Silicon wafer and method for manufacturing silicon wafer

A silicon wafer with controlled oxygen concentration and vacancy complex defects, produced via rapid thermal processing, addresses the issues of high oxygen content and BMDs in Czochralski method wafers, enhancing gettering ability and reducing leakage current.

JP2024148525APending Publication Date: 2024-10-18GLOBALWAFERS JAPAN
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023061727
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional silicon wafers manufactured by the Czochralski method contain high oxygen concentrations, leading to oxygen precipitates (BMDs) that cause leakage current and heavy metal contamination, making them unsuitable for advanced power devices requiring low oxygen content and effective gettering ability.

Method used

A silicon wafer with controlled oxygen concentration and vacancy complex defects is produced through rapid thermal processing, reducing BMD density and enhancing gettering ability by adjusting oxygen partial pressure and temperature during heat treatment.

Benefits of technology

The silicon wafer achieves low oxygen concentration and suppressed BMD density, providing sufficient gettering for heavy metals, thus improving device yield and reducing leakage current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148525000001_ABST
    Figure 2024148525000001_ABST
Patent Text Reader

Abstract

To provide a silicon wafer that has a low oxygen concentration and a low BMD density but has gettering capability for heavy metal, and to provide a method for manufacturing a silicon wafer.SOLUTION: A silicon wafer 1 with a bulk region of which oxygen concentration is 1×1016 atoms / cm3 or more and 7×1017 atoms / cm3 or less has a region of which density of vacancy-related compound defect is 1×1012 atoms / cm3 or more in a region within 100 μm in a depth direction from a wafer surface and has a BMD density of less than 1×105 atoms / cm3 in a region within 50 μm in the depth direction from the wafer surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon wafer and a method for manufacturing the silicon wafer, and more particularly to a silicon wafer having gettering capability and a method for manufacturing the silicon wafer. [Background technology]

[0002] Metal-oxide-semiconductor field-effect transistors (MOSFETs) are a type of field-effect transistor (FET) and are the most commonly used structure in LSIs. For example, insulated-gate bipolar transistors (IGBTs), which are used for power control, are a type of semiconductor device, and are bipolar transistors that incorporate MOSFETs into their main components. Conventionally, wafers used in such MOS power transistors such as IGBTs are required to have low oxygen content in order to avoid a decrease in lifetime, and high-resistance silicon wafers with low oxygen content achieved by the FZ method (floating zone method) as described in Patent Document 1 and epitaxial wafers having low-oxygen epitaxial layers stacked thereon have been used.

[0003] However, when manufacturing silicon wafers using the FZ method, it is difficult to produce large-diameter single crystals, for example, with a diameter of 300 mm or more, and the yield of devices is low with small-diameter silicon wafers. Therefore, there was an issue that it was difficult to apply the method to green devices (power devices directly linked to energy conservation), the demand of which is expected to increase significantly in the future.

[0004] In addition, epitaxial wafers, for example in the case of MOS power transistors, require a large epitaxial film thickness when manufacturing vertical devices, which increases costs, and so, like silicon wafers manufactured by the FZ method, they are not suitable for green devices. In addition, by making the epitaxial film thickness thicker, the integrity of the epitaxial layer is easily compromised, increasing the possibility of generating leakage current that causes problems in MOS power transistors and other devices. Therefore, attention is being focused on applying silicon wafers manufactured by the MCZ method (a method in which the crystal growth conditions are controlled by applying a magnetic field in the Czochralski method) to power devices. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-118283 Summary of the Invention [Problem to be solved by the invention]

[0006] For example, silicon single crystals pulled by the Czochralski method are produced using a quartz crucible, so the normal MCZ method requires at least 5 × 10 17 atoms / cm 3 This silicon wafer contains oxygen precipitates (called BMD) that are formed during crystal growth, and the dissolved oxygen atoms form new BMD during the power device manufacturing process, and these BMDs are the cause of leakage current in power devices. Therefore, in order to apply these silicon wafers manufactured by the MCZ method to more advanced power devices (high voltage resistance and high switching speed), it was necessary to suppress BMD, which causes defects.

[0007] On the other hand, in order to suppress leakage current in power devices, it is also important to reduce contamination by heavy metals. Therefore, there is a demand for silicon wafers that have a low oxygen concentration, suppress the formation of BMD, and have gettering capabilities.

[0008] Under these circumstances, the inventors of the present application conducted extensive research and found that when a silicon wafer with a low oxygen concentration is subjected to rapid thermal processing (RTP), in which the wafer is heated to a high temperature (1250°C or higher) for a time scale of several tens of seconds or less, large-sized defects such as BMDs that deteriorate the breakdown voltage are not generated. On the other hand, it has been found that microvacancy-oxygen complex defects (hereinafter referred to as vacancy complex defects) that contribute to the gettering of heavy metals are generated, which has led to the present invention.

[0009] An object of the present invention is to provide a silicon wafer having a low oxygen concentration and a low BMD density, but with gettering capability, and a method for manufacturing the silicon wafer. [Means for solving the problem]

[0010] The silicon wafer according to the present invention, which has been made to solve the above problems, has an oxygen concentration in the bulk region of 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 The following silicon wafers are characterized in that the concentration of vacancy-based complex defects is 1×10 in a region within 100 μm in the depth direction from the wafer surface. 12 atoms / cm 3 or more, and the BMD density is 1×10 5 atoms / cm 3 It is characterized by being less than In addition, in the region within 30 μm in the depth direction from the wafer surface, the concentration of vacancy-based complex defects is 1×10 12 atoms / cm 3 It is desirable to have the above areas.

[0011] Thus, the oxygen concentration in the bulk region of a silicon wafer is 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 In the region within 100 μm deep from the wafer surface, the concentration of vacancy-based complex defects gradually increases with increasing depth from the surface. Preferably, in the region within 30 μm deep from the wafer surface, the concentration of vacancy-based complex defects is 1×10 12 atoms / cm 3In addition, the silicon wafer has a BMD density of 1×10 within 50 μm from the surface. 5 atoms / cm 3 is less than. Therefore, although the bulk region has a low oxygen concentration and the gettering ability of BMD is low, the vacancy-based complex defects can provide sufficient gettering ability for heavy metals.

[0012] In order to solve the above problems, the method for producing a silicon wafer according to the present invention is characterized in that the silicon wafer cut from a silicon single crystal has an oxygen concentration of 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 The method includes the steps of placing the wafer described below in a chamber, introducing an inert gas having an oxygen partial pressure of 1% to 10% into the chamber, and performing heat treatment at a maximum temperature of 1250° C. to 1350° C.

[0013] In order to solve the above problems, the method for producing a silicon wafer according to the present invention is characterized in that the silicon wafer cut from a silicon single crystal has an oxygen concentration of 1×10 16 atoms / cm 3 More than 1×10 17 atoms / cm 3 the step of placing a wafer of less than 10% oxygen in a chamber; the step of introducing into the chamber a mixed gas of oxygen gas having an oxygen partial pressure higher than 10% and an inert gas; and the step of performing a heat treatment at a maximum attainable temperature within a region surrounded by a line segment connecting two points (x, y)=(10%, 1250°C) and (x, y)=(100%, 1350°C) with a straight line, a line segment connecting two points (x, y)=(100%, 1350°C) and (x, y)=(10%, 1350°C) with a straight line, and a line segment connecting two points (x, y)=(10%, 1350°C) and (x, y)=(10%, 1250°C) with a straight line, where the horizontal axis x is the logarithm of the oxygen partial pressure and the vertical axis y is the maximum attainable temperature of the rapid temperature increase / decrease heat treatment.

[0014] In order to solve the above problems, the method for producing a silicon wafer according to the present invention is characterized in that the silicon wafer cut from a silicon single crystal has an oxygen concentration of 1×10 17 atoms / cm 3 More than 7×10 17 atoms / cm 3 The present invention relates to a process for producing a silicon wafer having a silicon wafer thickness of 100 nm or less and a silicon wafer thickness of 100 nm or less, comprising the steps of: placing a silicon wafer in a chamber; introducing a mixed gas of oxygen gas having an oxygen partial pressure higher than 10% and an inert gas into the chamber; and, assuming that the horizontal axis x is the logarithm of the oxygen partial pressure and the vertical axis y is the maximum temperature achieved in the rapid temperature increase / decrease heat treatment, determining whether the maximum temperature achieved in the rapid temperature increase / decrease heat treatment is within the range of 100 nm or less. and a step of performing heat treatment at the maximum attainable temperature within a region surrounded by a line segment connecting the two points (100%, 1300°C) and (x, y) = (100%, 1350°C) with a straight line, a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line, and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1250°C) with a straight line.

[0015] According to this manufacturing method, the oxygen concentration in the bulk region is 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 The oxygen concentration is low, at 1×10 or less, and the concentration of vacancy-based complex defects is 1×10 or less in the region within 100 μm in the depth direction from the wafer surface. 12 atoms / cm 3 or more, and the BMD density is 1×10 5 atoms / cm 3 In this way, silicon wafers having a diameter of less than 100 mm can be obtained. Effect of the Invention

[0016] According to the present invention, it is possible to provide a silicon wafer having a low oxygen concentration and a low BMD density but with a heavy metal gettering capability, and a method for manufacturing the silicon wafer. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view illustrating a silicon wafer of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an outline of an example of a heat treatment apparatus used for manufacturing the silicon wafer of FIG. [Diagram 3] FIG. 3 is a flow chart showing a process flow of a first embodiment of a method for producing a silicon wafer according to the present invention. [Figure 4] FIG. 4 is a flow chart showing the flow of a second embodiment of the method for producing a silicon wafer according to the present invention. [Diagram 5] FIG. 5 is a flow chart showing a process flow of a third embodiment of a method for producing a silicon wafer according to the present invention. [Figure 6] FIG. 6 is a graph showing the results of Experiment 1 of an embodiment of the present invention. [Figure 7] FIG. 7 is a graph showing other results of Experiment 1 in an embodiment of the present invention. [Figure 8] FIG. 8 is a graph showing the results of Experiment 2 of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. Fig. 1 is a cross-sectional view showing a silicon wafer according to the present invention. As shown in Fig. 1, a DZ layer 2, which is a defect-free region (denuded zone), is formed on the surface side of a silicon wafer 1. Below the DZ layer 2 is a bulk region 3, and this bulk layer 3 is formed at a depth of 30 µm or less, more preferably 50 µm or less, from the wafer surface.

[0019] The silicon wafer 1 has an oxygen concentration of 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3In the region A within 100 μm from the wafer surface, the concentration of vacancy-based complex defects (microvacancy-oxygen complex defects) gradually increases with increasing depth from the surface, and in the region B within 30 μm from the wafer surface, the concentration of vacancy-based complex defects (microvacancy-oxygen complex defects) is 1×10 12 atoms / cm 3 This is the result. In this way, 1 × 10 12 atoms / cm 3 By having a concentration of vacancy-based complex defects of this or higher level, it is possible to provide a sufficient gettering ability for heavy metals such as Ni and Cu. In addition, in the silicon wafer 1, the BMD density in the region C within 50 μm from the surface is 1×10 5 atoms / cm 3 Although the gettering ability of the BMDs is reduced due to the low BMD density, the generation of leakage current can be suppressed, making the material suitable for use in imaging elements such as power devices and CMOS image sensors.

[0020] Fig. 2 is a cross-sectional view showing an overview of an example of a heat treatment apparatus (RTP apparatus) used for manufacturing the silicon wafer of Fig. 1. As shown in Fig. 2, the heat treatment apparatus 10 includes a chamber (reaction tube) 20 having an atmospheric gas inlet 20a and an atmospheric gas outlet 20b, a plurality of lamps 30 arranged at a distance from each other on the upper part of the chamber 20, and a wafer support part 40 that supports the silicon wafer 1 in the reaction space 25 in the chamber 20. In addition, although not shown, the heat treatment apparatus includes a rotation means for rotating the silicon wafer 1 around its central axis at a predetermined speed.

[0021] The wafer support 40 includes an annular susceptor 40a that supports the outer periphery of the silicon wafer 1, and a stage 40b that supports the susceptor 40a. The chamber 20 is made of, for example, quartz. The lamp 30 is made of, for example, a halogen lamp. The susceptor 40a is made of, for example, SIC. The stage 40b is made of, for example, quartz.

[0022] 2, the silicon wafer 1 is introduced into the reaction space 25 through a substrate inlet (not shown) provided in the chamber 20, and the silicon wafer 1 is placed on the susceptor 40a of the wafer support 40. Then, an atmospheric gas, which will be described later, is introduced through the atmospheric gas inlet 20a, and the silicon wafer 1 is rotated by a rotating means (not shown) while the wafer surface is irradiated with light from the lamps 30.

[0023] The temperature in the reaction space 25 in the heat treatment device 10 is controlled by measuring the average temperature at multiple points (e.g., nine points) on the wafer surface in the radial direction of the lower part of the silicon wafer 1 using a plurality of radiation thermometers 50 embedded in the stage 40b of the wafer support part 40, and controlling the plurality of halogen lamps 30 (individual ON-OFF control of each lamp, control of the emission intensity of the emitted light, etc.) based on the measured temperatures.

[0024] Next, a first embodiment of a method for producing a silicon wafer according to the present invention will be described with reference to the flow chart of FIG. In the method for producing a silicon wafer according to the present invention, a silicon wafer sliced ​​from a silicon single crystal ingot grown by, for example, the Czochralski method (CZ method) is subjected to a heat treatment under predetermined production conditions.

[0025] The growth of a silicon single crystal ingot by the Czochralski method is carried out by a well-known method. That is, polycrystalline silicon filled in a quartz crucible is heated to form silicon melt, a seed crystal is brought into contact with the silicon melt from above the liquid surface, and the seed crystal and the quartz crucible are pulled up while rotating, and the diameter is expanded to a desired diameter to grow a straight body portion, thereby producing a silicon single crystal ingot. The silicon single crystal ingot pulled up here has an oxygen concentration of 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3In order to achieve the following, it is desirable to suppress convection of the silicon melt by applying a magnetic field by the MCZ method, and to grow the single crystal by slowing down the rotation speed of the single crystal and the crucible, etc. However, the method for pulling the silicon single crystal is not limited to the MCZ method, and the silicon single crystal may be grown by, for example, the CZ method or the FZ method in which no magnetic field is applied.

[0026] The pulled silicon single crystal ingot is processed into silicon wafers by a well-known method (step S1 in FIG. 3). That is, a silicon single crystal ingot is sliced ​​into plates using an inner peripheral blade or a wire saw, and then processed to form silicon wafers through processes such as chamfering the outer periphery, lapping, etching, and polishing. 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 The following silicon wafers are obtained: It should be noted that the processing steps described here are merely examples, and the present invention is not limited to these processing steps.

[0027] Next, the obtained silicon wafer is subjected to a heat treatment under predetermined manufacturing conditions. Specifically, in a heat treatment apparatus 10 as shown in Fig. 2, the silicon wafer is placed in a chamber 20 maintained at a desired initial temperature (step S2 in Fig. 3). After the silicon wafer is placed, a gas mixture of oxygen (O2) and an inert gas is introduced at a predetermined flow rate from the atmospheric gas inlet 20a into the chamber 20, preferably with an oxygen partial pressure set in the range of 1% to 10%. Examples of the inert gas include Ar gas and nitrogen gas.

[0028] Then, the inside of the chamber 20 is heated by the halogen lamps 30 at a temperature increase rate (30° C. / sec or more and 100° C. / sec or less), and a rapid temperature increase / decrease thermal process (RTP) is performed at a maximum temperature of 1250° C. or more and 1350° C. or less for a predetermined time (e.g., 10 seconds or more and 50 seconds or less) (step S3 in FIG. 3). In order to control the oxygen partial pressure in the heat treatment space to a constant value, the gas within the chamber is exhausted from exhaust port 20b at a predetermined flow rate. When the high-temperature heat treatment is completed, the temperature inside the chamber is lowered to a predetermined temperature at a predetermined rate (for example, 10° C. / sec to 150° C. / sec) to finish the heat treatment (Step S4 in FIG. 3).

[0029] By such rapid temperature increase and decrease heat treatment, BMDs, which are likely to be a source of leakage current when devices are formed, are hardly formed in the surface layer of the silicon wafer which becomes the active layer of the device. Instead, vacancies introduced by the heat treatment react with extremely low concentration oxygen to form vacancy-oxygen complex defects (vacancy complex defects), which act as a gettering source for heavy metals such as Fe, Ni, and Cu. Specifically, silicon wafer 1 has a vacancy complex defect concentration of 1×10 12 atoms / cm 3 In the region within 100 μm from the wafer surface, the concentration of vacancy-based complex defects gradually increases with increasing depth from the surface, and in the region within 30 μm from the wafer surface, the concentration exceeds 1×10 12 atoms / cm 3 That's all. In addition, the silicon wafer 1 has a BMD density of 1×10 in a region within 50 μm from the surface. 5 atoms / cm 3 Therefore, the generation of leakage current due to BMD can be suppressed.

[0030] After the heat treatment of the silicon wafer 1, the silicon wafer 1 is taken out of the chamber 20, and the oxide film formed on the surface of the silicon wafer 1 by the heat treatment is removed by, for example, HF cleaning, to obtain the silicon wafer 1 of the present invention.

[0031] Next, a second embodiment of the method for producing a silicon wafer according to the present invention will be described with reference to the flow chart of FIG. In the second embodiment, similarly to the first embodiment, a silicon wafer sliced ​​from a silicon single crystal ingot grown by, for example, the Czochralski method (CZ method) is subjected to a heat treatment under predetermined manufacturing conditions.

[0032] The growth of a silicon single crystal ingot by the Czochralski method is carried out by a well-known method. That is, polycrystalline silicon filled in a quartz crucible is heated to form silicon melt, a seed crystal is brought into contact with the silicon melt from above the liquid surface, and the seed crystal and the quartz crucible are pulled up while rotating, and the diameter is expanded to a desired diameter to grow a straight body portion, thereby producing a silicon single crystal ingot. The silicon single crystal ingot pulled up here has an oxygen concentration of 1×10 16 atoms / cm 3 More than 1×10 17 atoms / cm 3 In order to keep the above temperature below 1000° C., it is desirable to suppress convection of the silicon melt by applying a magnetic field in the MCZ method and to grow the silicon single crystal by slowing down the rotation speed of the single crystal and the crucible, etc. However, the method for pulling the silicon single crystal is not limited to the MCZ method, and the silicon single crystal may be grown by using, for example, the CZ method or the FZ method in which no magnetic field is applied.

[0033] The pulled silicon single crystal ingot is processed into silicon wafers by a well-known method (Step St1 in FIG. 4). That is, a silicon single crystal ingot is sliced ​​into plates using an inner peripheral blade or a wire saw, and then processed to form silicon wafers through processes such as chamfering the outer periphery, lapping, etching, and polishing. 16 atoms / cm 3 More than 1×10 17 atoms / cm 3 Silicon wafers of less than 100 mm can be obtained. It should be noted that the processing steps described here are merely examples, and the present invention is not limited to these processing steps.

[0034] Next, the obtained silicon wafer is subjected to a heat treatment under predetermined manufacturing conditions. Specifically, in a heat treatment apparatus 10 as shown in Fig. 2, the silicon wafer is placed in a chamber 20 maintained at a desired initial temperature (Step St2 in Fig. 4). After the silicon wafer is placed, a gas mixture of oxygen (O2) and an inert gas, with the oxygen partial pressure set to be higher than 10% (e.g., 70%), is introduced at a predetermined flow rate from the atmospheric gas inlet 20a into the chamber 20. Examples of the inert gas include Ar gas and nitrogen gas.

[0035] Then, the inside of the chamber 20 is heated by the halogen lamps 30 at a temperature increase rate (30° C. / sec to 100° C. / sec), and rapid temperature ramping (RTP) is performed for a predetermined time (e.g., 10 seconds to 50 seconds) (step St3 in FIG. 4). Here, the oxygen partial pressure and the maximum temperature are set within a region surrounded by a line segment connecting the two points (x, y) = (10%, 1250°C) and (x, y) = (100%, 1350°C) with a straight line, a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line, and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1250°C) with a straight line, as shown in FIG. 6, where the horizontal axis x is the logarithm of the oxygen partial pressure and the vertical axis y is the maximum temperature achieved in the rapid temperature increase / decrease heat treatment. In order to control the oxygen partial pressure in the heat treatment space to a constant value, the gas within the chamber is exhausted from exhaust port 20b at a predetermined flow rate. When the high-temperature heat treatment is completed, the temperature inside the chamber is lowered to a predetermined temperature at a predetermined temperature lowering rate (for example, 10° C. / sec to 150° C. / sec), and the heat treatment is terminated (step St4).

[0036] By such rapid temperature increase and decrease heat treatment, BMDs, which are likely to be a source of leakage current when devices are formed, are hardly formed in the surface layer of the silicon wafer which becomes the active layer of the device. Instead, vacancies introduced by the heat treatment react with extremely low concentration oxygen to form vacancy-oxygen complex defects (vacancy complex defects), which act as a gettering source for heavy metals such as Fe, Ni, and Cu. Specifically, silicon wafer 1 has a vacancy complex defect concentration of 1×10 12 atoms / cm 3 In the region within 100 μm from the wafer surface, the concentration of vacancy-based complex defects gradually increases with increasing depth from the surface, and in the region within 30 μm from the wafer surface, the concentration exceeds 1×10 12 atoms / cm 3 That's all. In addition, the silicon wafer 1 has a BMD density of 1×10 in a region within 50 μm from the surface. 5 atoms / cm 3 Therefore, the generation of leakage current due to BMD can be suppressed.

[0037] After the heat treatment of the silicon wafer 1, the silicon wafer 1 is taken out of the chamber 20, and the oxide film formed on the surface of the silicon wafer 1 by the heat treatment is removed by, for example, HF cleaning, to obtain the silicon wafer 1 of the present invention.

[0038] Next, a third embodiment of the method for producing a silicon wafer according to the present invention will be described with reference to the flow chart of FIG. In the third embodiment, similarly to the first and second embodiments, a silicon wafer sliced ​​from a silicon single crystal ingot grown by, for example, the Czochralski method (CZ method) is subjected to a heat treatment under predetermined manufacturing conditions.

[0039] The growth of a silicon single crystal ingot by the Czochralski method is carried out by a well-known method. That is, polycrystalline silicon filled in a quartz crucible is heated to form silicon melt, a seed crystal is brought into contact with the silicon melt from above the liquid surface, and the seed crystal and the quartz crucible are pulled up while rotating, and the diameter is expanded to a desired diameter to grow a straight body portion, thereby producing a silicon single crystal ingot. The silicon single crystal ingot pulled up here has an oxygen concentration of 1×10 17 atoms / cm 3 More than 7×10 17 atoms / cm3 In order to achieve the following, it is desirable to suppress convection of the silicon melt by applying a magnetic field by the MCZ method, and to grow the single crystal by slowing down the rotation speed of the single crystal and the crucible, etc. However, the method for pulling the silicon single crystal is not limited to the MCZ method, and the silicon single crystal may be grown by, for example, the CZ method or the FZ method in which no magnetic field is applied.

[0040] The pulled silicon single crystal ingot is processed into silicon wafers by a well-known method (Step Sp1 in FIG. 5). That is, a silicon single crystal ingot is sliced ​​into plates using an inner peripheral blade or a wire saw, and then processed to form silicon wafers through processes such as chamfering the outer periphery, lapping, etching, and polishing. 17 atoms / cm 3 More than 7×10 17 atoms / cm 3 The following silicon wafers are obtained: It should be noted that the processing steps described here are merely examples, and the present invention is not limited to these processing steps.

[0041] Next, the obtained silicon wafer is subjected to a heat treatment under predetermined manufacturing conditions. Specifically, in a heat treatment apparatus 10 as shown in Fig. 2, the silicon wafer is placed in a chamber 20 maintained at a desired initial temperature (step Sp2 in Fig. 5). After the silicon wafer is placed, a gas mixture of oxygen (O2) and an inert gas, with the oxygen partial pressure set to be higher than 10% (e.g., 70%), is introduced at a predetermined flow rate from the atmospheric gas inlet 20a into the chamber 20. Examples of the inert gas include Ar gas and nitrogen gas.

[0042] Then, the inside of the chamber 20 is heated by the halogen lamps 30 at a temperature increase rate (30° C. / sec to 100° C. / sec), and rapid temperature ramping (RTP) is performed for a predetermined time (e.g., 10 seconds to 50 seconds) (step Sp3 in FIG. 5). Here, the oxygen partial pressure and the maximum temperature are set within a region surrounded by a line segment connecting the two points (x, y) = (10%, 1250°C) and (x, y) = (100%, 1300°C) with a straight line, a line segment connecting the two points (x, y) = (100%, 1300°C) and (x, y) = (100%, 1350°C) with a straight line, a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line, and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line. In order to control the oxygen partial pressure in the heat treatment space to a constant value, the gas within the chamber is exhausted from exhaust port 20b at a predetermined flow rate. When the high-temperature heat treatment is completed, the temperature inside the chamber is lowered to a predetermined temperature at a predetermined rate (for example, 10° C. / sec to 150° C. / sec), and the heat treatment is terminated (step Sp4 in FIG. 5).

[0043] By such rapid temperature increase and decrease heat treatment, BMDs, which are likely to be a source of leakage current when devices are formed, are hardly formed in the surface layer of the silicon wafer which becomes the active layer of the device. Instead, vacancies introduced by the heat treatment react with extremely low concentration oxygen to form vacancy-oxygen complex defects (vacancy complex defects), which act as a gettering source for heavy metals such as Fe, Ni, and Cu. Specifically, silicon wafer 1 has a vacancy complex defect concentration of 1×10 12 atoms / cm 3 In the region within 100 μm from the wafer surface, the concentration of vacancy-based complex defects gradually increases with increasing depth from the surface, and in the region within 30 μm from the wafer surface, the concentration exceeds 1×10 12 atoms / cm 3 That's all. In addition, the silicon wafer 1 has a BMD density of 1×10 in a region within 50 μm from the surface. 5 atoms / cm 3Therefore, the generation of leakage current due to BMD can be suppressed.

[0044] After the heat treatment of the silicon wafer 1, the silicon wafer 1 is taken out of the chamber 20, and the oxide film formed on the surface of the silicon wafer 1 by the heat treatment is removed by, for example, HF cleaning, to obtain the silicon wafer 1 of the present invention.

[0045] As described above, according to the embodiment of the present invention, the oxygen concentration in the bulk region of the silicon wafer 1 is 1×10 16 atoms / cm 3 More than 7×10 17 atoms / cm 3 In the region within 100 μm deep from the wafer surface, the concentration of vacancy-based complex defects gradually increases with increasing depth from the surface, reaching 1×10 12 atoms / cm 3 That's all. Therefore, although the bulk region has a low oxygen concentration and the gettering ability of BMD is low, the vacancy-based complex defects can provide a sufficient gettering ability for heavy metals and the like. In addition, the silicon wafer 1 has a BMD density of 1×10 in a region within 50 μm from the surface. 5 atoms / cm 3 Since the thickness is less than 100 nm, the occurrence of leakage current due to BMD can be suppressed.

[0046] In the above embodiment, silicon wafers are manufactured using silicon single crystals grown by the CZ method. However, the present invention is not limited to this. For example, silicon wafers may be manufactured using silicon single crystals grown by the FZ method. EXAMPLES

[0047] The silicon wafer and the method for manufacturing the silicon wafer according to the present invention will be further described with reference to examples. In the examples, the following experiments were carried out based on the above-described embodiment.

[0048] (Experiment 1) (Condition 1~21) In conditions 1 to 21, in order to grow silicon single crystals with a low oxygen concentration, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 1×10 16 atoms / cm 3 The silicon single crystal was then sliced ​​to a diameter of 300 mm, a thickness of 775 μm, and an oxygen concentration of 1×10 16 atoms / cm 3 This was placed in the chamber shown in Figure 2, and RTP (heating rate 75°C / sec, holding time at the maximum temperature for 20 seconds, cooling rate 120°C / sec) was performed to measure the BMD density and the concentration of vacancy-based complex defects formed on the silicon wafer. Conditions 1 to 21 were combinations (21 combinations) of maximum temperatures of 1350° C., 1300° C., and 1250° C. and oxygen partial pressures of 100%, 70%, 30%, 10%, 7%, 3%, and 1%.

[0049] After the heat treatment, the oxide film formed on the silicon wafer surface was removed by HF cleaning, and then, in order to visualize and confirm oxygen defects, the silicon wafer was placed in a chamber and heat-treated in a 100% oxygen atmosphere at 780°C for 3 hours, followed by another heat treatment at 1000°C for 8 hours. The BMD density and the concentration of vacancy-based complex defects were measured using IR tomography (System Seiko MO-441). The concentration of vacancy-based complex defects is set to 1×10 in a region 100 μm deep (preferably within 30 μm) from the wafer surface in the depth direction because this sufficiently increases the gettering ability of Ni and Cu. 12 atoms / cm 3 The above was considered preferable. In addition, the BMD density is set to 1×10 in the region within 50 μm in the depth direction from the wafer surface to suppress leakage current generation. 5 atoms / cm 3 Less than this was preferred.

[0050] The results of conditions 1 to 21 are shown in Table 1. In Table 1, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Less than was marked as ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3 Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0051] [Table 1]

[0052] As shown in Table 1, when the oxygen concentration of a silicon wafer is 1×10 16 atoms / cm 3 In the case of the 1350°C maximum temperature, good results were obtained regardless of the oxygen partial pressure. That is, the concentration of vacancy-type oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 It became less than. When the maximum temperature is 1300°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 70% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0053] (Condition 22~42) In conditions 22 to 42, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 5 × 10 16 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 5×10 16 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results of conditions 22 to 42 are shown in Table 2. In Table 2, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Those below this were marked with an ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3 Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0054] [Table 2]

[0055] As shown in Table 2, when the oxygen concentration of a silicon wafer is 5×10 16 atoms / cm 3 In the case of the maximum temperature of 1350°C, good results were obtained regardless of the oxygen partial pressure. That is, the concentration of vacancy-type oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 It became less than. When the maximum temperature is 1300°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 70% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0056] (Condition 43~63) In conditions 43 to 63, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 9 × 10 16 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 9×10 16 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 43 to 63 are shown in Table 3. In Table 3, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Those below this were marked with an ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3 Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0057] [Table 3]

[0058] As shown in Table 3, when the oxygen concentration of a silicon wafer is 9×10 16 atoms / cm 3 In the case of the maximum temperature of 1350°C, good results were obtained regardless of the oxygen partial pressure. That is, the concentration of vacancy-type oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×105 atoms / cm 3 It became less than. When the maximum temperature is 1300°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 70% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0059] (Condition 64~84) In conditions 64 to 84, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 1×10 17 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 1×10 17 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 64 to 84 are shown in Table 4. In Table 4, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Those below this were marked with an ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3 Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0060] [Table 4]

[0061] As shown in Table 4, when the oxygen concentration of a silicon wafer is 1×10 17 atoms / cm 3 In the case of the maximum temperature of 1350°C and 1300°C, good results were obtained regardless of the oxygen partial pressure. 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0062] (Condition 85~105) In conditions 85 to 105, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 5×10 17 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 5×10 17 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 85 to 105 are shown in Table 5. In Table 5, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Those below this were marked with an ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3 Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0063] [Table 5]

[0064] As shown in Table 5, when the oxygen concentration of a silicon wafer is 5×10 17 atoms / cm 3 In the case of the maximum temperature of 1350°C and 1300°C, good results were obtained regardless of the oxygen partial pressure.12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0065] (Condition 106~126) In conditions 106 to 126, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 7 × 10 17 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 7×10 17 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 106 to 126 are shown in Table 6. In Table 6, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 Those below this were marked with an ◎. In addition, the density of BMDs on the wafer surface is 1×10 5 atoms / cm 3 The concentration of vacancy-based oxygen defects is less than 1×10 12 atoms / cm 3Those less than this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0066] [Table 6]

[0067] As shown in Table 6, when the oxygen concentration of a silicon wafer is 7×10 17 atoms / cm 3 In the case of the maximum temperature of 1350°C and 1300°C, good results were obtained regardless of the oxygen partial pressure. 12 atoms / cm 3 or more, and the density of BMDs is less than 1×10 5 atoms / cm 3 It became less than. When the maximum temperature is 1250°C, the density of BMDs is 1×10 5 atoms / cm 3 However, when the oxygen partial pressure was 30% or more, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 It became less than. The concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 There was nothing more.

[0068] (Condition 127~147) In conditions 127 to 147, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 8 × 10 17 atoms / cm3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 8×10 17 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 127 to 147 are shown in Table 7. In Table 7, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 Those above this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0069] [Table 7]

[0070] As shown in Table 7, when the oxygen concentration of a silicon wafer is 8×10 17 atoms / cm 3 In the case of the maximum temperature of 1350°C and 1300°C, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 That was all. In addition, when the maximum temperature is 1250°C, the oxygen partial pressure is 30% or less, and the concentration of vacancy-type oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 That was all. In addition, when the oxygen partial pressure is 70% or less, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 That was all.

[0071] (Condition 148~168) In conditions 148 to 168, the rotation speed of the quartz glass crucible was controlled at a low speed while applying a magnetic field by the MCZ method, and the oxygen concentration was kept at 1×10 18 atoms / cm 3 The silicon single crystal was then sliced, and the resulting oxygen concentration was 1×10 18 atoms / cm 3 The other conditions were the same as those in Conditions 1 to 21. The results for conditions 148 to 168 are shown in Table 8. In Table 8, the concentration of vacancy-based oxygen defects was 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 Those above this were rated as △. In addition, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 Those that met the above criteria were marked as x.

[0072] [Table 8]

[0073] As shown in Table 8, when the oxygen concentration of a silicon wafer is 1×10 18 atoms / cm 3 In the case of the maximum temperature of 1350°C and 1300°C, the concentration of vacancy-based oxygen defects is 1×1012 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 That was all. In addition, when the maximum temperature is 1250°C, the oxygen partial pressure is 30% or less, and the concentration of vacancy-type oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 That was all. In addition, when the oxygen partial pressure is 70% or less, the concentration of vacancy-based oxygen defects is 1×10 12 atoms / cm 3 The density of BMDs is less than 1×10 5 atoms / cm 3 That was all.

[0074] As shown in Tables 1 to 8, when the oxygen concentration of the silicon wafer is 1×10 16 atoms / cm 3 More than 1×10 17 atoms / cm 3 In the case where the concentration of vacancy-type oxygen defects is less than 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 It was confirmed that it was less than In addition, when the oxygen partial pressure is higher than 10%, as shown in FIG. 6, where the horizontal axis x is the logarithm of the oxygen partial pressure and the vertical axis y is the maximum temperature achieved in the rapid temperature increase / decrease heat treatment, it is necessary to perform the heat treatment at an oxygen partial pressure and maximum temperature achieved within the region surrounded by a line segment connecting the two points (x, y) = (10%, 1250°C) and (x, y) = (100%, 1350°C) with a straight line, a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line, and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1250°C) with a straight line.

[0075] In addition, the oxygen concentration of the silicon wafer is 1×10 17 atoms / cm 3 More than 7×10 17 atoms / cm 3 In the case of , under the heat treatment conditions in the region surrounded by the dashed line as shown in the graph of FIG. 7, the concentration of vacancy-type oxygen defects is 1×10 12 atoms / cm 3 or more, and the density of BMDs is 1×10 5 atoms / cm 3 It was confirmed that it was less than In addition, when the oxygen partial pressure is higher than 10%, as shown in the graph of FIG. 7, if the horizontal axis x is the logarithm of the oxygen partial pressure and the vertical axis y is the maximum temperature reached in the rapid temperature increase / decrease heat treatment, the line segment connecting the two points (x, y)=(10%, 1250°C) and (x, y)=(100%, 1300°C) with a straight line and the line segment connecting the two points (x, y)=(100%, 1300°C) and (x, y)=(100%, Heat treatment must be performed at the oxygen partial pressure and maximum temperature within the area surrounded by the line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C), the line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1250°C), and the line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C). In addition, the oxygen concentration of the silicon wafer is 7×10 17 atoms / cm 3 If it is larger, the vacancy-based oxygen defects and the BMD density cannot satisfy the conditions of the silicon wafer of the present invention.

[0076] (Experiment 2) In experiment 2, an example that satisfied the heat treatment conditions within the dashed lines in Figures 6 and 7 and a comparative example that did not satisfy the heat treatment conditions were carried out, and 100 power devices were manufactured using the obtained wafers, and the yield rate (%) was calculated. The conditions for Example 1 were: maximum temperature of 1350°C, oxygen partial pressure of 3%, oxygen concentration of silicon wafer of 5×10 16 atoms / cm 3 It was decided. The conditions for Example 2 were: maximum temperature of 1250°C, oxygen partial pressure of 10%, oxygen concentration of silicon wafer of 5×10 17 atoms / cm 3 It was decided. The conditions for Example 3 were: maximum temperature of 1300°C, oxygen partial pressure of 30%, oxygen concentration of silicon wafer of 7×10 17 atoms / cm 3 It was decided. The conditions for Comparative Example 1 were: maximum temperature of 1350°C, oxygen partial pressure of 30%, oxygen concentration of silicon wafer of 1×10 18 atoms / cm 3 It was decided. The conditions of Comparative Example 2 were: maximum temperature reached 1250°C, oxygen partial pressure 100%, oxygen concentration of silicon wafer 1×10 18 atoms / cm 3 It was decided.

[0077] The results of Examples 1 to 3 and Comparative Examples 1 and 2 are shown in the graph of Fig. 8. The vertical axis of the graph in Fig. 8 is the yield rate (%) of the power device manufacturing. As shown in the graph of FIG. 8, in Examples 1 to 3, the yield rate was 90% or more, but in Comparative Examples 1 and 2, the yield rate was significantly reduced, confirming the effect of the silicon wafer of the present invention. [Explanation of symbols]

[0078] 1. Silicon wafer 2 DZ layer 3. Bulk Region 10 Heat treatment device 20 Chamber 20a Atmospheric gas inlet 20b Atmospheric gas exhaust port 25 Reaction Space 30 Lamp 40 Wafer support

Claims

1. The oxygen concentration in the bulk region is 1×10 16 atoms / cm 3 Above 7 x 10 17 atoms / cm 3 A silicon wafer comprising: In a region within 100 μm in the depth direction from the wafer surface, the concentration of vacancy-based complex defects is 1×10 12 atoms / cm 3 With the above areas, In a region within 50 μm in the depth direction from the wafer surface, the BMD density is 1×10 5 atoms / cm 3 A silicon wafer, comprising:

2. In a region within 30 μm in the depth direction from the wafer surface, the concentration of vacancy-based complex defects is 1×10 12 atoms / cm 3 2. The silicon wafer according to claim 1, comprising the above-mentioned regions.

3. A method for manufacturing a silicon wafer, comprising the steps of: The oxygen concentration of silicon cut from a single crystal is 1×10 16 atoms / cm 3 Above 7 x 10 17 atoms / cm 3 placing a silicon wafer in a chamber; introducing a mixed gas of oxygen gas having an oxygen partial pressure of 1% to 10% and an inert gas into the chamber, and performing a rapid temperature increase and decrease heat treatment with a maximum temperature of 1250° C. to 1350° C.

4. A method for manufacturing a silicon wafer, comprising the steps of: The oxygen concentration of silicon cut from a single crystal is 1×10 16 atoms / cm 3 Above 1 x 10 17 atoms / cm 3 placing a wafer less than 1 mm in a chamber; introducing a mixed gas of oxygen gas having an oxygen partial pressure higher than 10% and an inert gas into the chamber; a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line; a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line; and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1250°C) with a straight line, where the horizontal axis x is the logarithm of oxygen partial pressure and the vertical axis y is the maximum temperature reached in rapid temperature increase and decrease heat treatment.

5. A method for manufacturing a silicon wafer, comprising the steps of: The oxygen concentration of silicon cut from a single crystal is 1×10 17 atoms / cm 3 Above 7 x 10 17 atoms / cm 3 placing a silicon wafer in a chamber; introducing a mixed gas of oxygen gas having an oxygen partial pressure higher than 10% and an inert gas into the chamber; 4. A method for manufacturing a silicon wafer, comprising: performing a heat treatment at a maximum attainable temperature within a region surrounded by a line segment connecting the two points (x, y) = (10%, 1250°C) and (x, y) = (100%, 1300°C) with a straight line; a line segment connecting the two points (x, y) = (100%, 1300°C) and (x, y) = (100%, 1350°C) with a straight line; a line segment connecting the two points (x, y) = (100%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line; and a line segment connecting the two points (x, y) = (10%, 1350°C) and (x, y) = (10%, 1350°C) with a straight line, wherein the horizontal axis x is the logarithm of oxygen partial pressure and the vertical axis y is the maximum attainable temperature of a rapid temperature increase / decrease heat treatment.

Citation Information

Patent Citations

  • Method of evaluating oxygen concentration of silicon sample

    JP2021118283A