Multilayered substrate
A multilayer substrate with controlled silicon and carbon distribution in the gallium nitride layer addresses the non-uniformity of n-type carrier concentration, enhancing semiconductor device performance by balancing breakdown voltage and resistance.
Patent Information
- Application Number
- JP2023062140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-06
AI Technical Summary
The in-plane non-uniformity of n-type carrier concentration in GaN layers due to silicon concentration distribution is significant, particularly at the outer circumferential side, which affects the production efficiency of semiconductor devices.
A multilayer substrate design with a gallium nitride layer having a specific silicon and carbon concentration distribution is implemented, where the outer silicon concentration is higher than the central concentration, and carbon is added to compensate for the excess n-type carrier concentration, thereby reducing the in-plane non-uniformity.
The design effectively suppresses the in-plane non-uniformity of n-type carrier concentration, improving the uniformity and performance of semiconductor devices by balancing breakdown voltage and resistance characteristics.
Smart Images

Figure 2024148750000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated substrate. [Background technology]
[0002] A laminated substrate in which a gallium nitride (GaN) layer is epitaxially grown on various base substrates is used as a material for manufacturing a semiconductor device (see, for example, Patent Document 1). In order to improve the production efficiency of semiconductor devices, the diameter of the laminated substrate is being increased. Silicon (Si) is used as an n-type impurity added to the GaN layer.
[0003] As described in detail below, the inventors of the present application have investigated a multilayer substrate having a large diameter, a low concentration of added Si, and a thick GaN layer, and have discovered that the GaN layer is prone to in-plane non-uniformity in the Si concentration distribution (specifically, non-uniformity in which the Si concentration is higher on the outer periphery of the GaN layer). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-199601 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a multilayer substrate in which the in-plane non-uniformity of the n-type carrier concentration resulting from the in-plane non-uniformity of the Si concentration distribution in a GaN layer is suppressed. [Means for solving the problem]
[0006] According to one aspect of the present invention A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of gallium nitride doped with silicon; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 More than 2×10 16 cm -3 is less than the carbon concentration on the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is higher than a central carbon concentration at the center of the upper surface; Multilayer Substrate is provided. Effect of the Invention
[0007] A laminated substrate is provided in which the in-plane non-uniformity of the n-type carrier concentration resulting from the in-plane non-uniformity of the Si concentration distribution in the GaN layer is suppressed. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating a laminated substrate according to an embodiment. [Diagram 2] FIG. 2 is a top view of a GaN layer for explaining a method for measuring the Si concentration and the C concentration in the GaN layer. [Diagram 3] FIG. 3 is a schematic side view showing a manufacturing apparatus for a GaN layer according to an embodiment. [Figure 4] FIG. 4 is a graph showing an example of a C concentration distribution in the upper surface of a GaN layer according to an embodiment. [Diagram 5] FIG. 5 is a timing chart that illustrates a supply state of the C doping source gas at a representative position on the periphery. [Figure 6] FIG. 6 is a schematic cross-sectional view illustrating a GaN layer according to an embodiment. [Figure 7] FIG. 7 is a schematic side view showing a comparative example of a GaN layer manufacturing apparatus. [Figure 8] FIG. 8 is a graph showing an example of a Si concentration distribution in the upper surface of a GaN layer according to the embodiment or the comparative embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A laminated substrate 100 according to an embodiment of the present invention will be described. Fig. 1 is a schematic cross-sectional view illustrating the laminated substrate 100. The laminated substrate 100 has at least an underlayer structure 10 and a gallium nitride (GaN) layer 20 formed on the underlayer structure 10.
[0010] The base structure 10 has at least a base substrate which is a crystal substrate for epitaxially growing the GaN layer 20. The base structure 10 may have a buffer layer between the base substrate and the GaN layer 20, as required. The structure of the buffer layer may be appropriately selected as required.
[0011] As the base substrate, a GaN substrate, a sapphire substrate, a silicon (Si) substrate, a silicon carbide (SiC) substrate, or the like may be appropriately used. For example, when the base substrate is a GaN substrate, the base structure 10 may be a GaN substrate. For example, when the base substrate is a Si substrate, the base structure 10 may have a Si substrate and an aluminum nitride (AlN) layer provided as a nucleation layer, or the like.
[0012] The laminated substrate 100 may have an upper layer 30 formed on the GaN layer 20 as necessary. The structure of the upper layer 30 may be appropriately selected depending on the operation of a semiconductor device to be fabricated using the laminated substrate 100. The upper layer 30 may be, for example, a Group III nitride layer epitaxially grown on the GaN layer 20.
[0013] The GaN layer 20 according to the embodiment has the following characteristics. The GaN layer 20 has a top surface 25 with a radius of 50 mm or more (a diameter of 100 mm or more). In other words, the multilayer substrate 100 has a circular shape with a diameter of 100 mm or more. The multilayer substrate 100 may have an orientation flat or a notch as necessary.
[0014] Silicon (Si) is contained as an n-type impurity in GaN layer 20. The Si concentration in upper surface 25 of GaN layer 20 has a distribution in which a central Si concentration CSi0 at the center of upper surface 25 is higher than a peripheral Si concentration CSi1 at the periphery of upper surface 25.
[0015] The central Si concentration CSi0 is 10 15 cm -3 This is a low concentration where a concentration fluctuation of the order of 4×10 15 cm -3 More than 2×10 16 cm -3 The central Si concentration CSi0 is less than 1×10 16 cm -3 Less than (i.e. 10 15 cm -3 In an embodiment where the thickness of the GaN layer 20 is on the order of 100 μm or more, such an effect is more pronounced. The thickness of the GaN layer 20 is, for example, 4 μm or less.
[0016] The GaN layer 20 is a layer that functions as at least a part of an operating layer in a semiconductor device including the laminated substrate 100. For this reason, it is preferable that the GaN layer 20 has a well-balanced breakdown voltage characteristic and resistance characteristic. From the viewpoint of improving the breakdown voltage, the central Si concentration CSi0 of the GaN layer 20 is 2×10 16 cm -3 From the viewpoint of improving the breakdown voltage, the thickness of the GaN layer 20 is preferably 4 μm or more. From the viewpoint of reducing the resistance, the central Si concentration CSi0 of the GaN layer 20 is preferably 4×10 15 cm -3From the viewpoint of reducing resistance, the thickness of the GaN layer 20 is preferably 40 μm or less.
[0017] As will be described in detail later, the peripheral Si contamination concentration (i.e., CSi1-CSi0), which is the excess of the peripheral Si concentration CSi1 from the central Si concentration CSi0, is the concentration of Si that has been introduced into the periphery of the GaN layer 20 due to the Si-containing deposition 230. The central Si concentration CSi0 is approximately equal to the target addition concentration, which is the Si concentration that is intentionally added.
[0018] Due to the inclusion of Si, an excess of the n-type carrier concentration occurs at the periphery relative to the center. GaN layer 20 contains carbon (C) as an impurity that compensates for the excess of the n-type carrier concentration at the periphery. The C concentration at upper surface 25 of GaN layer 20 has a distribution in which a peripheral C concentration CC1 at the periphery of upper surface 25 is higher than a central C concentration CC0 at the center of upper surface 25. The peripheral C doping concentration (i.e., CC1-CC0), which is the excess of the peripheral C concentration CC1 from the central C concentration CC0, is the concentration of C doped to compensate for the excess of the n-type carrier concentration at the periphery.
[0019] In the following description, the radius of the GaN layer 20 is 50 mm, the thickness of the GaN layer 20 is 4 μm, and the target Si doping concentration in the GaN layer 20 is 9×10 15 cm -3 The embodiment in which
[0020] A method for measuring the Si concentration and the C concentration in the GaN layer 20 will be described. Hereinafter, for common content between the Si concentration and the C concentration, the term "concentration" may be used to avoid complication of explanation. Fig. 2 is a top view of the GaN layer 20 for explaining a method for measuring the concentrations in the GaN layer 20. An XY Cartesian coordinate system is set on the top surface 25 of the GaN layer 20, with the center of the top surface 25 as the origin.
[0021] First, the measurement positions within the surface will be described. At least five measurement points, including a central measurement point and four outer periphery measurement points, are set as the measurement points for the concentration on upper surface 25. The central measurement point is set at the center of upper surface 25. The four outer periphery measurement points are set at radial positions 10 mm from the edge of upper surface 25 (i.e., every 90° in the circumferential direction) for each of the X positive direction, X negative direction, Y positive direction, and Y negative direction. Here, a radial position 10 mm from the edge of upper surface 25 is set as a representative position of the outer periphery when specifying the concentration on the outer periphery of upper surface 25.
[0022] The Si concentration at the central measurement point is the central Si concentration CSi0. The Si concentration obtained by averaging the Si concentration CSiX+ at the peripheral measurement points in the positive X direction, the Si concentration CSiX- at the peripheral measurement points in the negative X direction, the Si concentration CSiY+ at the peripheral measurement points in the positive Y direction, and the Si concentration CSiY- at the peripheral measurement points in the negative Y direction is the peripheral Si concentration CSi1. In other words, the peripheral Si concentration CSi1 indicates the circumferentially averaged Si concentration on the periphery. The excess of the peripheral Si concentration CSi1 from the central Si concentration CSi0, i.e., CSi1-CSi0, is the peripheral Si contamination concentration.
[0023] The C concentration at the central measurement point is the central C concentration CC0. The C concentration obtained by averaging the C concentration CCX+ at the peripheral measurement points in the positive X direction, the C concentration CCX- at the peripheral measurement points in the negative X direction, the C concentration CCY+ at the peripheral measurement points in the positive Y direction, and the C concentration CCY- at the peripheral measurement points in the negative Y direction is the peripheral C concentration CC1. In other words, the peripheral C concentration CC1 indicates the circumferentially averaged C concentration on the outer periphery. The excess of the peripheral C concentration CC1 from the central C concentration CC0, i.e., CC1-CC0, is the peripheral C addition concentration.
[0024] In this example, the radius of the upper surface 25 is 50 mm. The four outer periphery measurement points are set at radial positions 40 mm from the center in each of the X positive direction, X negative direction, Y positive direction, and Y negative direction.
[0025] In addition to the center measurement point and the four outer circumference measurement points, intermediate measurement points may be set at radial positions intermediate between the center measurement point and the outer circumference measurement points. In this example, intermediate measurement points are set at radial positions 10 mm, 20 mm, and 30 mm from the center in the X positive direction, X negative direction, Y positive direction, and Y negative direction, respectively. In FIG. 2, for ease of illustration, the center measurement point and the outer circumference measurement points are indicated by large black circles, and the intermediate measurement points are indicated by small black circles.
[0026] Note that even in an embodiment in which the radius of upper surface 25 of GaN layer 20 exceeds 50 mm, the four outer periphery measurement points are set at radial positions of 10 mm from the edge of upper surface 25. Also, even in an embodiment in which the radius of upper surface 25 of GaN layer 20 exceeds 50 mm, the intermediate measurement points may be set at radial positions every 10 mm from the center in each of the X-positive direction, the X-negative direction, the Y-positive direction, and the Y-negative direction.
[0027] The concentrations obtained by averaging the concentrations at four measurement points in the X positive direction, X negative direction, Y positive direction, and Y negative direction, which are set at equal radial positions from the center of upper surface 25, that is, the concentrations averaged in the circumferential direction for each radial position, are referred to as the average Si concentration and average C concentration for Si and C. The peripheral Si concentration CSi1 and the peripheral C concentration CC1 are the average Si concentration and average C concentration on the periphery, respectively.
[0028] As described later, the GaN layer 20 is grown so as to be uniform in the circumferential direction. However, in reality, there are variations in concentration even among four measurement points set at equal radial positions. In order to reduce the effect of such variations, the radial distribution of the concentration in the GaN layer 20 is evaluated using an average Si concentration, which is the circumferentially averaged Si concentration, and an average C concentration, which is the circumferentially averaged C concentration, for each of Si and C. The concentration of the mixed Si is the excess of the average Si concentration from the central Si concentration CSi0 at each radial position. The concentration of the added C is the excess of the average C concentration from the central C concentration CC0 at each radial position.
[0029] In addition, when specifying that "the peripheral Si concentration CSi1 is higher than the central Si concentration CSi0", it is not only the peripheral Si concentration CSi1, i.e., the average value of the Si concentrations at the four peripheral measurement points, being higher than the central Si concentration CSi0 that is satisfied, but also the condition that the Si concentrations at at least three (preferably four) of the four peripheral measurement points are higher than the central Si concentration CSi0.
[0030] In addition, when specifying that "the peripheral C concentration CC1 is higher than the central C concentration CC0," it does not simply mean that the peripheral C concentration CC1, i.e., the average value of the C concentration at the four peripheral measurement points, is higher than the central C concentration CC0, but also that the C concentration at at least three (preferably four) of the four peripheral measurement points is higher than the central C concentration CC0.
[0031] Next, the measurement position in the height direction will be described. Concentrations (Si concentration and C concentration) in GaN layer 20 are measured at upper surface 25 by secondary ion mass spectrometry (SIMS). However, "concentration at upper surface 25" does not mean the concentration at the exact height of upper surface 25, but means the concentration in the vicinity of upper surface 25, as will be described below. Upper surface 25 is the top surface of laminated substrate 100 in a mode in which upper layer 30 is not laminated, and is the interface between upper layer 30 and GaN layer 20 in a mode in which upper layer 30 is laminated.
[0032] In general, the reliability of SIMS measurement at the surface position is not high. For this reason, it is preferable to perform SIMS measurement at a height slightly toward the underlayer structure 10 from the upper surface 25, that is, slightly inside the GaN layer 20. It is also preferable to use a measurement value averaged over a certain height range (depth range, thickness range). Here, the concentration at the upper surface 25 is defined as the average value of the SIMS measurement values in a depth range of 100 nm to 200 nm from the upper surface 25 for each measurement point in the plane. For example, in an embodiment in which the thickness of the GaN layer 20 is 4 μm, the average value of the concentration by SIMS measurement in a range of 3.8 μm to 3.9 μm from the lower surface of the GaN layer 20 is defined as the concentration at the upper surface 25.
[0033] The concentration at the midpoint between upper surface 25 of GaN layer 20 and the lower surface of GaN layer 20 (the concentration at a predetermined depth from upper surface 25 of GaN layer 20) is defined according to the concentration at upper surface 25. Specifically, the average value of SIMS measurement values in a depth range of 100 nm to 200 nm from the predetermined depth is defined as the concentration at the predetermined depth.
[0034] Before further describing the embodiment, a comparative embodiment will be described. Fig. 7 is a schematic side view showing a manufacturing apparatus 200 for a GaN layer 20 according to a comparative embodiment. The manufacturing apparatus 200 is a metal-organic vapor phase epitaxy (MOVPE) apparatus, and has a susceptor 210 on which a wafer 40 is placed. The wafer 40 is a processing target (an intermediate of the laminated substrate 100) at the stage when the growth process of the GaN layer 20 is performed by the manufacturing apparatus 200, and specifically, the wafer 40 is an underlayer structure 10 when the growth of the GaN layer 20 starts, and is a laminate of the underlayer structure 10 and the GaN layer 20 after the growth of the GaN layer 20 starts.
[0035] The manufacturing apparatus 200 is a lateral flow type MOVPE apparatus in which a source gas 220 is supplied in a direction parallel to the upper surface of the wafer 40. The source gas 220 includes a GaN source gas for growing GaN constituting the GaN layer 20, and a Si doping source gas for supplying Si to be added to the GaN layer 20. The GaN source gas includes a gallium (Ga) source gas and a nitrogen (N) source gas. For example, trimethylgallium (TMG) gas is used as the Ga source gas, and for example, ammonia (NH3) gas is used as the N source gas. For example, silane (SiH4) gas is used as the Si doping source gas.
[0036] The growth temperature can be selected, for example, in the range of 900° C. to 1400° C., and the V / III ratio, which is the flow rate ratio of the group V source gas to the group III source gas, can be selected, for example, in the range of 10 to 5000. The Si doping source gas has a target doping concentration in the GaN layer 20 of 4×10 15 cm -3 More than 2×10 16 cm -3 Less than a given value, e.g., 9×10 15 cm -3 The input signal is supplied so that:
[0037] Susceptor 210 holds wafer 40 so as to rotate wafer 40 about the center of wafer 40. By growing GaN layer 20 while rotating in this manner, the growth conditions of GaN layer 20 can be made uniform in the circumferential direction of wafer 40.
[0038] The susceptor inner peripheral edge 211 is the position of the susceptor 210 where the edge of the wafer 40 is located in a plan view. The susceptor peripheral upper surface 213 is the upper surface of the susceptor 210 between the susceptor inner peripheral edge 211 and the susceptor outer peripheral edge 212.
[0039] As the GaN layer 20 is grown, the Si-containing deposition 230 adheres to the susceptor edge upper surface 213, and Si is mixed into the GaN layer 20 from the Si-containing deposition 230. The inclusion of Si in the GaN layer 20 due to the Si-containing deposition 230 is called "mixing" and is to be distinguished from "addition" in which Si is intentionally included in the GaN layer 20 by a Si-doping source gas. The Si concentration in the upper surface 25 of the GaN layer 20 is the sum of the concentration of Si added by the Si-doping source gas and the concentration of Si mixed in due to the Si-containing deposition 230.
[0040] The concentration of Si added by the Si doping source gas is typically constant over the entire area of the upper surface 25 of the GaN layer 20. The concentration of Si mixed in due to the Si-containing deposition 230 is higher at a position closer to the inner periphery 211 of the susceptor, that is, at a position closer to the edge of the wafer 40 on the outer periphery side.
[0041] 8 is a graph showing an example of the Si concentration distribution in the upper surface 25 of the GaN layer 20 according to the comparative example. The horizontal axis shows the in-plane measurement position in mm, and the vertical axis shows the Si concentration in 10 15 cm -3 The Si concentration at each measurement point in the X direction is indicated by a black circle, and the Si concentration at each measurement point in the Y direction is indicated by a white square. The average Si concentration is indicated by a cross.
[0042] In addition, here, a comparative embodiment will be described assuming that no C is added in the embodiment described later. Therefore, the comparative embodiment is the same as the embodiment except for the absence of C addition, and the Si concentration distribution shown in FIG. 8 is the same between the comparative embodiment and the embodiment.
[0043] The central Si concentration CSi0 is the target doping concentration of 9×10 15 cm -3 is approximately equal to 9.01 × 10 15 cm -3 The Si concentration is almost constant up to about 10 mm from the center. This means that the mixed Si does not reach the center of the wafer 40.
[0044] At radial positions 20 mm or more away from the center, the concentration of mixed Si, which is the excess over the central Si concentration CSi0, is significantly higher. The concentration of mixed Si also increases toward the outer periphery. The outer periphery Si concentration CSi1 is 10.65×10 15 cm -3 The peripheral Si contamination concentration, which is the excess of the peripheral Si concentration CSi1 from the central Si concentration CSi0, is 1.64 × 10 15 cm -3 It is.
[0045] The Si resulting from the Si-containing deposition 230 is mixed in from the edge of the wafer 40 to a width of about 40 mm in the radial direction. In the case of a large-diameter wafer 40 such as that of a 50 mm radius, as in this example, no Si is mixed in at the center. In contrast, in a case where a wafer with a smaller diameter, such as a 25 mm radius, is used, Si is mixed in at the center of the wafer.
[0046] In the case of a small diameter embodiment where Si is mixed in the center, the mixed Si from both edges on either side of the center overlaps at the center, so that the Si concentration due to the mixed Si is high even at the center. As a result, the Si concentration distribution due to the mixed Si approaches uniformity within the surface.
[0047] In contrast, in the case of a large-diameter wafer such as this example, where no Si is mixed in the center, the Si concentration distribution due to the mixed Si is non-uniform with a large difference between the center and the periphery. Thus, in a large-diameter wafer 40, specifically a wafer with a radius of 50 mm or more, the in-plane non-uniformity of the Si concentration distribution due to the mixed Si becomes significant.
[0048] Although a 50 mm radius is shown as an example, even in wafers 40 with a radius of more than 50 mm, the concentration of contaminating Si at the outer periphery (a radial position 10 mm from the edge of the wafer 40) is approximately the same as in the case of a 50 mm radius.
[0049] The peripheral Si concentration, which is the difference in Si concentration between the center and the periphery, is 1.64 × 10 15 cm-3 On the other hand, the target concentration of Si, that is, the central Si concentration CSi0, is 10 15 cm -3 Therefore, the influence of the peripheral Si contamination concentration on the in-plane Si concentration distribution becomes significant.
[0050] In this way, when the radius of the upper surface 25 is 50 mm or more and the central Si concentration CSi0 is 4×10 15 cm -3 More than 2×10 16 cm -3 Less than (even 1×10 16 cm -3 In the GaN layer 20 having a thickness of less than 100 nm, the difference in Si concentration between the center and the periphery becomes significant due to the mixed Si. That is, the difference in n-type carrier concentration between the center and the periphery becomes significant due to the difference in Si concentration. As described below, in the embodiment, a technique is proposed that can suppress such a difference in n-type carrier concentration between the center and the periphery as compared to the comparative embodiment.
[0051] The embodiment will be further described. As described above, Fig. 8 is also a graph showing the Si concentration distribution in the upper surface 25 of the GaN layer 20 according to the embodiment. The Si concentration distribution will be further described.
[0052] The lower limit of the target doping concentration, that is, the lower limit of the central Si concentration CSi0, is 4×10 15 cm -3 The Si concentration is 0.4×10 15 cm -3 is defined as the contamination standard value ΔSi. A region where the concentration of contamination Si is equal to or less than the contamination standard value ΔSi is called a contamination low concentration region 23. A region where the concentration of contamination Si is greater than the contamination standard value ΔSi is called a contamination high concentration region 24.
[0053] The mixed-Si high concentration region 24 becomes a circular ring-shaped region on the edge side of the upper surface 25 of the GaN layer 20. (The entire area of) the circular region inside the circular ring-shaped region that is the mixed-Si high concentration region 24 becomes the mixed-Si low concentration region 23. The width of the circular ring-shaped region that becomes the mixed-Si high concentration region 24 from the edge of the upper surface 25 is approximately 30 mm.
[0054] The mixed Si high concentration region 24 is a region where the excess of n-type carrier concentration caused by mixed Si is large. In the embodiment, C is added to the mixed Si high concentration region 24 to compensate for at least a part of the excess of the n-type carrier concentration, thereby suppressing the difference in n-type carrier concentration between the center and the periphery.
[0055] 3 is a schematic side view showing a manufacturing apparatus 200 for a GaN layer 20 according to an embodiment. The manufacturing apparatus 200 according to the embodiment is a lateral flow type MOVPE apparatus, as in the comparative example, and main source gas 220 (GaN source gas and Si doping source gas) is supplied in a direction parallel to the upper surface of the wafer 40.
[0056] The manufacturing apparatus 200 according to the embodiment further includes a mechanism for supplying a compensating raw material gas 240. The compensating raw material gas 240 includes a C doping raw material gas for supplying C to be added to the GaN layer 20. As the C doping raw material gas, for example, methane (CH4) gas is used.
[0057] Since the Ga source gas (e.g., TMG gas) contained in the main source gas 220 is an organic source gas, C resulting from the Ga source gas is also contained in the GaN layer 20. The inclusion of C in the GaN layer 20 due to the Ga source gas is called "mixing" and is distinguished from "addition" in which C is intentionally contained in the GaN layer 20 by a C doping source gas. The C concentration on the upper surface of the GaN layer 20 is the sum of the concentration of C added by the C doping source gas and the concentration of C mixed in due to the Ga source gas.
[0058] The concentration of C mixed in due to the Ga raw material gas is typically constant over the entire area of upper surface 25 of GaN layer 20. Compensating raw material gas 240, that is, C doping raw material gas, is selectively supplied to mixed Si high concentration region .
[0059] In the embodiment, in order to preferentially add C to the mixed Si high concentration region 24, the C doping source gas is selectively supplied to the mixed Si high concentration region 24, that is, to a predetermined range on the outer periphery side in the radial direction (specifically, in this example, a range with a width of about 30 mm from the edge of the upper surface 25). Note that, in the mixed Si low concentration region 23, the Si concentration is slightly higher in the outer periphery side portion, so the C doping source gas may be supplied to this portion as well as a supplementary supply.
[0060] The C doping source gas is supplied from a direction perpendicular to the upper surface of the wafer 40. Specifically, the C doping source gas is supplied from a perpendicular direction onto the mixed Si high concentration region 24 on the downstream side of the main source gas 220 with respect to the rotation center of the wafer 40. This allows selective supply to the mixed Si high concentration region 24.
[0061] The concentration of mixed Si in the mixed Si high concentration region 24 is greater toward the outer periphery. For this reason, the C doping source gas is preferably supplied to a plurality of radial positions in the mixed Si high concentration region 24, and the supply amount of the C doping source gas supplied to the plurality of radial positions is preferably controlled so as to be greater toward the outer periphery.
[0062] The growth conditions of the GaN layer 20 of the embodiment are the same as those of the comparative embodiment, except for the supply conditions of the C doping source gas. The supply conditions of the C doping source gas (the supply position, supply amount, supply timing, etc. of the C doping source gas) may be appropriately set by experimental consideration so that the excess of the n-type carrier concentration caused by the mixed Si is compensated. As a rough guideline, the supply conditions of the C doping source gas may be set so that the concentration of the mixed Si and the concentration of the added C are equal at each position in the radial direction. However, since it is not easy to determine how much of the added C compensates for the n-type carriers, the concentration of the added C may be appropriately adjusted.
[0063] It should be noted that the addition of C has the effect of compensating for at least a part of the excess of the n-type carrier concentration, compared to a comparative embodiment in which no C is added. For this reason, it is not essential to add C so as to completely compensate for the excess of the n-type carrier concentration.
[0064] For example, it is not essential that the peripheral C doping concentration is equal to (or higher than) the peripheral Si contamination concentration. However, the peripheral C doping concentration is preferably 0.5 times or more the peripheral Si contamination concentration. In order to prevent the peripheral C doping concentration from becoming excessive, the peripheral C doping concentration is preferably 2 times or less the peripheral Si contamination concentration.
[0065] The concentration of C mixed in due to the Ga source gas, i.e., the central C concentration CC0, is, for example, 2×10 15 cm -3 However, it is preferable that the central C concentration CC0 is as low as possible so as to be equal to or lower than the lower limit of the central Si concentration CSi0. The concentration of added C is an excess of the central C concentration CC0, and such an excess C concentration contributes to the effect of compensating for the excess of the n-type carrier concentration in the embodiment.
[0066] 4 is a graph showing an example of the C concentration distribution in the upper surface 25 of the GaN layer 20 according to the embodiment. The horizontal axis shows the in-plane measurement position in mm, and the vertical axis shows the C concentration in 10 15 cm -3 The C concentration at each measurement point in the X direction is indicated by a black circle, and the C concentration at each measurement point in the Y direction is indicated by a white square. The average C concentration is indicated by a cross.
[0067] The central C concentration CC0 is 2.01×10 15 cm -3 In the mixed Si high concentration region 24, the C concentration is higher than the central C concentration CC0, that is, C is added. In response to the higher concentration of mixed Si toward the outer periphery, C is added so that the concentration of added C becomes higher toward the outer periphery. The peripheral C concentration CC1 is 3.26×10 15 cm -3 The peripheral C concentration, which is the excess of the peripheral C concentration CC1 from the central C concentration CC0, is 1.25×10 15 cm -3 The peripheral C concentration is 1.25×10 15 cm -3 is the peripheral Si contamination concentration 1.64×10 15 cm -3 It is 0.76 times.
[0068] Further, the characteristics of the C addition in the height direction (depth direction, thickness direction) according to the embodiment will be described below. The concentration of mixed Si in the GaN layer 20 generally tends to increase as the GaN layer 20 becomes thicker. This is because the Si-containing deposits 230 adhering to the susceptor edge upper surface 213 increase as the growth time of the GaN layer 20 increases. Therefore, the supply of the C doping source gas may be started at the timing when the growth thickness reaches a value at which the mixed Si has a predetermined concentration or more.
[0069] 5 is a timing chart showing a typical supply state of the C doping source gas at a representative position on the periphery (a radial position 10 mm from the edge). The horizontal axis shows the growth thickness of the GaN layer 20, and the vertical axis shows the supply amount of the C doping source gas. When the peripheral Si contamination concentration reaches a predetermined concentration, for example, the above-mentioned contamination reference value ΔSi (0.4×10 15 cm -3 The supply of the C doping source gas is started at the timing when the growth thickness reaches a growth thickness T1, which is equal to the growth thickness T2 of the GaN layer 20. Thereafter, the peripheral Si contamination concentration increases until the GaN layer 20 reaches the final growth thickness T2. Therefore, it is preferable to increase the supply amount of the C doping source gas as the growth thickness increases so as to correspond to the increase in the peripheral Si contamination concentration.
[0070] Incidentally, the amount of mixed Si is less on the central side than on the peripheral representative position. Therefore, the timing of starting the supply of the C doping source gas may be delayed on the central side than on the peripheral representative position. Also, the amount of mixed Si is more on the further outer periphery side (edge side) than on the peripheral representative position. Therefore, the timing of starting the supply of the C doping source gas may be advanced on the further outer periphery side (edge side) than on the peripheral representative position. The supply amount of the C doping source gas may be increased as the growth thickness increases, so as to correspond to the increase in the concentration of mixed Si on the central side or on the further outer periphery side (edge side) than on the peripheral representative position.
[0071] 6 is a schematic cross-sectional view illustrating a GaN layer 20 according to an embodiment. A region to which the C doping source gas is not supplied is a C non-doped region 21, and a region to which the C doping source gas is supplied is a C doped region 22. A representative position on the outer periphery (a radial position 10 mm from the edge) is described below as an example. A range of thickness T2 downward from an upper surface 25 of the GaN layer 20 is the C doped region 22, and a range of thickness T1 downward from the lower end of the C doped region 22 is the C non-doped region 21.
[0072] In C-doped region 22, the C concentration is highest at upper surface 25 and decreases downward from upper surface 25. The C concentration in C-non-doped region 21 is lower than the C concentration at upper surface 25. That is, in GaN layer 20, at a representative position on the periphery (a radial position 10 mm from the edge), at a predetermined depth position from upper surface 25, there is a region where the C concentration is lower than the peripheral C concentration at upper surface 25.
[0073] As described above, the concentration of mixed Si in GaN layer 20 generally tends to increase as GaN layer 20 becomes thicker. In other words, the concentration of mixed Si in GaN layer 20 generally tends to decrease toward the lower side of GaN layer 20. That is, in GaN layer 20, at a representative position on the periphery (a radial position 10 mm from the edge), at a predetermined depth position from upper surface 25, there exists a region where the Si concentration is lower than the peripheral Si concentration at upper surface 25.
[0074] The following further describes the characteristics of the GaN layer 20 according to the embodiment. The concentration of mixed Si typically decreases monotonically from the outer periphery toward the center of the GaN layer 20. Therefore, the GaN layer 20 according to the embodiment has a characteristic that the intermediate Si concentration CSi2 at the radial position midway between the center and the outer periphery is higher than the central Si concentration CSi0 and lower than the outer periphery Si concentration CSi1.
[0075] The intermediate Si concentration CSi2 is, for example, the average Si concentration at a radial position 30 mm from the center. In the example shown in FIG. 8, the intermediate Si concentration CSi2 (9.94×10 15 cm -3 ) is the central Si concentration CSi0(9.01×10 15 cm -3 ), and the peripheral Si concentration CSi1 (10.65 × 10 15 cm -3 ) lower.
[0076] In order to correspond to the concentration distribution shape of the mixed Si, the concentration of added C also preferably decreases monotonically from the outer periphery toward the center of the GaN layer 20. That is, the GaN layer 20 of the embodiment preferably has a feature that a middle C concentration CC2 at a radial position midway between the center and the outer periphery is higher than the center C concentration CC0 and lower than the outer periphery C concentration CC1.
[0077] The intermediate C concentration CC2 is, for example, the average C concentration at a radial position 30 mm from the center. In the example shown in FIG. 4, the intermediate C concentration CC2 (2.73×10 15 cm -3 ) is the central C concentration CC0(2.01×10 15 cm -3 ) and the peripheral C concentration CC1 (3.26 × 10 15 cm -3 ) lower.
[0078] <Preferred embodiment of the present invention> Preferred aspects of the present invention will be described below.
[0079] (Appendix 1) A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of gallium nitride doped with silicon; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 More than 2×10 16 cm -3 is less than the carbon concentration on the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is higher than a central carbon concentration at the center of the upper surface; Laminated board.
[0080] (Appendix 2) In the gallium nitride layer, a region having a carbon concentration lower than the peripheral carbon concentration in the upper surface exists at a radial position 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface. 2. The laminated substrate according to claim 1.
[0081] (Appendix 3) In the gallium nitride layer, a region having a silicon concentration lower than the peripheral silicon concentration in the upper surface exists at a radial position 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface. 3. The laminated substrate according to claim 1 or 2.
[0082] (Appendix 4) The silicon concentration on the top surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the top surface is higher than the central silicon concentration and lower than the peripheral silicon concentration. 4. The laminated substrate according to claim 1.
[0083] (Appendix 5) the carbon concentration on the upper surface of the gallium nitride layer has a distribution in which a median carbon concentration at a radial position 30 mm from the center of the upper surface is higher than the central carbon concentration and lower than the peripheral carbon concentration; 5. The laminated substrate according to any one of claims 1 to 4. [Explanation of symbols]
[0084] 10...underlying structure, 20...GaN layer, 21...C-non-doped region, 22...C-doped region, 23...mixed Si low concentration region, 24...mixed Si high concentration region, 25...top surface (of GaN layer), 30...upper layer, 40...wafer, 100...laminated substrate, 200...manufacturing apparatus, 210...susceptor, 211...susceptor inner periphery, 212...susceptor outer periphery, 213...susceptor edge upper surface, 220...(main) source gas, 230...Si-containing deposition, 240...compensatory source gas
Claims
1. A base substrate; a gallium nitride layer epitaxially grown on the base substrate and made of gallium nitride doped with silicon; Equipped with the gallium nitride layer has a top surface with a radius of 50 mm or greater; The thickness of the gallium nitride layer is 4 μm or more, a silicon concentration distribution in the upper surface of the gallium nitride layer has a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface that is higher than a central silicon concentration at the center of the upper surface; The central silicon concentration is 4×10 15 cm -3 Above 2 x 10 16 cm -3 is less than the carbon concentration in the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is higher than a central carbon concentration at the center of the upper surface; Laminated board.
2. In the gallium nitride layer, a region having a carbon concentration lower than the peripheral carbon concentration in the upper surface is present at a radial position 10 mm from an edge of the upper surface and at a predetermined depth from the upper surface. The laminated substrate according to claim 1 .
3. In the gallium nitride layer, a region having a silicon concentration lower than the peripheral silicon concentration in the upper surface is present at a radial position 10 mm from an edge of the upper surface and at a predetermined depth from the upper surface. The laminated substrate according to claim 1 or 2.
4. The silicon concentration on the top surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the top surface is higher than the central silicon concentration and lower than the peripheral silicon concentration. The laminated substrate according to claim 1 or 2.
5. The carbon concentration on the upper surface of the gallium nitride layer has a distribution in which a median carbon concentration at a radial position 30 mm from the center of the upper surface is higher than the central carbon concentration and lower than the peripheral carbon concentration. The laminated substrate according to claim 1 or 2.
Citation Information
Patent Citations
Susceptor, and vapor deposition device
JP2009252969A
Nitride semiconductor substrate, semiconductor device, and method of manufacturing nitride semiconductor substrate
JP2017183582A
Method of manufacturing semiconductor device and semiconductor device
JP2018041878A
Group iii nitride laminated substrate and semiconductor light emitting element
JP2021082781A
Nitride crystal substrate, semiconductor laminate, method of manufacturing semiconductor laminate, and method of manufacturing semiconductor device
JP2018199601A