Multilayered substrate

The multilayer substrate design with a controlled silicon concentration distribution in the GaN layer, using an annular dummy wafer, addresses the non-uniformity issue, enhancing semiconductor device performance and efficiency.

JP2024148749AActive Publication Date: 2024-10-18SUMITOMO CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023062139
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Laminated substrates with gallium nitride (GaN) layers exhibit significant in-plane non-uniformity in silicon concentration distribution, particularly on the outer circumferential side, which affects the performance and efficiency of semiconductor devices.

Method used

A multilayer substrate design with a gallium nitride layer having a diameter of 50 mm or more and a thickness of 4 μm or more, where the silicon concentration on the outer periphery is controlled by using an annular dummy wafer to reduce the excess silicon concentration relative to the center, maintaining a difference of 1.2×10^15 cm^-3 or less, and ensuring uniformity through controlled growth conditions.

Benefits of technology

The solution effectively suppresses in-plane non-uniformity of silicon concentration in the GaN layer, improving the breakdown voltage characteristics and resistance characteristics of semiconductor devices while maintaining efficient production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148749000001_ABST
    Figure 2024148749000001_ABST
Patent Text Reader

Abstract

To provide a multilayered substrate in which in-plane non-uniformity of a Si concentration distribution in a GaN layer is suppressed.SOLUTION: A multilayered substrate includes an underlying substrate, and a gallium nitride layer epitaxially grown above the underlying substrate and comprising gallium nitride containing silicon. The gallium nitride layer has a top surface with a radius of 50 mm or more, and the gallium nitride layer has a thickness of 4 μm or more. A silicon concentration on the top surface of the gallium nitride layer has a distribution in which an outer circumferential silicon concentration at a radial position 10 mm from an edge of the top surface is higher than a central silicon concentration at a center of the top surface, the central silicon concentration is 4×1015 cm-3 or more and less than 2×1016 cm-3, and an outer circumferential silicon contamination concentration, which is an excess of the outer circumferential silicon concentration from the central silicon concentration, is 1.2×1015 cm-3 or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated substrate. [Background technology]

[0002] A laminated substrate in which a gallium nitride (GaN) layer is epitaxially grown on various base substrates is used as a material for manufacturing a semiconductor device (see, for example, Patent Document 1). In order to improve the production efficiency of semiconductor devices, the diameter of the laminated substrate is being increased. Silicon (Si) is used as an n-type impurity added to the GaN layer.

[0003] As described in detail below, the inventors of the present application have investigated a multilayer substrate having a large diameter, a low concentration of added Si, and a thick GaN layer, and have discovered that the GaN layer is prone to in-plane non-uniformity in the Si concentration distribution (specifically, non-uniformity in which the Si concentration is higher on the outer periphery of the GaN layer). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-199601 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a multilayer substrate in which the in-plane non-uniformity of the Si concentration distribution in a GaN layer is suppressed. [Means for solving the problem]

[0006] According to one aspect of the present invention A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of silicon-containing gallium nitride; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 More than 2×10 16 cm -3 is less than The peripheral silicon contamination concentration, which is the excess of the peripheral silicon concentration from the central silicon concentration, is 1.2×10 15 cm -3 Below is the Multilayer Substrate is provided. Effect of the Invention

[0007] A laminated substrate is provided in which the in-plane non-uniformity of the Si concentration distribution in the GaN layer is suppressed. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating a laminated substrate according to an embodiment. [Diagram 2] FIG. 2 is a top view of a GaN layer for explaining a method for measuring the Si concentration in the GaN layer. [Diagram 3] FIG. 3 is a schematic side view showing a manufacturing apparatus for a GaN layer according to an embodiment. [Figure 4] FIG. 4 is a graph showing an example of a Si concentration distribution in the upper surface of the GaN layer in the first example of the embodiment. [Diagram 5] FIG. 5 is a graph that diagrammatically shows the Si concentration distribution of the first example similar to FIG. [Figure 6] FIG. 6 is a graph showing an example of a Si concentration distribution in the upper surface of the GaN layer in the second example of the embodiment. [Figure 7]FIG. 7 is a graph that illustrates a Si concentration distribution of a second example similar to that of FIG. [Figure 8] FIG. 8 is a schematic side view showing a manufacturing apparatus for a GaN layer according to a comparative embodiment. [Figure 9] FIG. 9 is a graph showing an example of the Si concentration distribution in the upper surface of the GaN layer according to the comparative example. [Figure 10] FIG. 10 is a graph showing a schematic diagram of the Si concentration distribution in a comparative example similar to that in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] A laminated substrate 100 according to an embodiment of the present invention will be described. Fig. 1 is a schematic cross-sectional view illustrating the laminated substrate 100. The laminated substrate 100 has at least an underlayer structure 10 and a gallium nitride (GaN) layer 20 formed on the underlayer structure 10.

[0010] The base structure 10 has at least a base substrate which is a crystal substrate for epitaxially growing the GaN layer 20. The base structure 10 may have a buffer layer between the base substrate and the GaN layer 20, as required. The structure of the buffer layer may be appropriately selected as required.

[0011] As the base substrate, a GaN substrate, a sapphire substrate, a silicon (Si) substrate, a silicon carbide (SiC) substrate, or the like may be appropriately used. For example, when the base substrate is a GaN substrate, the base structure 10 may be a GaN substrate. For example, when the base substrate is a Si substrate, the base structure 10 may have a Si substrate and an aluminum nitride (AlN) layer provided as a nucleation layer, or the like.

[0012] The laminated substrate 100 may have an upper layer 30 formed on the GaN layer 20 as necessary. The structure of the upper layer 30 may be appropriately selected depending on the operation of a semiconductor device to be fabricated using the laminated substrate 100. The upper layer 30 may be, for example, a Group III nitride layer epitaxially grown on the GaN layer 20.

[0013] The GaN layer 20 according to the embodiment has the following characteristics. The GaN layer 20 has a top surface 25 with a radius of 50 mm or more (a diameter of 100 mm or more). In other words, the multilayer substrate 100 has a circular shape with a diameter of 100 mm or more. The multilayer substrate 100 may have an orientation flat or a notch as necessary.

[0014] Silicon (Si) is contained as an n-type impurity in GaN layer 20. The Si concentration in upper surface 25 of GaN layer 20 has a distribution in which a central Si concentration C0 at the center of upper surface 25 is higher than a peripheral Si concentration C1 at the periphery of upper surface 25.

[0015] The central Si concentration C0 is 10 15 cm -3 This is a low concentration where a concentration fluctuation of the order of 4×10 15 cm -3 More than 2×10 16 cm -3 The central Si concentration C0 is less than 1×10 16 cm -3 Less than (i.e. 10 15 cm -3 In the case where the Si concentration C1 is in the order of 1.2×10, this effect is more significant. The excess of the peripheral Si concentration C1 from the central Si concentration C0, Δ (i.e., C1−C0), is 1.2×10 15 cm -3 In other words, the peripheral Si concentration C1 is higher than the central Si concentration C0, but the peripheral Si contamination concentration Δ, which is the difference between the two, is set to 1.2×10 15 cm -3 The thickness of the GaN layer 20 is suppressed to be equal to or less than 4 μm. The thickness of the GaN layer 20 is, for example, equal to or less than 40 μm.

[0016] The GaN layer 20 is a layer that functions as at least a part of an operating layer in a semiconductor device including the multilayer substrate 100. For this reason, it is preferable that the GaN layer 20 has a well-balanced breakdown voltage characteristic and resistance characteristic. From the viewpoint of improving the breakdown voltage, the central Si concentration C0 of the GaN layer 20 is 2×1016 cm -3 From the viewpoint of improving the breakdown voltage, the thickness of the GaN layer 20 is preferably 4 μm or more. From the viewpoint of reducing the resistance, the central Si concentration C0 of the GaN layer 20 is preferably 4×10 15 cm -3 From the viewpoint of reducing resistance, the thickness of the GaN layer 20 is preferably 40 μm or less.

[0017] As will be described in detail later, the peripheral Si contamination concentration Δ is the concentration of Si that is introduced into the periphery of the GaN layer 20 due to the Si-containing deposition 230. The central Si concentration C0 is approximately equal to the target addition concentration, which is the Si concentration that is intentionally added. The peripheral Si contamination concentration Δ is the excess of the central Si concentration C0 at the periphery due to the introduced Si. The GaN layer 20 according to the embodiment has a feature that the peripheral Si contamination concentration Δ is suppressed compared to the comparative embodiment.

[0018] In the following description, the radius of the GaN layer 20 is 50 mm, the thickness of the GaN layer 20 is 4 μm, and the target Si doping concentration in the GaN layer 20 is 9×10 15 cm -3 Such conditions are common to the embodiment and comparative example.

[0019] A method for measuring the Si concentration in GaN layer 20 will be described. Fig. 2 is a top view of GaN layer 20 for explaining a method for measuring the Si concentration in GaN layer 20. An XY Cartesian coordinate system is set on top surface 25 of GaN layer 20, with the center of top surface 25 as the origin.

[0020] First, the measurement positions within the surface will be described. At least five measurement points, including a central measurement point and four outer periphery measurement points, are set as the measurement points for the Si concentration on upper surface 25. The central measurement point is set at the center of upper surface 25. The four outer periphery measurement points are set at radial positions 10 mm from the edge of upper surface 25 (i.e., every 90° in the circumferential direction) for each of the X positive direction, X negative direction, Y positive direction, and Y negative direction. Here, a radial position 10 mm from the edge of upper surface 25 is set as a representative position of the outer periphery when specifying the Si concentration on the outer periphery of upper surface 25.

[0021] The Si concentration at the central measurement point is the central Si concentration C0. The Si concentration obtained by averaging the Si concentration CX+ at the peripheral measurement point in the positive X direction, the Si concentration CX- at the peripheral measurement point in the negative X direction, the Si concentration CY+ at the peripheral measurement point in the positive Y direction, and the Si concentration CY- at the peripheral measurement point in the negative Y direction is the peripheral Si concentration C1. In other words, the peripheral Si concentration C1 indicates the circumferentially averaged Si concentration on the periphery. The excess of the peripheral Si concentration C1 from the central Si concentration C0, i.e., C1-C0, is the peripheral Si contamination concentration Δ.

[0022] In this example, the radius of the upper surface 25 is 50 mm. The four outer periphery measurement points are set at radial positions 40 mm from the center in each of the X positive direction, X negative direction, Y positive direction, and Y negative direction.

[0023] In addition to the center measurement point and the four outer circumference measurement points, intermediate measurement points may be set at radial positions intermediate between the center measurement point and the outer circumference measurement points. In this example, intermediate measurement points are set at radial positions 10 mm, 20 mm, and 30 mm from the center in the X positive direction, X negative direction, Y positive direction, and Y negative direction, respectively. In FIG. 2, for ease of illustration, the center measurement point and the outer circumference measurement points are indicated by large black circles, and the intermediate measurement points are indicated by small black circles.

[0024] Note that even in an embodiment in which the radius of upper surface 25 of GaN layer 20 exceeds 50 mm, the four outer periphery measurement points are set at radial positions of 10 mm from the edge of upper surface 25. Also, even in an embodiment in which the radius of upper surface 25 of GaN layer 20 exceeds 50 mm, the intermediate measurement points may be set at radial positions every 10 mm from the center in each of the X-positive direction, the X-negative direction, the Y-positive direction, and the Y-negative direction.

[0025] The average Si concentration is the Si concentration obtained by averaging the Si concentrations at four measurement points in the X positive direction, the X negative direction, the Y positive direction, and the Y negative direction, which are set at equal radial positions from the center of the upper surface 25, that is, the Si concentration averaged in the circumferential direction for each radial position. The peripheral Si concentration C1 is the average Si concentration on the peripheral edge.

[0026] As described later, the GaN layer 20 is grown so as to be uniform in the circumferential direction. However, in reality, there is variation in the Si concentration even among four measurement points set at equal radial positions. To reduce the effect of such variation, the radial distribution of the Si concentration in the GaN layer 20 is evaluated using an average Si concentration, which is the Si concentration averaged in the circumferential direction. The concentration of the mixed Si is the excess of the average Si concentration from the central Si concentration C0 at each radial position.

[0027] Next, the measurement position in the height direction will be described. As the Si concentration in GaN layer 20, the Si concentration in upper surface 25 is measured by secondary ion mass spectrometry (SIMS). However, "Si concentration in upper surface 25" does not mean the Si concentration just at the height of upper surface 25, but means the Si concentration in the vicinity of upper surface 25, as described below. Upper surface 25 is the top surface of laminated substrate 100 in a mode in which upper layer 30 is not laminated, and is the interface between upper layer 30 and GaN layer 20 in a mode in which upper layer 30 is laminated.

[0028] In general, the reliability of SIMS measurement at the surface position is not high. For this reason, it is preferable to perform SIMS measurement at a height slightly toward the underlayer structure 10 from the upper surface 25, that is, slightly inside the GaN layer 20. It is also preferable to use a measurement value averaged over a certain height range (depth range, thickness range). Here, the average value of SIMS measurement values ​​in a depth range of 100 nm to 200 nm from the upper surface 25 for each measurement point in the plane is defined as the Si concentration at the upper surface 25. For example, in an embodiment in which the thickness of the GaN layer 20 is 4 μm, the average value of the Si concentration by SIMS measurement in a range of 3.8 μm to 3.9 μm from the lower surface of the GaN layer 20 is defined as the Si concentration at the upper surface 25.

[0029] Before further describing the embodiment, a comparative embodiment will be described. Fig. 8 is a schematic side view showing a manufacturing apparatus 200 for a GaN layer 20 according to a comparative embodiment. The manufacturing apparatus 200 is a metal-organic vapor phase epitaxy (MOVPE) apparatus, and has a susceptor 210 on which a wafer 40 is placed. The wafer 40 is a processing target (an intermediate of the laminated substrate 100) at the stage when the growth process of the GaN layer 20 is performed by the manufacturing apparatus 200, and specifically, the wafer 40 is an underlayer structure 10 when the growth of the GaN layer 20 starts, and is a laminate of the underlayer structure 10 and the GaN layer 20 after the growth of the GaN layer 20 starts.

[0030] The manufacturing apparatus 200 is a lateral flow type MOVPE apparatus in which a source gas 220 is supplied in a direction parallel to the upper surface of the wafer 40. The source gas 220 includes a GaN source gas for growing GaN constituting the GaN layer 20, and a Si doping source gas for supplying Si to be added to the GaN layer 20. The GaN source gas includes a gallium (Ga) source gas and a nitrogen (N) source gas. For example, trimethylgallium (TMG) gas is used as the Ga source gas, and ammonia (NH 3 ) gas is used. As the Si doping source gas, for example, silane (SiH 4 ) gas is used.

[0031] The growth temperature can be selected, for example, in the range of 900° C. to 1400° C., and the V / III ratio, which is the flow rate ratio of the group V source gas to the group III source gas, can be selected, for example, in the range of 10 to 5000. The Si doping source gas has a target doping concentration in the GaN layer 20 of 4×10 15 cm -3 More than 2×10 16 cm -3 Less than a given value, e.g., 9×10 15 cm -3 The input signal is supplied so that:

[0032] Susceptor 210 holds wafer 40 so as to rotate wafer 40 about the center of wafer 40. By growing GaN layer 20 while rotating in this manner, the growth conditions of GaN layer 20 can be made uniform in the circumferential direction of wafer 40.

[0033] The susceptor inner peripheral edge 211 is the position of the susceptor 210 where the edge of the wafer 40 is located in a plan view. The susceptor peripheral upper surface 213 is the upper surface of the susceptor 210 between the susceptor inner peripheral edge 211 and the susceptor outer peripheral edge 212.

[0034] During the growth process of the GaN layer 20, the Si-containing deposition 230 adheres to the susceptor edge upper surface 213, and Si is mixed into the GaN layer 20 from the Si-containing deposition 230. The Si-containing deposition 230 is a defective GaN and contains Si. It is presumed that the Si contained in the Si-containing deposition 230 mainly comes from the Ga source gas or the Si doping source gas (one or both of them), but the details are unclear. In addition, it is not realistic to prevent the Si-containing deposition 230 from adhering to the susceptor edge upper surface 213. The mixing of Si from the Si-containing deposition 230 into the GaN layer 20 cannot be controlled by conventional techniques.

[0035] The concentration of Si mixed in from the Si-containing deposition 230 becomes higher toward the inner peripheral edge 211 of the susceptor, that is, toward the outer peripheral side closer to the edge of the wafer 40. The inclusion of Si in the GaN layer 20 due to the Si-containing deposition 230 is called "mixing" and is distinguished from "addition" in which Si is intentionally included in the GaN layer 20 by a Si doping source gas.

[0036] Ideally, the concentration of Si contained in GaN layer 20 is controlled to a target concentration, which is a concentration desired to be added by a Si doping source gas, over the entire area of ​​upper surface 25. Therefore, as will be described in the embodiment below, it is preferable to reduce the amount of Si mixed in from Si-containing deposition 230 as much as possible.

[0037] The concentration of Si mixed into the GaN layer 20 from the Si-containing deposition 230 is approximately the same when grown under the above-mentioned range of growth conditions and when grown under the above-mentioned range of target doping concentrations. Specifically, as described below, the concentration of mixed Si at the outer periphery (a radial position 10 mm from the edge of the wafer 40, and a radial position 10 mm from the inner peripheral edge 211 of the susceptor in the comparative example) is 1.6×10 15 cm -3 It will be about that amount.

[0038] 9 is a graph showing an example of the Si concentration distribution in the upper surface 25 of the GaN layer 20 according to the comparative example. The horizontal axis indicates the in-plane measurement position in mm, and the vertical axis indicates the Si concentration in 10 15 cm -3 The Si concentration at each measurement point in the X direction is shown by a black circle, and the Si concentration at each measurement point in the Y direction is shown by a white square. The average Si concentration is shown by a cross. This method of display is also used in the graphs of FIG. 4 and FIG. 6 relating to the embodiment.

[0039] The central Si concentration C0 is the target doping concentration of 9×10 15 cm -3 The Si concentration is almost constant up to about 10 mm from the center. This means that the mixed Si does not reach the center of the wafer 40.

[0040] At radial positions 20 mm or more away from the center, the concentration of contaminating Si, which is the excess over the central Si concentration C0, is significantly higher. Also, the concentration of contaminating Si increases toward the outer periphery.

[0041] In the comparative example, the central Si concentration C0 is 9.01×10 15 cm -3 The peripheral Si concentration C1 is 10.65×10 15 cm -3 The peripheral Si contamination concentration Δ is 1.64×10 15 cm -3 It is.

[0042] Fig. 10 is a graph showing a schematic diagram of a comparative Si concentration distribution similar to that of Fig. 9. For ease of understanding, Fig. 10 shows the wafer 40 and the inner peripheral edge 211 of the susceptor together with the Si concentration distribution.

[0043] The added distribution D0 is a constant Si concentration distribution equal to the central Si concentration C0 throughout the entire surface of the wafer 40, and typically represents the Si concentration distribution due to Si added by the Si doping source gas. The mixed distribution D1 typically represents the Si concentration distribution due to Si mixed in from the Si-containing deposition 230. The overall Si concentration distribution is expressed as the sum of the added distribution D0 and the mixed distribution D1.

[0044] The Si resulting from the Si-containing deposition 230 is mixed in from the edge of the wafer 40 to a width of about 40 mm in the radial direction. In the case of a large-diameter wafer 40 such as that of a 50 mm radius, as in this example, no Si is mixed in at the center. In contrast, in a case where a wafer with a smaller diameter, such as a 25 mm radius, is used, Si is mixed in at the center of the wafer.

[0045] In the case of a small diameter embodiment where Si is mixed in the center, the mixed Si from both edges on either side of the center overlaps at the center, so that the Si concentration due to the mixed Si is high even at the center. As a result, the Si concentration distribution due to the mixed Si approaches uniformity within the surface.

[0046] In contrast, in the case of a large-diameter wafer such as this example, where no Si is mixed in the center, the Si concentration distribution due to the mixed Si is non-uniform with a large difference between the center and the periphery. Thus, in a large-diameter wafer 40, specifically a wafer with a radius of 50 mm or more, the in-plane non-uniformity of the Si concentration distribution due to the mixed Si becomes significant.

[0047] Although an embodiment with a radius of 50 mm is shown as an example, even in the case of a wafer 40 with a radius of more than 50 mm, the concentration of contaminating Si at the outer periphery (a radial position 10 mm from the edge of the wafer 40, which is a radial position 10 mm from the inner peripheral edge 211 of the susceptor in the comparative embodiment) is approximately the same as in the case of a radius of 50 mm.

[0048] In the comparative example, the peripheral Si contamination concentration Δ, which is the difference in Si concentration between the center and the periphery, is 1.64×10 15 cm -3 On the other hand, the target concentration of Si, that is, the central Si concentration C0, is 10 15 cm -3 Therefore, the influence of the peripheral Si contamination concentration Δ on the in-plane Si concentration distribution becomes significant.

[0049] In this way, when the radius of the upper surface 25 is 50 mm or more and the central Si concentration C0 is 4×10 15 cm -3 More than 2×10 16 cm -3 Less than (even 1×10 16 cm -3 In the GaN layer 20 having a Si concentration of less than 100 nm, the difference in Si concentration between the center and the periphery becomes significant due to the Si contamination. As described below, the embodiment proposes a technique that can suppress such in-plane nonuniformity of the Si concentration compared to the comparative example, that is, a technique that can suppress the peripheral Si contamination concentration Δ compared to the comparative example.

[0050] In addition, the peripheral Si contamination concentration Δ generally tends to increase as the GaN layer 20 becomes thicker. This is because the Si-containing deposits 230 adhering to the susceptor edge upper surface 213 increase as the growth time of the GaN layer 20 becomes longer.

[0051] The comparative example (and the embodiment) illustrates the peripheral Si contamination concentration Δ in the GaN layer 20 having a thickness of 4 μm. If the thickness of the GaN layer 20 is sufficiently thin, the Si contamination caused by the Si-containing deposition 230 may not be enough to cause the above-mentioned in-plane nonuniformity. However, when the GaN layer 20 having a thickness of 4 μm (or more) is grown, the above-mentioned in-plane nonuniformity will occur. As described below, the embodiment proposes a technique that can reduce the peripheral Si contamination concentration Δ in the GaN layer 20 having a thickness of 4 μm compared to the comparative example, and further proposes a technique that can similarly reduce the peripheral Si contamination concentration Δ in the GaN layer 20 having a thickness of more than 4 μm.

[0052] The embodiment will be further described below. Fig. 3 is a schematic side view showing a manufacturing apparatus 200 for a GaN layer 20 according to the embodiment. The manufacturing apparatus 200 according to the embodiment is a lateral flow type MOVPE apparatus, similar to the comparative embodiment.

[0053] In the embodiment, the GaN layer 20 is grown in a state where a circular dummy wafer 50 is arranged on the outer side of the wafer 40 in a plan view. The dummy wafer 50 has a radial width WD and the same thickness as the wafer 40. The material of the dummy wafer 50 (dummy base substrate) at the start of growth of the GaN layer 20 is a base material for epitaxially growing GaN, such as GaN or sapphire. After the start of growth of the GaN layer 20, a structure in which the grown GaN layer is stacked on the dummy base substrate becomes the dummy wafer 50.

[0054] The whole wafer 60 is a structure combining the wafer 40 and the dummy wafer 50. In the embodiment, the object to be processed by the manufacturing apparatus 200 is the whole wafer 60. The edge of the whole wafer 60, that is, the position where the outer periphery of the dummy wafer 50 is located, becomes the inner periphery 211 of the susceptor.

[0055] In the embodiment, since the dummy wafer 50 is disposed outside the wafer 40, the Si released from the Si-containing deposition 230 is preferentially mixed into the GaN grown on the dummy wafer 50. The Si released from the Si-containing deposition 230 and exceeding the width WD of the dummy wafer 50 is mixed into the GaN layer 20 of the wafer 40. In this way, by using the dummy wafer 50, it is possible to reduce the amount of Si mixed into the GaN layer 20 from the Si-containing deposition 230, as compared to the comparative embodiment.

[0056] Next, a first example of the embodiment will be described. In the first example of the embodiment, a mode in which the width WD of the dummy wafer 50 is 10 mm will be illustrated. The growth conditions of the GaN layer 20 in the first example of the embodiment are the same as those in the comparative example described above.

[0057] 4 is a graph showing an example of a Si concentration distribution in the upper surface 25 of the GaN layer 20 in the first example of the embodiment. Although the inclusion of Si on the outer periphery side is observed in the first example of the embodiment as in the comparative example, it is suppressed more than in the comparative example.

[0058] In the first example of the embodiment, specifically, the central Si concentration C0 is 9.00×10 15 cm -3 The peripheral Si concentration C1 is 10.05×10 15 cm -3 The peripheral Si contamination concentration Δ is 1.05×10 15 cm -3 The peripheral Si contamination concentration in the comparative example is Δ1.64×10 15 cm -3 is suppressed compared to

[0059] Peripheral Si contamination concentration in the comparative form: Δ1.64×1015 cm -3 The first concentration standard value is set to 1.2 × 10 15 cm -3 The peripheral Si contamination concentration Δ in the first example of the embodiment is set to the first concentration reference value of 1.2×10 15 cm -3 In FIG. 4 (and FIG. 9), the first concentration standard value is indicated as Δ1.2.

[0060] Fig. 5 is a graph showing a schematic Si concentration distribution in a first example of an embodiment similar to Fig. 4. For ease of understanding, Fig. 5 shows the wafer 40, the dummy wafer 50, and the inner peripheral edge 211 of the susceptor together with the Si concentration distribution.

[0061] The contamination distribution D1 in the comparative embodiment is shown on the center side of the wafer 40, and the contamination distribution D1 in the first example of the embodiment is shown on the outer periphery side of the wafer 40. The dummy wafer 50 has the function of moving the inner peripheral edge 211 of the susceptor away from the wafer 40 compared to the comparative embodiment. This allows the contamination distribution D1 to be shifted 10 mm toward the outer periphery of the wafer 40, which is the width of the dummy wafer 50, compared to the comparative embodiment. In this way, in the first example of the embodiment, the contamination Si concentration can be suppressed to a low level at the bottom side of the contamination distribution D1, compared to the comparative embodiment.

[0062] Next, a second example of the embodiment will be described. In the second example of the embodiment, a mode in which the width WD of the dummy wafer 50 is 20 mm is illustrated. The growth conditions of the GaN layer 20 in the second example of the embodiment are the same as those in the comparative example (or the first example of the embodiment) described above.

[0063] 6 is a graph showing an example of a Si concentration distribution in the upper surface 25 of the GaN layer 20 in the second example of the embodiment. The inclusion of Si on the outer periphery side is seen in the second example of the embodiment as in the comparative example and the first example of the embodiment, but is further suppressed than in the first example of the embodiment.

[0064] In the second example of the embodiment, specifically, the central Si concentration C0 is 8.91×10 15 cm -3 The peripheral Si concentration C1 is 9.44×10 15 cm -3 The peripheral Si contamination concentration Δ is 0.53×10 15 cm -3 In the first embodiment, the peripheral Si contamination concentration Δ is 1.05×10 15 cm -3 is even more suppressed than

[0065] First concentration standard value 1.2 x 10 15 cm -3 The second and third concentration standards are set to be lower than 0.9×10 15 cm -3 and 0.6 × 10 15 cm -3 The peripheral Si contamination concentration Δ in the second example of the embodiment is set to the first concentration reference value of 1.2×10 15 cm -3 The peripheral Si contamination concentration Δ in the second example of the embodiment is preferably suppressed to a second concentration reference value of 0.9×10 15 cm -3 More preferably, the third concentration standard value is 0.6×10 15 cm -3 In FIG. 6, the third concentration standard value is indicated as Δ0.6.

[0066] Fig. 7 is a graph showing a schematic Si concentration distribution in a second example of an embodiment similar to Fig. 6. For ease of understanding, Fig. 7 shows the wafer 40, the dummy wafer 50, and the inner peripheral edge 211 of the susceptor together with the Si concentration distribution.

[0067] The contamination distribution D1 in the comparative example is shown on the center side of the wafer 40, and the contamination distribution D1 in the second example of the embodiment is shown on the outer periphery side of the wafer 40. In the second example of the embodiment, the contamination distribution D1 can be shifted to the outer periphery side of the wafer 40 by 20 mm, the width of the dummy wafer 50, compared to the comparative example. In this way, in the second example of the embodiment, the contamination Si concentration can be suppressed to a lower level further to the bottom side of the contamination distribution D1, compared to the first example of the embodiment.

[0068] As in the second example, by increasing the width WD of the dummy wafer 50, it is possible to further suppress the inclusion of Si on the outer periphery side of the wafer 40. However, increasing the width WD of the dummy wafer 50 increases the area of ​​the entire wafer 60, that is, increases the area of ​​the GaN layer to be grown.

[0069] A horizontal flow type MOVPE apparatus has a characteristic that the larger the area of ​​the GaN layer to be grown, the lower the raw material efficiency (the proportion of raw materials contributing to growth). In the embodiment, since a thick GaN layer 20 with a thickness of 4 μm or more is grown, the lower raw material efficiency leads to a decrease in production efficiency and an increase in costs. In addition, the larger the growth area, the more likely it is that the downstream side will run out of raw materials.

[0070] Therefore, from the viewpoint of favorable growth of the GaN layer 20 on the wafer 40, the area of ​​the entire wafer 60, that is, the width WD of the dummy wafer 50, is preferably small within a range in which the effect of suppressing the inclusion of Si can be appropriately obtained.

[0071] For this reason, the width WD of the dummy wafer 50 is not increased excessively so that the peripheral Si contamination concentration Δ becomes zero. 15 cm -3 The width WD of the dummy wafer 50 is set so that the peripheral Si contamination concentration Δ is equal to or smaller than the fourth concentration reference value 0.3×10 15 cm -3 Keep it to a size equal to or greater than this.

[0072] In this manner, in the embodiment, the peripheral Si contamination concentration Δ is suppressed by using the dummy wafer 50, but the peripheral Si contamination concentration Δ is not reduced to zero. In other words, the peripheral Si concentration C1 remains higher than the central Si concentration C0. Specifically, the peripheral Si contamination concentration Δ is reduced to 0.5×10 15 cm -3 The concentration is suppressed to be equal to or lower than the second concentration standard value of 0.9×10 15 cm -3 More preferably, the third concentration standard value is suppressed to 0.6×10 or less. 15 cm -3 However, the peripheral Si contamination concentration Δ is suppressed to the fourth concentration standard value of 0.3×10 15 cm -3 That's all.

[0073] In addition, when defining that "the peripheral Si concentration C1 is higher than the central Si concentration C0," it is assumed that not only the first condition that the value of the peripheral Si concentration C1 is greater than the value of the central Si concentration C0 is satisfied, but also the second condition described below is satisfied.

[0074] The peripheral Si concentration C1 is the average value of the four peripheral measurement points. If only the average value is considered, for example (hypothetically), the Si concentration at three peripheral measurement points is lower than the central Si concentration C0, but due to the variation in the Si concentration at one peripheral measurement point being extremely high, it may include an inappropriate situation in which the average value, i.e., the peripheral Si concentration C1, is higher than the central Si concentration C0.

[0075] In the embodiment, as described above, the GaN layer 20 is grown while rotating so as to achieve uniformity in the circumferential direction. For this reason, it is preferable to specify the circumferential direction uniformity. Here, when specifying that "the peripheral Si concentration C1 is higher than the central Si concentration C0", an additional second condition is also satisfied, that is, the Si concentration at at least three (preferably four) of the four peripheral measurement points is higher than the central Si concentration C0.

[0076] In the above description, an embodiment in which the thickness of the GaN layer 20 is 4 μm is exemplified. As described above, the longer the growth time of the GaN layer 20, that is, the thicker the GaN layer 20, the more the Si-containing deposition 230 tends to be. As a result, when the width WD of the dummy wafer 50 is constant, the thicker the GaN layer 20, the higher the peripheral Si contamination concentration Δ.

[0077] Therefore, in an embodiment in which the thickness of the GaN layer 20 is thicker than 4 μm, it is preferable to appropriately increase the width WD of the dummy wafer 50 according to the thickness of the GaN layer 20 so that the peripheral Si contamination concentration Δ is reduced to a predetermined value, compared to an embodiment in which the thickness of the GaN layer 20 is 4 μm. In this manner, by appropriately increasing the width WD of the dummy wafer 50 according to the thickness of the GaN layer 20, the peripheral Si contamination concentration Δ can be reduced to a predetermined value even in an embodiment in which the thickness of the GaN layer 20 is thicker than 4 μm.

[0078] The following further describes the features of the GaN layer 20 according to the embodiment. As described above, in the embodiment, the peripheral Si contamination concentration Δ is suppressed by using the dummy wafer 50. This allows the region with low concentration of contaminated Si on the central side of the upper surface 25 of the GaN layer 20 to be expanded toward the outer periphery more than in the comparative embodiment. In other words, the width of the region with high concentration of contaminated Si on the outer periphery side of the upper surface 25 of the GaN layer 20 can be made smaller than in the comparative embodiment.

[0079] The concentration of the mixed Si is 4×10, which is the lower limit of the target concentration, i.e., the lower limit of the central Si concentration C0. 15 cm -3 The Si concentration of 0.4×10 15 cm -3 The region where the Si concentration exceeds 0.4×10 15 cm -3) is denoted as ΔSi. The mixed Si high concentration region is an annular region on the edge side of upper surface 25 of GaN layer 20. The (entire) circular region inside the annular region that is the mixed Si high concentration region is the mixed Si low concentration region. The width from the edge of upper surface 25 of the annular region that is the mixed Si high concentration region is W1, and the diameter of the circular region that is the mixed Si low concentration region is W0.

[0080] The width W1 of the mixed Si high concentration region is approximately 30 mm in the comparative example (FIG. 9), but is smaller at approximately 20 mm in the first example (FIG. 4) and second example (FIG. 6) of the embodiment. The width W1 in the second example is even smaller than the width W1 in the first example. The width W1 of the mixed Si high concentration region in the first and second examples of the embodiment is suppressed to 20 mm or less.

[0081] In this manner, in the GaN layer 20 of the embodiment, the concentration of mixed Si (the excess of the average Si concentration from the central Si concentration C0) in the (entire) circular region inside the annular region having a width of 20 mm from the edge of the upper surface 25 is 0.4×10 15 cm -3 The present invention has the following characteristics:

[0082] In the embodiment (and the comparative embodiment), the concentration of the mixed Si decreases monotonically from the outer periphery toward the center of the GaN layer 20. Therefore, the GaN layer 20 of the embodiment has a feature that the intermediate Si concentration C2 at the radial position intermediate between the center and the outer periphery is higher than the central Si concentration C0 and is lower than the outer periphery Si concentration C1.

[0083] The intermediate Si concentration C2 is, for example, the average Si concentration at a radial position 30 mm from the center. In the first example of the embodiment shown in FIG. 4, the intermediate Si concentration C2 (9.40×10 15 cm -3 ) is the central Si concentration C0(9.00×10 15 cm -3 ), and the peripheral Si concentration C1 (10.05×10 15 cm -36, the intermediate Si concentration C2 (9.25×10 15 cm -3 ) is the central Si concentration C0(8.91×10 15 cm -3 ), and the peripheral Si concentration C1 (9.44 × 10 15 cm -3 ) lower.

[0084] <Preferred embodiment of the present invention> Preferred aspects of the present invention will be described below.

[0085] (Appendix 1) A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of silicon-containing gallium nitride; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 More than 2×10 16 cm -3 is less than The peripheral silicon contamination concentration, which is the excess of the peripheral silicon concentration from the central silicon concentration, is 1.2×10 15 cm -3 Less than or equal to 0.9×10 15 cm -3 Less than or equal to 0.6×10 15 cm -3 (below) Laminated board.

[0086] (Appendix 2) In a circular region inside a 20 mm-wide annular region from the edge of the top surface, the excess of the silicon concentration at the top surface of the gallium nitride layer from the central silicon concentration is 0.4×10 15 cm -3 Below is the 2. The laminated substrate according to claim 1.

[0087] (Appendix 3) The silicon concentration on the top surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the top surface is higher than the central silicon concentration and lower than the peripheral silicon concentration. 3. The laminated substrate according to claim 1 or 2. [Explanation of symbols]

[0088] Reference Signs List 10...underlying structure, 20...GaN layer, 25...top surface (of GaN layer), 30...upper layer, 40...wafer, 50...dummy wafer, 60...whole wafer, 100...laminated substrate, 200...manufacturing apparatus, 210...susceptor, 211...inner periphery of susceptor, 212...outer periphery of susceptor, 213...upper surface of susceptor edge, 220...source gas, 230...Si-containing deposition

Claims

1. A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of silicon-containing gallium nitride; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 Above 2 x 10 16 cm -3 is less than The peripheral silicon contamination concentration, which is the excess of the peripheral silicon concentration from the central silicon concentration, is 1.2×10 15 cm -3 Below is the Laminated board.

2. In a circular region inside a 20 mm-wide annular region from the edge of the top surface, the excess of the silicon concentration at the top surface of the gallium nitride layer from the central silicon concentration is 0.4×10 15 cm -3 Below is the The laminated substrate according to claim 1 .

3. The silicon concentration on the top surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the top surface is higher than the central silicon concentration and lower than the peripheral silicon concentration. The laminated substrate according to claim 1 or 2.

Citation Information

Patent Citations

  • Susceptor, and vapor deposition device

    JP2009252969A

  • Crystal production method and gas phase growth apparatus

    JP2017178767A

  • Method of manufacturing semiconductor device and semiconductor device

    JP2018041878A

  • Group iii nitride laminated substrate and semiconductor light emitting element

    JP2021082781A

  • Nitride crystal substrate, semiconductor laminate, method of manufacturing semiconductor laminate, and method of manufacturing semiconductor device

    JP2018199601A