn from one of the corners of the square. Then, the number of voids present on the diagonal, that is, voids having a size of 1 mm x 1 mm or more among the gaps formed between the expanded beads, was counted. If the number of voids was 2 or less, it was judged as passing, and if the number was 3 or more, it was judged as failing.
[0188] - Weldability The foamed bead molding was broken into roughly equal parts in the longitudinal direction. At least 100 foamed beads randomly selected from the foamed beads exposed on the fracture surface were visually observed to determine whether they had broken inside the beads (i.e., foamed beads with material destruction) or at the interface between the foamed beads. The ratio of the number of foamed beads that had broken inside the beads to the total number of foamed beads observed was calculated as a percentage (i.e., material destruction rate), and this value was taken as the fusion rate. A fusion rate of 80% or more was judged to be acceptable, and a fusion rate of less than 80% was judged to be unacceptable.
[0189] ·Recovery In a plan view of the expanded bead molding from the thickness direction, the thickness of the expanded bead molding was measured at four positions 10 mm inward from each apex toward the center, and at the center. Next, the ratio (unit: %) of the thickness of the thinnest part to the thickness of the thickest part among the measured parts was calculated. If the thickness ratio thus obtained was 95% or more, it was judged as passing, and if it was less than 95%, it was judged as failing.
[0190] [Density of Molded Body] Molding was performed in the mold at the lowest molding pressure within the above-mentioned moldable range to obtain an expanded bead molding. The mass (unit: g) of this expanded bead molding was divided by the volume (unit: L) calculated from the outer dimensions of the molding, and the density (unit: kg / m) of the molding was calculated by converting the unit. 3 ) was calculated.
[0191] [Closed cell ratio of molded body] Molding was performed in the mold at the lowest molding pressure within the above-mentioned moldable range to obtain a foamed bead molding. A test specimen measuring 25 mm in length × 25 mm in width × 30 mm in height was cut out from the center of this molding, and the geometric volume Va (unit: cm 3 ), that is, the product of the vertical dimension (unit: cm), horizontal dimension (unit: cm), and height dimension (unit: cm), was calculated. Next, in accordance with procedure C described in ASTM-D2856-70, the true volume value Vx of the test specimen was measured using an air comparison pycnometer (specifically, a "Beckman Model 1000 Air Comparison Pycnometer" manufactured by Tokyo Science Co., Ltd.). The true volume value Vx obtained using the air comparison pycnometer is the sum (unit: cm) of the volume of the resin constituting the measurement sample and the total volume of the air bubbles in the closed cell portion of the measurement sample. 3 ).
[0192] The mass W (unit: g) of the specimen obtained above and the density ρ (unit: g / cm 3) and the geometric volume Va and true volume Vx of the test specimen obtained by the above-mentioned method were used to calculate the closed cell ratio (unit: %) of the test specimen according to the following formula (2). Closed cell ratio = (Vx-W / ρ)×100 / (Va-W / ρ) (2)
[0193] The above procedure was carried out for five test specimens, the closed cell ratio of each test specimen was calculated, and the arithmetic mean value of the closed cell ratios of these five test specimens was regarded as the closed cell ratio of the molded article.
[0194] [50% compression strength of molded body] Molding was performed in the mold at the lowest molding pressure within the above-mentioned moldable range, to obtain an expanded bead molding. A rectangular parallelepiped test piece measuring 50 mm in length, 50 mm in width, and 25 mm in thickness was taken from the center of this molding. A compression test was performed on the test piece at a compression speed of 10 mm / min based on the method specified in JIS K7220:2006, and a stress-strain curve was obtained. The compression test was performed in a laboratory at 23°C. The 50% deformation compressive stress of the test piece was calculated based on this stress-strain curve, and this value was used as the 50% compression strength of the molding. The "50% compression strength / density" column in Tables 3 and 4 shows the value obtained by dividing the 50% compression strength value by the density of the molding (unit: kPa / (kg / m 3 )) was described.
[0195] [Table 3]
[0196] [Table 4]
[0197] As shown in Table 3, the resin composition A used in the manufacturing methods of Examples 1 to 5 contains a polypropylene-based resin composition a derived from a post-consumer material, and has a melting point Tm within the specific range. A and bending modulus M A Similarly, resin B has a melting point Tm within the above-mentioned specific range. Band bending modulus M B The resin particles in Examples 1 to 5 are composed of a melt-kneaded product obtained by mixing such resin composition A and resin B in a mass ratio within the specific range. Therefore, the expanded beads obtained by expanding such resin particles have good moldability in a mold. In addition, the molded articles obtained from the expanded beads obtained by expanding the resin particles in Examples 1 to 5 showed good compression properties.
[0198] On the other hand, as shown in Table 4, the resin particles in the manufacturing method of Comparative Example 1 do not contain resin B, and are composed only of resin composition A. Therefore, when the expanded beads obtained at various molding pressures were molded in a mold to evaluate the moldable range, a good molded product could not be obtained at any molding pressure.
[0199] The ratio M of the flexural modulus of the resin composition A and the resin B used in the manufacturing method of Comparative Example 2 B / M A does not satisfy the above-mentioned specific range. Therefore, in the evaluation of the moldable range, the expanded beads obtained at various molding pressures were molded in a mold, but no good molded product could be obtained at any molding pressure.
[0200] The flexural modulus M of resin B used in the manufacturing method of Comparative Example 3 B is higher than the specific range. Therefore, in the evaluation of the moldable range, the expanded beads obtained at various molding pressures were molded in a mold, but no good molded product could be obtained at any molding pressure.
[0201] The above describes specific aspects of the expanded beads and the manufacturing method thereof according to the present invention based on the examples. However, the specific aspects of the expanded beads and the manufacturing method thereof according to the present invention are not limited to the aspects of the examples, and the configurations can be changed as appropriate within the scope that does not depart from the spirit of the present invention. [Explanation of symbols]
[0202] A Polypropylene resin composition
Claims
1. A method for producing expanded beads by expanding polypropylene-based resin beads to obtain expanded beads, comprising the steps of: The resin particles contain a polypropylene-based resin composition a derived from post-consumer materials and have a melting point Tm A is 160° C. or more, and the flexural modulus M A A polypropylene resin composition A having a melting point Tm B is less than 160°C, and the flexural modulus M B and polypropylene-based resin B having a modulus of elasticity of 900 MPa or more and 1400 MPa or less, The bending elastic modulus M A The bending elastic modulus M B Ratio of M B / M A is 1 or more, The method for producing expanded beads, wherein a mass ratio of the polypropylene-based resin composition A to the polypropylene-based resin B in the resin beads is polypropylene-based resin composition A:polypropylene-based resin B=10:90 to 70:
30.
2. The resin particles have a melting point Tm r is 150°C or more and 162°C or less, and the flexural modulus M r The method for producing expanded beads according to claim 1, wherein the expanded beads are composed of a polypropylene-based resin composition r having a modulus of elasticity of 900 MPa or more and 1,300 MPa or less.
3. The melting point Tm of the polypropylene resin composition A A and the melting point Tm of the polypropylene resin B B Difference Tm A -Tm B The method for producing expanded beads according to claim 1 or 2, wherein the temperature is 5° C. or higher and 20° C. or lower.
4. The method for producing expanded beads according to claim 1 or 2, wherein the polypropylene resin composition A has a melt mass flow rate of 10 g / 10 min or more and 40 g / 10 min or less when measured at a temperature of 230° C. and a load of 2.16 kg.
5. 3. The method for producing expanded beads according to claim 1, wherein the polypropylene-based resin composition A exhibits a morphology in which a polypropylene-based resin is a matrix and a rubber-like body containing an ethylene-propylene-based rubber is a domain.
6. The bulk density of the expanded particles is 10 kg / m 3 More than 200kg / m 3 The method for producing expanded beads according to claim 1 or 2, wherein the method is as follows:
7. The method for producing expanded beads according to claim 1 or 2, wherein the expanded beads have a closed cell rate of 90% or more.
8. The polypropylene resin composition a is derived from post-consumer materials and has a melting point Tm R is 150°C or more and 162°C or less, and the flexural modulus M R The expanded particles are composed of a polypropylene-based resin composition R having a compressive strength of 900 MPa or more and 1,300 MPa or less.
9. The bulk density of the expanded particles is 10 kg / m 3 More than 200kg / m 3 9. The expanded beads according to claim 8, wherein:
10. 10. The expanded beads according to claim 8, wherein the expanded beads have a closed cell rate of 90% or more.
Citation Information
Patent Citations
Method for producing polypropylene-based resin-foamed particle
JP2005023302A
Method for producing polypropylene-based resin expanded particle molding
JP2005325179A
Polypropylene-based resin pre-expandable beads, method for producing the same, and in-mold expansion-molded form
JP2009126914A
Propylene-based resin foaming particle and foaming particle molded body
JP2017019980A
Method for producing foam molding
JP2020152781A
Cited By
Polypropylene resin foam particles
WO2026163889A1
Method for producing polypropylene-based resin foam particles, method for discriminating polypropylene-based resin, and method for producing polypropylene-based resin