film

A film with a resin composition of cellulose ester, aliphatic polyester, and acrylic polymer balances impact resistance and transparency, offering enhanced mechanical properties and decorative qualities for various applications.

JP2024148792AInactive Publication Date: 2024-10-18MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023062238
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Films laminated on the surfaces of articles often require impact resistance and transparency to allow visibility of the underlying product, but existing films do not adequately balance these properties.

Method used

A film composed of a resin composition containing cellulose ester compound, aliphatic polyester, and acrylic polymer, with specific ratios and properties to enhance impact resistance and transparency, featuring a sea-island structure with a continuous phase of cellulose ester and aliphatic polyester and a dispersed phase of acrylic polymer.

Benefits of technology

The film achieves excellent transparency, impact resistance, and matte appearance, suitable for decorative and protective applications, with improved mechanical properties and designability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148792000001
    Figure 2024148792000001
  • Figure 2024148792000002
    Figure 2024148792000002
  • Figure 2024148792000003
    Figure 2024148792000003
Patent Text Reader

Abstract

To provide a film having excellent transparency and impact resistance.SOLUTION: There is provided a film composed of a resin composition comprising a cellulose ester compound (A), an aliphatic polyester (B) and an acrylic polymer (C), wherein the tensile modulus in the MD direction is 1300 MPa or less and the tensile elongation at break in the MD direction is 80% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film. [Background technology]

[0002] Films that are laminated on the surfaces of various articles are known. For example, protective films for polarizing plates, retardation films, viewing angle expansion films, etc., used in liquid crystal display devices It is used as an optical film such as an anti-reflection film for films and plasma displays. USP 5,333,636 describes cellulose ester films which can be used. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-54100 A Summary of the Invention [Problem to be solved by the invention]

[0004] Impact resistance is sometimes required for films laminated on the surface of articles. In some cases, transparency is required to allow the surface of the article underneath to be seen. An object of the present invention is to provide a film that is excellent in transparency and impact resistance. [Means for solving the problem]

[0005] The present invention has the following aspects. [1] A cellulose ester compound (A), an aliphatic polyester (B), and an acrylic polymer A film made of a resin composition containing the composite (C), having a tensile modulus of elasticity in the MD direction of 1300 MPa or less and a tensile elongation at break in the MD direction of 80% or more. [2] The content of the cellulose ester compound (A) relative to the total mass of the resin composition. The film according to [1], wherein the amount is 10% by mass or more and 60% by mass or less. [3] The content of the aliphatic polyester (B) relative to the total mass of the resin composition is 1. The film according to [1] or [2], wherein the content is 0% by mass or more and 50% by mass or less. [4] The content of the acrylic polymer (C) relative to the total mass of the resin composition is 10% by mass. The film according to any one of [1] to [3], wherein the content is from 50% by mass to 50% by mass. [5] The aliphatic polyester (B) comprises a constitutional unit derived from an aliphatic polycarboxylic acid and an aliphatic Any of [1] to [4], which is a polymer having a structural unit derived from an aromatic polyhydric alcohol. The film described. [6] The film according to any one of [1] to [5], having a total light transmittance of 90% or more. . [7] Any of [1] to [6] whose puncture impact at 23°C is 1.5 J or more. The film described in any one of the above. Effect of the Invention

[0006] According to the present invention, a film having excellent transparency and excellent impact resistance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] In this specification, the term "structural unit" of a polymer refers to a unit (atom) formed from one monomer molecule. It means a group. In this specification, the symbol "~" indicating a range of values ​​indicates that the values ​​before and after the symbol are the lower limit and the It means inclusive as an upper limit.

[0008] ≪Resin composition (X)≫ The resin composition (X) of the present embodiment comprises a cellulose ester compound (A), an aliphatic polyester compound (B), and a cellulose ester compound (C). The copolymer contains a terephthalate (B) and an acrylic polymer (C).

[0009] <Cellulose ester compound (A)> The cellulose ester compound (A) is, for example, cellulose propionate (CP ), cellulose butyrate (CB), cellulose acetate propionate (CAP), Cellulose acetate butyrate (CAB), Cellulose acetate isobutyrate (C AIB), cellulose propionate butyrate (CPB), etc. From the viewpoint of film transparency, cellulose acetate propionate is preferred. The ester compound (A) may be used alone or in combination of two or more kinds. The resin composition (X) is a cellulose ester compound which is a substance derived from a renewable organic resource. By including this, the environmental impact can be reduced.

[0010] The glass transition temperature (Tg) of the cellulose ester compound (A) depends on the function of the resulting film. From the viewpoint of mechanical properties, the temperature is preferably 120°C or higher, and more preferably 130°C or higher. From this viewpoint, the temperature is preferably 180° C. or lower, and more preferably 170° C. or lower. The glass transition temperature (Tg) of the cellulose ester compound (A) is determined according to JIS K7244- 4:1999, using a viscoelastic spectrometer at a heating rate of 3°C / min. It is calculated from the peak top temperature of the loss tangent (tan δ) when the temperature is raised by can be done.

[0011] <Aliphatic polyester (B)> The aliphatic polyester (B) is a polyester having a constitutional unit derived from an aliphatic hydroxycarboxylic acid. The polymer (b-1) has a constitutional unit derived from an aliphatic polyvalent carboxylic acid and a constitutional unit derived from an aliphatic polyhydric alcohol. and polymers (b-2) having the following structural units.

[0012] The polymer (b-1) contains, with respect to all structural units, a structure derived from an aliphatic hydroxycarboxylic acid. The proportion of the structural unit is preferably 80% by mass or more, and more preferably 90% by mass or more. It may be 100% by mass, which is preferable. Specific examples of the polymer (b-1) include polyglycolic acid, polylactic acid, poly(3-hydroxyl) acid, and the like. Poly(4-hydroxybutyric acid), Poly(4-hydroxyvaleric acid), Poly(3-hydroxyhexanoic acid) Examples of the polycaprolactone include acrylic acid and polycaprolactone.

[0013] The polymer (b-2) contains, relative to all structural units, structural units derived from aliphatic polyvalent carboxylic acids. and the total proportion of structural units derived from aliphatic polyhydric alcohols is preferably 80 mass % or more. It is preferably 90% by mass or more, and may be 100% by mass. Specific examples of the polymer (b-2) include polyethylene adipate and polypropylene adipate. Polybutylene adipate, Polyhexene adipate, Polybutylene succinate ( Examples include polybutylene succinate adipate (PBSA), etc.

[0014] Of the above, aliphatic polyester (B) is preferred from the viewpoints of impact resistance and matte finish of the film. , polybutylene succinate-based resin is preferable, and polybutylene succinate ( More preferably, the polybutylene succinate is poly(butylene phosphate buffered saline) or polybutylene succinate adipate (PBSA). Among them, polybutylene succinate (PBS) is more preferable. Aliphatic polyesters (B) are made from renewable organic resources. preferable.

[0015] <Acrylic polymer (C)> The acrylic polymer (C) includes the following polymer (Ca) and the following polymer (Cb). Acrylic polymer (c-1), polymer (Cd) alone consisting of acrylic polymer (c-2), etc. Some examples include:

[0016] =Acrylic polymer (c-1)= The acrylic polymer (c-1) is a polymer (Ca) obtained by polymerizing the monomer components described below. It is preferable that the polymer (Cb) is a polymer obtained by polymerizing the monomer components of the polymer (Cb) in the presence of stomach. The acrylic polymer (c-1) is a polymer having a core layer and at least one shell layer covering the core layer. The acrylic polymer (c-1) may be a multilayer structure polymer. In the case of the above, the innermost layer is composed of a polymer (Ca) and the outermost layer is composed of a polymer (Cb). It is preferable that

[0017] The acrylic polymer (c-1) may further contain a polymer (Cc). The acrylic polymer (c-1) is a polymer (Ca), a polymer (Cb), and a polymer (Cc). In the case where the acrylic polymer (c-1) contains the polymer (Cc) in the presence of the polymer (Ca), A polymer obtained by polymerizing the monomer component of (Cb) and then polymerizing the monomer component of polymer (Cb). It is preferable that there is. Acrylic polymers (c-1) including polymer (Ca), polymer (Cb), and polymer (Cc) When the polymer has a multi-layer structure, the innermost layer is made of polymer (Ca) and the outermost layer is made of polymer (Cb ), and between the outermost layer and the innermost layer there is a layer composed of a polymer (Cc). preferable.

[0018] [Polymer (Ca)] The polymer (Ca) has an alkyl group having 1 to 8 carbon atoms and one double bond in each molecule. A structural unit derived from (meth)acrylic acid ester (MA1) and a double bond in one molecule. It contains a constituent unit derived from a monomer (MA2) having at least one of the above units.

[0019] In the (meth)acrylic acid ester (MA1), the alkyl group having 1 to 8 carbon atoms is It may be either linear or branched. A specific example of the (meth)acrylic acid ester (MA1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate These may be used alone or in combination of two or more. Among them, those having a low Tg in the homopolymer are preferred, and acrylic acid alkyl esters are preferred. is more preferred, with butyl acrylate being particularly preferred.

[0020] The content of (meth)acrylic acid ester (MA1) is the monomer constituting the polymer (Ca). The total amount of the above is preferably 40% by mass or more, and more preferably 50% by mass or more, based on 100% by mass of the total amount of the above. It is preferably 70% by mass or more, more preferably 90% by mass or more, and particularly preferably 99. It is preferably 9% by mass or less, and more preferably 99.7% by mass or less.

[0021] The monomer (MA2) is copolymerizable with the (meth)acrylic acid ester (MA1). It is a monomer that has two or more double bonds in one molecule. Specific examples of the monomer (MA2) include ethylene glycol di(meth)acrylate, 1 ,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate alkylene glycols such as acrylate, propylene glycol di(meth)acrylate, etc. vinyl di(meth)acrylate; polyvinylbenzene such as divinylbenzene and trivinylbenzene Cyanurate monomers such as triallyl cyanurate and triallyl isocyanurate Allyl esters and methallyl esters of α,β-unsaturated carboxylic acids or dicarboxylic acids These may be used alone or in combination of two or more. They may also be used in combination. Of the above, alkylene glycol di(meth)acrylate, acrylic acid, methacrylate Preferred are allyl esters of allylic acid, maleic acid or fumaric acid, among which allyl methacrylate is preferred. Acrylates are more preferred.

[0022] The content of the monomer (MA2) is set to be equal to or smaller than the content of the monomer constituting the polymer (Ca) from the viewpoint of impact resistance. The content is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, based on 100% by mass of the total amount of the body. From the viewpoint of film formability, the content is preferably 60% by mass or less, and more preferably 50% by mass or less. The content is more preferably 30% by mass or less, further preferably 10% by mass or less.

[0023] The glass transition temperature (Tg) of the polymer (Ca) is set to 25°C or lower from the viewpoint of the impact resistance of the film. Preferably, the temperature is below 10°C, more preferably below 0°C, and particularly preferably below 0°C. From the viewpoint of film formability, Tg is preferably -100°C or higher, and more preferably -80 ° C. or higher is more preferable. The glass transition temperature (Tg) of the polymer (Ca) is HandBook (J. Brandrup, Interscience, 1989)〕 Using the values ​​listed in the table, the monomers that make up the polymer (Ca) are calculated using the FOX formula. In addition, the viscoelasticity spectrum can be calculated using a method conforming to JIS K7244-4:1999. The loss tangent (tan δ) when the temperature was increased at a heating rate of 3°C / min using a trometer It can be determined from the peak top temperature. The glass transition temperatures of the polymers (Cb), (Cc), and (Cd) described below are also similar. do.

[0024] [Polymer (Cb)] The polymer (Cb) has an alkyl group having 1 to 4 carbon atoms and one double bond in each molecule. A polymer containing a structural unit derived from a (meth)acrylic acid ester (MB1) (provided that the polymer The polymer (Cb) is a polymer having a constitutional unit derived from the monomer (MA2). Does not include.

[0025] In the (meth)acrylic acid ester (MB1), the alkyl group having 1 to 4 carbon atoms is It may be either linear or branched. A specific example of the (meth)acrylic acid ester (MB1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate These may be used alone or in combination of two or more. Among these, those having a low Tg in the homopolymer are preferred, and alkyl acrylates are preferred. Esters are more preferred, with butyl acrylate being especially preferred.

[0026] The content of (meth)acrylic acid ester (MB1) is the monomer constituting polymer (Cb). The total amount of the above is preferably 50% by mass or more, and more preferably 80% by mass or more, based on 100% by mass of the total amount of the above. It may be 100% by mass.

[0027] The glass transition temperature (Tg) of the polymer (Cb) may be different from that of the polymer (Ca); The Tg of the polymer (Cb) is preferably higher than the Tg of the polymer (Ca). From the viewpoint of mechanical properties, 60°C or higher is preferable, 70°C or higher is more preferable, and 80°C or higher is even more preferable. From the viewpoint of film formability, the temperature is preferably 150° C. or less, and more preferably 130° C. or less. is more preferred.

[0028] [Polymer (Cc)] The polymer (Cc) has an alkyl group having 1 to 8 carbon atoms and one double bond in each molecule. The structural unit derived from (meth)acrylic acid ester (MC1) and the double bond are two in one molecule. It is preferable that the monomer (MC1) contains a structural unit derived from a monomer (MC2) having at least one of the above units. A preferred embodiment of the (meth)acrylic acid ester (MC1) is the same as that of the polymer (Ca). The preferred embodiment of the monomer (MC2) is the same as that of the polymer (Ca). This is similar to (MA2) mentioned above. The composition (type and ratio) of the monomers constituting the polymer (Cc) and the It is preferable that the compositions (types and ratios) of the monomers constituting the polymerization copolymer (polymerization copolymer) are not the same. The monomer composition of the polymer (Cc) is different from that of the polymer (Ca). This makes it easier to improve the mechanical properties of the rubber.

[0029] The content of the (meth)acrylic acid ester (MC1) is the same as that of the monomer constituting the polymer (Cc). The amount is preferably 40% by mass or more, more preferably 50% by mass or more, based on 100% by mass of the total amount of the monomers. It is preferably 70% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more. It is preferably 9.9% by mass or less, and more preferably 99.7% by mass or less.

[0030] The content of the monomer (MC2) is set to be equal to or less than the content of the monomer constituting the polymer (Cc) from the viewpoint of impact resistance. The content is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, based on 100% by mass of the total amount of the body. From the viewpoint of film formability, the content is preferably 60% by mass or less, and more preferably 50% by mass or less. The content is more preferably 30% by mass or less, further preferably 10% by mass or less.

[0031] The glass transition temperature (Tg) of the polymer (Cc) is determined from the viewpoint of the mechanical properties of the film. Ca). Specifically, from the viewpoint of mechanical properties, it is preferably 0° C. or higher. It is preferable that the temperature is higher than 0°C, and more preferable that the temperature is higher than 10°C. A temperature of 0°C or lower is preferable, and a temperature of 80°C or lower is more preferable. For example, if the glass transition temperature (Tg) of polymer (Cc) is higher than the glass transition temperature (Tg) of polymer (Ca), The absolute value of the difference is preferably 10 to 80°C, and more preferably 20 to 70°C. It is more preferable that the absolute value of the difference between the two is equal to or greater than the lower limit of the above range. When the content is equal to or less than the upper limit, the film can be easily molded. It will be good.

[0032] The content of the polymer (Ca) relative to the total mass of the acrylic polymer (c-1) is From the viewpoints of the properties, transparency and moldability, the content is preferably 5% by mass or more, and more preferably 10% by mass or more. The content is preferably 60% by mass or less, and more preferably 55% by mass or less. Below is more preferable. The content of the polymer (Cb) relative to the total mass of the acrylic polymer (c-1) is 40% by mass. When the content is more than the above lower limit, the impact resistance of the film is reduced. In addition, it has excellent transparency and moldability. % by mass or less is more preferable, 80% by mass or less is even more preferable, and 70% by mass or less is even more preferable. Preferred. In addition, when the acrylic polymer (c-1) contains the polymer (Cc), the acrylic polymer (c- The content of the polymer (Cc) relative to the total mass of 1) is 1 mass% or more from the viewpoint of mechanical properties. The content is preferably 35% by mass or less. The content of the polymer (Ca), the content of the polymer (Cb), and the content of the polymer ( The total content of Cc) does not exceed 100% by mass. It may be 100% by mass.

[0033] =Acrylic polymer (c-2)= [Polymer (Cd)] The polymer (Cd) has an alkyl group having 1 to 18 carbon atoms and one double bond in each molecule. It is a polymer containing structural units derived from a (meth)acrylic acid ester (MD1).

[0034] In the (meth)acrylic acid ester (MD1), the alkyl group having 1 to 18 carbon atoms is The alkyl group may be either linear or branched. A specific example of the (meth)acrylic acid ester (MD1) is methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl ( (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, desic (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate acrylate, stearyl (meth)acrylate, icosyl (meth)acrylate, heminecosyl (Meth)acrylate, behenyl (meth)acrylate and other linear alkyl (meth)acrylates acrylate; isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec -Butyl (meth)acrylate, t-Butyl (meth)acrylate, Isopentyl (meth)acrylate ) acrylate, neopentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, iso Decyl (meth)acrylate, Isostearyl (meth)acrylate, Isoicosyl (meth)acrylate Branched alkyl (meth)acrylates such as cyclohexyl (meth)acrylate; acrylate, t-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, adamantyl (Meth)acrylate and other alicyclic (meth)acrylates. Among these, T in homopolymers may be used. Those having a low g are preferred, and alkyl acrylates are more preferred, and methyl methacrylates are more preferred. Rate is particularly preferred.

[0035] The content of (meth)acrylic acid ester (MD1) is the monomer that constitutes the polymer (Cd). The total amount of the above is preferably 50% by mass or more, and more preferably 80% by mass or more, based on 100% by mass of the total amount of the above. It may be 100% by mass.

[0036] The glass transition temperature (Tg) of the polymer (Cd) is set to 60°C or higher from the viewpoint of the mechanical properties of the film. Preferably, the temperature is 70°C or higher, more preferably 80°C or higher. From the viewpoint of gas permeability of the rubber, the temperature is preferably 150° C. or lower, and more preferably 130° C. or lower.

[0037] Preferred embodiments of the acrylic polymer (C) include the following embodiments 1, 2 and 3. [Aspect 1] The acrylic polymer (C) contains a polymer (Ca) and a polymer (Cb), Relative to the total mass of the polymer (C), The content of the polymer (Ca) is 5 to 60% by mass, preferably 10 to 60% by mass, more preferably Preferably, the content is 20 to 55 mass %. The content of the polymer (Cb) is 40 to 95% by mass, preferably 40 to 90% by mass, more preferably A preferred embodiment is 45 to 80% by mass. [Aspect 2] The acrylic polymer (C) is a polymer (Ca), a polymer (Cb), and a polymer ( Cc), based on the total mass of the acrylic polymer (C), The content of the polymer (Ca) is 5 to 59% by mass, preferably 10 to 55% by mass, and more preferably Preferably, the content is 20 to 55 mass %. The content of the polymer (Cb) is 40 to 94% by mass, preferably 40 to 90% by mass, more preferably Preferably, it is 45 to 80 mass %. The content of the polymer (Cc) is 1 to 35% by mass, preferably 3 to 30% by mass, and more preferably Or, in an embodiment, the content is 5 to 25 mass %. [Aspect 3] The acrylic polymer (C) contains a polymer (Cd), and the total amount of the acrylic polymer (C) is With respect to mass, The content of the polymer (Cd) is 60 to 100% by mass, preferably 65 to 99.5% by mass. More preferably, the content is 70 to 99% by mass.

[0038] [Method for producing acrylic polymer (C)] The acrylic polymer (C) can be produced, for example, by a sequential multi-stage emulsion polymerization method, an emulsion suspension polymerization method, or the like. polymerization method, suspension polymerization method, etc. The acrylic polymer (c-1) can be produced by a sequential multi-stage emulsion polymerization method, for example. The emulsion prepared by mixing the monomer components, water and surfactant to obtain the polymer (Ca) is reacted. After feeding the polymer to the reactor and polymerizing, the monomer components that are the raw materials for the polymer (Cc) are reacted as necessary. After the polymerization is carried out in the reactor, the monomer components that are the raw materials for the polymer (Cb) are fed to the reactor. A method of polymerizing the compound by polymerization is mentioned. The acrylic polymer (c-1) can be produced by emulsion suspension polymerization, for example. In the presence of polymer (Ca), monomer components which are raw materials for polymer (Cc) are successively added as necessary. After multi-stage emulsion polymerization, the suspension polymerization system is used during polymerization of the monomer components that are the raw materials for polymer (Cb). An example of such a method is an emulsion suspension polymerization method in which the copolymer is converted into the copolymer. The acrylic polymer (c-1) obtained by the above-mentioned sequential multistage emulsion polymerization method or emulsion suspension polymerization method is used. The film obtained by this method is preferred because it has the characteristic of having a small number of fish eyes in the film. It is nice. The acrylic polymer (c-2) can be produced, for example, by reacting the polymer (Cd) A known method for this purpose is suspension polymerization.

[0039] The average particle size of the acrylic polymer (C) is determined from the viewpoints of the mechanical properties and transparency of the resulting film. , 0.03 μm or more is preferable, 0.07 μm or more is more preferable, and 0.09 μm or more is It is particularly preferable that the thickness is 0.3 μm or less, more preferably 0.15 μm or less, and 0. .13 μm or less is particularly preferred. The average particle size is a cumulonimbus measured by a dynamic light scattering method using a light scattering photometer. These are measurements taken using optical fiber analysis.

[0040] The mass average molecular weight (Mw) of the acetone soluble portion of the acrylic polymer (C) is preferably 20,000 or more. It is preferable that the molecular weight is 150,000 or less, and more preferably 100,000 or less. If Mw is 20,000 or more, the impact resistance of the obtained film is improved, and cracks during molding are prevented. In addition, when the Mw is 150,000 or less, the resulting film has excellent formability.

[0041] The mass average molecular weight (Mw) is determined based on the acetone soluble content in the acrylic polymer (C). The measured values ​​were determined by gel permeation chromatography (GPC) using the following method. (1) 1 g of acrylic polymer is dissolved in 50 g of acetone and refluxed at 70°C for 6 hours to obtain acetone. Extract ton soluble matter. (2) The obtained extract was incubated at 4°C using a CRG SERIES (Hitachi, Ltd.). The mixture is centrifuged at 14,000 rpm for 30 minutes. (3) Remove the acetone insoluble matter by decantation, and simmer in a vacuum dryer at 50°C for 24 hours. The acetone solubles were then dried for 1 hour and the resulting solution was subjected to GPC measurement under the following conditions. The mass average molecular weight is determined from a calibration curve using styrene. Equipment: Tosoh Corporation "HLC8220" Column: Tosoh "TSKgel SuperMultiporeHZ-H" (Inner diameter 4.6 mm x length 15 cm x 2 pieces, exclusion limit 4 x 10 7 (Estimated) Eluent: Tetrahydrofuran Eluent flow rate: 0.35mL / min Measurement temperature: 40℃ Sample injection volume: 10 μL (sample concentration 0.1%)

[0042] The melt viscosity of the acrylic polymer (C) at 200°C is preferably 4,000 Pa·s or more. Preferably, the viscosity is 5,000 Pa·s or more, more preferably 6,000 Pa·s or more. In addition, the viscosity is preferably 30,000 Pa·s or less, and more preferably 27,000 Pa·s or less. It is preferable that the viscosity is 25,000 Pa·s or less. If the melt viscosity of the acrylic polymer (C) is equal to or higher than the lower limit above, minute recesses may appear on the film surface. When the content is equal to or less than the upper limit of the above range, the surface roughness is easily improved. Acrylic polymer (C), cellulose ester compound (A) and aliphatic polyester (B) Interfacial peeling is unlikely to occur, and the film has excellent impact resistance and formability. When the acrylic polymer (C) has a multilayer structure, the melt viscosity of the acrylic polymer (C) is This can be adjusted by the ratio of the core layer to the shell layer, the mass average molecular weight (Mw) of the shell layer, etc. For example, the ratio of the shell layer is decreased or the mass average molecular weight (Mw) of the shell layer is increased. This tends to increase the melt viscosity of the acrylic polymer (C).

[0043] In the resin composition (X), the melt viscosity of the acrylic polymer (C) is It is preferable that the melt viscosity is higher than that of the mixture of the compound (A) and the aliphatic polyester (B). The absolute value of the difference in melt viscosity at 200°C between the acrylic polymer (C) and the mixture ( Hereinafter, this is also referred to as the "melt viscosity difference".) is preferably 2000 Pa·s or more, and more preferably 3000 Pa·s or more. s or more is more preferable, and 4000 Pa s or more is even more preferable. a·s or less is preferable, 25,000 Pa·s or less is more preferable, and 20,000 Pa·s or less is more preferable. s or less is even more preferable. When the melt viscosity difference is equal to or greater than the lower limit, fine irregularities tend to appear on the film surface. On the other hand, when the melt viscosity difference is equal to or less than the upper limit, a fine matte finish is easily obtained. and an acrylic polymer (C), a cellulose ester compound (A) and an aliphatic polyester. Interfacial peeling with (B) is unlikely to occur, and the film has excellent impact resistance and formability.

[0044] The melt viscosity of the resin composition (X) at 200°C is preferably 100 to 9000 Pa·s. The viscosity is preferably from 300 to 7000 Pa·s, more preferably from 500 to 6000 Pa·s. When the melt viscosity of the resin composition (X) is equal to or higher than the above lower limit, the resin composition (X) is excellent in moldability, and when the melt viscosity of the resin composition (X) is equal to or higher than the above upper limit, the resin composition (X) is excellent in moldability. If it is less than this, the mechanical properties of the film will be excellent.

[0045] <Optional ingredients> The resin composition (X) may contain various additives as required. Examples of such additives include antioxidants, heat stabilizers, light stabilizers, plasticizers, lubricants, antistatic agents, flame retardants, Fillers, matting agents, processing aids, impact resistance aids, antibacterial agents, antifungal agents, foaming agents, release agents, colorants , ultraviolet absorbers, and thermoplastic polymers. The resin composition (X) is also recyclable. Polysaccharides such as starch may be blended as a material derived from organic resources.

[0046] As the antioxidant, phenol-based, sulfur-based, phosphorus-based, etc. antioxidants can be used. Heat stabilizers include hindered phenol-based, sulfur-based, and hydrazine-based heat stabilizers. The plasticizers that can be used include phthalate esters, phosphate esters, and fats. Acid ester type, aliphatic dibasic acid ester type, oxybenzoic acid ester type, epoxy type, poly As lubricants, fatty acid esters, fatty Use lubricants such as acid-based, metal soap-based, fatty acid amide-based, higher alcohol-based, and paraffin-based. It is possible.

[0047] The antistatic agent may be a cationic, anionic, nonionic, or amphoteric antistatic agent. Flame retardants can be used. Bromine-based, phosphorus-based, chlorine-based, nitrogen-based, aluminum-based, etc. Uses flame retardants such as nium, antimony, magnesium, boron, and zirconium. Fillers include calcium carbonate, barium sulfate, talc, rosewood, and kaolin. etc. can be used.

[0048] As the ultraviolet absorbing agent, a benzotriazole type, a triazine type, or the like is used. As the light stabilizer, a hindered amine-based light stabilizer or the like can be used. The blocking agent is a compound capable of blocking the carboxyl end group of the polymer. There are no particular limitations on the type of compound, and examples include epoxy compounds, oxazoline compounds, oxazine compounds, and carbamide compounds. These compounds are used as blocking agents for the carboxyl ends of polymers, such as carboxyimide compounds. The compatibilizer may be a polymer type compatibilizer, a low molecular weight organic compound, or an inorganic Compounds, organic-inorganic composites, etc. can be used. These compounding agents may be used alone. Two or more of them may be used in combination.

[0049] <Content> The content of the cellulose ester compound (A) relative to the total mass of the resin composition (X) is 1 It is preferably 0% by mass or more, more preferably 20% by mass or more, and particularly preferably 30% by mass or more. In addition, the content is preferably 80% by mass or less, more preferably 70% by mass or less, and more preferably 65% ​​by mass or less. When the content of the cellulose ester compound (A) is within the above range, The resulting film tends to have good impact resistance and transparency.

[0050] The content of the aliphatic polyester (B) is 10% by mass based on the total mass of the resin composition (X). It is preferably 15% by mass or more, more preferably 15% by mass or more, and particularly preferably 20% by mass or more. 50% by mass or less is preferable, 45% by mass or less is more preferable, and 40% by mass or less is particularly preferable. When the content of the aliphatic polyester (B) is within the above range, good mechanical properties are obtained. And transparency is easily achieved.

[0051] The content of the acrylic polymer (C) is 5% by mass or more based on the total mass of the resin composition (X). It is preferably 10% by mass or more, more preferably 15% by mass or more. % by mass or less is preferable, 40% by mass or less is more preferable, and 35% by mass or less is particularly preferable. When the content of the acrylic polymer (C) is within the above range, the resulting film has Good mechanical properties are easily obtained. In addition, good matte properties are easily obtained.

[0052] The ratio of the cellulose ester compound (A) and the aliphatic polyester compound (B) to the total mass of the resin composition (X) is The total content of the ster (B) is preferably 50% by mass or more, more preferably 60% by mass or more. It is preferably 90% by mass or less, and more preferably 85% by mass or less. It is more preferable that the content is 80 mass % or less, and particularly preferable that the content is 80 mass % or less.

[0053] The ratio of the cellulose ester compound (A) and the aliphatic polyester compound (B) to the total mass of the resin composition (X) is The total content of the styrene (B) and the acrylic polymer (C) is preferably 80% by mass or more, and more preferably 90% by mass or more. It is more preferable that the content is at least 10% by mass. It may be 100% by mass.

[0054] In the resin composition (X), the content of the cellulose ester compound (A) is 100 parts by mass. In this case, the content of the aliphatic polyester (B) is preferably 20 parts by mass or more, and more preferably 30 parts by mass or more. parts by mass or more is more preferable, 40 parts by mass or more is even more preferable, and 45 parts by mass or more is even more preferable. It is preferably 50 parts by mass or more, particularly preferably 150 parts by mass or less, and more preferably 100 The amount of the aliphatic polyester ( When the content of B) is equal to or more than the lower limit, the transparency is good, and when it is equal to or less than the upper limit, the filter is not easily formed. This improves the moldability of the molded product.

[0055] In the resin composition (X), the content of the cellulose ester compound (A) is 100 parts by mass. In this case, the content of the acrylic polymer (C) is preferably 10 parts by mass or more, and more preferably 20 parts by mass or more. More preferably, the amount is 25 parts by mass or more, particularly preferably 25 parts by mass or more. Also, the amount is preferably 150 parts by mass or less. The amount of the acrylic polymer is more preferably 130 parts by mass or less, and particularly preferably 100 parts by mass or less. When the content of the polymer (C) is equal to or greater than the above lower limit, good transparency and matte finish are easily obtained. When the content is equal to or less than the upper limit, good impact resistance is likely to be obtained.

[0056] <Film manufacturing method> The film of the present embodiment is a polymer film made of a cellulose ester compound (A), an aliphatic polyester (B (C) and an acrylic polymer (C) are molded into a film (film formation) An example of a method for producing a film is shown below. For example, the resin composition (X) is melt extruded by a melt casting method, a T-die method, an inflation method, or the like. The film can be formed by known methods such as the casting method, the calendering method, etc. The T-die method is preferred because of its good operability. The stretching method is uniaxial stretching (machine direction or transverse direction (direction perpendicular to the machine direction)), biaxial stretching (sequential stretching) A stretching step such as secondary biaxial stretching or simultaneous biaxial stretching may be provided. In addition, various structures can be formed on the film surface by known methods such as thermal transfer and etching. This is also fine.

[0057] <Film> The film of this embodiment is made of a resin composition (X). When the resin composition (X) is molded into a film, the components may be modified. Except for the component modification, the composition of the resin composition (X) is the same as the composition of the film.

[0058] The film of the present embodiment preferably has a sea-island structure consisting of a continuous phase and a dispersed phase. The continuous phase (sea portion) in the sea-island structure is composed of a cellulose ester compound (A) and an aliphatic polyester compound (B). It is preferred that the dispersion phase (islands) contains an acrylic polymer (C).

[0059] The thickness of the film of this embodiment is preferably 10 μm or more, more preferably 30 μm or more. The thickness is preferably 50 μm or more, and more preferably 500 μm or less, and more preferably 300 μm or less. It is more preferable that the thickness is 200 μm or less, and further more preferable that the thickness is 200 μm or less. Suitable rigidity can be obtained, and the exterior design can be more satisfactorily imparted.

[0060] The arithmetic mean roughness Ra of the surface of the film of this embodiment is preferably 0.10 μm or more, and more preferably 0 More preferably, the thickness is 20 μm or more. Also, the thickness is preferably 3.00 μm or less, and more preferably 2.00 μm or less. more preferably 1.00 μm or less, even more preferably 0.50 μm or less. I wish. If Ra is equal to or greater than the lower limit, the glare is low, and the design and decorative properties such as a sense of luxury and depth are excellent. When Ra is equal to or less than the upper limit, the surface appearance is excellent. a is a value measured by a method conforming to JIS B0601:2001.

[0061] The maximum height Rz of the surface of the film of this embodiment is preferably 0.5 μm or more, and more preferably 1.0 μm or more. It is more preferably 1.5 μm or more, and further preferably 15.0 μm or more. The thickness is preferably 10.0 μm or less, more preferably 5.0 μm or less. If Rz is equal to or greater than the lower limit, the glare is low, and the design and decorativeness such as a sense of luxury and depth are poor. When Rz is equal to or less than the above upper limit, the external design is excellent. The maximum height Rz is a value measured using a method conforming to JIS B0601:2001. be.

[0062] In particular, the film of the present embodiment satisfies both the Ra and Rz at the same time, thereby achieving high The film has excellent design and decorative properties, such as a sense of class and depth.

[0063] The total light transmittance of the film of this embodiment is preferably 80% or more, more preferably 83% or more. It is preferable that the content is 100% or less, and more preferably 99% or less. It is preferable that the content is 98% or less, and more preferable that the content is 98% or less. When the total light transmittance is within the above range, the transparency is good. The total light transmittance was measured according to a method conforming to JIS K7361-1:1997. value.

[0064] The total haze of the film of this embodiment is preferably 90% or less, more preferably 85% or less. More preferably, the ratio is 80% or less. Also, the ratio is preferably 10% or more, and more preferably 20% or more. When the total haze is within the above range, the matte finish and transparency are excellent. will be good. The total haze is a value measured by a method conforming to JIS K7136:2000.

[0065] The design quality of a film, such as its luxurious feel and depth, is determined by its surface gloss and haze. . Generally, it is preferable that the surface gloss is low. Specifically, the 20° surface gloss of the film is is preferably 0.1% or more, more preferably 0.3% or more, and even more preferably 0.5% or more. In addition, it is preferably 70% or less, more preferably 50% or less, and even more preferably 30% or less. The 60° surface gloss of the film is preferably 5% or more, and more preferably 6% or more. More preferably, the ratio is 7% or more. Also, the ratio is preferably 70% or less, and more preferably 50% or less. The 85° surface gloss of the film is preferably 5% or more, and more preferably 30% or less. More preferably, the ratio is 6% or more, and even more preferably, 7% or more. Also, the ratio is preferably 90% or less, and even more preferably, 80% or less. 0% or less is more preferable, 70% or less is even more preferable, and 60% or less is even more preferable. stomach. In particular, when the surface gloss at 20°, 60°, and 85° is within the above range, glare is reduced. The film has excellent design and decorative properties, such as a luxurious feel and a sense of depth. The 20°, 60°, and 85° surface gloss values ​​are determined according to JIS Z8741:1997 The values ​​were measured using a method conforming to the above.

[0066] The film of the present embodiment preferably has a tensile modulus of elasticity of 100 MPa or more. The elastic modulus is more preferably 300 MPa or more, and particularly preferably 400 MPa or more. If it is equal to or higher than the limit value, the film has excellent formability. Also, from the viewpoint of impact resistance, 3000MP a or less is preferable, 1500 MPa or less is more preferable, and 1300 MPa or less is particularly preferable. It is nice.

[0067] The film of the present embodiment preferably has a tensile breaking elongation of 80% or more. The elongation is more preferably 100% or more, and particularly preferably 120% or more. If it is equal to or more than the limit value, the impact resistance is excellent. From the viewpoint of moldability, it is preferably 600% or less. It is preferable that the ratio is 500% or less. The tensile test for measuring the tensile modulus and tensile elongation at break was performed according to JIS K712 7:1999, initial chuck distance 100 mm, tensile speed 50 mm / s The test was performed under conditions of 2 min and 23°C.

[0068] The film of this embodiment preferably has a puncture impact of 1.0 J or more at 23° C. 1.3 J or more is more preferable, and 1.5 J or more is even more preferable. Also, 10.0 J or less is preferable, 8.0 J or less is more preferable, and 5.0 J or less is even more preferable. In addition, the puncture impact at -20°C is preferably 0.1 J or more, and 0.3 J or more is preferable. More preferably, it is 0.5 J or more, and even more preferably, it is 10.0 J or less, and 8. 0 J or less is more preferable, and 5.0 J or less is even more preferable. If the puncture impact at 23°C is equal to or higher than the lower limit, the formability of the film is good. If the puncture impact at 23°C is equal to or less than the upper limit, good mechanical properties are obtained. It is easy to get. If the puncture impact at -20°C is equal to or greater than the lower limit above, the film has good formability. If the puncture impact at -20°C is equal to or less than the upper limit, good mechanical properties are obtained. Easy to obtain. The puncture impact was measured according to the method compliant with JIS K7124-2:1999. This is the value.

[0069] According to this embodiment, the impact resistance of the film can be improved. The reason is clear. However, the following reasons may be considered: In the film of this embodiment, the aliphatic polyester (B) and the acrylic polymer (C) By adding a cellulose ester compound (A), aliphatic polyester (B ) crystallization can be suppressed, improving the flexibility of the film and improving impact resistance. It is thought that this is the case. In the film of this embodiment, the (meth)acrylic acid in the polymer (Cb) or (Cd) The structural unit derived from the ester (MB1) or (MD1) is a cellulose ester compound (A). and contributes to compatibility between the mixture of the aliphatic polyester (B) and the acrylic polymer (C), It is believed that these interfaces become less susceptible to peeling. A preferred embodiment of the film of this embodiment has a sea-island structure, and the dispersed phase is an acrylic polymer ( C), the continuous phase being a mixture of a cellulose ester compound (A) and an aliphatic polyester (B). In this embodiment, the (meth)acrylic acid ester (MB) in the polymer (Cb) is 1) The structural unit derived from the polymer contributes to the compatibility between the continuous phase and the dispersed phase, and the interface between the continuous phase and the dispersed phase is It is believed that peeling becomes difficult.

[0070] The film of the present embodiment has good transparency. The reason for this is not clear. For example, the following reasons may be considered: Cellulose esterification for aliphatic polyester (B) and acrylic polymer (C) By adding the compound (A), the crystallization of the aliphatic polyester (B) can be suppressed. It is believed that the transparency is improved because the total light transmittance can be increased.

[0071] The film of this embodiment has a good matte appearance. The reason for this is unclear. However, the following reasons may be considered: In the process of forming the resin composition (X) into a film, the resin composition (X) is When subjected to internal shear force, the acrylic polymer (C) in the resin composition (X) is stretched. Then, the resin composition (X) is discharged from a die or the like. In some cases, when the acrylic polymer (C) has a suitable fluidity, it is difficult to release elastic energy. This causes the acrylic polymer (C) to return to its original shape. If the elastic modulus of the polymer (C) is higher than that of the surrounding area, the difference in elastic modulus will cause the film to It is believed that the surface shrinks and fine irregularities appear. In particular, cellulose ester compounds ( The higher the content of the aliphatic polyester (B) relative to A), the greater the amount of the acrylic polymer (C) around the The fluidity of the surrounding area increases, and the difference in fluidity between the acrylic polymer (C) and its surrounding area becomes larger. As a result, the film surface becomes rougher and a higher degree of matte finish is achieved. do. In this respect, the film of the present embodiment is advantageous in that minute irregularities are easily generated due to the difference in elastic modulus. has an island-in-a-sea structure, the dispersed phase contains an acrylic polymer (C), and the continuous phase contains a cellulose ester It is preferable that the composition contains a compound (A) and an aliphatic polyester (B). The fluidity when molding into a film is determined by the melt viscosity at around the molding temperature. The lower the melt viscosity, the higher the fluidity.

[0072] <Application> The film of the present embodiment has good transparency, flexibility and impact resistance, and can be used to coat the surfaces of various articles. It is suitable as a film to be laminated on top of the substrate. For example, interior and exterior materials for buildings, interior and exterior materials for automobiles, various items (mobile phones, It can be used as a decorative film or surface protection film for electronic products, etc. In particular, the film has excellent transparency and low surface gloss, and is called a matte film. The use of a matte film as the outermost layer of an article gives it a luxurious feel. It can impart a sense of depth, calmness, etc. The film of the present embodiment is suitable as a film constituting the outermost layer of an article. EXAMPLES

[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, the unit of content is "parts" unless otherwise specified. The units represent "parts by mass."

[0074] [Evaluation method / measurement method] <Total light transmittance, total haze> Total light transmittance is based on JIS K7361-1:1997, and total haze is based on JIS K7136 :2000, using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd.), light source D65, The total light transmittance of the film was measured at a temperature of 25°C.

[0075] <Surface gloss> Compliant with JIS Z8741:1997, using a portable gloss meter (Konica Minolta, Inc.) The surface gloss of the film was measured using a meter (product name: GM-268Plus). Measurement angle The angles of incidence were 20°, 60°, and 85°.

[0076] <Arithmetic mean roughness Ra> Using a surface roughness measuring instrument (Tokyo Seimitsu Co., Ltd., product name: SURFCOM 1400D), Based on JIS B0601:2001, measurement length 4.0mm, evaluation length 4.0mm, The arithmetic mean roughness R of the film was measured under the conditions of a cut-off wavelength of 0.8 mm and a measurement speed of 0.3 mm / s. a was measured.

[0077] <Maximum height Rz> Using a surface roughness measuring instrument (Tokyo Seimitsu Co., Ltd., product name: SURFCOM 1400D), Based on JIS B0601:2001, measurement length 4.0mm, evaluation length 4.0mm, The maximum height Rz of the film was measured under the conditions of a drop-off wavelength of 0.8 mm and a measurement speed of 0.3 mm / s. Measured.

[0078] <Tensile elongation at break, tensile modulus> Shimadzu Corporation Model: AGS-X Precision Universal Testing Machine (Autograph) was used. The tensile elongation at break and the tensile modulus of elasticity were measured in accordance with K7127:1999. μm film is cut to 150 mm in the machine direction (MD) and 15 mm in the cross direction (TD). The specimen was cut into pieces. The initial chuck distance was 100 mm, and the tensile speed was 50 mm / min. The tensile elongation at break and the tensile modulus of the film (MD) were measured at an ambient temperature of 23°C. The average of the measurements was recorded.

[0079] <Puncture impact test> Compliant with JIS K7124-2:1999, high-speed puncture impact test machine Hydros The temperature was measured at 23℃ and -20℃ using a shot HITS-P10 (Shimadzu Corporation). The energy to fracture was measured under the conditions of a punch diameter of 0.5 inches and a test speed of 3 m / sec. The resistance (unit: J) was measured and the average value of five measurements was recorded.

[0080] <Melt viscosity> Based on JIS K7244:2007, a rheometer (Thermo Fisher Scientific A 0.5% strain, 1Hz frequency, and 240°C temperature were measured using a 300-mV meter (MARS, manufactured by Flexo Corporation). Temperature dispersion measurement was performed at a temperature drop rate of 3.0℃ / min from ℃, and the melt viscosity at 200℃ was measured. did.

[0081] <Raw materials> The abbreviations in Table 1 represent the following raw materials. MMA: Methyl methacrylate n-BA: n-butyl acrylate AMA: Allyl methacrylate 1,3-BD: 1,3-butylene glycol dimethacrylate MA: Methyl acrylate RS610NA: Sodium mono-n-dodecyloxytetraoxyethylene phosphate (phosphate Osphanol RS-610NA: manufactured by Toho Chemical Industry Co., Ltd. OTP: Sodium di-2-ethylhexyl sulfosuccinate (Perex OT-P: Flower (Manufactured by Wang Co., Ltd.) CHP: Cumene hydroperoxide t-BH: t-butyl hydroperoxide n-OM: n-octyl mercaptan

[0082] The abbreviations in Table 2 represent the following raw materials. Cellulose ester (A1): Cellulose acetate propionate (CAP), glass Transition temperature: 158℃ Aliphatic polyester (B1): Polybutylene succinate (PBS) Acrylic polymer (C1): Acrylic rubber synthesized in Production Example 1 below Acrylic polymer (C2): Acrylic rubber synthesized in Production Example 2 below Acrylic polymer (C3): Acrylic rubber synthesized in Production Example 3 below Acrylic polymer (C4): Acrylic polymer synthesized in Production Example 4 below

[0083] (Production Example 1: Production of Acrylic Polymer (C1)) The composition of the raw materials (unit: parts by mass) is shown in Table 1. 8.5 parts of ion-exchanged water was placed in a vessel equipped with a stirrer and a cooler, and then (meth)acrylic acid was added. As the ester (MA1-1), 0.3 parts of MMA and 4.5 parts of n-BA, 2-1) 0.2 parts of 1,3-BD and 0.05 parts of AMA as well as CHP as an initiator 0.025 parts of the monomer component (Ca1-1) was added and mixed with stirring. Add 1.1 parts of RS610NA as a mixing agent to the above container while stirring, and continue stirring for 20 minutes. An emulsion containing the monomer component (Ca1-1) was prepared. Next, 186.5 parts of ion-exchanged water was added to a reaction vessel equipped with a cooler and the temperature was raised to 70°C. Heat it, add 5 parts of ion-exchanged water and SFS (sodium formaldehyde sulfoxylate) 0.20 parts, ferrous sulfate 0.0001 parts, EDTA (disodium ethylenediaminetetraacetate The mixture was then added in one portion without stirring under nitrogen. Then, the emulsion containing the monomer component (Ca1-1) was dropped into the reaction vessel over a period of 8 minutes. The reaction was continued for 15 minutes to obtain a polymer consisting of the monomer component (Ca1-1). Next, MMA1. 5 parts and n-BA22.5 parts, 1,3-BD1.0 part as monomer (MA2-2) and A A monomer component (Ca1-) consisting of 0.25 parts of MA and 0.016 parts of CHP as an initiator After adding 2) over 90 minutes, the reaction was continued for 60 minutes to obtain a polymer (Ca1). The Tg of the polymer (Ca1) was -47°C. Next, 6.0 parts of MMA and nB A4.0 parts, AMA0.075 parts as monomer (MC2-1), and CH A monomer component (Cc1-1) consisting of 0.013 parts of P was added dropwise to the reaction vessel over a period of 45 minutes. The reaction was continued for 60 minutes to form an intermediate polymer. The Tg of the polymer (Cc1) composed of 1) was 20°C. Next, 55.2 parts of MMA and n- BA 4.8 parts, n-OM 0.22 parts as chain transfer agent, and t-BH 0.01 parts as initiator. 0.75 parts of monomer component (Cb1-1) was added dropwise to the reaction vessel over a period of 140 minutes. The reaction was continued for 60 minutes to obtain a latex of acrylic polymer (C1). The Tg of the polymer (Cb1) composed of the monomer component (Cb1-1) was 84°C. The obtained latex of the acrylic polymer (C1) was filtered through a SUS mesh (average mesh size) After filtering using a vibrating filter equipped with a 62 μm aperture, the mixture was diluted with 3 parts calcium acetate. The resulting product was salted out in an aqueous solution containing 1,000 ppm of acrylic acid, washed with water, recovered, and then dried to obtain a powdery acrylic polymer (C1). The average particle size of the acrylic polymer (C1) is 0.12 μm, Mw is 59,000, and the temperature is 200° C. The melt viscosity at 1000 Pa·s was 16,000 Pa·s.

[0084] (Production Example 2: Production of Acrylic Polymer (C2)) The composition of the raw materials (unit: parts by mass) is shown in Table 1. 195 parts of ion-exchanged water was charged into a vessel equipped with a stirrer and a cooler, and the same procedure as in Production Example 1 was repeated. An emulsion containing the monomer component (Ca2-1) shown in Table 1 was prepared by the method described above. Next, the temperature of the emulsion was raised to 75° C., and 0.20 parts of SFS and 0.20 parts of sulfur were added to 5 parts of ion-exchanged water. A mixture of 0.0001 parts of ferrous acid and 0.0003 parts of EDTA was added all at once. After confirming the temperature rise peak, the reaction was continued for 15 minutes to separate the monomer component (Ca2-1 ) polymer was obtained. Next, the monomer component (Ca2-2) shown in Table 1 was added to the container, and the mixture was mixed to obtain the same mixture as in Production Example 1. Polymer (Ca2) was obtained in the same manner. The Tg of polymer (Ca2) was -10°C. Next, the monomer component (Cc2-1) shown in Table 1 was dropped into the reaction vessel, and the same procedure as in Production Example 1 was repeated. An intermediate polymer was formed by the above method. Here, the intermediate polymer composed of the monomer component (Cc2-1) was The Tg of the composite (Cc2) was 60°C. Next, the monomer component (Cb2-1) shown in Table 1 was added dropwise to the reaction vessel, and the mixture was mixed to obtain Production Example 1. In the same manner, a latex of an acrylic polymer (C2) was obtained. The Tg of the polymer (Cb2) composed of -1) was 99°C. The obtained latex of the acrylic polymer (C2) was filtered through a SUS mesh (average mesh size) After filtering using a vibrating filter equipped with a filter (62 μm opening), 3.5 parts of calcium acetate were added. The resulting mixture was salted out in an aqueous solution containing 1,000,000,000, and then washed and collected, followed by drying to obtain a powdered acrylic polymer (C2). Ta. The average particle size of the acrylic polymer (C2) is 0.11 μm, Mw is 58,000, and the temperature is 200°C. The melt viscosity at 20,500 Pa·s was found to be

[0085] (Production Example 3: Production of Acrylic Polymer (C3)) The composition of the raw materials (unit: parts by mass) is shown in Table 1. 244 parts of ion-exchanged water was charged into a vessel equipped with a stirrer and a cooler, and the same procedure as in Production Example 1 was repeated. An emulsion containing the monomer component (Ca3-1) shown in Table 1 was prepared by the method described above. Next, 244 parts of ion-exchanged water was added to a reaction vessel equipped with a cooler, and the temperature was raised to 80°C. In addition, 5 parts of ion-exchanged water, 0.60 parts of SFS, 0.00012 parts of ferrous sulfate, EDTA The mixed aqueous solution prepared by adding 0.0003 parts of ethyl acetate was then added. Then, 1 / 15 (by mass) of the emulsion containing the monomer component (Ca3-1) was added, and the mixture was stirred for 15 minutes. The remaining emulsion was then added at an increase rate of 8% by mass per hour to the water. After the dropwise addition, the reaction was continued for 60 minutes to obtain a polymer consisting of the monomer component (Ca3-1). Ta. 0.6 parts of SFS was added to the latex of this polymer and the mixture was kept for 15 minutes. Then, the mixture was cooled in a nitrogen atmosphere. At 80°C under atmospheric pressure, 3.0 parts of MMA, 47 parts of n-BA, 0.8 parts of AMA, and C A monomer component (Ca3-2) consisting of 0.05 parts of HP was added to water at an increase rate of 4% by mass / hour. After the dropwise addition so that the temperature was kept constant, the reaction was continued for 120 minutes to obtain a polymer (Ca3). The Tg of the body (Ca3) was -47°C. 0.4 parts of SFS was added to the latex of this polymer and the mixture was kept for 15 minutes. Then, the mixture was cooled in a nitrogen atmosphere. At 80°C under atmospheric pressure, 40.5 parts of MMA, 4.5 parts of n-BA, 0.3 parts of n-OM, The monomer component (Cb3-1) consisting of 0.02 parts and t-BH0.063 parts was added to water at an increased After dripping so that the rate was 10 mass% / hour, the reaction was continued for 60 minutes to polymerize the acrylic. A latex of the polymer (C3) was obtained. Here, the polymer was composed of the monomer component (Cb3-1). The Tg of the form (Cb3) was 79°C. The obtained latex of the acrylic polymer (C3) was filtered through a SUS mesh (average mesh size) After filtering using a vibrating filter equipped with a filter (150 μm opening), 3.5 g of calcium acetate was added. The resulting mixture is salted out in an aqueous solution containing acrylic acid, washed with water, and then dried to obtain a powdered acrylic polymer (C3). The acrylic polymer (C3) had a Mw of 45,000 and a melt viscosity of 10 at 200°C. ,900 Pa·s.

[0086] (Production Example 4: Production of Acrylic Polymer (C4)) An acrylic polymer (C) consisting of 87 parts of methyl methacrylate and 13 parts of methyl acrylate 4) was produced by known suspension polymerization. The Mw of the acrylic polymer (C4) was 100,000. The melt viscosity at 200°C was 5,890 Pa·s.

[0087] [Table 1]

[0088] <Examples 1 to 8 and Comparative Examples 1 to 6> The cellulose ester compound (A) was mixed to obtain the composition shown in Tables 2 and 3 (unit: mass %). Then, the aliphatic polyester (B) and the acrylic polymer (C) were dry blended. The resin composition (X) was kneaded at 220°C using a 25 mm diameter co-rotating twin screw extruder, and then passed through a T-die. The mixture was then extruded by a casting roll at about 80°C and quenched to a thickness of 100 μm. A film was produced. The evaluation results of various properties of the obtained film are shown in Tables 2 and 3.

[0089] [Table 2]

[0090] [Table 3]

[0091] The films of Examples 1 to 8 have a sea-island structure, and the acrylic polymer (C) is the dispersed phase (the islands of the sea). A mixture of the cellulose ester compound (A) and the aliphatic polyester compound (B) is formed. It is thought to form a continuous phase (sea part of the sea island). As shown in the results in Tables 2 and 3, the films of Examples 1 to 8 had a tensile modulus of 1,300 MPa or less, and the tensile elongation at break is 80% or more, and the impact resistance is excellent. It has high total light transmittance and excellent transparency.

[0092] Comparative Example 1, which did not contain the acrylic polymer (C), had a high tensile modulus and poor impact resistance. Comparative Example 2, which did not contain the acrylic polymer (C), had low tensile elongation at break and poor impact resistance. In addition, the transparency is insufficient and the transparency is poor. Comparative Example 3, which was a film made of the acrylic polymer (C) alone, had low impact resistance. In Comparative Example 4, which does not contain the cellulose ester compound (A), the impact resistance was also low. In addition, the internal haze of the film was high and transparency was poor. It is believed that (B) has crystallized. Comparative Example 5, which does not contain the aliphatic polyester (B), has a low tensile elongation at break and poor impact resistance. I did.

[0093] A cellulose ester compound (A), an aliphatic polyester (B), and an acrylic polymer ( C), and the tensile modulus and tensile elongation at break are within appropriate ranges, providing good impact resistance. It can be seen that it has

Claims

1. A cellulose ester compound (A), an aliphatic polyester (B), and an acrylic polymer ( C), a film made of a resin composition containing the film, and having a tensile modulus in the MD direction of 1300 MPa or less, and the tensile breaking elongation in the MD direction is 80% or more.

2. The content of the cellulose ester compound (A) relative to the total mass of the resin composition is 1 The film according to claim 1 , wherein the content is 0% by weight or more and 60% by weight or less.

3. The content of the aliphatic polyester (B) relative to the total mass of the resin composition is 10 mass %.

2. The film according to claim 1, wherein the content of the polyimide is from 0.1 to 50% by weight.

4. The content of the acrylic polymer (C) is 10% by mass or more based on the total mass of the resin composition. The film according to claim 1 , wherein the content is 50% by weight or less.

5. The aliphatic polyester (B) comprises a structural unit derived from an aliphatic polycarboxylic acid and an aliphatic polycarboxylic acid. The film according to claim 1 , which is a polymer having structural units derived from an alcohol.

6. The film according to claim 1 , having a total light transmittance of 90% or more.

7. 2. The method according to claim 1, wherein the puncture impact at 23° C. is 1.5 J or more. of film.

Citation Information

Patent Citations

  • Cellulose ester film, hard coat film and antireflection film

    JP2005054100A