Steel material
The steel material with controlled Mn sulfide distribution addresses the loss of non-magnetic properties by preventing chip retention and strain introduction, ensuring long-term magnetic stability and improved bending workability.
Patent Information
- Application Number
- JP2023062216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Steel materials used in magnetic field environments lose non-magnetic properties over time due to deformation-induced martensitic transformation caused by chips remaining after cutting and clogging of cutting tools, which introduce excessive strain.
A steel material with a specific chemical composition and controlled distribution of Mn sulfides, ensuring a density of 1.0×10^2 to 5.0×10^3 pieces/mm^2 of MnS inclusions with a diameter of 1.0 to 5.0 μm, which prevents chip retention and strain introduction during cutting.
Maintains non-magnetic properties and enhances bending workability by preventing deformation-induced martensitic transformation and improving chip disposal efficiency.
Smart Images

Figure 2024148780000001 
Figure 2024148780000002 
Figure 2024148780000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to steel materials, and more preferably to steel materials suitable for use in magnetic field environments and requiring non-magnetic properties. [Background technology]
[0002] Steel materials used in magnetic field environments, such as strong magnetic fields such as those found in linear motor car related equipment, or weak magnetic fields such as those found in medical equipment and geomagnetic measuring instruments, are required to have non-magnetic properties (low magnetic permeability) to suppress energy loss and noise generation caused by the excitation of induced currents.
[0003] Steel materials with a face-centered cubic structure (fcc) are known to have non-magnetic properties. Austenitic stainless steel materials such as SUS304 and SUS316, and high-Mn steel materials containing a large amount of Mn are known as steel materials with a face-centered cubic structure having such non-magnetic properties. Of these steel materials, austenitic stainless steel materials contain large amounts of alloy elements such as Ni and Cr, and are expensive. For this reason, the use of high-Mn steel materials as steel materials with non-magnetic properties is progressing.
[0004] However, the steel materials for the above-mentioned applications are usually used in a magnetic field environment after being cut or bent, so these steel materials are required to have not only excellent non-magnetic properties but also excellent bending workability.
[0005] Techniques for improving the bending workability of steel materials having non-magnetic properties are disclosed in JP 3-13544 A (Patent Document 1) and JP 2014-205908 A (Patent Document 2).
[0006] The steel material disclosed in Patent Document 1 has a chemical composition containing, by mass%, C: 0.55-0.80%, Si: 0.5% or less, Mn: 11-17%, Al: 0.02-0.06%, N: 0.02-0.06%, and P: 0.02% or less, with the balance being Fe and unavoidable impurities. In Patent Document 1, the C content of the steel material is kept low to improve bending workability, and the strength of the steel material is ensured by the inclusion of Al and N.
[0007] The steel material disclosed in Patent Document 2 contains, in mass%, C: 0.8-1.2%, Si: 0.1-0.6%, Mn: more than 13-20%, Al: 0.001-less than 0.02%, P: 0.040% or less, S: 0.045% or less, and N: 0.025-0.05%, with the balance being Fe and inevitable impurities. Furthermore, 99.0 area % or more of the microstructure is an austenite structure, and the austenite grain size number is 8.0-10.5. Furthermore, the steel surface contains at least one of Mn and Cr, and has an oxide scale with a thickness of 0.5 to 8.0 μm. In Patent Document 2, the austenite grains are set within a predetermined range to improve bending workability at room temperature, and further, the above-mentioned oxide scale is formed to improve bending workability at low temperatures. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 3-13544 [Patent Document 2] JP 2014-205908 A Summary of the Invention [Problem to be solved by the invention]
[0009] As described above, steel materials used in a magnetic field environment are not only bent but also cut to a predetermined length. The present inventors discovered for the first time that the non-magnetic properties of steel materials may be lost after a long period of time has passed since the cutting process. The present inventors investigated and considered the cause of the deterioration of the non-magnetic properties of steel materials after a long period of time has passed since the cutting process. As a result, it was found that the non-magnetic properties deteriorate due to the following mechanism.
[0010] When cutting high-Mn steel, chips such as burrs may be too long and remain in the steel without peeling off. If the chips remain in the steel without peeling off, plastic deformation may occur in the area near the chips that were not peeled off, and excessive strain may be introduced. This introduction of strain causes deformation-induced martensitic transformation after a long period of time, and martensite is formed locally in the steel. As martensite is ferromagnetic, the nonmagnetic properties of the steel deteriorate.
[0011] Furthermore, if the chips are too short, the cutting tools used for cutting, such as saw blades, become clogged, even though the chips are easily removed from the steel. If a clogged cutting tool is used to cut steel, plastic deformation occurs on the cut surface of the steel, and excessive strain is introduced into the steel. This introduction of strain causes deformation-induced martensitic transformation after a long period of time.
[0012] Based on the above findings, in order to suppress the deterioration of the non-magnetic properties of steel over a long period of time, excellent chip disposal properties are required, in which the length of the chips is sufficient to suppress the chips from remaining on the steel or clogging the cutting tool.
[0013] An object of the present disclosure is to provide a steel material that has non-magnetic properties, provides excellent bending workability, and improves chip disposal during processing. [Means for solving the problem]
[0014] The steel material according to the present disclosure is Chemical composition, in mass%, C: 0.75-1.10%, Si: 0.10 to 0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%, The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 There are 10 pieces.
[0015] The steel material according to the present disclosure is Chemical composition, in mass%, C: 0.75-1.10%, Si: 0.10 to 0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%, Further, it contains one or more selected from the group consisting of Groups 1 to 4, The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 There are 10 pieces. [Group 1] Cu: 0.40% or less, and Ni: 0.40% or less, one or more selected from the group consisting of [Group 2] Cr: 1.50% or less, V: 0.25% or less, Ti: 0.100% or less, Mo: 1.00% or less Al: 0.100% or less, and Nb: 0.050% or less, one or more selected from the group consisting of [Group 3] B: 0.0050% or less [Group 4] Bi: 0.20% or less, Pb: 0.09% or less, and Ca: 0.0100% or less, one or more selected from the group consisting of Effect of the Invention
[0016] The steel material according to the present disclosure has non-magnetic properties, provides excellent bending workability, and improves chip disposal during processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The inventors first conducted a study on a steel material that can provide excellent non-magnetic properties and excellent bending workability from the viewpoint of chemical composition. As a result, the inventors found that the steel material contains, in mass%, C: 0.75-1.10%, Si: 0.10-0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010-0.070%, N: 0.005-0.024%, Cu: 0-0.40%, Ni: 0-0.40%, Cr: 0-1.50%, V: 0-0.25%, Ti: 0- It was believed that excellent non-magnetic properties and excellent bending workability could be obtained with a steel material having a chemical composition of: 0.100%, Mo: 0-1.00%, Al: 0-0.100%, Nb: 0-0.050%, B: 0-0.0050%, Bi: 0-0.20%, Pb: 0-0.09%, Ca: 0-0.0100%, and the balance being Fe and impurities.
[0018] Therefore, the present inventors further investigated means for improving chip disposability during machining of a steel material having the above-mentioned chemical composition, and as a result, the present inventors obtained the following findings.
[0019] In the steel material having the above-mentioned chemical composition, multiple Mn sulfides are generated in the steel material. The interface between the Mn sulfides and the parent phase in the steel material becomes a stress concentration source during cutting. If Mn sulfides with a circle equivalent diameter of 1.0 to 5.0 μm are present at an appropriate number density, stress is concentrated at the interface between the multiple Mn sulfides and the parent phase during cutting, and cracks are generated. If multiple cracks are connected, the cracks propagate. In this case, before excessive plastic deformation occurs during cutting, the cracks propagate and the cutting chips peel off from the steel material. Therefore, the introduction of strain during cutting is suppressed, and processing-induced martensitic transformation after a long period of time can be suppressed.
[0020] If the number density of Mn sulfides is too low, cracks do not occur sufficiently at the interface between the Mn sulfides and the parent phase. In this case, long chips remain in the steel while undergoing plastic deformation. As a result, excessive strain is introduced into the steel. On the other hand, if the number density of Mn sulfides is too high, the length of the chips becomes extremely short. In this case, the extremely short chips cause clogging of cutting tools such as saw blades. If a steel is cut using a clogged cutting tool, deformation occurs on the cut surface of the steel, and excessive strain is introduced into the steel. The introduced strain causes processing-induced martensitic transformation after a long period of time, deteriorating the nonmagnetic properties of the steel. The remaining chips may scratch the surface of other steel. In a steel with scratches, stress concentrates near the scratches during bending, and excessive strain is introduced.
[0021] Based on the above findings, the inventors investigated and examined the number density of Mn sulfides having an equivalent circle diameter of 1.0 to 5.0 μm. As a result, the inventors obtained the following findings. In a steel material having the above chemical composition, the number density of Mn sulfides having an equivalent circle diameter of 1.0 to 5.0 μm is 1.0×10 2 ~5.0×10 3 pieces / mm 2If the thickness is 100 mm, the chips produced during cutting can be made to an appropriate length, improving chip disposal. This makes it possible to suppress the introduction of excessive strain. As a result, the occurrence of deformation-induced martensitic transformation after a long period of time can be suppressed, and non-magnetic properties can be maintained.
[0022] The steel material according to this embodiment, which has been completed based on the above findings, has the following configuration.
[0023] [1] A steel material, Chemical composition, in mass%, C: 0.75-1.10%, Si: 0.10 to 0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%, The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 Individual Steel material.
[0024] [2] A steel material, Chemical composition, in mass%, C: 0.75-1.10%, Si: 0.10 to 0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%, Further, it contains one or more selected from the group consisting of Groups 1 to 4, The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 Individual Steel material. [Group 1] Cu: 0.40% or less, and Ni: 0.40% or less, one or more selected from the group consisting of [Group 2] Cr: 1.50% or less, V: 0.25% or less, Ti: 0.100% or less, Mo: 1.00% or less Al: 0.100% or less, and Nb: 0.050% or less, one or more selected from the group consisting of [Group 3] B: 0.0050% or less [Group 4] Bi: 0.20% or less, Pb: 0.09% or less, and Ca: 0.0100% or less, one or more selected from the group consisting of
[0025] [3] [2] The steel material according to the present invention, The chemical composition contains the first group, Steel material.
[0026] [4] The steel material according to [2] or [3], The chemical composition contains the second group, Steel material.
[0027] [5] The steel material according to any one of [2] to [4], The chemical composition contains the third group, Steel material.
[0028] [6] The steel material according to any one of [2] to [5], The chemical composition contains the fourth group, Steel material.
[0029] The steel material of this embodiment will be described in detail below. Note that "%" for elements means mass % unless otherwise specified.
[0030] [Features of the steel material of this embodiment] The steel material of this embodiment has the following characteristics. (Feature 1) The chemical composition, in mass%, is C: 0.75-1.10%, Si: 0.10-0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010-0.070%, N: 0.005-0.024%, Cu: 0-0.40%, Ni: 0-0.40%, Cr: 0-1.50%, V: 0-0.25%, Ti: 0-0.100%, Mo: 0-1.00%, Al: 0-0.100%, Nb: 0-0.050%, B: 0-0.0050%, Bi: 0-0.20%, Pb: 0-0.09%, Ca: 0-0.0100%, and the remainder is Fe and impurities. (Feature 2) When the diameter of a steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing 70% or more in area ratio and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 There are 10 pieces. Features 1 and 2 will be explained below.
[0031] [(Feature 1) Chemical composition] The chemical composition of the steel material of this embodiment contains the following elements.
[0032] C: 0.75-1.10% Carbon (C) stabilizes austenite and suppresses processing-induced martensitic transformation. Therefore, sufficient non-magnetic properties are obtained. If the C content is less than 0.75%, the above effect is not sufficiently obtained. On the other hand, if the C content exceeds 1.10%, carbides are excessively precipitated at the grain boundaries. The carbides precipitated at the grain boundaries become the starting point of cracks during bending. Therefore, sufficient bending workability is not obtained. Therefore, the C content is 0.75 to 1.10%. The lower limit of the C content is preferably 0.80%, more preferably 0.83%, and further preferably 0.85%. The upper limit of the C content is preferably 1.05%, more preferably 1.03%, and further preferably 1.00%.
[0033] Silicon: 0.10 to 0.70% Silicon (Si) deoxidizes steel. Furthermore, Si increases the strength of steel by solid solution strengthening. If the Si content is less than 0.10%, the above effects cannot be sufficiently obtained. On the other hand, if the Si content exceeds 0.70%, bending workability decreases. Therefore, the Si content is 0.10 to 0.70%. The lower limit of the Si content is preferably 0.15%, more preferably 0.18%, and further preferably 0.20%. The upper limit of the Si content is preferably 0.60%, more preferably 0.55%, and further preferably 0.50%.
[0034] Mn: 11.00-18.00% Manganese (Mn) stabilizes austenite and suppresses processing-induced martensitic transformation. Therefore, sufficient non-magnetic properties are obtained. Mn also generates Mn sulfides to suppress the remaining of chips during processing. If the Mn content is less than 11.00%, the above effects are not sufficiently obtained. On the other hand, if the Mn content exceeds 18.00%, the strength of the steel material increases excessively and the workability of the steel material decreases. Therefore, the Mn content is 11.00 to 18.00%. The lower limit of the Mn content is preferably 12.00%, more preferably 12.50%, and further preferably 13.00%. The upper limit of the Mn content is preferably 17.00%, more preferably 16.50%, and further preferably 16.00%.
[0035] P:0.050% or less Phosphorus (P) is an impurity. P segregates at the grain boundaries of austenite crystal grains and reduces bending workability. Therefore, the P content is 0.050% or less. It is preferable that the P content is as low as possible. However, an extreme reduction in the P content significantly increases the production cost. Therefore, in consideration of industrial production, the preferable lower limit of the P content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%. The upper limit of the P content is preferably 0.035%, more preferably 0.030%, and further preferably 0.025%.
[0036] S: 0.010~0.070% Sulfur (S) combines with Mn to form Mn sulfides. Mn sulfides suppress the remaining of cutting chips during processing. Therefore, sufficient non-magnetic properties are maintained in the steel material after processing. If the S content is less than 0.010%, the above effects cannot be sufficiently obtained. On the other hand, if the S content exceeds 0.070%, the Mn sulfides become coarse. In this case, sufficient bending workability cannot be obtained. Therefore, the S content is 0.010 to 0.070%. The lower limit of the S content is preferably 0.015%, more preferably 0.018%, and further preferably 0.020%. The upper limit of the S content is preferably 0.060%, more preferably 0.055%, and further preferably 0.050%.
[0037] N: 0.005~0.024% Nitrogen (N) stabilizes austenite and suppresses processing-induced martensitic transformation. Therefore, sufficient non-magnetic properties are obtained. N also increases the strength of the steel material by solid solution strengthening. If the N content is less than 0.005%, the above effects are not sufficiently obtained. On the other hand, if the N content exceeds 0.024%, defects such as blowholes are likely to occur in the steel material. Therefore, the manufacturability of the steel material decreases. Therefore, the N content is 0.005 to 0.024%. The lower limit of the N content is preferably 0.007%, more preferably 0.010%, and further preferably 0.012%. The upper limit of the N content is preferably 0.022%, more preferably 0.020%, and further preferably 0.018%.
[0038] The balance of the chemical composition of the steel material of the present embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to those that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and are not intentionally contained, but are allowed within a range that does not adversely affect the steel material of the present embodiment.
[0039] [Optional Elements] The chemical composition of the steel material of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of first to fourth groups. [Group 1] Cu: 0.40% or less, and Ni: 0.40% or less, one or more selected from the group consisting of [Group 2] Cr: 1.50% or less, V: 0.25% or less, Ti: 0.100% or less, Mo: 1.00% or less Al: 0.100% or less, and Nb: 0.050% or less, one or more selected from the group consisting of [Group 3] B: 0.0050% or less [Group 4] Bi: 0.20% or less, Pb: 0.09% or less, and Ca: 0.0100% or less, one or more selected from the group consisting of The optional elements will be described below.
[0040] [Group 1: Cu and Ni] The chemical composition of the steel material of this embodiment may further contain the above-mentioned first group elements in place of a portion of Fe. These elements are optional elements, and all of them improve the non-magnetic properties of the steel material and increase the toughness of the steel material. Each element will be described below.
[0041] Cu: 0.40% or less Copper (Cu) is an optional element and may not be contained. In other words, the Cu content may be 0%. When it is contained, that is, when the Cu content is more than 0%, Cu stabilizes austenite and improves the non-magnetic properties of the steel. Cu also increases the toughness of the steel. Even if even a small amount of Cu is contained, the above effects can be obtained to some extent. However, when the Cu content exceeds 0.40%, the hot workability of the steel is reduced. Therefore, the Cu content is 0 to 0.40%, and when it is contained, it is 0.40% or less. The lower limit of the Cu content is preferably 0.01%, more preferably 0.02%, more preferably 0.05%, more preferably 0.07%, and even more preferably 0.10%. The upper limit of the Cu content is preferably 0.35%, more preferably 0.30%, further preferably 0.20%, and further preferably 0.15%.
[0042] Ni: 0.40% or less Nickel (Ni) is an optional element and may not be contained. In other words, the Ni content may be 0%. When contained, that is, when the Ni content is more than 0%, Ni stabilizes austenite and improves the non-magnetic properties of the steel material. Ni also increases the toughness of the steel material. Even if even a small amount of Ni is contained, the above effects can be obtained to some extent. However, when the Ni content exceeds 0.40%, chips during processing are not sufficiently peeled off and tend to remain in the steel material. Therefore, the Ni content is 0 to 0.40%, and when contained, it is 0.40% or less. The lower limit of the Ni content is preferably 0.01%, more preferably 0.02%, more preferably 0.05%, more preferably 0.07%, more preferably 0.10%, and more preferably 0.15%. The upper limit of the Ni content is preferably 0.35%, more preferably 0.30%, further preferably 0.20%, and further preferably 0.15%.
[0043] [Group 2: Cr, V, Ti, Mo, Al and Nb] The chemical composition of the steel material of this embodiment may further contain the above-mentioned second group elements in place of a portion of Fe. These elements are optional elements, and all of them increase the strength of the steel material. Each element will be described below.
[0044] Cr:1.50% or less Chromium (Cr) is an optional element and may not be contained. In other words, the Cr content may be 0%. When contained, that is, when the Cr content is more than 0%, Cr forms carbides and increases the strength of the steel material by precipitation strengthening. Cr also stabilizes austenite and improves the non-magnetic properties of the steel material. If even a small amount of Cr is contained, the above effects can be obtained to some extent. However, if the Cr content exceeds 1.50%, coarse Cr carbides are generated and the strength of the steel material decreases. Therefore, the Cr content is 0 to 1.50%, and if contained, it is 1.50% or less. The lower limit of the Cr content is preferably 0.01%, more preferably 0.02%, more preferably 0.05%, more preferably 0.10%, more preferably 0.20%, more preferably 0.30%, and more preferably 0.40%. The upper limit of the Cr content is preferably 1.40%, more preferably 1.30%, and further preferably 1.10%.
[0045] V: 0.25% or less Vanadium (V) is an optional element and may not be contained. In other words, the V content may be 0%. When it is contained, that is, when the V content is more than 0%, V forms carbides and increases the strength of the steel material by precipitation strengthening. Even if even a small amount of V is contained, the above effect can be obtained to some extent. However, when the V content exceeds 0.25%, the hot workability of the steel material is reduced. Therefore, the V content is 0 to 0.25%, and when it is contained, it is 0.25% or less. The lower limit of the V content is preferably 0.01%, more preferably 0.03%, further preferably 0.05%, and further preferably 0.10%. The upper limit of the V content is preferably 0.20%, more preferably 0.18%, and further preferably 0.15%.
[0046] Ti:0.100% or less Titanium (Ti) is an optional element and may not be contained. In other words, the Ti content may be 0%. When titanium is contained, that is, when the Ti content is more than 0%, Ti forms nitrides and increases the strength of the steel material by precipitation strengthening. Even if even a small amount of Ti is contained, the above effects can be obtained to some extent. However, when the Ti content exceeds 0.100%, the hot workability and cold workability of the steel material are reduced. Therefore, the Ti content is 0 to 0.100%, and when contained, it is 0.100% or less. The lower limit of the Ti content is preferably 0.001%, more preferably 0.005%, more preferably 0.010%, more preferably 0.015%, and more preferably 0.020%. The upper limit of the Ti content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, and further preferably 0.050%.
[0047] Mo: 1.00% or less Molybdenum (Mo) is an optional element and may not be contained. In other words, the Mo content may be 0%. When it is contained, that is, when the Mo content exceeds 0%, Mo forms carbides and increases the strength of the steel material by precipitation strengthening. Even if even a small amount of Mo is contained, the above effect can be obtained to a certain extent. However, when the Mo content exceeds 1.00%, the above effect becomes saturated and the manufacturing cost of the steel material increases. Therefore, the Mo content is 0 to 1.00%, and when it is contained, it is 1.00% or less. The lower limit of the Mo content is preferably 0.01%, more preferably 0.03%, further preferably 0.10%, and further preferably 0.15%. The upper limit of the Mo content is preferably 0.80%, more preferably 0.70%, and further preferably 0.60%.
[0048] Al: 0.100% or less Aluminum (Al) is an optional element and may not be contained. In other words, the Al content may be 0%. When aluminum is contained, that is, when the Al content is more than 0%, Al forms nitrides and refines austenite grains by a pinning effect. The refinement of austenite grains increases the strength of the steel material. Even if even a small amount of Al is contained, the above effect can be obtained to some extent. However, when the Al content exceeds 0.100%, excessive Al nitrides are generated. In this case, the amount of solid-solubilized N in the steel material decreases, and the stability of austenite decreases. Therefore, the Al content is 0 to 0.100%, and when contained, it is 0.100% or less. The lower limit of the Al content is preferably 0.001%, more preferably 0.005%, still more preferably 0.010%, still more preferably 0.015%, and still more preferably 0.020%. The upper limit of the Al content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, and further preferably 0.050%. In the chemical composition of the steel material of this embodiment, the Al content means the total Al content.
[0049] Nb: 0.050% or less Niobium (Nb) is an optional element and may not be contained. In other words, the Nb content may be 0%. When it is contained, that is, when the Nb content is more than 0%, Nb forms nitrides and refines austenite grains by a pinning effect. The refinement of austenite grains increases the strength of the steel material. Even if even a small amount of Nb is contained, the above effect can be obtained to some extent. However, when the Nb content exceeds 0.050%, the workability of the steel material decreases. Therefore, cracks are likely to occur during hot rolling and continuous casting. Therefore, the Nb content is 0 to 0.050%, and when it is contained, it is 0.050% or less. The lower limit of the Nb content is preferably 0.001%, more preferably 0.005%, more preferably 0.010%, more preferably 0.020%, and even more preferably 0.030%. The upper limit of the Nb content is preferably 0.045%, more preferably 0.043%, and further preferably 0.040%.
[0050] [Group 3: B] The chemical composition of the steel material of this embodiment may further contain the above-mentioned third group (B) in place of a portion of Fe.
[0051] B: 0.0050% or less Boron (B) is an optional element and may not be contained. In other words, the B content may be 0%. When it is contained, that is, when the B content exceeds 0%, B segregates at the grain boundaries to increase the grain boundary strength. As a result, the manufacturability of the steel material is improved. If even a small amount of B is contained, the above effect can be obtained to some extent. However, if the B content exceeds 0.0050%, B segregates excessively at the grain boundaries of the austenite grains. In this case, the grain boundary strength is rather reduced, and the manufacturability of the steel material is reduced. Therefore, the B content is 0 to 0.0050%, and when it is contained, it is 0.0050% or less. The lower limit of the B content is preferably 0.0001%, more preferably 0.0005%, more preferably 0.0010%, more preferably 0.0015%, and even more preferably 0.0020%. The upper limit of the B content is preferably 0.0040%, more preferably 0.0035%, and further preferably 0.0030%.
[0052] [Group 4: Bi, Pb and Ca] The chemical composition of the steel material of this embodiment may further contain the above-mentioned fourth group instead of a part of Fe. These elements are optional elements, and each of them suppresses the remaining of chips during processing. Each element will be described below.
[0053] Bi:0.20% or less Bismuth (Bi) is an optional element and may not be contained. In other words, the Bi content may be 0%. When contained, that is, when the Bi content is more than 0%, Bi suppresses the remaining of chips during processing. Even if even a small amount of Bi is contained, the above effect can be obtained to some extent. However, when the Bi content exceeds 0.20%, the hot workability of the steel material is reduced. Therefore, the Bi content is 0 to 0.20%, and when contained, it is 0.20% or less. The lower limit of the Bi content is preferably 0.01%, more preferably 0.03%, further preferably 0.05%, and further preferably 0.07%. The upper limit of the Bi content is preferably 0.18%, more preferably 0.15%, and further preferably 0.10%.
[0054] Pb: 0.09% or less Lead (Pb) is an optional element and may not be contained. In other words, the Pb content may be 0%. When it is contained, that is, when the Pb content is more than 0%, Pb suppresses the remaining of chips during processing. Even if even a small amount of Pb is contained, the above effect can be obtained to some extent. However, when the Pb content exceeds 0.09%, the hot workability of the steel material is reduced. Therefore, the Pb content is 0 to 0.09%, and when it is contained, it is 0.09% or less. The lower limit of the Pb content is preferably 0.01%, more preferably 0.04%, further preferably 0.05%, and further preferably 0.06%. The upper limit of the Pb content is preferably 0.08%, and more preferably 0.07%.
[0055] Ca:0.0100% or less Calcium (Ca) is an optional element and may not be contained. In other words, the Ca content may be 0%. When it is contained, that is, when the Ca content is more than 0%, Ca bonds with S to form Ca sulfides, or is contained in Mn sulfides to modify the form of Mn sulfides. As a result, the remaining of chips during processing is suppressed. If even a small amount of Ca is contained, the above effect can be obtained to a certain extent. However, if the Ca content exceeds 0.0100%, the above effect is saturated. Therefore, the Ca content is 0 to 0.0100%, and if it is contained, it is 0.0100% or less. The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0005%, further preferably 0.0010%, and further preferably 0.0015%. The upper limit of the Ca content is preferably 0.0080%, more preferably 0.0070%, and further preferably 0.0050%.
[0056] [(Feature 2) Number density of sulfides in steel] In the steel material of this embodiment, when the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present within 1 mm 2 The number of winning pieces is 1.0 x 10 2 ~5.0×10 3 The following definitions apply to Mn sulfides that contain 70% or more MnS by area and have a circle equivalent diameter of 1.0 to 5.0 μm. 2 The number of Mn sulfides per unit area is expressed as the Mn sulfide number density ND (units / mm 2 In this specification, Mn sulfides refer to particles (inclusions) in which the area ratio of MnS is 70% or more. Hereinafter, the Mn sulfide number density ND will be explained.
[0057] As described above, the steel material of this embodiment is cut to a predetermined length. Specifically, the steel material is cut using a cutting tool, typically a saw blade. In the cutting process, the steel material is cut by cutting the steel material with the cutting tool. When the cutting tool cuts the steel material, chips are generated. If the chips are long and difficult to peel off, local plastic deformation occurs near the chips when the chips are generated, and strain is introduced. On the other hand, if the chips are short, clogging occurs in the cutting tool, such as a saw blade. If the steel material is cut using a clogged cutting tool, deformation occurs on the cut surface of the steel material, and excessive strain is introduced into the steel material. These introduced strains cause processing-induced martensitic transformation after a long period of time. Since martensite exhibits ferromagnetic properties, sufficient non-magnetic properties cannot be obtained in the steel material.
[0058] If the chips generated during processing are of an appropriate length and the chip disposability is improved, excessive strain is unlikely to be introduced. In this case, processing-induced martensitic transformation is unlikely to occur even after a long period of time has passed. Therefore, sufficient non-magnetic properties are maintained even after a long period of time has passed.
[0059] The interface between Mn sulfides and the parent phase in the steel material becomes a source of stress concentration during processing. If Mn sulfides with a circle equivalent diameter of 1.0 to 5.0 μm are present at an appropriate number density, stress will concentrate at the interface between multiple Mn sulfides and the parent phase during cutting processing, and cracks will occur. If multiple cracks are connected, the cracks will propagate. In this case, the cracks will propagate and the cutting chips will peel off from the steel material before excessive plastic deformation occurs during cutting processing. Therefore, the introduction of strain during cutting processing is suppressed, and processing-induced martensitic transformation after a long period of time can be suppressed.
[0060] In order to generate cracks at the interface between the Mn sulfide and the parent phase during cutting and to link a plurality of cracks, it is effective to adjust the number density of Mn sulfides having an equivalent circle diameter of 1.0 to 5.0 μm.
[0061] The Mn sulfide number density N is 1.0×10 2 pieces / mm 2 If the Mn sulfide number density ND is less than 5.0×10, the number density of Mn sulfides is too low. Therefore, cracks do not occur sufficiently at the interface between the Mn sulfides and the matrix. As a result, the chips generated during cutting become long, and chip disposal becomes difficult. In this case, the long chips remain in the steel material while undergoing plastic deformation. As a result, excessive strain is introduced into the steel material. On the other hand, if the Mn sulfide number density ND is more than 5.0×10, the number density of Mn sulfides is too low. Therefore, cracks do not occur sufficiently at the interface between the Mn sulfides and the matrix. As a result, the chips become long, and chip disposal becomes difficult. In this case, the long chips remain in the steel material while undergoing plastic deformation. As a result, excessive strain is introduced into the steel material. 3 pieces / mm 2 If the cutting length exceeds , the length of the chips becomes excessively short, and chip disposal becomes poor. In this case, excessively short chips cause clogging of cutting tools such as saw blades. If a steel material is cut using a clogged cutting tool, deformation occurs on the cut surface of the steel material, and excessive strain is introduced into the steel material. The introduced strain causes processing-induced martensitic transformation after a long period of time, deteriorating the nonmagnetic properties of the steel material. The remaining chips may scratch the surface of other steel materials. In steel material with scratches, stress is concentrated near the scratches during bending, and excessive strain is introduced.
[0062] The Mn sulfide number density N is 1.0×10 2 ~5.0×10 3 pieces / mm 2If so, the Mn sulfide number density ND is appropriate. Therefore, the length of the chips is in an appropriate range, and chip disposability is improved. Therefore, during cutting, the chips peel off from the steel material without introducing excessive strain. Therefore, the occurrence of processing-induced martensitic transformation after a long period of time is suppressed, and sufficient non-magnetic properties are maintained.
[0063] The preferred lower limit of the Mn sulfide number density N is 2.0×10 2 pieces / mm 2 and more preferably 3.0×10 2 pieces / mm 2 and more preferably 4.0×10 2 pieces / mm 2 and more preferably 5.0×10 2 pieces / mm 2 The preferred upper limit of the Mn sulfide number density N is 4.5×10 3 pieces / mm 2 and more preferably 4.0×10 3 pieces / mm 2 and more preferably 3.5×10 3 pieces / mm 2 and more preferably 3.0×10 3 pieces / mm 2 It is.
[0064] [Method for measuring Mn sulfide number density ND] The Mn sulfide number density ND is measured by the following method.
[0065] The cross section including the central axis of the steel material and parallel to the axial direction (central axis direction) is taken as the investigation surface. The diameter of the steel material is D. If the steel material is a deformed steel material, the nominal diameter of the steel material is D. A test piece is taken from the investigation surface including a depth position of D / 4 in the radial direction from the steel material surface. The taken test piece is embedded in resin. The investigation surface of the test piece embedded in resin is mirror polished. After mirror polishing, a 200x optical microscope is used to observe 30 arbitrary fields of view including the D / 4 depth position on the investigation surface to generate photographic images. The area of each field of view is 0.3 mm 2 Let us assume that.
[0066] In each field of view, Mn sulfides are identified based on the contrast. Specifically, MnS is identified as a light gray area. The parent phase is identified as a white area brighter than MnS. Inclusions, precipitates, etc. other than MnS are identified as areas with lower brightness than Mn sulfides (areas that are darker gray or black than MnS). Therefore, a person skilled in the art can identify MnS in the field of view based on the contrast. Among the particles in the field of view, particles with an area ratio of MnS recognized by the contrast of 70% or more are identified as "Mn sulfides". In other words, Mn sulfides may be inclusions with an area ratio of MnS of 100%, or may be composite inclusions of MnS and other elements.
[0067] Among the identified Mn sulfides, sulfides with an equivalent circle diameter of 1.0 to 5.0 μm are identified. The equivalent circle diameter can be measured by known image processing. Based on the total number of Mn sulfides with an equivalent circle diameter of 1.0 to 5.0 μm in the 30 visual fields and the total area of the 30 visual fields, the Mn sulfide number density ND (number / mm 2 ) is required.
[0068] [Effects of the steel material according to this embodiment] The steel material of this embodiment satisfies the above-mentioned features 1 and 2. Therefore, it is possible to sufficiently suppress the remaining chips during processing. Therefore, it is possible to sufficiently suppress the processing-induced martensitic transformation after processing. In addition, excellent bending workability is obtained, and excellent nonmagnetic properties are obtained after processing.
[0069] [Shape of steel material in this embodiment] The steel material of this embodiment is a steel material having a circular cross section perpendicular to the axial direction. The steel material of this embodiment may be a deformed steel material having a rim portion. The steel material of this embodiment is, for example, a steel bar or a wire rod. The steel material may be wound in a coil shape or may be cut to a predetermined length.
[0070] [Use of the steel material according to this embodiment] As described above, the steel material of this embodiment is suitable for use in structural members used in a magnetic field environment. The steel material of this embodiment is suitable for use in linear motor car-related facilities, for example. However, the steel material of this embodiment may be used for applications other than the structural members used in the magnetic field environment described above.
[0071] [Steel manufacturing method] An example of a method for manufacturing the steel material of this embodiment will be described. The method for manufacturing the steel material described below is one example for manufacturing the steel material of this embodiment. Therefore, the steel material having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing the steel material of this embodiment.
[0072] An example of a method for manufacturing a steel material according to this embodiment includes the following steps. (Process 1) Material preparation process (Process 2) Rough rolling process (Process 3) Finish rolling process Each step will be described below.
[0073] [(Process 1) Material preparation process] In the material preparation step, a material for the steel material of this embodiment is prepared. Specifically, molten steel having a chemical composition that satisfies characteristic 1 is produced. The refining method is not particularly limited, and any known method may be used. The produced molten steel is used to produce a material by a known casting method. For example, an ingot may be produced by an ingot casting method using the molten steel. Also, a bloom may be produced by a continuous casting method using the molten steel. The material (ingot or bloom) is produced by the above method.
[0074] [(Process 2) Rough rolling process] In the rough rolling process, the material (ingot or bloom) prepared in the material preparation process is subjected to rough rolling to produce a billet. Specifically, the material is heated using a heating furnace. The heating temperature is not particularly limited. The heating temperature is, for example, 1000 to 1250°C.
[0075] The heated material is subjected to hot rolling to produce a billet. For example, the heated material is hot rolled using a blooming mill to produce a billet. The billet after blooming may be further hot rolled using a continuous rolling mill to produce a smaller billet. The billet produced by the above rough rolling process is allowed to cool (air-cool) to room temperature.
[0076] [(Process 3) Finish rolling process] In the finish rolling process, the billet produced in the rough rolling process is heated. The heated billet is subjected to hot rolling using a continuous rolling mill equipped with a number of rolling stands arranged in a row to produce a steel material. Mn sulfides are produced in the casting process. The Mn sulfides produced in the casting process are coarse. Therefore, the size and number density of the Mn sulfides are adjusted by heating in the finish rolling process. Specifically, the following conditions are satisfied in the finish rolling process. (Condition 1) The heating temperature T of the billet is set to more than 1200°C to 1250°C. (Condition 2) The holding time t at the heating temperature T is set to more than 10 minutes and up to 150 minutes. (Condition 3) M defined by the following formula (1) is set to 14,000 to 15,500. M = (T + 273) × (10 + log (t / 60)) (1) Here, the heating temperature (°C) in the finish rolling process is substituted for T in the formula (1), and the holding time (min) at the heating temperature T is substituted for t. (Condition 4) The finish rolling temperature FT is set to 1000°C or higher. Here, the finish rolling temperature FT means the surface temperature (° C.) of a steel material at the exit side of a rolling stand that has applied the final reduction in a continuous rolling mill having a plurality of rolling stands arranged in a row. Each condition of the finish rolling process will be described below.
[0077] [(Condition 1) Heating temperature T] If the heating temperature T is 1200°C or less, the coarse Mn sulfides generated in the casting process are not sufficiently broken down. As a result, the Mn sulfide number density ND becomes extremely low. On the other hand, if the heating temperature T exceeds 1250°C, the Mn sulfides are excessively broken down. As a result, the Mn sulfide number density ND becomes excessively high. If the heating temperature T is more than 1200 to 1250°C, the Mn sulfide number density ND becomes an appropriate amount.
[0078] [(Condition 2) Retention time t] If the holding time t at the heating temperature T is 10 minutes or less, the coarse Mn sulfides generated in the casting process are not sufficiently broken down. As a result, the Mn sulfide number density ND becomes extremely low. On the other hand, if the holding time t exceeds 150 minutes, the Mn sulfides are excessively broken down. As a result, the Mn sulfide number density ND becomes excessively high. If the holding time t at the heating temperature T is more than 10 minutes to 150 minutes, the Mn sulfide number density ND becomes an appropriate amount.
[0079] [(Condition 3) Regarding M] Even if the heating temperature T and the holding time t satisfy the conditions 1 and 2, if M is less than 14000, the coarse Mn sulfides generated in the casting process are not sufficiently broken down. As a result, the number density ND of the Mn sulfides becomes extremely small. On the other hand, if M exceeds 15500, the Mn sulfides are excessively broken down. As a result, the number density ND of the Mn sulfides becomes excessively large. If M is 14000 to 15500, the number density ND of the Mn sulfides becomes appropriate.
[0080] [(Condition 4) Finish rolling temperature FT] The heated billet is hot-rolled by a continuous rolling mill. Even during this hot rolling, the Mn sulfides in the steel are broken down by external forces from the rolls of the rolling stand. If the finishing rolling temperature FT is less than 1000°C, the temperature of the steel during hot rolling is too low. In this case, the coarse Mn sulfides in the steel are not broken down sufficiently. As a result, the Mn sulfide number density ND becomes extremely low. If the finishing rolling temperature FT is 1000°C or higher, the Mn sulfide number density ND becomes an appropriate amount.
[0081] The steel material of this embodiment is manufactured by the above manufacturing process. EXAMPLES
[0082] The effect of the steel material of this embodiment will be described more specifically with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the steel material of this embodiment is not limited to this one example of conditions.
[0083] Steel materials having the chemical compositions shown in Table 1 (Tables 1A to 1D) were produced by the following method.
[0084] [Table 1A]
[0085] [Table 1B]
[0086] [Table 1C]
[0087] [Table 1D]
[0088] Steel materials (blooms) having the chemical compositions of the respective test numbers were manufactured. The produced bloom was subjected to a rough rolling process to produce a billet. Specifically, the bloom was heated at 1000 to 1250°C using a heating furnace. The heated bloom was rolled (rough rolling) using a blooming mill and a continuous rolling mill to produce a billet. The billet produced in the rough rolling process was allowed to cool to room temperature.
[0089] The manufactured billets were subjected to a finish rolling process. Specifically, the billets of each test number were heated at the heating temperature T (°C) and the holding time at the heating temperature T for the period t (min) shown in Table 2 (Tables 2A and 2B). The M value for each test number was as shown in Table 2. The heated billets were subjected to hot rolling using a continuous rolling mill. At this time, the finish rolling temperature FT (°C) was as shown in Table 2 (Tables 2A and 2B).
[0090] [Table 2A]
[0091] [Table 2B]
[0092] The steel material (wire rod) after the finish rolling was allowed to cool to room temperature. Through the above manufacturing process, steel materials (wire rods) having a diameter of 20 mm and each test number were manufactured.
[0093] [About the evaluation test] The following steel evaluation tests (Tests 1 to 4) were carried out on the manufactured steel materials having each test number. [Steel material evaluation test] (Test 1) Mn sulfide number density ND measurement test (Test 2) Chip disposal evaluation test (Test 3) Bendability evaluation test (Test 4) Non-magnetic property evaluation test Each test will be explained below.
[0094] [(Test 1) Mn sulfide number density ND measurement test] Based on the above [Method for measuring Mn sulfide number density ND], the Mn sulfide number density ND (pieces / mm 2 The Mn sulfide number density ND was calculated as shown in Table 2. 2 ) column.
[0095] [(Test 2) Evaluation test of chip disposal] The following chip disposal evaluation test was conducted on the steel material with each test number. A test piece with a diameter of 18 mm and a length of 100 mm was taken from the steel material with each test number. The central axis of the test piece was coaxial with the central axis of the steel material. The peripheral turning process was performed on the test piece under the following conditions. The cutting tool was an uncoated ultra-high alloy equivalent to M20 specified in JIS B 4053 (2013). The cutting speed was 100 m / min, the feed rate was 0.20 mm / rev, and the cutting depth was 1.0 mm. Water-soluble cutting oil was used during turning. Under the above conditions, the peripheral turning process was performed on the test piece with each test number until the diameter reached 10 mm.
[0096] The length of the longest chip (maximum chip length) was determined among the chips obtained by peripheral turning. The length of the longest chip was defined as the length of the line segment (straight line) connecting the two ends of each chip. The ratio of the maximum chip length of each test number to the maximum chip length of the test piece with test number 60 was determined. The obtained value was defined as the maximum chip length ratio LR. The maximum chip length obtained is shown in the "Maximum chip length (mm)" column of Table 2. The maximum chip length ratio LR obtained is shown in the "Maximum chip length ratio LR" column of Table 2. If the maximum chip length ratio LR was 0.10 to 0.80, it was determined that the chip disposal property during processing was excellent.
[0097] [(Test 3) Bendability evaluation test] The following bending workability test was conducted on the steel material of each test number. Ten test pieces with a diameter of 14 mm and a length of 100 mm were taken from the steel material of each test number. The central axis of the test piece was coaxial with the central axis of the steel material. A bending test in accordance with JIS Z2248 (2022) was conducted using the 10 test pieces taken. Specifically, each test piece was bent 180°. The presence or absence of cracks in the 10 test pieces after bending was completed was confirmed. If no cracks were confirmed in any of the 10 test pieces, it was determined that excellent bending workability was obtained (indicated by "○" in the "Bending workability" column in Table 2). On the other hand, if a crack was confirmed in even one of the test pieces, it was determined that sufficient bending workability was not obtained (indicated by "×" in the "Bending workability" column in Table 2).
[0098] [(Test 4) Non-magnetic property evaluation test] The relative permeability was measured at the bent portion of the 10 test pieces after the above-mentioned bending test. Specifically, using a permeability / magnetic field strength measuring device (Förster Magnetscope), the relative permeability of the convex side after bending was measured for the 10 test pieces of each test number according to a method conforming to ASTM A342M. The maximum value of the 10 relative permeabilities was taken as the relative permeability of the steel material of that test number. The obtained relative permeability is shown in the "Relative Permeability" column of Table 2. If the obtained relative permeability was 1.100 or less, it was determined that excellent non-magnetic properties were obtained.
[0099] [Evaluation Results] The evaluation results are shown in Table 2 (Table 2A and Table 2B). Test Nos. 1 to 49 satisfied features 1 and 2. Therefore, excellent chip disposal during processing was achieved, and excellent bending workability was also achieved. Furthermore, sufficient non-magnetic properties were achieved.
[0100] On the other hand, in test number 50, the C content was too low, and therefore sufficient non-magnetic properties were not obtained.
[0101] In test number 51, the C content was too high, and therefore sufficient bending workability was not obtained.
[0102] In test number 52, the Si content was too high, and therefore sufficient bending workability was not obtained.
[0103] In test number 53, the Mn content was too low, so sufficient non-magnetic properties were not obtained.
[0104] In test number 54, the P content was too high, and therefore sufficient bending workability was not obtained.
[0105] In test number 55, the S content was too low, so the maximum cutting length ratio LR exceeded 0.80, and sufficient chip disposability was not obtained.
[0106] In test number 56, the S content was too high, and therefore sufficient bending workability was not obtained.
[0107] In test number 57, the N content was too low, so sufficient non-magnetic properties were not obtained.
[0108] In test numbers 58 to 60, the heating temperature T was too low, and therefore the Mn sulfide number density ND was too low, resulting in a maximum chip length ratio LR exceeding 0.80, and insufficient chip disposability being obtained.
[0109] In test numbers 61 and 62, the holding time t was too short, and therefore the Mn sulfide number density ND was too low, and as a result, the maximum chip length ratio LR exceeded 0.80, and sufficient chip disposability was not obtained.
[0110] In the test numbers 63 and 64, the holding time t was too long, and therefore the Mn sulfide number density ND was too high, and as a result, the maximum chip length ratio LR was less than 0.10, and sufficient chip disposability was not obtained.
[0111] In test numbers 65 and 66, the M value was too low, and therefore the Mn sulfide number density ND was too low, resulting in a maximum cutting length ratio LR exceeding 0.80, and insufficient chip disposability being obtained.
[0112] In test numbers 67 to 69, the M value was too high, and therefore the Mn sulfide number density ND was too high, and as a result, the maximum chip length ratio LR was less than 0.10, and sufficient chip disposability was not obtained.
[0113] In the test numbers 70 and 71, the finish rolling temperature FT was too low, and therefore the Mn sulfide number density ND was too low, resulting in a maximum chip length ratio LR exceeding 0.80, and insufficient chip disposability being obtained.
[0114] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. A steel material, The chemical composition, in mass%, is C: 0.75-1.10%, Si: 0.10-0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%; The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present. 2 The number of winning pieces is 1.0 x 10 2 ~5.0 x 10 3 Individual Steel material.
2. A steel material, The chemical composition, in mass%, is C: 0.75-1.10%, Si: 0.10-0.70%, Mn: 11.00-18.00%, P: 0.050% or less, S: 0.010 to 0.070%, and N: 0.005 to 0.024%; Further, the composition contains one or more selected from the group consisting of Groups 1 to 4, The balance is Fe and impurities. When the diameter of the steel material is D, in a cross section parallel to the axial direction of the steel material, at a depth position of D / 4 in the radial direction from the surface of the steel material, Mn sulfides containing MnS at an area ratio of 70% or more and having a circle equivalent diameter of 1.0 to 5.0 μm are present. 2 The number of winning pieces is 1.0 x 10 2 ~5.0 x 10 3 Individual Steel material. [Group 1] Cu: 0.40% or less, and Ni: 0.40% or less, one or more selected from the group consisting of [Group 2] Cr: 1.50% or less, V: 0.25% or less, Ti: 0.100% or less, Mo: 1.00% or less, Al: 0.100% or less, and Nb: 0.050% or less, one or more selected from the group consisting of [Group 3] B: 0.0050% or less [Group 4] Bi: 0.20% or less, Pb: 0.09% or less; and Ca: 0.0100% or less, one or more selected from the group consisting of
3. The steel material according to claim 2, The chemical composition contains the first group, Steel material.
4. The steel material according to claim 2, The chemical composition contains the second group, Steel material.
5. The steel material according to claim 2, The chemical composition contains the third group, Steel material.
6. The steel material according to claim 2, The chemical composition contains the fourth group. Steel material.
Citation Information
Patent Citations
High-mn nonmagnetic reinforcing steel bar and its production
JP1991013544A
Non-magnetic steel excellent in low temperature bendability
JP2014205908A